Glass powder for sealing titanium alloy, preparation method and application

By preparing and applying glass powder for titanium alloy sealing, combined with pre-oxidation and high-temperature sealing technology, the problems of insulation, air tightness and low production efficiency in the titanium alloy sealing process are solved, and high-performance titanium alloy glass is realized Sealing device.

CN118754447APending Publication Date: 2024-10-11LIAONING GLASS CERAMIC TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410921374.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-10
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

During the sealing process of titanium alloy, there are problems such as unqualified insulation resistance, poor air tightness, easy oxidation of titanium alloy at high temperature, poor wettability of glass and titanium alloy, and high sealing temperature, which leads to phase change and dimensional change of titanium alloy. The existing market is mature for sealing production. Glass sealing is difficult and production efficiency is low.

Method used

Provided is a glass powder for titanium alloy sealing, including silica, aluminum oxide, boron trioxide, alkali metal oxides, alkaline earth metal oxides and transition metal oxides, which are heated and melted through a lifting furnace, quenched with water, It is prepared through ball milling, granulation and other steps, combined with pre-oxidation and high-temperature sealing technology, to control the sealing temperature below the phase transition temperature of titanium alloy, and use the borosilicate glass system to reduce the surface tension of the glass and improve the wettability and sealing properties.

Benefits of technology

It achieves high electrical insulation, air tightness and sealing strength of titanium alloy glass sealing devices, reduces production difficulty and cost, improves production efficiency, and avoids dimensional changes caused by titanium alloy phase transformation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118754447A_ABST
    Figure CN118754447A_ABST
Patent Text Reader

Abstract

The invention discloses glass powder for titanium alloy sealing and a preparation method and application thereof.The glass powder for titanium alloy sealing is prepared from, by mass, 55%-62% of silicon dioxide, 15%-20% of aluminum oxide, 12%-18% of diboron trioxide, 5%-8% of alkali metal oxide and the balance glass powder. The mass fraction of the alkaline earth metal oxide is 2-8%, the mass fraction of the titanium dioxide is 0.5-2%, and the mass fraction of the transition metal oxide is 3-5%. The preparation method comprises the steps of material preparation, homogenization, heating, melting, water quenching, drying, ball milling, granulation and the like. The glass powder for sealing the titanium alloy is compact in space structure, high in chemical stability, low in surface tension and good in wettability with the titanium alloy, and the air tightness of a sealed product can be improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of electronic sealing glass, and in particular provides a glass powder for titanium alloy sealing, a preparation method and application thereof. Background Art

[0002] Glass sealing devices, including aviation plugs, sensors, electrode plugs and other types of products, have a basic structure composed of a metal shell, a glass insulator, and an internal core column. The glass insulator is used as a solder to achieve a sealed connection between the metal shell and the internal core column. It has basic properties such as insulation and sealing, and completes the transmission of electrical signals. It is widely used in aerospace, underwater detection, oil drilling, chemical industry and other fields.

[0003] Conventional glass-sealed devices have metal shells made of stainless steel, Kovar, etc. depending on their service environment. At present, the domestic and foreign markets for sealing glass for metal shells and Kovar are mature, the sealing glass powder used is of many types, has stable performance, and has low production costs. Metal sealing with stainless steel and Kovar has developed maturely.

[0004] As my country's defense, aerospace and other fields have increased their demand for lightweight and precision equipment, titanium alloy sealing devices have become an important choice to replace stainless steel sealing devices. Titanium alloy has the characteristics of light weight, low density, high specific strength, low thermal conductivity, impact resistance and corrosion resistance. It is known as the "metal of the 21st century" and is expected to replace stainless steel and Kovar alloy glass sealing devices and become a new generation of high-performance glass sealing products.

[0005] However, there are many problems in the titanium alloy sealing process, such as: the insulation resistance between the metal shell and the internal core column is unqualified, the device is poorly airtight, the titanium alloy is easily oxidized at high temperature, the wettability of glass and titanium alloy is poor, the high glass sealing temperature causes the titanium alloy to undergo phase change and dimensional changes, the existing market is mature, the production of sealed glass is difficult, and the production efficiency is low.

[0006] Therefore, proposing a glass powder for titanium alloy sealing, a preparation method and an application thereof have become issues to be solved urgently. Summary of the invention

[0007] In view of this, the object of the present invention is to provide a glass powder for titanium alloy sealing, a preparation method and an application thereof, so as to solve the problems existing in the prior art.

[0008] On the one hand, the present invention provides a glass powder for titanium alloy sealing, which includes the following raw materials, by mass percentage: 55-62% by mass of silicon dioxide, 15%-20% by mass of aluminum oxide, 12%-18% by mass of boron trioxide, 5%-8% by mass of alkali metal oxide, 2%-8% by mass of alkaline earth metal oxide, 0.5%-2% by mass of titanium dioxide, and 3%-5% by mass of transition metal oxide.

[0009] Preferably, the alkali metal oxide includes at least one of K2O and Na2O, and the mass fraction of K2O is greater than the mass fraction of Na2O.

[0010] More preferably, the alkaline earth metal oxide includes at least one of CaO and MgO.

[0011] Further preferably, the transition oxide includes at least one of WO3, V2O3, and Cr2O3.

[0012] The present invention also provides a method for preparing the titanium alloy sealing glass powder, comprising the following steps:

[0013] a) preparing raw materials according to mass percentage;

[0014] b) using a lifting furnace to uniformly mix, heat, and melt the raw materials, and then quench with water to obtain glass cullets, and then dry them to obtain dried glass cullets;

[0015] c) ball milling the dried glass shreds with a planetary ball mill to obtain titanium alloy sealing glass raw powder, and then granulating the titanium alloy sealing glass raw powder to obtain the titanium alloy sealing glass powder.

[0016] Preferably, in step b), the raw materials are placed in an alumina crucible with a height not exceeding one-half of the height of the crucible, and are mixed evenly using a glass rod. Thereafter, the alumina crucible is placed in a lifting furnace, heated to 850°C at a rate of 10°C / min at room temperature, kept warm for 4 hours, and then heated to 1400-1500°C at a rate of 3-5°C / min, and kept warm for 2-4 hours.

[0017] Further preferably, in step c), the dried glass chips are evenly placed in a ball mill filled with zirconia balls for 1-2 hours, and then 3%-6% of a binder is added to the glass raw powder obtained after ball milling. After granulation and sieving, 40-120 mesh granulated powder is obtained, i.e., glass powder for titanium alloy sealing.

[0018] The present invention also provides an application of the titanium alloy sealing glass powder. The titanium alloy glass sealing is realized by using the titanium alloy sealing glass powder, which comprises the following steps:

[0019] 1) preparing the titanium alloy sealing glass powder into a glass insulator;

[0020] 2) pre-oxidizing the titanium alloy shell and the Kovar alloy core column to be sealed;

[0021] 3) According to the product structure, assemble the graphite mold, titanium alloy shell, Kovar alloy core column and glass insulator, put the assembled parts into the graphite mold, place the graphite mold in a tubular atmosphere furnace, introduce protective gas into the tubular atmosphere furnace, heat it from room temperature to 800℃, keep it warm for 30 minutes, then heat it to 860-950℃, keep it warm for 30 minutes, seal it, drop the temperature to 450-550℃ after high-temperature sealing, keep it warm for 30 minutes, then cool it with the furnace to complete the titanium alloy glass sealing.

[0022] Preferably, in step 1), the titanium alloy sealing glass powder is dry-pressed and then wax-removed and vitrified to obtain a glass insulator of the required size; in step 2), the pre-oxidation temperature of the titanium alloy shell is 550°C, the pre-oxidation time is 30 minutes, and the pre-oxidation temperature of the Kovar alloy core column is 450°C, and the pre-oxidation time is 30 minutes.

[0023] Further preferably, in step 3), the protective gas is nitrogen or argon, the gas flow rate is 12-15L / min, the temperature is increased from room temperature to 800°C at a rate of 10°C / min, kept warm for 30 minutes, then increased to 860-950°C at a rate of 5°C / min, kept warm for 30 minutes, and after high-temperature sealing, the temperature is reduced to 450-550°C at a rate of 8°C / min, and kept warm for 30 minutes.

[0024] The titanium alloy sealing glass powder provided by the present invention uses lead-free borosilicate glass as a basic system, has a dense glass space structure, and has strong chemical stability. By adding alkali metal ions K2O, the surface tension of the glass can be reduced. By adding alkaline earth metal oxides, the activity of alkali metal ions can be suppressed by the mixed alkali effect, thereby avoiding the decrease of insulation resistance caused by the migration of alkali metal ions at high temperature. In addition, the transition metal oxides in the components can reduce the surface tension of the glass to a certain extent. The thermal expansion coefficient of the titanium alloy sealing glass powder is α=58-68×10 -7 / ℃, softening point is 665-695℃, and sealing temperature is 860~950℃.

[0025] The borosilicate titanium alloy sealing glass powder has good wettability with titanium alloy, which can improve the airtightness of the product after sealing. At high temperature, the glass insulator fully melts and chemically combines with the metal to achieve a sealed seal between the titanium alloy and the glass. During the sealing process, the sealing temperature is controlled below the phase change temperature of the titanium alloy TC4, which can avoid the problem that the existing sealing glass powder sealing temperature is too high, causing the titanium alloy to undergo phase change and dimensional changes during the sealing process. Before sealing, the titanium alloy shell and the Kovar alloy core column are pre-oxidized, and a heat preservation platform is set during the heating process, which can increase the wettability of the borosilicate glass and the titanium alloy, and achieve high-performance sealing of the titanium alloy.

[0026] The thermal expansion coefficient of the glass powder for titanium alloy sealing provided by the present invention is lower than that of the titanium alloy, and is suitable for compression sealing. The obtained titanium alloy sealing device has high electrical insulation, high air tightness and high sealing strength. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] The present invention is further described in detail below in conjunction with the accompanying drawings and embodiments:

[0028] Figure 1 It is a schematic diagram of the structure of a titanium alloy glass sealing device;

[0029] In the figure, 1. Titanium alloy shell; 2. Glass insulator; 3. Kovar alloy core column. DETAILED DESCRIPTION

[0030] The present invention will be further explained below in conjunction with specific implementation schemes, but the present invention is not limited thereto.

[0031] On the one hand, the present invention provides a glass powder for sealing titanium alloys, which adopts a borosilicate glass system, wherein the glass powder for sealing titanium alloys comprises the following raw materials, calculated by mass percentage: 55-62% by mass of silicon dioxide, 15%-20% by mass of aluminum oxide, 12%-18% by mass of boron trioxide, 5%-8% by mass of alkali metal oxides, 2%-8% by mass of alkaline earth metal oxides, 3%-5% by mass of transition metal oxides, and 0.5%-2% by mass of titanium dioxide.

[0032] Preferably, the alkali metal oxide includes at least one of K2O and Na2O, and the mass fraction of K2O is greater than the mass fraction of Na2O.

[0033] More preferably, the alkaline earth metal oxide includes at least one of CaO and MgO.

[0034] Further preferably, the transition metal oxide includes at least one of WO3, V2O3, and Cr2O3.

[0035] The present invention also provides a method for preparing the titanium alloy sealing glass powder, comprising the following steps:

[0036] a) preparing raw materials according to mass percentage;

[0037] b) using a lifting furnace to uniformly mix, heat, and melt the raw materials, and then quench with water to obtain glass cullets, and then dry them to obtain dried glass cullets;

[0038] c) ball milling the dried glass shreds with a planetary ball mill to obtain titanium alloy sealing glass raw powder, and then granulating the titanium alloy sealing glass raw powder to obtain the titanium alloy sealing glass powder.

[0039] Preferably, in step b), the raw materials are placed in an alumina crucible with a height not exceeding one-half of the height of the crucible, and are mixed evenly using a glass rod. Thereafter, the alumina crucible is placed in a lifting furnace, heated to 850°C at a rate of 10°C / min at room temperature, kept warm for 4 hours, and then heated to 1400-1500°C at a rate of 3-5°C / min, and kept warm for 2-4 hours.

[0040] Further preferably, in step c), the dried glass chips are evenly placed in a ball mill filled with zirconia balls for 1-2 hours, and then 3%-6% of a binder is added to the glass raw powder obtained after ball milling. After granulation and sieving, a granulated powder with a mesh size of 40-120 is obtained, i.e., glass powder for titanium alloy sealing, wherein the binder includes but is not limited to paraffin wax, polyvinyl alcohol, etc.

[0041] The present invention also provides an application of the titanium alloy sealing glass powder. The titanium alloy glass sealing is realized by using the titanium alloy sealing glass powder, which comprises the following steps:

[0042] 1) using a dry pressing mold to prepare the titanium alloy sealing glass powder into a glass insulator;

[0043] 2) pre-oxidizing the titanium alloy shell and the Kovar alloy core column to be sealed;

[0044] 3) According to the product structure, assemble the graphite mold, titanium alloy shell, Kovar alloy core column and glass insulator, put the assembled parts into the graphite mold, place the graphite mold in a tubular atmosphere furnace, introduce protective gas into the tubular atmosphere furnace, heat it from room temperature to 800℃ and keep it for 30 minutes, then heat it to 860-950℃ and keep it for 30 minutes for sealing, after high-temperature sealing, reduce the temperature to 450-550℃ and keep it for 30 minutes, then cool it with the furnace to complete the titanium alloy glass sealing.

[0045] Preferably, in step 1), the glass powder is dry-pressed and then wax-removed and vitrified to obtain a glass insulator of a desired size.

[0046] More preferably, in step 2), the pre-oxidation temperature of the titanium alloy shell is 550° C., the pre-oxidation time is 30 min, and the pre-oxidation temperature of the Kovar alloy core column is 450° C., the pre-oxidation time is 30 min.

[0047] Further preferably, in step 3), the protective gas is nitrogen or argon, the gas flow rate is 12-15L / min, the temperature is increased from room temperature to 800°C at a rate of 10°C / min, and kept warm for 30 minutes, so that the glass insulator and the metal material are fully heated up and the internal and external temperatures are kept consistent, then the temperature is increased to 860-950°C at a rate of 5°C / min, and kept warm for 30 minutes, the glass insulator is fully melted at high temperature, the gas is removed, and after high-temperature sealing, the temperature is reduced to 450-550°C at a rate of 8°C / min and kept warm for 30 minutes to eliminate the stress of the sealed device.

[0048] Example 1

[0049] A method for preparing glass powder for titanium alloy sealing comprises the following steps:

[0050] a) preparing raw materials according to mass percentage, as shown in Table 1;

[0051] b) placing the raw materials in an alumina crucible, with the height of the raw materials not exceeding one-half of the height of the crucible, and mixing them uniformly using a glass rod, then placing the alumina crucible in a lifting furnace, heating the temperature to 850° C. at a rate of 10° C. / min at room temperature, keeping the temperature for 4 hours, then heating the temperature to 1400° C. at a rate of 3° C. / min, keeping the temperature for 2 hours, then quenching with water to obtain glass cullets, and then drying to obtain dried glass cullets;

[0052] c) The dried glass chips are evenly placed in a ball mill filled with zirconium oxide balls and the ball milling time is 1 hour. After that, 3% of a binder paraffin is added to the glass raw powder obtained after ball milling. After granulation and sieving, granulated powder with a mesh size of 40-120 is obtained, i.e., glass powder for titanium alloy sealing.

[0053] Example 2

[0054] A method for preparing glass powder for titanium alloy sealing comprises the following steps:

[0055] a) preparing raw materials according to mass percentage, as shown in Table 1;

[0056] b) placing the raw materials in an alumina crucible, with the height of the raw materials not exceeding one-half of the height of the crucible, and mixing them uniformly using a glass rod, then placing the alumina crucible in a lifting furnace, heating the temperature to 850° C. at a rate of 10° C. / min at room temperature, keeping the temperature for 4 hours, then heating the temperature to 1500° C. at a rate of 5° C. / min, keeping the temperature for 4 hours, then quenching with water to obtain glass cullets, and then drying the cullets to obtain dried glass cullets;

[0057] c) The dried glass chips are evenly placed in a ball mill filled with zirconium oxide balls and the ball milling time is 2 hours. After that, 6% of the binder polyvinyl alcohol is added to the glass raw powder obtained after ball milling. After granulation and sieving, granulated powder with a mesh size of 40-120 is obtained, i.e., glass powder for titanium alloy sealing.

[0058] Example 3

[0059] The difference from Example 1 is that the mass percentage of raw materials is different, see Table 1.

[0060] Example 4

[0061] The difference from Example 2 is that the mass percentage of raw materials is different, see Table 1.

[0062] Table 1 Raw material mass percentage and basic physical and chemical properties of glass powder for titanium alloy sealing in Examples 1-4:

[0063]

[0064] From Table 1, it can be seen that the physical and chemical properties of the titanium alloy sealing glass powder prepared by the present invention are as follows: the thermal expansion coefficient is α=58~68×10 -7 / ℃, softening point is 665-695℃, and sealing temperature is 860~950℃.

[0065] Example 5

[0066] The titanium alloy glass sealing device is obtained by using the titanium alloy sealing glass powder in Examples 1 to 4 to perform titanium alloy glass sealing, including the following steps:

[0067] 1) Dry-pressing titanium alloy sealing glass powder into shape using a dry-pressing mold, followed by wax removal and vitrification to obtain a glass insulator of the required size;

[0068] 2) pre-oxidizing the titanium alloy shell (TC4 titanium alloy) and the Kovar alloy core column (4J29 Kovar alloy) to be sealed, wherein the pre-oxidation temperature of the titanium alloy shell is 550° C., the pre-oxidation time is 30 min, and the pre-oxidation temperature of the Kovar alloy core column is 450° C., and the pre-oxidation time is 30 min;

[0069] 3) According to product structure (such as Figure 1As shown, it includes a glass insulator 2 with two through holes, a Kovar alloy core column 3 arranged in the through holes of the glass insulator, and a titanium alloy shell 1 wrapping the glass insulator 2. A graphite mold, a titanium alloy shell, a Kovar alloy core column and a glass insulator are assembled, and the assembled parts are put into a graphite mold. The graphite mold is placed in a tubular atmosphere furnace. Nitrogen is introduced into the tubular atmosphere furnace with a gas flow rate of 15L / min. The temperature is increased from room temperature to 800℃ at a rate of 10℃ / min and kept warm for 30min, and then the temperature is increased to 860℃ at a rate of 5℃ / min and kept warm for 30min for sealing. After high-temperature sealing, the temperature is reduced to 550℃ at a rate of 8℃ / min and kept warm for 30min, and then cooled with the furnace to complete the titanium alloy glass sealing.

[0070] Example 6

[0071] The titanium alloy glass sealing device is obtained by using the titanium alloy sealing glass powder in Examples 1 to 4 to perform titanium alloy glass sealing, including the following steps:

[0072] 1) Dry-pressing titanium alloy sealing glass powder into shape using a dry-pressing mold, followed by wax removal and vitrification to obtain a glass insulator of the required size;

[0073] 2) pre-oxidizing the titanium alloy shell (TC4 titanium alloy) and the Kovar alloy core column (4J29 Kovar alloy) to be sealed, wherein the pre-oxidation temperature of the titanium alloy shell is 550° C., the pre-oxidation time is 30 min, and the pre-oxidation temperature of the Kovar alloy core column is 450° C., and the pre-oxidation time is 30 min;

[0074] 3) According to product structure (such as Figure 1 As shown, it includes a glass insulator 2 with two through holes, a Kovar alloy core column 3 arranged in the through holes of the glass insulator, and a titanium alloy shell 1 wrapping the glass insulator 2. A graphite mold, a titanium alloy shell, a Kovar alloy core column and a glass insulator are assembled, and the assembled parts are put into a graphite mold. The graphite mold is placed in a tubular atmosphere furnace. Argon gas is introduced into the tubular atmosphere furnace with a gas flow rate of 12L / min. The temperature is increased from room temperature to 800℃ at a rate of 10℃ / min and kept warm for 30min, and then the temperature is increased to 950℃ at a rate of 5℃ / min and kept warm for 30min for sealing. After high-temperature sealing, the temperature is reduced to 450℃ at a rate of 8℃ / min and kept warm for 30min, and then cooled with the furnace to complete the titanium alloy glass sealing.

[0075] The performance of the titanium alloy glass sealing devices obtained in Example 5 and Example 6 was tested, and the results are as follows:

[0076] 1. The insulation resistance between the titanium alloy shell and the Kovar alloy core column is ≥1GΩ (500V DC);

[0077] 2. Use helium mass spectrometer leak detector, leakage rate ≤1.0×10 -9 Pa·m3 / s.

[0078] Compared with traditional titanium alloy sealing glass, the glass system of the present invention improves the wettability with titanium alloy, and the sealing temperature is controlled below the TC4 phase transition point of titanium alloy, which simplifies the subsequent dimensional precision refinement and other processes of titanium alloy glass sealing devices. The thermal expansion coefficient between titanium alloy and Kovar alloy realizes compression sealing, and good wettability and coordination ensure the performance of the product.

[0079] The embodiments of the present invention are described in detail above with reference to the accompanying drawings, but the present invention is not limited to the above embodiments, and various changes can be made within the knowledge scope of ordinary technicians in this field without departing from the purpose of the present invention.

Claims

1. Glass powder for titanium alloy sealing, It is characterized in that Calculated by mass percentage, the raw materials include: 55-62% silicon dioxide, 15-20% aluminum oxide, 12-18% boron oxide, 5-8% alkali metal oxide, 2-8% alkaline earth metal oxide, 0.5-2% titanium dioxide and 3-5% transition metal oxide.

2. The titanium alloy sealing glass powder according to claim 1, Features: The alkali metal oxides include K 2 O、Na 2 At least one of O and K 2 O mass fraction>Na 2 The mass fraction of O.

3. The titanium alloy sealing glass powder according to claim 1, Features: The alkaline earth metal oxide includes at least one of CaO and MgO.

4. The titanium alloy sealing glass powder according to claim 1, Features: The transition metal oxide includes WO 3 、V 2 O 3 Cr 2 O 3 At least one of .

5. A method for preparing the glass powder for titanium alloy sealing according to any one of claims 1 to 4, It is characterized in that The steps include: a) preparing raw materials according to mass percentage; b) using a lifting furnace to uniformly mix, heat, and melt the raw materials, and then quench with water to obtain glass cullets, and then dry them to obtain dried glass cullets; c) ball milling the dried glass shreds with a planetary ball mill to obtain titanium alloy sealing glass raw powder, and then granulating the titanium alloy sealing glass raw powder to obtain the titanium alloy sealing glass powder.

6. The method for preparing the glass powder for titanium alloy sealing according to claim 5, Features: In step b), the raw materials are placed in an alumina crucible with a height not exceeding one-half of the height of the crucible, and are mixed evenly using a glass rod. Thereafter, the alumina crucible is placed in a lifting furnace, heated to 850°C at a rate of 10°C / min at room temperature, kept warm for 4 hours, and then heated to 1400-1500°C at a rate of 3-5°C / min, and kept warm for 2-4 hours.

7. The method for preparing the glass powder for titanium alloy sealing according to claim 5, Features: In step c), the dried glass chips are evenly placed in a ball mill filled with zirconium oxide balls for 1-2 hours. After that, 3%-6% of a binder is added to the glass raw powder obtained after ball milling. Granulation and sieving are performed to obtain granulated powder of 40-120 mesh, i.e., glass powder for titanium alloy sealing.

8. Application of the glass powder for titanium alloy sealing according to any one of claims 1 to 4, Features: The titanium alloy glass sealing is realized by using the titanium alloy sealing glass powder, which comprises the following steps: 1) preparing the titanium alloy sealing glass powder into a glass insulator; 2) pre-oxidizing the titanium alloy shell and the Kovar alloy core column to be sealed; 3) According to the product structure, assemble the graphite mold, titanium alloy shell, Kovar alloy core column and glass insulator, put the assembled parts into the graphite mold, place the graphite mold in a tubular atmosphere furnace, introduce protective gas into the tubular atmosphere furnace, heat it from room temperature to 800℃, keep it warm for 30 minutes, then heat it to 860-950℃, keep it warm for 30 minutes, seal it, drop the temperature to 450-550℃ after high-temperature sealing, keep it warm for 30 minutes, then cool it with the furnace to complete the titanium alloy glass sealing.

9. Application of the glass powder for titanium alloy sealing according to claim 8, Features: In step 1), the titanium alloy sealing glass powder is dry-pressed and then wax-removed and vitrified to obtain a glass insulator of the required size; in step 2), the pre-oxidation temperature of the titanium alloy shell is 550°C, the pre-oxidation time is 30 minutes, and the pre-oxidation temperature of the Kovar alloy core column is 450°C, and the pre-oxidation time is 30 minutes.

10. Application of the glass powder for titanium alloy sealing according to claim 8, Features: In step 3), the protective gas is nitrogen or argon, the gas flow rate is 12-15L / min, the temperature is increased from room temperature to 800°C at a rate of 10°C / min, kept warm for 30 minutes, then increased to 860-950°C at a rate of 5°C / min, kept warm for 30 minutes, and after high-temperature sealing, the temperature is reduced to 450-550°C at a rate of 8°C / min, and kept warm for 30 minutes.