Silver catalyst for producing ethylene oxide through ethylene epoxidation as well as preparation method and application of silver catalyst

By optimizing the load ratio of silver, alkali metal and rhenium in the silver catalyst, a high-activity and high-selectivity silver catalyst was prepared, which solved the problem of insufficient activity and selectivity of existing catalysts under high load conditions and improved ethylene epoxy Production efficiency of alkane and stability of catalyst.

CN118925724APending Publication Date: 2024-11-12CHINA PETROLEUM & CHEMICAL CORP +1

Patent Information

Application Number
CN202310538775.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-12
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Existing silver catalysts have problems with insufficient activity and selectivity in ethylene epoxidation reaction. Especially under high load reaction conditions, the stability and selectivity of the catalyst are reduced rapidly, which affects the production of ethylene oxide. efficiency.

Method used

By optimizing the load ratio of silver, alkali metal, rhenium and rhenium co-adjuvant in the silver catalyst, a silver catalyst with high activity and selectivity was prepared, including 15 to 36 wt% silver, 50 to 3000 ppm alkali metal oxide, 25 to 25 to 3000 ppm alkali metal oxide, 15 to 36 wt% silver, 15 to 36 ppm alkali metal oxide, 15 to 36 ppm 1500 ppm rhenium oxide and 5 to 300 ppm rhenium co-adjuvant metal element oxide, the support is porous α-alumina, and the catalyst is prepared by preparation of impregnation liquid and heat treatment.

Benefits of technology

It improves the activity and selectivity of the catalyst, is suitable for ethylene epoxidation reaction under high load conditions, extends the activity and selectivity stability of the catalyst, and improves the production efficiency of ethylene oxide.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004230013640000081
    Figure BDA0004230013640000081
  • Figure BDA0004230013640000111
    Figure BDA0004230013640000111
  • Figure BDA0004230013640000121
    Figure BDA0004230013640000121
Patent Text Reader

Abstract

The invention belongs to the technical field of silver catalysts, and discloses a silver catalyst for producing ethylene oxide through ethylene epoxidation and a preparation method and application of the silver catalyst. The silver catalyst comprises silver, alkali metal oxide, rhenium oxide, rhenium co-aid metal element oxide and a carrier; based on the total weight of the silver catalyst, the content of silver is 15-36 wt%, the content of alkali metal oxide (calculated as alkali metal) is 50-3000 ppm, the content of rhenium oxide (calculated as rhenium) is 25-1500 ppm, the content of rhenium co-additive metal element oxide (calculated as metal element) is 5-300 ppm, and the balance is the carrier; wherein the molar ratio of the silver to the alkali metal is 150-800 / 1, the molar ratio of the alkali metal to the rhenium is 0.5-10 / 1, and the molar ratio of the rhenium to the rhenium co-additive metal element is 5-50 / 1. The silver catalyst provided by the invention has high activity and selectivity, and is especially suitable for a reaction device with high load for producing ethylene oxide through ethylene epoxidation.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of silver catalysts, and more specifically, to a silver catalyst for producing ethylene oxide by epoxidation of ethylene, and a preparation method and application thereof. Background Art

[0002] In recent years, the global ethylene oxide / ethylene glycol (EO / EG) production capacity has increased year by year, and Asia, especially China, is both a major production area and a major consumption area. EO / EG is mainly produced by ethylene epoxidation reaction, and silver catalyst is the core catalyst for the production of ethylene oxide / ethylene glycol. At present, the global EOE (equivalent EO) production capacity has exceeded 30 million tons / year, and the annual demand for catalysts has reached about 6,000 tons; with the rapid development of chemical and ethylene-related industries in various countries, especially in the Middle East, the future EO / EG market and silver catalyst demand are huge.

[0003] Silver catalyst is a catalyst used in industry for the production of ethylene oxide (EO) by epoxidation of ethylene. Shell, Dow Chemical (UCC), SD and Sinopec have conducted extensive research on silver catalysts. The current market is dominated by high-selectivity and high-efficiency silver catalysts suitable for high space-time yields, with a demand ratio of more than 99%. Ethylene epoxidation under the action of silver catalysts mainly produces ethylene oxide (EO), while carbon dioxide and water are produced as side reactions. Among them, activity, selectivity and stability are the main performance indicators of silver catalysts. Activity refers to the reaction temperature required when the ethylene oxide production process reaches a certain reaction load. The lower the reaction temperature, the higher the activity of the catalyst; selectivity refers to the ratio of the number of moles of ethylene converted into ethylene oxide in the reaction to the total number of moles of ethylene in the reaction; stability is expressed as the rate of decrease of activity and selectivity. The smaller the rate of decrease, the better the stability of the catalyst. The performance of silver catalysts is not only related to the performance of the carrier used and its preparation method, but also to the composition and preparation method of the catalyst.

[0004] From the perspective of catalyst composition, the active component is metallic silver, and additives are added to improve the selectivity of the product. Patents for the addition of additives have basically covered all elements in the periodic table. However, the additive components of silver catalysts mainly include alkali metals, alkaline earth metals, rare earth metals and precious metals, and the composition of different types of catalysts is also different. One of the more important additives is alkali metals. Literature reports that it can make the silver particles more evenly distributed on the carrier, and can promote the formation of electrophilic oxygen and ethylene epoxidation transition state oxygen heterometallic ring (OMC); there are also literatures introducing that alkali metals can make silver generate more lattice defects on the carrier surface, which is easy to adsorb subsurface oxygen and then generate EO. USP6762311 alkali metals are preferably added in the form of hydroxides, and USP6815395 alkali metals are preferably added in the form of nitrates, and the catalyst performance is improved by impregnating different alumina carriers.

[0005] Another very important additive is rhenium. The difference between high-activity catalysts and medium / high-selectivity and high-efficiency silver catalysts is that the latter catalysts contain rhenium additives, which significantly improves the selectivity of the catalysts. US patent application USP4761394 first reported the use of rhenium (Re) as an additive in silver catalysts. USP4548921 describes the role of rhenium additives in silver catalysts. Re exists on the carrier as uniformly dispersed metal particles, and the active component silver is loaded on the outer surface of rhenium to improve the performance of silver catalysts. There are also literatures that believe that the rhenium additive competes with the adsorbed oxygen on the catalyst surface and attracts electrons in the silver lattice, resulting in a decrease in the electron density of the adsorbed oxygen and an increase in the selectivity of the product EO. In USP7259129, the rhenium additive can be added in the form of chloride, rhenate and perrhenate. In Chinese patent applications CN201010622856.4 and CN201010534019.6, the rhenium additive is an inorganic compound containing rhenium, such as perrhenic acid, perrhenate, or a mixture thereof.

[0006] As a co-promoter of the rhenium promoter, it can keep the rhenium promoter at a higher valence and ensure that the catalyst has a higher selectivity. US Patent Application No. 7538235 describes that the co-promoter of the rhenium promoter includes one or more compounds containing tungsten, chromium, molybdenum and sulfur, preferably a tungsten compound.

[0007] In addition, the loading amount of each auxiliary agent during the preparation of the impregnation solution and the ratio between silver and auxiliary agents and between different auxiliary agents also have an important influence on the synergistic effect and catalyst performance. The amount of alkali metal auxiliary agent added in US10865189 is 10-3000ppm, preferably 15-2000ppm, further preferably 20-1500ppm, and most preferably 50-1000ppm. BASF's US2021 / 0046459 Al provides a catalyst that effectively converts ethylene oxidation into ethylene oxide, the catalyst composition comprising 20-45% silver by weight of the catalyst; the cesium loading C (Cs) per kilogram of catalyst is at least 2.0mmol; the rhenium loading C (Re) per kilogram of catalyst is at least 3.0mmol; the tungsten loading c (W) per kilogram of catalyst is at least 1.6mmol. Shell patent EP 3187493 B1 provides a catalyst for olefin epoxidation, which includes a carrier and silver, a rhenium promoter, a first co-promoter and a second co-promoter deposited on the carrier; the rhenium promoter is at least 1.5 mmole / kg and at most 10 mmole / kg relative to the weight of the catalyst in terms of element; the molar ratio of the first co-promoter to the second co-promoter is greater than 1; the catalyst also contains a potassium promoter, and the potassium loading is at least 0.5 mmole / kg relative to the weight of the catalyst.

[0008] The generally accepted mechanism of ethylene epoxidation to produce ethylene oxide is the atomic oxygen mechanism, that is, ethylene reacts with atomic oxygen adsorbed on silver to generate the product ethylene oxide. The additive can adjust the amount and strength of oxygen adsorbed on silver, and thus affect the performance of the catalyst. The above reference introduces the preferred range of the loading amount of the additive in the catalyst, but does not limit or optimize the synergistic ratio between silver and the additives. Summary of the invention

[0009] The purpose of the present invention is to provide a silver catalyst for producing ethylene oxide by epoxidation of ethylene, a preparation method and application thereof, and the prepared silver catalyst has better catalyst performance by optimizing the loading ratio between silver and alkali metal, alkali metal and rhenium, and rhenium and rhenium co-promoter metal elements.

[0010] The first aspect of the present invention provides a silver catalyst for producing ethylene oxide by epoxidation of ethylene, the silver catalyst comprising: silver, an alkali metal oxide, an oxide of rhenium, an oxide of a co-promoter metal element of rhenium, and a carrier;

[0011] Based on the total weight of the silver catalyst, the content of silver is 15-36wt%, the content of the alkali metal oxide is 50-3000ppm based on the alkali metal, the content of the rhenium oxide is 25-1500ppm based on rhenium, the content of the oxide of the co-promoter metal element of rhenium is 5-300ppm based on the metal element, and the balance is carrier;

[0012] Among them, the auxiliary components in the silver catalyst are calculated as metals, the molar ratio of silver to alkali metal is 150-800 / 1, the molar ratio of alkali metal to rhenium is 0.5-10 / 1, and the molar ratio of rhenium to the co-auxiliary metal element of rhenium is 5-50 / 1.

[0013] A second aspect of the present invention provides a method for preparing the above-mentioned silver catalyst, the preparation method comprising:

[0014] (1) preparing an impregnation solution of the silver catalyst;

[0015] (2) The carrier is impregnated in the impregnation solution, and then leached and heated to obtain the silver catalyst.

[0016] The third aspect of the present invention provides an application of the above silver catalyst in the production of ethylene oxide by epoxidation of ethylene.

[0017] The technical solution of the present invention has the following beneficial effects: the silver catalyst of the present invention has high activity and selectivity, and is particularly suitable for a reaction device for producing ethylene oxide by epoxidation of ethylene with a high load.

[0018] Other features and advantages of the present invention will be described in detail in the following detailed description. DETAILED DESCRIPTION

[0019] The preferred embodiments of the present invention will be described in more detail below. Although the preferred embodiments of the present invention are described below, it should be understood that the present invention can be implemented in various forms and should not be limited to the embodiments set forth herein.

[0020] The first aspect of the present invention provides a silver catalyst for producing ethylene oxide by epoxidation of ethylene, the silver catalyst comprising: silver, an alkali metal oxide, an oxide of rhenium, an oxide of a co-promoter metal element of rhenium, and a carrier;

[0021] Based on the total weight of the silver catalyst, the content of silver is 15-36wt%, the content of the alkali metal oxide is 50-3000ppm based on the alkali metal, the content of the rhenium oxide is 25-1500ppm based on rhenium, the content of the oxide of the co-promoter metal element of rhenium is 5-300ppm based on the metal element, and the balance is carrier;

[0022] Among them, the auxiliary components in the silver catalyst are calculated as metals, the molar ratio of silver to alkali metal is 150-800 / 1, the molar ratio of alkali metal to rhenium is 0.5-10 / 1, and the molar ratio of rhenium to the co-auxiliary metal element of rhenium is 5-50 / 1.

[0023] According to the present invention, preferably, the content of the rhenium oxide calculated as rhenium is 100-2500 ppm, the content of the rhenium oxide calculated as rhenium is 50-1200 ppm, and the content of the oxide of the co-promoter metal element of rhenium calculated as the metal element is 10-250 ppm.

[0024] According to the present invention, preferably, the molar ratio of silver to alkali metal is 200-650 / 1, the molar ratio of alkali metal to rhenium is 1-8 / 1, and the molar ratio of rhenium to the co-additive metal element of rhenium is 10-40 / 1.

[0025] In the present invention, the inventors have conducted in-depth research on the preparation of domestically produced high-efficiency silver-containing rhenium catalysts. By adjusting the amount of alkali metal additives, rhenium additives and co-additives added in the impregnation solution on the basis of selecting a carrier with suitable physical properties and the original catalyst preparation process, the loading amount of silver and alkali metal, alkali metal and rhenium, and rhenium and its co-additives in the prepared finished catalyst is in a certain ratio to further improve the performance of the high-efficiency silver catalyst. The silver amine solution is prepared in a traditional manner. According to the physical properties of the carrier, the amount of additives added is strictly controlled during the preparation of the impregnation solution. After the catalyst is leached and thermally decomposed, there is an optimal ratio range between the active component silver and the loading amount of each additive, and the prepared silver catalyst has good performance.

[0026] The auxiliary agents used in the present invention include alkali metal auxiliary agents, rhenium auxiliary agents and co-auxiliaries thereof. The auxiliary agents with a synergistic ratio in the catalyst can achieve the best effect of its auxiliary catalytic effect and improve the performance of the prepared silver catalyst.

[0027] In the present invention, the rhenium auxiliary agent used to prepare the impregnation solution can be at least one of rhenium oxide, perrhenic acid and perrhenate, preferably perrhenic acid and / or perrhenate, and more preferably at least one of perrhenic acid, cesium perrhenate and ammonium perrhenate.

[0028] According to the present invention, preferably, the alkali metal is at least one of lithium, sodium, potassium, rubidium and cesium.

[0029] According to the present invention, preferably, the co-promoter metal element of rhenium is a transition metal element in the periodic table, preferably at least one of Group VIB and Group VIIB elements, and more preferably at least one of tungsten, molybdenum and chromium.

[0030] In the present invention, the rhenium co-agent for preparing the impregnation solution is at least one of the compounds of transition metals in the periodic table; preferably at least one of the compounds of VIB group and VIIB group elements; further preferably at least one of the oxyacids of VIB group elements, oxyacids of VIB group elements, oxyacids of VIIB group elements and oxyacids of VIIB group elements; more preferably at least one of tungstic acid, ammonium tungstate, molybdic acid, ammonium molybdate and ammonium chromate.

[0031] According to the present invention, preferably, the carrier is an α-alumina carrier;

[0032] Preferably, the α-alumina carrier is prepared by a method comprising the following steps: uniformly mixing inert α-A12O3 powder, pseudo-monohydrate alumina, a pore-forming agent, a silicon-containing compound and a zirconium-containing compound to obtain a mixed material; then kneading, extruding, drying and calcining the mixed material, an extrusion aid and a cellulose polymer colloid solution to obtain the α-alumina carrier.

[0033] In the present invention, the carrier used is a porous α-alumina, and the α-alumina content in the carrier is more than 90%.

[0034] In the present invention, preferably, based on the total weight of the mixed material, the inert α-A1 2 O 3 The amount of powder is 75% to 95%, the amount of pseudo-monohydrate alumina is 2.0% to 15%, the amount of pore-forming agent is 2.0% to 15%, the amount of silicon-containing compound is 0.1% to 1.5%, and the amount of zirconium-containing compound is 0.2% to 2.0%;

[0035] Based on the total weight of the mixed material, the amount of the extrusion aid is 0.5% to 10%, and the amount of the cellulose polymer colloid solution is 20% to 40%.

[0036] In the present invention, preferably, the inert α-A1 2 O 3 The particle size of the powder is 1 to 5 μm; the particle size of pseudo-monohydrate alumina is less than 75 μm.

[0037] In the present invention, the cellulose polymer colloidal solution is used as a binder and the calcination temperature is 1200-1450°C.

[0038] The α-alumina carrier of the present invention has the following characteristics: the crushing strength of the α-alumina carrier is 40 to 150 N / grain, preferably 50 to 140 N / grain; the specific surface area is 0.5 to 2.5 m 2 / g, preferably 0.7 to 2.0 m 2 / g; the pore volume is 0.30 to 0.65 ml / g, preferably 0.35 to 0.60 ml / g.

[0039] According to the present invention, preferably, the oxide of the co-promoter metal element of rhenium is a high-valent metal oxide, preferably a hexavalent metal oxide and / or a heptavalent metal oxide.

[0040] The second aspect of the present invention provides a method for preparing the above-mentioned silver catalyst, the preparation method comprising:

[0041] (1) preparing an impregnation solution of the silver catalyst;

[0042] (2) The carrier is impregnated in the impregnation solution, and then leached and heated to obtain the silver catalyst.

[0043] In the present invention, preferably, the impregnation solution comprises: a silver-containing compound, an alkali metal additive, a rhenium additive, and an inorganic co-additive of rhenium. Further, the impregnation solution preferably comprises: a silver-containing compound, an alkali metal additive, a rhenium additive, an inorganic co-additive of rhenium, and a solvent; the solvent is water and / or an organic solvent, and the organic solvent is preferably an organic amine.

[0044] According to the present invention, preferably, the preparation method further comprises step (3): repeatedly performing step (2) on the prepared silver catalyst.

[0045] According to the present invention, preferably, the carrier is immersed in the impregnation liquid under the condition that the vacuum degree is less than 10 mmHg;

[0046] The heating is carried out in an air flow or a nitrogen-oxygen mixed gas with an oxygen content of not more than 21%.

[0047] In the present invention, the impregnation time of the support is preferably 10 to 60 minutes.

[0048] In the present invention, the alkali metal auxiliary agent may be applied to the support before, simultaneously with or after the impregnation of silver, or may be impregnated on the support after the silver compound is reduced.

[0049] In the present invention, the rhenium-containing additive and its co-additive can be applied to the carrier before, at the same time or after the silver is impregnated, or can be impregnated on the carrier after the silver compound is reduced. The activity, selectivity and stability of the activity and selectivity of the obtained silver catalyst can be further improved by adding the rhenium-containing additive and its co-additive.

[0050] The third aspect of the present invention provides the use of the above silver catalyst in the production of ethylene oxide by epoxidation of ethylene.

[0051] The present invention is further described below by examples:

[0052] The carriers used for the catalysts of the following examples and comparative examples were prepared by the following method:

[0053] 1~5μm inert α-A1 2 O 3 500g of powder, 50g of pseudo-monohydrate alumina less than 75μm, 50g of petroleum coke, 3.0g of calcium silicate and 5.0g of zirconium dioxide are put into a mixer and mixed evenly, then transferred to a kneader, 25g of vaseline and 160g of 2.5% methyl cellulose colloidal aqueous solution are added, and kneaded into a paste that can be extruded. Extrusion molding is a single-hole column with an outer diameter of 8.0mm, a length of 6.0mm, and an inner diameter of 3.0mm. Dry at 100℃ for more than 2 hours to reduce the free water content to less than 10%. The carrier after kneading is placed in a bell kiln, and the temperature is raised from room temperature to 1400℃ over 33 hours. It is calcined at 1400℃ for 4 hours to obtain a carrier (α-alumina carrier) for a white silver catalyst. The carrier crushing strength is 68N / grain; the specific surface area is 1.16m 2 / g; pore volume is 0.44ml / g.

[0054] The activity and selectivity of various silver catalysts of the present invention are tested by a laboratory reactor (hereinafter referred to as "micro-reactor") evaluation device. The reactor used in the micro-reactor evaluation device is a stainless steel tube with an inner diameter of 4 mm, and the reactor is placed in a heating jacket. The filling volume of the catalyst is 1 ml, and there is an inert filler at the bottom, so that the catalyst bed is located in the constant temperature zone of the heating jacket.

[0055] The activity and selectivity test conditions used in the present invention are as follows: The gas composition at the reactor inlet (mol%): ethylene (C 2 H 4 ), 28.0% ± 1.0; oxygen (O 2 ), 7.4% ± 0.2; carbon dioxide (CO2 ), <1.0%; inhibitor dichloroethane 0.1ppm~2.0ppm; stabilizing gas (N 2 ), balance; reaction pressure, 2.1MPa; space velocity, 6000 / h; reactor outlet EO concentration (mol%): 2.50%

[0056] When the above reaction conditions are stably reached, the gas composition at the reactor inlet and outlet is continuously measured. The selectivity is calculated according to the following formula after volume shrinkage correction is performed on the measured results:

[0057]

[0058] Among them, ΔEO is the difference in ethylene oxide concentration between the outlet gas and the inlet gas, and the average of more than 10 groups of test data is taken as the test result of the day.

[0059] Catalyst Preparation Comparative Example 1

[0060] 16.82 g of ethylenediamine and 6.53 g of ethanolamine were dissolved in 35.92 g of deionized water. Silver oxalate was slowly added to the mixture under stirring. The temperature was kept below 40° C. to dissolve all the silver oxalate. The amount of silver oxalate added was such that the silver content in the silver catalyst was 24 wt % (based on the total weight of the silver catalyst). 0.055 g of cesium nitrate and deionized water were then added to make the total mass of the solution reach 100 g to prepare an impregnation solution for standby use.

[0061] Catalyst Preparation Comparative Example 2

[0062] 16.82 g of ethylenediamine and 6.53 g of ethanolamine were dissolved in 35.92 g of deionized water. Silver oxalate was slowly added to the mixture under stirring. The temperature was kept below 40° C. to dissolve all the silver oxalate. The amount of silver oxalate added was such that the silver content in the silver catalyst was 24 wt % (based on the total weight of the silver catalyst). 0.074 g of cesium nitrate, 0.251 g of perrhenic acid and deionized water were then added to make the total mass of the solution reach 100 g to prepare an impregnation solution for standby use.

[0063] Catalyst Preparation Comparative Example 3

[0064] 16.82g of ethylenediamine and 6.53g of ethanolamine were dissolved in 35.92g of deionized water. Silver oxalate was slowly added to the mixture under stirring. The temperature was kept below 40°C to dissolve all the silver oxalate. The amount of silver oxalate added was such that the silver content in the silver catalyst was 24wt% (based on the total weight of the silver catalyst). Then, 0.462g of cesium nitrate, 0.042g of perrhenic acid, 0.013g of ammonium chromate and deionized water were added to make the total mass of the solution reach 100g, and the mixture was prepared into an impregnation solution for standby use.

[0065] Catalyst Preparation Example 1

[0066] 16.82g of ethylenediamine and 6.53g of ethanolamine were dissolved in 35.92g of deionized water. Silver oxalate was slowly added to the mixture under stirring. The temperature was kept below 40°C to dissolve all the silver oxalate. The amount of silver oxalate added was such that the silver content in the silver catalyst was 24wt% (based on the total weight of the silver catalyst). Then, 0.074g of cesium nitrate, 0.186g of perrhenic acid, 0.002g of ammonium chromate and deionized water were added to make the total mass of the solution reach 100g, and the mixture was prepared into an impregnation solution for standby use.

[0067] Catalyst Preparation Example 2

[0068] 16.82 g of ethylenediamine and 6.53 g of ethanolamine were dissolved in 35.92 g of deionized water. Silver oxalate was slowly added to the mixture under stirring. The temperature was kept below 40° C. to dissolve all the silver oxalate. The amount of silver oxalate added was such that the silver content in the silver catalyst was 24 wt % (based on the total weight of the silver catalyst). 0.110 g of cesium nitrate, 0.136 g of perrhenic acid, 0.002 g of ammonium chromate and deionized water were then added to make the total mass of the solution reach 100 g to prepare an impregnation solution for standby use.

[0069] Catalyst Preparation Example 3

[0070] 16.82g of ethylenediamine and 6.53g of ethanolamine were dissolved in 35.92g of deionized water. Silver oxalate was slowly added to the mixture under stirring. The temperature was kept below 40°C to dissolve all the silver oxalate. The amount of silver oxalate added was such that the silver content in the silver catalyst was 24wt% (based on the total weight of the silver catalyst). Then, 0.174g of cesium nitrate, 0.093g of perrhenic acid, 0.003g of ammonium chromate and deionized water were added to make the total mass of the solution reach 100g, and the mixture was prepared into an impregnation solution for standby use.

[0071] Catalyst Preparation Example 4

[0072] 16.82 g of ethylenediamine and 6.53 g of ethanolamine were dissolved in 35.92 g of deionized water. Silver oxalate was slowly added to the mixture under stirring. The temperature was kept below 40° C. to dissolve all the silver oxalate. The amount of silver oxalate added was such that the silver content in the silver catalyst was 24 wt % (based on the total weight of the silver catalyst). Then, 0.221 g of cesium nitrate, 0.051 g of perrhenic acid, 0.004 g of ammonium chromate and deionized water were added to make the total mass of the solution reach 100 g to prepare an impregnation solution for standby use.

[0073] Catalyst Preparation Example 5

[0074] 16.82 g of ethylenediamine and 6.53 g of ethanolamine were dissolved in 35.92 g of deionized water. Silver oxalate was slowly added to the mixture under stirring. The temperature was kept below 40° C. to dissolve all the silver oxalate. The amount of silver oxalate added was such that the silver content in the silver catalyst was 24 wt % (based on the total weight of the silver catalyst). Then, 0.221 g of cesium nitrate, 0.051 g of perrhenic acid, 0.003 g of ammonium chromate and deionized water were added to make the total mass of the solution reach 100 g to prepare an impregnation solution for standby use.

[0075] Catalyst Preparation Example 6

[0076] 16.82 g of ethylenediamine and 6.53 g of ethanolamine were dissolved in 35.92 g of deionized water. Silver oxalate was slowly added to the mixture under stirring. The temperature was kept below 40° C. to dissolve all the silver oxalate. The amount of silver oxalate added was such that the silver content in the silver catalyst was 24 wt % (based on the total weight of the silver catalyst). Then, 0.331 g of cesium nitrate, 0.043 g of perrhenic acid, 0.005 g of ammonium chromate and deionized water were added to make the total mass of the solution reach 100 g to prepare an impregnation solution for standby use.

[0077] The impregnation solutions prepared in the above catalyst preparation comparative examples and catalyst preparation examples were used to prepare catalysts (Comparative Examples 1-3 and Examples 1-6) according to the following method. The main compositions of the prepared catalysts and the molar ratios of the components are shown in Table 1.

[0078] Take 20g of the carrier sample, put it into a vacuum container, evacuate to above 10mmHg, introduce the above impregnation solution, keep it for 30 minutes, and filter out the excess solution. The impregnated carrier is heated in an air flow at 350℃ for 10 minutes, and after cooling, it is made into a primary impregnation catalyst; repeat the above steps for secondary impregnation to obtain the finished catalyst.

[0079] Table 1 Main composition of catalyst and molar ratio of each component

[0080]

[0081] The activity and selectivity of the catalyst sample were measured under the aforementioned process conditions using a microreactor evaluation device. The space-time yield was 295 gEO / mlCat. / h. The experimental results are listed in Table 2 below.

[0082] Table 2 Effect of additive composition on silver catalyst performance

[0083]

[0084] The embodiments of the present invention have been described above, and the above description is exemplary, not exhaustive, and is not limited to the disclosed embodiments. Many modifications and changes will be apparent to those skilled in the art without departing from the scope and spirit of the described embodiments.

Claims

1. A silver catalyst for producing ethylene oxide by epoxidation of ethylene, characterized in that: The silver catalyst comprises: silver, alkali metal oxide, rhenium oxide, oxide of a co-promoter metal element of rhenium and a carrier; Based on the total weight of the silver catalyst, the content of silver is 15-36wt%, the content of the alkali metal oxide is 50-3000ppm based on the alkali metal, the content of the rhenium oxide is 25-1500ppm based on rhenium, the content of the oxide of the co-promoter metal element of rhenium is 5-300ppm based on the metal element, and the balance is carrier; Among them, the auxiliary components in the silver catalyst are calculated as metals, the molar ratio of silver to alkali metal is 150-800 / 1, the molar ratio of alkali metal to rhenium is 0.5-10 / 1, and the molar ratio of rhenium to the co-auxiliary metal element of rhenium is 5-50 / 1.

2. The silver catalyst according to claim 1, wherein The content of the rhenium oxide calculated as rhenium is 100 to 2500 ppm, the content of the rhenium oxide calculated as rhenium is 50 to 1200 ppm, and the content of the oxide of the co-promoter metal element of rhenium calculated as the metal element is 10 to 250 ppm.

3. The silver catalyst according to claim 1, wherein The molar ratio of silver to alkali metal is 200-650 / 1, the molar ratio of alkali metal to rhenium is 1-8 / 1, and the molar ratio of rhenium to the co-additive metal element of rhenium is 10-40 / 1.

4. The silver catalyst according to any one of claims 1 to 3, wherein The alkali metal is at least one of lithium, sodium, potassium, rubidium and cesium.

5. The silver catalyst according to any one of claims 1 to 3, wherein The co-promoter metal element of rhenium is a transition metal element in the periodic table, preferably at least one of Group VIB and Group VIIB elements, and more preferably at least one of tungsten, molybdenum and chromium.

6. The silver catalyst according to any one of claims 1 to 3, wherein The carrier is an α-alumina carrier; Preferably, the α-alumina carrier is prepared by a method comprising the following steps: uniformly mixing inert α-A12O3 powder, pseudo-monohydrate alumina, a pore-forming agent, a silicon-containing compound and a zirconium-containing compound to obtain a mixed material; then kneading, extruding, drying and calcining the mixed material, an extrusion aid and a cellulose polymer colloid solution to obtain the α-alumina carrier.

7. The silver catalyst according to any one of claims 1 to 3, wherein The oxide of the co-promoter metal element of rhenium is a high-valent metal oxide, preferably a hexavalent metal oxide and / or a heptavalent metal oxide.

8. A method for preparing the silver catalyst according to any one of claims 1 to 7, characterized in that: The preparation method comprises: (1) preparing an impregnation solution of the silver catalyst; (2) The carrier is impregnated in the impregnation solution, and then leached and heated to obtain the silver catalyst.

9. The preparation method according to claim 8, wherein: The preparation method further comprises step (3): repeatedly performing step (2) on the prepared silver catalyst.

10. The preparation method according to claim 8, wherein: Immersing the carrier in the impregnation liquid under a condition where the vacuum degree is less than 10 mmHg; The heating is carried out in an air flow or a nitrogen-oxygen mixed gas with an oxygen volume content of no more than 21%.

11. Use of the silver catalyst according to any one of claims 1 to 7 in the production of ethylene oxide by epoxidation of ethylene.

Citation Information

Patent Citations

  • Preparation method of silver catalyst for producing ethylene oxide, silver catalyst prepared thereby and application thereof

    CN102527384A

  • Silver catalyst and preparation method and application thereof

    CN106607028A

Cited By

  • Selective hydrogenation reaction Ag-based catalyst and preparation method thereof

    CN121372399A