A crystallized ion sieve and its preparation method and application

By developing crystallized ion sieve composed of specific crystal phases, the problem of the existing ion sieve's unsatisfactory removal effect in high-temperature salt bath is solved, and the effect of stably absorbing impurity ions in high-temperature salt bath is achieved, ensuring the glass strengthening process salt bath concentration and glass mass in it.

CN118270978BActive Publication Date: 2024-11-26CHONGQING AUREAVIA HI TECH GLASS CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202310588487.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-05-23
Publication Date
2024-11-26
Estimated Expiration
2043-05-23

AI Technical Summary

Technical Problem

The existing ion sieves have poor impurity removal after use in high-temperature salt baths, which can easily release impurities and reversely release impurities, affecting the apparent quality of the glass and the concentration of the salt bath.

Method used

A crystallized ion sieve containing specific crystal phase composition and structure was developed. The content of cherry stone crystal phase is not less than 45 wt%, with low thermal gravimetric analysis weight loss in the range of 30℃ to 500℃, and can continuously and stably absorb in a high-temperature salt bath. Impurity ions and reduce the effect on salt bath pH.

Benefits of technology

The crystallized ion sieve maintains the structure stable in the high-temperature salt bath, continuously absorbs impurity ions, avoids the release of impurities, prolongs the use time, ensures that the salt bath concentration meets the requirements of glass strengthening, reduces the impact on the pH of the salt bath, and avoids the Glass corrosion.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118270978B_ABST
    Figure CN118270978B_ABST
Patent Text Reader

Abstract

The present invention discloses a crystallized ion sieve and a preparation method and application thereof. The crystallized ion sieve contains SiO 2 、Al 2 O 3 and alkali metal oxides; the crystallized ion sieve contains nepheline crystal phase, and the content of nepheline crystal phase in the crystallized ion sieve is not less than 45.00wt% based on the total mass of the ion sieve; the crystallized ion sieve has a thermogravimetric weight loss of less than or equal to 1.60% by weight in the range of 30°C to 500°C. The crystallized ion sieve provided by the present invention that meets the specific crystal phase content and thermal weight loss has excellent high-temperature stability, can maintain a stable structure in a high-temperature salt bath, is not easy to release impurities that affect the surface quality of the glass into the salt bath, and can still continuously and stably absorb impurity ions in the salt bath even if it exists in a high-temperature salt bath for a long time. At the same time, the crystallized ion sieve has a smaller effect on the pH of the salt bath after being added to the salt bath for use than other crystallized ion sieves of the same system.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of glass chemical strengthening, and in particular to a crystallized ion sieve that can be used as a salt bath purification additive material, and a preparation method and application thereof. Background Art

[0002] In the glass processing industry, chemical strengthening methods are often used to improve the mechanical strength of the base glass. That is, the base glass is immersed in a high-temperature molten salt bath, and the alkali metal cations with small ion radius in the glass are replaced with alkali metal cations with large ion radius in the salt bath, thereby generating a compressive stress layer on the glass surface, thereby achieving the purpose of improving the strength of the glass.

[0003] During industrial continuous production, as ion exchange proceeds, impure alkali metal ions in the salt bath (i.e., cations diffused from the substrate glass into the salt bath) gradually accumulate, causing poisoning of the salt bath, hindering the normal ion exchange and affecting the size and stress strength of the strengthened glass.

[0004] In order to ensure the stable quality of chemically strengthened glass during mass production and improve its production efficiency, production plants often use ion impurity removal methods to ensure that the concentration of impurity ions in the long-term salt bath meets the requirements of the salt bath for glass strengthening.

[0005] At present, the commonly used methods for removing impurity ions in the industry mainly include: adding phosphates (sodium phosphate, potassium phosphate), ion sieves, etc. to the salt bath as removal materials or adsorption materials for impurity ions in the salt bath.

[0006] Among them, sodium phosphate and / or potassium phosphate are used as impurity ion removal materials. This impurity removal method often requires the suspension of strengthening work to allow the impurity ions to fully react and precipitate with phosphates, which is not conducive to improving mass production efficiency. Moreover, the precipitate after the reaction is deposited at the bottom of the salt bath furnace, which increases the difficulty of cleaning and replacing the salt bath. In addition, phosphates, especially sodium phosphates, will exchange with potassium on the surface of the glass in the salt bath to form potassium phosphate. Potassium phosphate has a relatively high melting point and will easily form solid crystals attached to the glass surface, affecting the quality of the glass.

[0007] The use of ion sieves as impurity ion adsorption materials can effectively solve the problems existing in the use of sodium phosphate and / or potassium phosphate as impurity ion removal materials. In the use of salt baths, the free alkali metal cations in the ion sieve network structure are used to exchange ions with impurity ions in the salt bath, so that the impurity ions in the salt bath can diffuse into the ion sieve channel and be selectively absorbed by the ion sieve. The selective ion exchange of the ion sieve and the ion exchange during glass chemical strengthening can be carried out simultaneously, and the ion sieve can be completely free of contact with the glass sample. Summary of the invention

[0008] However, the inventors found during use that the impurity removal effect of the ion sieve material in the prior art is not ideal in a long-term high-temperature salt bath environment. Specifically, after being used in a high-temperature salt bath for a long time, the ion sieve material in the prior art is not only easy to release impurities that affect the surface quality of the glass into the salt bath, such as many small fragments. The small fragments are easy to adhere to the glass surface and affect the apparent quality of the glass product in the salt bath, but also release the impurity ions originally absorbed from the salt bath into the salt bath in reverse, affecting the concentration of impurity ions in the salt bath. In other words, the ion sieve material in the prior art cannot continuously and stably absorb impurity ions in a high-temperature salt bath for a long time.

[0009] In view of the above-mentioned deficiencies in the prior art, the inventors of the present invention have developed a crystallized ion sieve containing a specific crystal phase composition and structure. The crystallized ion sieve has excellent high-temperature stability, is not easy to release impurities that affect the surface quality of the glass into the salt bath, and can continuously and stably absorb impurity ions in a high-temperature salt bath for a long time, thereby ensuring that the concentration of impurity ions in the salt bath meets the requirements of the salt bath for glass strengthening, thereby solving the problem of the ion sieve in the prior art that the impurity removal effect is not ideal after being placed in a high-temperature salt bath for a long time.

[0010] After further in-depth research on the crystallized ion sieve, the inventor unexpectedly discovered that the crystallized ion sieve that meets the specific crystal phase content and heat loss weight will have less impact on the pH of the salt bath after being added to the salt bath than other crystallized ion sieves of the same system. Reducing the impact of the ion sieve material on the pH of the salt bath during use is more conducive to extending the use time of the ion sieve material in the salt bath, because if the ion sieve material has a large impact on the pH of the salt bath during use, it will more easily cause the pH of the salt bath to become strongly alkaline, which will cause the glass to be strengthened in the salt bath to be corroded.

[0011] Based on this, the present invention provides the following technical solutions:

[0012] In the first aspect, a crystallized ion sieve is provided, which contains SiO2, Al2O3 and alkali metal oxides in terms of oxides; the crystallized ion sieve contains nepheline crystal phase, and the content of nepheline crystal phase in the crystallized ion sieve is not less than 45.00wt% calculated based on the total mass of the ion sieve; the crystallized ion sieve has a thermogravimetric analysis weight loss of less than or equal to 1.60% by weight in the range of 30°C to 500°C.

[0013] In some embodiments of the present invention, the nepheline crystal phase includes sodium nepheline crystal phase and / or potassium nepheline crystal phase.

[0014] In some embodiments of the present invention, the nepheline crystal phase includes a sodium nepheline crystal phase; or, the nepheline crystal phase includes a sodium nepheline crystal phase and a potassium nepheline crystal phase.

[0015] In some embodiments of the present invention, the content of the nepheline crystal phase is not less than 50.00 wt%, preferably not less than 60.00 wt%, and more preferably not less than 70.00 wt%.

[0016] In some embodiments of the present invention, the crystallized ion sieve has a thermogravimetric weight loss of less than or equal to 1.50% by weight in the range of 30°C to 500°C; preferably, the crystallized ion sieve has a thermogravimetric weight loss of 0.30% to 1.50% by weight in the range of 30°C to 500°C.

[0017] In some embodiments of the present invention, the crystallized ion sieve includes the following components, calculated as molar percentage of oxides:

[0018] 28.00mol% to 60.00mol% SiO2, preferably 30.00mol% to 55.00mol% SiO2;

[0019] 8.00 mol% to 28.00 mol% Al2O3, preferably 8.00 mol% to 25.00 mol% Al2O3;

[0020] 25.00 mol% to 55.00 mol% of alkali metal oxide, preferably 30.00 mol% to 50.00 mol% of alkali metal oxide.

[0021] In some embodiments of the present invention, in the crystallized ion sieve, the molar percentage of SiO2 is 30.00mol% to 50.00mol%; and / or, the molar percentage of Al2O3 is 10.00mol% to 20.00mol%; and / or, the molar percentage of alkali metal oxide is 35.00mol% to 50.00mol%.

[0022] In some embodiments of the present invention, the alkali metal oxide includes at least one or two of Na2O and K2O.

[0023] In some embodiments of the present invention, the alkali metal oxide does not contain lithium oxide; the alkali metal oxide includes at least Na2O, or the alkali metal oxide includes at least Na2O and K2O.

[0024] In some embodiments of the present invention, the alkali metal oxide comprises 25.00 mol% to 55.00 mol% of Na2O and 0 to 6.00 mol% of K2O, calculated as the molar percentage of the oxide.

[0025] In some embodiments of the present invention, the crystallized ion sieve further comprises the following components, calculated by molar percentage of oxides: 0 to 8.00 mol % of TiO2 and 0 to 12.00 mol % of ZrO2.

[0026] In some embodiments of the present invention, in the crystallized ion sieve, the sum of the molar percentages of TiO2 and ZrO2 is 2.00 mol% to 16.00 mol%.

[0027] In some embodiments of the present invention, the crystallized ion sieve further comprises the following components, calculated as molar percentage of oxides: 0 to 5.00 mol % of P2O5 and 0 to 5.00 mol % of B2O3.

[0028] In some embodiments of the present invention, the crystallized ion sieve is in a granular, sheet-like or porous form; preferably, the crystallized ion sieve is in a granular form; preferably, the particle size of the granular crystallized ion sieve is 1 mm to 10 mm.

[0029] In some embodiments of the present invention, based on the mass of the salt bath, 1 wt% of the crystallized ion sieve is added to a 500°C salt bath containing 90 ppm to 120 ppm of impurity lithium ions and reacted for 24 hours, and the growth rate of the salt bath pH is ≤40.00%.

[0030] In some embodiments of the present invention, based on the mass of the salt bath, the crystallized ion sieve with a mass proportion of 1 wt% is added to a 500°C salt bath containing 90 ppm to 120 ppm of impurity lithium ions and reacted for 24 hours. The absorption rate of the crystallized ion sieve to lithium ions is ≥50.00%.

[0031] In a second aspect, a method for preparing the above-mentioned crystallized ion sieve is provided, comprising the following steps:

[0032] (1) taking the raw materials of each component according to the proportion of the ion sieve component and mixing them uniformly, melting the obtained mixture, and then shaping and cooling the obtained molten liquid to prepare the ion sieve substrate;

[0033] (2) The ion sieve substrate is heat-treated to obtain a crystallized ion sieve; the crystallized ion sieve contains a nepheline crystal phase, and the content of the nepheline crystal phase in the crystallized ion sieve is not less than 45.00wt% based on the total mass of the ion sieve; the crystallized ion sieve has a thermogravimetric weight loss of less than or equal to 1.60% by weight in the range of 30°C to 500°C.

[0034] In some embodiments of the present invention, in step (2), when heat treatment is performed, the heat treatment temperature is 500°C to 900°C, and the heat treatment time is 1h to 6h; and / or, when heat treatment is performed, the heating rate is controlled to be 5°C / min to 15°C / min, preferably the heating rate is 10°C / min.

[0035] In some embodiments of the present invention, in step (1), the molten liquid is rolled or drawn into a sheet-like ion sieve substrate by external force; or, the molten liquid is poured into water and quenched to obtain a granular ion sieve substrate; or, a porous ion sieve substrate is prepared by adding a foaming agent to the molten liquid.

[0036] In a third aspect, an application of the crystallized ion sieve is provided, wherein the crystallized ion sieve is added into a molten salt bath for strengthening glass to adsorb impurity ions in the salt bath.

[0037] In some embodiments of the present invention, the salt bath contains potassium ions and / or sodium ions and / or lithium ions; the temperature of the salt bath is 350°C to 600°C, preferably the temperature of the salt bath is 450°C to 600°C.

[0038] In some embodiments of the present invention, the amount of the crystallized ion sieve used is 0.3 wt% to 5.0 wt% of the salt bath, and preferably the amount of the crystallized ion sieve used is 0.5 wt% to 3.0 wt% of the salt bath.

[0039] In a fourth aspect, a method for manufacturing chemically strengthened glass is provided, comprising:

[0040] The step of adding the crystallized ion sieve to a salt bath; and

[0041] A step of bringing the lithium-containing glass into contact with the salt bath to perform ion exchange.

[0042] In some embodiments of the present invention, the amount of the crystallized ion sieve is 0.3 wt % to 5.0 wt % of the salt bath.

[0043] Compared with the prior art, at least one of the above technical solutions has the following advantages or beneficial effects:

[0044] 1. The present invention unexpectedly discovered a crystallized ion sieve containing a specific crystal phase composition and structure, which has excellent high-temperature stability, can maintain a stable structure in a high-temperature salt bath, is not easy to release impurities that affect the surface quality of the glass into the salt bath, and can maintain the absorption effect of impurity ions in the salt bath, especially impurity lithium ions. Even if it exists in a high-temperature salt bath for a long time, it can still continuously and stably absorb impurity ions in the salt bath. It is precisely because the crystallized ion sieve material of the present invention has the above-mentioned characteristics, that is, it has excellent high-temperature stability, is not easy to release impurities that affect the surface quality of the glass into the salt bath, and can continuously and stably absorb impurity ions in the salt bath. Therefore, when the crystallized ion sieve of the present invention is used for salt bath online purification, even if the ion sieve material is to be added or replaced, it is not necessary to suspend the strengthening process to clean the ion sieve material used in the salt bath, but the newly added crystallized ion sieve material can be directly added to the salt bath, so that the concentration of impurity ions in the salt bath can be ensured to meet the requirements of the salt bath for glass strengthening without affecting production. On this basis, the present invention also unexpectedly found that the crystallized ion sieve that meets the specific crystal phase content and heat loss weight, after being added to the salt bath, has less impact on the pH of the salt bath than other crystallized ion sieves of the same system. Reducing the impact of the ion sieve material on the pH of the salt bath during use is more conducive to extending the use time of the ion sieve material in the salt bath.

[0045] 2. The present invention provides a method for preparing a crystallized ion sieve with high-temperature stability with simple process, low cost and scalable production. The crystallized ion sieve obtained by the preparation method has a stable structure in a high-temperature salt bath and can maintain the absorption effect of impurity ions in the salt bath, thereby ensuring the long-term continuous absorption effect of the ion sieve on impurity ions in the high-temperature salt bath. BRIEF DESCRIPTION OF THE DRAWINGS

[0046] Figure 1 Schematic diagram for comparing the XRD spectra of the ion sieve before and after absorbing lithium ions in Example 1 and Comparative Example 9.

[0047] Figure 2 Schematic diagram for comparing the XRD spectra of the ion sieve before and after absorbing lithium ions in Example 5 and Comparative Example 13.

[0048] Figure 3 Schematic diagram of the change of lithium ion concentration in the salt bath over time in Examples 1 to 5.

[0049] Figure 4 Schematic diagram of the change of lithium ion concentration in the salt bath over time in Comparative Examples 7 to 14.

[0050] Figure 5 The diagram is a schematic diagram of the change in the pH growth rate of the salt bath when the crystallized ion sieves of Examples 1 to 5 and Comparative Examples 1 to 6 are placed in a salt bath.

[0051] Figure 6 The thermogravimetric curves of the crystallized ion sieves of Examples 1 to 5 and Comparative Examples 1 to 6 are shown.

[0052] Figure 7 It is the DSC curve diagram of the ion sieve in Example 1, Comparative Example 1 and Comparative Example 5. DETAILED DESCRIPTION

[0053] The following will be combined with the accompanying drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments. All other embodiments obtained by ordinary technicians in this field based on the present invention belong to the scope of protection of the present invention.

[0054] Unless otherwise specified in specific circumstances, the numerical ranges listed herein include upper and lower limits, as well as all integers and fractions within the range, and are not limited to the specific values ​​listed when defining the range. "And / or" herein is inclusive, for example, "A; and / or B" means only A, or only B, or both A and B.

[0055] As used herein, the language "substantially free of" or "free of" when used to describe constituent components of a composition, batch, melt or article refers to constituent components that have not been actively added or dosed into the composition, batch, melt or article but may be present in small amounts of less than about 0.01% (on an oxide mole basis) as a contaminant and / or due to the inherent degree of uncertainty attributable to any measurement or analytical technique.

[0056] The relevant testing methods involved in the present invention are explained as follows.

[0057] 1. XRD test method

[0058] The ion sieve sample was crushed and ground into a sample with a particle size of less than 75 μm, and the ground sample was tested using an X-ray diffractometer. The XRD test results (RAW format) were then imported into the X-ray diffraction data Rietveld refinement software Jade for fitting and calculation to obtain the crystal phase composition and crystal phase content in the sample. Specifically, the ratio of the fitted crystal phase peak area to the fitted total peak area is the content of the corresponding crystal phase.

[0059] The X-ray diffractometer used in the present invention is Shimadzu XRD_6100, the angle range selected for the test is 2θ=10°~50°, the scanning speed is 6° / min, the working voltage is 40kV, and the working current is 30mA.

[0060] 2. Lithium ion concentration test method

[0061] The concentration of lithium ions in the salt bath was tested using an atomic absorption spectrophotometer AA-6880.

[0062] Specifically, an appropriate amount of molten salt bath of lithium ion concentration to be determined is taken out from the strengthening furnace. After the molten salt bath is cooled, 0.25 g of the cooled solid substance is accurately weighed into a 100 ml glass beaker, and an appropriate amount of deionized water is added to dissolve it. Then, the solution is filtered into a 100 ml volumetric flask with slow filter paper, and 1 ml of hydrochloric acid aqueous solution is added to the volumetric flask (the preparation method of the hydrochloric acid aqueous solution is as follows: according to the volume ratio, high-grade pure 36-38 wt % hydrochloric acid produced by Chongqing Wansheng Chuandong Chemical Group Co., Ltd. is used: deionized water = 1:1, and the hydrochloric acid aqueous solution is prepared by mixing and shaking), and then deionized water is added to the volumetric flask to make up the volume, and after shaking, the concentration of lithium ions in the salt bath is tested using an atomic absorption spectrophotometer using the corresponding standard curve.

[0063] 3. Salt bath pH test method

[0064] Take out an appropriate amount of molten salt bath whose pH is to be measured from the strengthening furnace. After the molten salt bath is cooled, accurately weigh 1.00g of the cooled solid substance into a 50ml beaker, add 10ml of deionized water, and shake until the solid substance is dissolved. Use a pH meter to measure the pH of the resulting solution, which is recorded as the pH of the salt bath. In the present invention, the pH meter can be an existing probe pH meter, such as the Leiji PHS-2F pH meter.

[0065] 4.TGA Thermogravimetric Analysis Test Method

[0066] The ion sieve sample was ground into fine powder and passed through a 200-mesh sieve to obtain a sample, which was placed in a 101-2AB electric blast drying oven at 100°C for 1 hour and then moved to a dryer to cool for 30 minutes. Then 10 mg of the sample was weighed and heated from room temperature to 1100°C at a heating rate of 10°C / min in an environment of 24°C and 42% humidity using a Mettler-Toledo TGA / DSC3+ thermogravimetric and synchronous thermal analyzer. The thermogravimetric analysis weight loss in the range of 30°C to 500°C and the endothermic and exothermic enthalpy values ​​from 30°C to 1100°C were measured.

[0067] In the prior art, an ion sieve is a solid-state complex that does not melt in a salt bath like sodium phosphate, but exists in a molten salt bath in solid form. It uses silicon dioxide as the main network structure, and uses a large amount of alkali metal oxides to provide free oxygen to disconnect Si-O-Si, forming a large amount of non-bridging oxygen Si-O. The network structure of the solid-state complex will exist in the form of chain-like and island-like [SiO4]. Other oxides, such as Al2O3, B2O3, and P2O5, are connected to it through the remaining oxygen to form chain-like and ring-like bodies. In this way, it is possible to ensure that the structure has a certain strength while widening the gap between the network structures. There are a large number of free alkali metal ions in the gaps, which form a three-dimensional ion channel with the chain-like and ring-like network structures in the structure. The diameter of the alkali metal determines the size of the channel, so that specific screening can be achieved, and ions with specific sizes outside the solid-state complex can be selectively absorbed.

[0068] However, during the use of the ion sieve, the inventors of the present invention found that the ion sieve material in the prior art is very prone to crystallization after being used for a long time in a high-temperature salt bath, and this crystallization phenomenon will cause the original structure of the ion sieve to change. After this transformation, the ion sieve is not only easy to release impurities that affect the surface quality of the glass into the salt bath, such as a large number of small fragments. These fragments are easy to adhere to the surface of the glass that is being chemically strengthened in the salt bath, thereby adversely affecting the apparent quality of the glass. What is more unfavorable is that this structural change will also cause the impurity ions that have been absorbed in the ion sieve to be reversely released into the salt bath, causing the concentration of impurity ions in the salt bath to increase, which is very unfavorable to achieve the salt bath impurity removal effect.

[0069] In order to solve the above-mentioned problems found by the inventors and existing in the ion sieves in the prior art, the inventors conducted further research on the ion sieves. The inventors unexpectedly found that the crystallized ion sieves with specific composition and structure have excellent high-temperature stability, can maintain a stable structure in a high-temperature salt bath, are not easy to release impurities that affect the surface quality of the glass into the salt bath, and can maintain the absorption effect of impurity ions in the salt bath, especially impurity lithium ions. Even if they exist in a high-temperature salt bath for a long time, they can still continuously and stably absorb impurity ions in the salt bath.

[0070] On this basis, the inventors of the present invention unexpectedly discovered that the crystallized ion sieve that meets the specific crystal phase content and heat loss weight has less impact on the pH of the salt bath after being added to the salt bath for use than other crystallized ion sieves of the same system. Reducing the impact of the ion sieve material on the pH of the salt bath during use is more conducive to extending the use time of the ion sieve material in the salt bath, because if the ion sieve material has a large impact on the pH of the salt bath during use, it will more easily cause the pH of the salt bath to become strongly alkaline, thereby causing the glass to be strengthened in the salt bath to be corroded.

[0071] The first aspect of the present invention provides a crystallized ion sieve, which contains SiO2, Al2O3 and alkali metal oxides in terms of oxides; the crystallized ion sieve contains nepheline crystal phase, and the content of nepheline crystal phase in the crystallized ion sieve is not less than 45.00wt% calculated based on the total mass of the ion sieve; the crystallized ion sieve has a thermogravimetric analysis weight loss of less than or equal to 1.60% by weight in the range of 30°C to 500°C.

[0072] In some embodiments, the content of the nepheline crystal phase in the crystallized ion sieve is preferably greater than or equal to 50.00 wt%, further preferably greater than or equal to 60.00 wt%, and preferably greater than or equal to 70.00 wt%.

[0073] In some embodiments, the content of the nepheline crystal phase in the crystallized ion sieve is preferably 45.00wt% to 95.00wt%, 45.00wt% to 95.00wt%, 50.00wt% to 95.00wt%, 60.00 to 95.00wt%, 50.00wt% to 86.00wt%, 60.00wt% to 86.00wt%, 60.00wt% to 70.00wt%, 60.00wt% to 80.00wt%, 68.00wt% to 84.00wt%, 6 3.00wt%~77.00wt%, 70.00wt%~90.00wt%, 75.00wt%~85.00wt%, 80.00wt%~90.00wt%; It can also be 45.00wt%, 50.00wt%, 60.00wt%, 65.00wt%, 70.00wt%, 75.00wt%, 80.00wt%, 86.00wt%, 90.00wt%, 95.00wt% or a value within the numerical range formed by any two of the above values ​​as endpoints. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges as long as the ion sieve with the desired performance of the present invention can be obtained. In the present invention, "implementation method" is also "implementation method".

[0074] In some embodiments, the crystallized ion sieve has a thermogravimetric weight loss of less than or equal to 1.60% by weight in the range of 30°C to 500°C, preferably, the crystallized ion sieve has a thermogravimetric weight loss of less than or equal to 1.50% by weight in the range of 30°C to 500°C, and more preferably, the crystallized ion sieve has a thermogravimetric weight loss of 0.30% by weight to 1.50% by weight in the range of 30 to 500°C. In some embodiments, the thermogravimetric weight loss of the crystallized ion sieve in the range of 30 to 500°C can be 1.50% by weight, 1.45% by weight, 1.40% by weight, 1.35% by weight, 1.30% by weight, 1.25% by weight, 1.20% by weight, 1.00% by weight, 0.80% by weight, 0.60% by weight, 0.40% by weight, 0.30% by weight, and all ranges and sub-ranges between the above values.

[0075] The inventors of the present invention have found that when the crystallized ion sieve composed of SiO2, Al2O3 and alkali metal oxides contains a specific content of nepheline crystal phase and satisfies a specific heat loss weight, the crystallized ion sieve can not only maintain a stable state for a long time in a high-temperature salt bath, but also maintain a continuous and stable absorption effect on impurity ions in the salt bath, especially impurity lithium ions. Even if it is placed in a high-temperature salt bath for a long time, the crystallized ion sieve is not easy to release impurities that affect the surface quality of the glass, such as a large number of small fragments, into the salt bath, which can avoid adverse effects on the apparent quality of the glass being chemically strengthened in the salt bath. Moreover, after the crystallized ion sieve is added to the salt bath for use, the effect on the pH of the salt bath will be smaller than that of other crystallized ion sieves of the same system.

[0076] In some embodiments, the nepheline crystal phase includes one or a mixture of sodium nepheline crystal phase (NaAlSiO4) and potassium nepheline crystal phase (KAlSiO4). Preferably, the nepheline crystal phase includes sodium nepheline crystal phase or the nepheline crystal phase includes sodium nepheline crystal phase and potassium nepheline crystal phase.

[0077] The inventors of the present invention have discovered that a crystallized ion sieve containing sodium nepheline crystal phase and / or potassium nepheline crystal phase not only has a more stable structure in a high-temperature salt bath, but can also selectively, long-term and continuously adsorb impurity ions (especially impure lithium ions) in the salt bath, thereby ensuring that the concentration of impurity ions in the salt bath meets the requirements of the salt bath for glass strengthening, and further ensuring that the strengthening effect of the glass during the chemical strengthening process will not be affected by impure alkali metal ions, such as impure lithium ions and impure sodium ions.

[0078] In some embodiments, the crystallized ion sieve includes the following components, calculated as mole percentage of oxides:

[0079] 28.00mol% to 60.00mol% SiO2, preferably 30.00mol% to 55.00mol% SiO2;

[0080] 8.00 mol% to 28.00 mol% Al2O3, preferably 8.00 mol% to 25.00 mol% Al2O3;

[0081] 25.00 mol% to 55.00 mol% of alkali metal oxide, preferably 30.00 mol% to 50.00 mol% of alkali metal oxide.

[0082] The inventors have found that in the crystallized ion sieve provided by the present invention:

[0083] SiO2 is an essential component for forming the framework of the ion sieve network structure, and its content directly affects the structure of the ion sieve, and further affects the stability of the ion sieve network structure and the performance of adsorption performance. Therefore, in order to ensure the stability of the ion sieve network structure and better play the adsorption and impurity removal performance, in the present invention, in terms of mol%, the content of SiO2 is preferably 28.00mol% to 60.00mol%, and more preferably 30.00mol% to 55.00mol%.

[0084] Alkali metal oxide is also a necessary component, and its content will directly affect the structure of the ion sieve, and then affect the selective adsorption effect of the ion sieve on impurity ions and the stability of the ion sieve network structure. If the alkali metal is too little, it is easy to cause the ion sieve to absorb less impurity ions, and if the alkali metal is too much, it is easy to cause the ion sieve to be unable to form, and it is also easy to increase the difficulty of storing the ion sieve. The presence of too much alkali metal is easy to cause the ion sieve to absorb water and hydrolyze during storage, and then cause the ion sieve to be unable to continue to be used. Therefore, in order to ensure better impurity removal effect and structural stability of the ion sieve, in the present invention, in terms of mol%, the content of alkali metal oxide is preferably 25.00mol% to 55.00mol%, and more preferably 30.00mol% to 50.00mol%.

[0085] At the same time, by ensuring the synergistic effect of the network framework components SiO2 and Al2O3 at a specific content, the high-temperature structural stability of the ion sieve can be better maintained, which is beneficial to improving the strain point and Tg point of the ion sieve, and is beneficial to its use in high-temperature environments. Moreover, an appropriate amount of Al2O3 is also beneficial to the formation of aluminum oxide tetrahedrons to widen the network channel, thereby increasing the absorption rate and degree of the ion sieve to the impurity ions, and better exerting the absorption performance of the ion sieve to the impurity ions. Therefore, in the present invention, in terms of mol%, the content of Al2O3 is preferably 8.00mol% to 28.00mol%, and more preferably 8.00mol% to 25.00mol%.

[0086] In some embodiments, the alkali metal oxide does not contain lithium oxide. Because the presence of lithium oxide in the ion sieve will affect the adsorption effect of the ion sieve, especially the effect of the ion sieve on the adsorption of impurity lithium ions, the alkali metal oxide of the present invention does not contain lithium oxide.

[0087] In some embodiments, the alkali metal oxide includes at least one or two of Na2O and K2O; preferably, the alkali metal oxide includes at least Na2O, or the alkali metal oxide includes at least Na2O and K2O. Among them, sodium oxide (Na2O) can provide sodium ions to achieve exchange with impurity lithium ions in the molten salt bath, and then absorb impurity lithium ions in the salt bath. Potassium oxide (K2O) can provide potassium ions to exchange with impurity sodium ions and impurity lithium ions in the salt bath, and then absorb impurity sodium ions and impurity lithium ions in the salt bath. The use of the two is generally selected according to the use scenario. At present, the impurity ions in the lithium aluminum silicate glass strengthening salt bath are mainly lithium ions, so an ion sieve in which the alkali metal oxide is mainly or entirely sodium oxide can be selected. If it is high aluminum silicate glass or substrate glass that only undergoes potassium-sodium exchange, the impurity ions in the strengthening salt bath are mainly sodium ions. At this time, a crystallized ion sieve in which the alkali metal oxide is mainly potassium oxide can be selected.

[0088] In some embodiments, the content of SiO2 can be 28.00mol% to 60.00mol%, 30.00mol% to 50.00mol%, 35.00mol% to 45.00mol%, 30.00mol% to 55.00mol%, 30.00mol% to 40.00mol%, 30.00mol% to 35.00mol%, 28.00mol% to 40.00mol%, 28.00mol% to 50.0 0mol%, 28.00mol% to 35.00mol%, 35.00mol% to 50.00mol%, 35.00mol% to 40.00mol%; it can also be 28.00mol%, 30.00mol%, 35.00mol%, 40.00mol%, 45.00mol%, 50.00mol%, 55.00mol%, 60.00mol% or a value within a numerical range consisting of any two of the above values ​​as endpoints. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges as long as the crystallized ion sieve with the desired performance of the present invention can be obtained.

[0089] In some embodiments, the content of Al2O3 can be 8mol% to 28mol%, 8mol% to 25mol%, 8.00mol% to 10.00mol%, 10.00mol% to 16.00mol%, 10.00mol% to 15.00mol%, 10.00mol% to 20.00mol%, 10.00mol% to 19.00mol%, 10.00mol% to 18.00mol%, 10.00mol% to 17.00mol%; it can also be 8.00mol%, 10.00mol%, 14.00mol%, 15.00mol%, 18.00mol%, 20.00mol%, 24.00mol%, 26.00mol%, 28.00mol% or a value within a numerical range consisting of any two of the above values ​​as endpoints. It should be understood that, in a specific embodiment, any of the above ranges can be combined with any other ranges as long as the crystallized ion sieve having the desired properties of the present invention can be obtained.

[0090] In some embodiments, the content of alkali metal oxide can be 25.00mol% to 55.00mol%, 30.00mol% to 50.00mol%, 35.00mol% to 50.00mol%, 25.00mol% to 45.00mol%, 30.00mol% to 40.00mol%, 30.00mol% to 45.00mol%, 40.00mol% to 45.00mol%, 40.00mol% to 55.00mol%; it can also be 25.00mol%, 30.00mol%, 35.00mol%, 40.00mol%, 45.00mol%, 50.00mol%, 55.00mol% or a value within the numerical range formed by any two of the above values ​​as endpoints. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the crystallized ion sieve with the desired performance of the present invention can be obtained.

[0091] In some embodiments, the alkali metal oxide comprises 25.00 mol % to 55.00 mol % Na2O, calculated as a mole percentage of the oxide.

[0092] In some embodiments, the alkali metal oxide further comprises 0-6.00 mol % K2O, calculated as the mole percentage of the oxide.

[0093] In some embodiments, the content of Na2O can be 25.00mol% to 55.00mol%, 35.00mol% to 50.00mol%, 25.00mol% to 40.00mol%, 25.00mol% to 35.00mol%, 35.00mol% to 40.00mol%, 40.00mol% to 45.00mol%, 45.00mol% to 50.00mol%; it can also be 25.00mol%, 30.00mol%, 35.00mol%, 40.00mol%, 45.00mol%, 50.00mol%, 55.00mol% or a value within the numerical range formed by any two of the above values ​​as endpoints. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the crystallized ion sieve with the desired performance of the present invention can be obtained.

[0094] In some embodiments, the content of K2O can be 0-6.00mol%, 1.00mol%-2.00mol%, 2.00mol%-4.00mol%, 4.00mol%-5.00mol%, 5.00mol%-6.00mol%; it can also be 0, 1.00mol%, 2.00mol%, 3.00mol%, 4.00mol%, 5.00mol%, 6.00mol% or a value within a numerical range consisting of any two of the above values ​​as endpoints. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the crystallized ion sieve with the desired performance of the present invention can be obtained.

[0095] In some embodiments of the present invention, the crystallized ion sieve further includes the following components, calculated by the molar percentage of the oxide: 0-8.00 mol% TiO2 and 0-12.00 mol% ZrO2. The inventors have found that in the crystallized ion sieve formula system provided by the present invention, by adding a specific content of ZrO2 and / or TiO2, it can not only promote the precipitation of crystal nuclei while playing a role in refining the grains, but also help to reduce the production of easily hydrolyzed sodium silicate, reduce the precipitation of alkaline substances during the storage and use of the ion sieve, and also help to increase the decomposition temperature of the ion sieve, and further improve the stability of the ion sieve in a high-temperature salt bath, but too much ZrO2 will reduce the absorption efficiency of the ion sieve for impurity ions. Therefore, in the present invention, in terms of mol%, the content of ZrO2 is preferably 0-12.00 mol%, and the content of TiO2 is preferably 0-8.00 mol%.

[0096] In some embodiments, the content of ZrO2 can be 0-12mol%, 5.00mol%-15.00mol%, 5.00mol%-8.00mol%, 5.00mol%-10.00mol%, 5.00mol%-11.00mol%, 5.00mol%-12.00mol%, 6.00mol%-9.00mol%, 6.00mol%-12.00mol%, 7.00mol%-12.00mol%, 8.00mol%-11.00mol%. %~11.00mol%, 8.00mol%~12.00mol%, 6.00mol%~11.00mol%; it can also be 0, 0.50mol%, 2.00mol%, 3.00mol%, 5.00mol%, 6.00mol%, 7.00mol%, 8.00mol%, 9.00mol%, 10.00mol%, 11.00mol%, 12.00mol% or a value within the numerical range consisting of any two of the above values ​​as endpoints. The content of TiO2 can be 0-8.00mol%, 0-8.00mol%, 0-5.00mol%, 1.00mol%-8.00mol%, 5.00mol%-8.00mol%, 3.00mol%-8.00mol%, 4.00mol%-5.00mol%, 2.00mol%-7.00mol%, 3.50mol%-6.50mol%, 0.50mol%-2.00mol%, 3.00mol%-5.00mol%; it can also be 0, 0.50mol%, 2.00mol%, 3.00mol%, 4.00mol%, 5.00mol%, 6.00mol%, 7.00mol%, 8.00mol% or a value within the numerical range formed by any two of the above values ​​as endpoints. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the crystallized ion sieve with the desired performance of the present invention can be obtained.

[0097] In some embodiments of the present invention, in the crystallized ion sieve, the sum of the molar percentages of TiO2 and ZrO2 is 2.00 mol% to 16.00 mol%.

[0098] In some embodiments, in the crystallized ion sieve, the sum of the molar percentages of TiO2 and ZrO2 can be 2.00mol% to 15.00mol%, 2.00mol% to 12.00mol%, 2.00mol% to 10.00mol%, 2.00mol% to 8.00mol%, 2.00mol% to 5.00mol%, 5.00mol% to 16.00mol%, 8.00mol% to 16.00mol%, 10.00mol% to 16.00mol%, 12.00mol% to 16.00mol%; it can also be 2.00mol%, 5.00mol%, 8.00mol%, 10.00mol%, 12.00mol%, 15.00mol%, 16.00mol% or a value within the numerical range consisting of any two of the above values ​​as endpoints. It should be understood that, in a specific embodiment, any of the above ranges can be combined with any other ranges as long as the crystallized ion sieve having the desired properties of the present invention can be obtained.

[0099] In some embodiments of the present invention, the crystallized ion sieve further comprises the following components, calculated by the molar percentage of the oxide: 0-5.00 mol% P2O5 and 0-5.00 mol% B2O3. The inventors have found that in the crystallized ion sieve formula system provided by the present invention, an appropriate amount of P2O5 and B2O3 is beneficial to reducing the generation of easily hydrolyzed sodium silicate and reducing the precipitation of alkaline substances during the storage and use of the ion sieve.

[0100] In some embodiments, the P2O5 content can be 0-5.00mol%, 0-1.00mol%, 0%-2.00mol%, 1.00mol%-4.00mol%, 1.00mol%-3.00mol%, 1.50mol%-4.50mol%, 2.80mol%-3.70mol%, 1.90mol%-3.50mol%, 1.40mol%-4.90mol%; it can also be 0, 1.00mol%, 2.00mol%, 3.00mol%, 4.00mol%, 5.00mol% or a value within the numerical range consisting of any two of the above values ​​as endpoints. The B2O3 content can be 0-5.00mol%, 0-1.50mol%, 0%-2.50mol%, 1.00mol%-4.00mol%, 1.00mol%-3.00mol%, 1.50mol%-4.50mol%, 2.80mol%-3.70mol%, 1.90mol%-3.50mol%, 1.40mol%-4.90mol%; it can also be 0, 1.00mol%, 2.00mol%, 3.00mol%, 4.00mol%, 5.00mol% or a value within a numerical range consisting of any two of the above values ​​as endpoints. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the crystallized ion sieve with the desired performance of the present invention can be obtained.

[0101] In some embodiments, the crystallized ion sieve is in a granular, sheet or porous form; preferably, the crystallized ion sieve is in a granular form; preferably, the particle size of the granular crystallized ion sieve is 1 mm to 10 mm. The granular crystallized ion sieve is easy to prepare and can fully contact with the salt bath to exert the effect of absorbing impurity ions in the salt bath.

[0102] In some embodiments, the crystallized ion sieve with a mass percentage of 1 wt% is added to a 500°C salt bath containing 90 ppm to 120 ppm of impurity lithium ions for 24 hours, and the growth rate of the salt bath pH is ≤40.00%. In some embodiments, the growth rate of the salt bath pH is 25.00% to 40.00%. In some embodiments, the growth rate of the salt bath pH is 30.00% to 40.00%.

[0103] In some embodiments, based on the mass of the salt bath, the crystallized ion sieve with a mass proportion of 1 wt% is added to a 500°C salt bath containing 90ppm to 120ppm of impurity lithium ions and reacted for 24 hours. The absorption rate of the crystallized ion sieve to lithium ions is ≥50.00%, and preferably, the absorption rate of the crystallized ion sieve to lithium ions is 50.00% to 70.00%.

[0104] The second aspect of the present invention provides a method for preparing the above-mentioned crystallized ion sieve, comprising the following steps:

[0105] (1) taking the raw materials of each component according to the proportion of the ion sieve component and mixing them uniformly, melting the obtained mixture, and then shaping and cooling the obtained molten liquid to prepare the ion sieve substrate;

[0106] (2) The ion sieve substrate is heat-treated to obtain the crystallized ion sieve; the crystallized ion sieve contains nepheline crystal phase, and the content of nepheline crystal phase in the crystallized ion sieve is not less than 45.00wt% based on the total mass of the ion sieve; the crystallized ion sieve has a thermogravimetric weight loss of less than or equal to 1.60% by weight in the range of 30°C to 500°C.

[0107] In some embodiments, in step (2), when heat treatment is performed, the heat treatment temperature is 500°C to 900°C, and the heat treatment time is 1h to 6h; and / or, when heat treatment is performed, the heating rate is controlled to be 5°C / min to 15°C / min.

[0108] In some embodiments, in step (2), when heat treatment is performed:

[0109] The heat treatment temperature may be 500°C to 900°C, 550°C to 800°C, 580°C to 680°C, 600°C to 700°C, 700°C to 800°C, 650°C to 850°C, 590°C to 780°C, 690°C to 850°C, 720°C to 850°C, or 550°C, 600°C, 750°C, 800°C, 900°C, or a value within a numerical range consisting of any two of the above values ​​as endpoints. The heat treatment time may be 1h to 6h, 1h to 5h, 1h to 4h, 2h to 6h, 3h to 6h, 4h to 6h, 2h to 5h, or 1h, 2h, 3h, 4h, 5h, 6h, or a value within a numerical range consisting of any two of the above values ​​as endpoints. The heating rate can be 5°C / min, 6°C / min, 7°C / min, 8°C / min, 9°C / min, 10°C / min, 11°C / min, 12°C / min, 13°C / min, 14°C / min, 15°C / min or a value within a numerical range consisting of any two of the above values ​​as endpoints.

[0110] In some embodiments, in step (1), oxides, carbonates, silicates, phosphates, hydroxides, etc. may be used as raw materials for providing the components.

[0111] It should be understood that when the ion sieve substrate is heat treated, one-step heat treatment can be performed, or two-step or multi-step heat treatment can be performed. If a one-step heat treatment is performed, it means that the nucleation treatment is not performed separately, and the nucleation and target crystal growth are directly performed in a one-step heating process, which can be understood as directly performing a crystallization treatment. If a two-step heat treatment is performed, it means that a two-step heating process is performed, first a nucleation treatment, i.e., a nucleation treatment, is performed, and then a target crystal growth treatment, i.e., a crystallization treatment, is performed. If a multi-step heat treatment is performed, then the nucleation treatment stage and / or the crystallization treatment stage adopts a step-by-step heating method, that is, the entire heat treatment process will be heated multiple times (more than twice).

[0112] In some embodiments, in step (1), the molten liquid is rolled or drawn into a sheet-like ion sieve substrate by external force; or, the molten liquid is poured into water and quenched to obtain a granular ion sieve substrate; or, a porous ion sieve substrate is prepared by adding a foaming agent to the molten liquid.

[0113] According to a third aspect of the present invention, there is provided an application of the crystallized ion sieve described above, wherein the crystallized ion sieve is added into a molten salt bath for strengthening glass to adsorb impurity ions in the salt bath.

[0114] In some embodiments, the salt bath contains potassium ions and / or sodium ions and / or lithium ions; the temperature of the salt bath is 350°C to 600°C, preferably the temperature of the salt bath is 450°C to 600°C. In some embodiments, the temperature of the salt bath can be 350°C to 600°C, 450°C to 600°C, 400°C to 500°C, 460°C to 550°C, 430°C to 580°C, 420°C to 550°C, 430°C to 580°C, 380°C to 500°C; it can also be 380°C, 400°C, 450°C, 500°C, 550°C, 600°C or a value within a numerical range consisting of any two of the above values ​​as endpoints.

[0115] In some embodiments, the amount of the crystallized ion sieve is 0.3 wt% to 5.0 wt% of the salt bath. In some embodiments, the amount of the crystallized ion sieve can be 0.8 wt% to 5.0 wt%, 0.5 wt% to 3.0 wt%, 0.9 wt% to 2.0 wt%, 1.0 wt% to 3.0 wt%, 1.5 wt% to 4.5 wt%, 1.0 wt% to 2.0 wt%, 1.0 wt% to 2.5 wt%, 1.8 wt% to 3.5 wt%, 2.5 wt% to 5.0 wt% of the salt bath; it can also be 0.3 wt%, 0.5 wt%, 1.0 wt%, 2.0 wt%, 2.5 wt%, 3.0 wt%, 3.5 wt%, 4.0 wt%, 4.5 wt%, 5.0 wt% of the salt bath or a value within a numerical range consisting of any two of the above values ​​as endpoints.

[0116] A fourth aspect of the present invention provides a method for manufacturing chemically strengthened glass, comprising:

[0117] The step of adding the crystallized ion sieve to a salt bath; and

[0118] A step of bringing the lithium-containing glass into contact with the salt bath to perform ion exchange.

[0119] In some embodiments, the amount of the crystallized ion sieve is 0.3 wt% to 5.0 wt% of the salt bath. In some embodiments, the amount of the crystallized ion sieve can be 0.8 wt% to 5.0 wt%, 0.5 wt% to 3.0 wt%, 0.9 wt% to 2.0 wt%, 1.0 wt% to 3.0 wt%, 1.5 wt% to 4.5 wt%, 1.0 wt% to 2.0 wt%, 1.0 wt% to 2.5 wt%, 1.8 wt% to 3.5 wt%, 2.5 wt% to 5.0 wt% of the salt bath; it can also be 0.3 wt%, 0.5 wt%, 1.0 wt%, 2.0 wt%, 2.5 wt%, 3.0 wt%, 3.5 wt%, 4.0 wt%, 4.5 wt%, 5.0 wt% of the salt bath or a value within a numerical range consisting of any two of the above values ​​as endpoints.

[0120] Below, the present invention is described by specific embodiments:

[0121] Example 1

[0122] <Preparation of Crystallized Ion Sieve>

[0123] Step 1: Convert the raw materials for ion sieve production into the raw materials according to the design of formula 3 in Table 1, mix the ingredients evenly, transfer the resulting mixture to a platinum crucible, and melt the resulting mixture. Specifically, heat the platinum crucible to 1500°C and keep it warm for 3 hours at this temperature, and stir the resulting mixture until it is molten to form a molten liquid.

[0124] The molten liquid is poured into water at a temperature of 25°C for quenching treatment, and after drying, it is placed in a 101-2AB electric heating blast drying oven at 100°C for 2 hours. After cooling, it is sieved with 16-mesh and 10-mesh metal wire mesh test sieves to obtain a granular ion sieve substrate with a particle size of 1mm to 2mm.

[0125] Step 2: Place the ion sieve substrate obtained in step 1 into a muffle furnace, heat treat it from room temperature to 800°C at a heating rate of 10°C / min for 2 hours, that is, heat treat it to 800°C at a heating rate of 10°C / min and keep it at this temperature for 2 hours, then cool it naturally with the furnace to obtain a crystallized ion sieve material.

[0126] <Application test of crystallized ion sieve>

[0127] The prepared crystallized ion sieve was placed in a molten salt bath at 500°C for testing, and the amount of crystallized ion sieve used was 1.00wt% of the weight of the salt bath. The test lasted up to 32.0 hours, during which the lithium ion concentration and pH value of the salt bath were regularly tested. Before and after the test, the ion sieve was subjected to XRD testing.

[0128] Preparation method of the molten salt bath for the test: Sodium nitrate is taken, and 0.1wt% of lithium nitrate (to provide lithium ions) is added to the sodium nitrate to obtain a mixed salt, and the mixed salt is melted to prepare a molten salt bath for the test. For example, if 1kg of sodium nitrate is taken, 1g of lithium nitrate is added to prepare a molten salt bath.

[0129] Embodiments 2 to 5

[0130] Except for adjusting the formula according to Table 1 and adjusting the relevant preparation parameters according to Table 2, the rest is the same as Example 1.

[0131] Comparative Examples 1-2, 4-6

[0132] Except for adjusting the formula according to Table 1 and adjusting the relevant preparation parameters according to Table 3, the rest is the same as Example 1.

[0133] Comparative Example 3

[0134] <Preparation of ion sieve>

[0135] Step 1: Convert the raw materials for ion sieve production into ingredients according to Formula 6 in Table 1, mix the ingredients evenly, transfer the resulting mixture to a platinum crucible, and melt the resulting mixture. Specifically, heat the platinum crucible to 1500°C and keep it warm for 3 hours at this temperature, and stir the resulting mixture until it is molten to form a molten liquid.

[0136] The molten liquid was poured into water at a temperature of 25°C for quenching treatment. After drying, it was placed in a 101-2AB electric hot air drying oven at 100°C for 2 hours. After cooling, it was sieved with 16-mesh and 10-mesh metal wire woven mesh test sieves to obtain a granular ion sieve substrate with a particle size of 1mm to 2mm. The granular ion sieve substrate is the ion sieve material prepared in Comparative Example 3.

[0137] <Application test of ion sieve>

[0138] The application test method of the ion sieve in Comparative Example 3 is the same as that in Example 1.

[0139] Comparative Examples 7 to 14

[0140] Except for adjusting the formula according to Table 1, the rest is the same as Comparative Example 3.

[0141] Table 1 Crystallized ion sieve formula

[0142]

[0143] Note: The content of each substance in Table 1 is molar percentage, i.e. mol%.

[0144] Table 2 Preparation process and characteristic parameters of crystallized ion sieve in Examples 1 to 5

[0145] Example Example 1 Example 2 Example 3 Example 4 Example 5 Ion Sieve Formula Recipe 3 Recipe 4 Recipe 5 Recipe 9 Recipe 10 Ion sieve form Granular Granular Granular Granular Granular Ion sieve particle size (mm) 1~2 1~2 1~2 1~2 1~2 Heat treatment temperature(℃) 800 800 800 600 600 Heat treatment time (h) 2 2 2 2 2 Heating rate (℃ / min) 10 10 10 10 10 Main crystal phase <![CDATA[NaAlSiO4]]> <![CDATA[NaAlSiO4]]> <![CDATA[NaAlSiO4]]> <![CDATA[NaAlSiO4]]> <![CDATA[NaAlSiO4]]> Main crystalline phase content (wt%) 70.9 79.07 82.8 76.46 87.38 TGA weight loss / % 1.46 1.17 0.73 1.48 1.09

[0146] Table 3 Preparation process and characteristic parameters of crystallized ion sieve in comparative examples 1 to 6

[0147] Comparative Example Comparative Example 1 Comparative Example 2 Comparative Example 3 Comparative Example 4 Comparative Example 5 Comparative Example 6 Ion Sieve Formula Recipe 1 Recipe 2 Recipe 6 Recipe 7 Recipe 8 Recipe 11 Ion sieve form Granular Granular Granular Granular Granular Granular Ion sieve particle size (mm) 1~2 1~2 1~2 1~2 1~2 1~2 Heat treatment temperature(℃) 600 800 / 600 600 600 Heat treatment time (h) 2 2 / 2 2 2 Heating rate (℃ / min) 10 10 / 10 10 10 Main crystal phase <![CDATA[NaAlSiO4]]> <![CDATA[NaAlSiO4]]> <![CDATA[ZrO2]]> <![CDATA[NaAlSiO4]]> <![CDATA[NaAlSiO4]]> <![CDATA[NaAlSiO4]]> Main crystalline phase content (wt%) 51.71 57.43 52.21 50.89 65.42 89.77 TGA weight loss / % 1.93 1.64 1.75 1.91 1.7 3.59

[0148] Note: “ / ” in Table 3 indicates that the corresponding process steps were not performed or the corresponding parameters were not tested; since the ion sieve of Comparative Example 3 experienced crystallization during the melting process, the ion sieve substrate corresponding to its formula was not subjected to heat treatment process, and the ion sieve also contained a large amount of crystalline phase.

[0149] Table 4 Ion sieve preparation process and ion sieve characteristic parameters in Comparative Examples 7 to 14

[0150]

[0151] Table 5 Application test results of crystallized ion sieves in Examples 1 to 5

[0152]

[0153]

[0154] Note: " / " in Table 5 indicates that the corresponding parameter is not tested, and "absorption time" indicates the time the ion sieve is placed in the salt bath. For example, if the absorption time is 1 hour, it means that the ion sieve is placed in the salt bath to absorb lithium ions for 1 hour. The same applies to other embodiments.

[0155] Table 6 Application test results of crystallized ion sieves in comparative examples 1 to 6

[0156]

[0157]

[0158] Note: “ / ” in Table 6 indicates that the corresponding parameter is not tested, and “absorption time” indicates the time the ion sieve is placed in the salt bath. For example, if the absorption time is 1h, it means that the ion sieve is placed in the salt bath to absorb lithium ions for 1h. The same applies to other comparative examples.

[0159] Table 7 Application test results of ion sieves in comparative examples 7 to 14

[0160]

[0161] Note: The "absorption time" in Table 7 indicates the time the ion sieve is placed in the salt bath. For example, if the absorption time is 1 hour, it means that the ion sieve is placed in the salt bath to absorb lithium ions for 1 hour. The same applies to other comparative examples.

[0162] The main crystalline phase of the crystallized ion sieves obtained in Examples 1 to 5 of the present invention is sodium nepheline (NaAlSiO4), and the content of sodium nepheline crystal phase in the crystallized ion sieve is not less than 45.00wt%, and even greater than 70wt%. At the same time, the crystallized ion sieve has a thermogravimetric analysis weight loss of less than or equal to 1.60% by weight in the range of 30°C to 500°C.

[0163] Although the main crystal phase of the ion sieves prepared in Comparative Examples 1-2 and 4-6 is also nepheline, they do not meet the thermal weight loss requirements of the ion sieves required by the present invention. The TGA weight loss of the ion sieves is very high, accounting for more than 1.60%.

[0164] Since the ion sieve of Comparative Example 3 experienced crystallization during the melting process, the ion sieve substrate corresponding to its formula was not subjected to a heat treatment process. The ion sieve also contained a large amount of crystalline phases. The main crystalline phase of the ion sieve was ZrO2, and it did not meet the thermal weight loss requirement of the ion sieve required by the present invention.

[0165] The ion sieves prepared in Comparative Examples 7 to 14 were not subjected to heat treatment. Figure 1 , Figure 2 It can be clearly seen that before use, no obvious crystal precipitation was found in the ion sieves in Comparative Examples 9 and 13, and the XRD spectrum was basically a glass phase bun peak.

[0166] After testing the application, we found that:

[0167] After the crystallized ion sieves prepared in Examples 1 to 5 were used in a high-temperature salt bath at 500°C for more than 24 hours, their structures were basically unchanged, and the main crystal phase was still the sodium nepheline crystal phase. This shows that the crystallized ion sieves prepared in Examples 1 to 5 can maintain structural stability after long-term use in a high-temperature salt bath. The crystallized ion sieves prepared in Examples 1 to 5 also have a long-term and continuous adsorption and removal effect on impurity lithium ions in a high-temperature salt bath. From Tables 5 and Figure 3It can be seen that the concentration of impurity lithium ions in the early salt bath showed a very significant downward trend. Although the decline gradually slowed down with the extension of time, the downward trend always exists. After the crystallized ion sieve was placed in a test salt bath at 500°C for more than 24 hours, its absorption rate of impurity lithium ions remained greater than or equal to 50.00%. This proves that the crystallized ion sieves prepared in Examples 1 to 5 can absorb impurity lithium ions in a high-temperature salt bath for a long time and stably. At the same time, after the crystallized ion sieve is placed in the salt bath, the effect on the pH of the salt bath is small. Even if the crystallized ion sieve is placed in a high-temperature salt bath for 24 hours, the growth rate of the salt bath pH does not exceed 40.00%, which shows that the crystallized ion sieve can be placed in the salt bath for a long time to achieve salt bath purification, and it is more convenient to put it into the salt bath together with the glass to be strengthened, and realize the online purification of the salt bath while the glass is chemically strengthened. The online purification referred to here refers to the impurity ion adsorption treatment (i.e., salt bath purification treatment) of the salt bath while the glass is chemically strengthened.

[0168] The ion sieves prepared in Comparative Examples 1-2 and 4-5 can maintain structural stability after being used in a high-temperature salt bath at 500°C for more than 24 hours, and the main crystal phase is still the sodium nepheline crystal phase, and the impurity lithium ions are absorbed for a long time and continuously, but the effect of the ion sieve on the pH of the salt bath is greater than that of the crystallized ion sieves in Examples 1-5. The main crystal phase of the ion sieve in Comparative Example 3 is ZrO2 crystal. The test results show that such a crystal phase structure is obviously not conducive to the adsorption of impurity lithium ions. Therefore, the adsorption effect of the ion sieve prepared in Comparative Example 3 on impurity lithium ions is not as good as that of the ion sieves prepared in Comparative Examples 1-2 and 4-5, nor as good as that of the crystallized ion sieve prepared in Examples 1-5. At the same time, the effect of the ion sieve in Comparative Example 3 on the pH of the salt bath is also greater than that of the crystallized ion sieve in Examples 1-5. Due to the large weight loss of TGA, the ion sieve in Comparative Example 6 is not only not as good as that of Examples 1-5 in terms of the absorption effect of impurity lithium ions, but also has a much greater effect on pH than the crystallized ion sieves in Examples 1-5.

[0169] From Table 6 and Figure 5 It can be seen that when the crystallized ion sieves in Comparative Examples 1 to 6 are placed in a high-temperature salt bath for 24 hours, the growth rate of the salt bath pH is higher than that of Examples 1 to 5, which indicates that, compared with the crystallized ion sieves in Examples 1 to 5 that meet the requirements of the present invention, the ion sieves in Comparative Examples 1 to 6 are more likely to cause the salt bath pH to increase, and will also cause the salt bath pH to be strongly alkaline more quickly. Therefore, the use time of the ion sieves in Comparative Examples 1 to 6 in the salt bath is obviously not as long as that of the crystallized ion sieves in Examples 1 to 5 of the present invention. This will result in that in actual production use, when the ion sieves in Comparative Examples 1 to 6 are used for salt bath online purification, the number of substrate glass batches that can be strengthened by the salt bath will be reduced, which is less than the case when the crystallized ion sieve of the present invention is used for salt bath online purification.

[0170] The ion sieves prepared in Comparative Examples 7 to 14 were placed in a high-temperature salt bath at 500°C. After 32 hours of use, their structures changed significantly, and a sodium nepheline crystal phase was produced. Figure 4 It can be seen that the ion sieves prepared in Comparative Examples 7 to 14 were placed in a high-temperature salt bath. Although they were able to absorb impurity lithium ions in the salt bath for a short time, causing the concentration of impurity lithium ions in the salt bath to show a downward trend, after the ion sieves were placed in the high-temperature salt bath for more than 16h to 24h, the concentration of impurity lithium ions in the salt bath showed a significant upward trend. This shows that after the ion sieves of Comparative Examples 7 to 14 were placed in a high-temperature salt bath for a long time, they released lithium ions in the reverse direction into the salt bath, and they were unable to achieve long-term, continuous and stable absorption of impurity lithium ions in the high-temperature salt bath.

[0171] After XRD tests were performed on the ion sieves of the embodiment and the comparative example, the XRD test results (RAW format) were first imported into the X-ray diffraction data Rietveld refinement software Jade for fitting, and the crystal phase composition in the sample was obtained. The test result data was then exported from Jade into a txt format, and imported into the origin software, and then smoothed and fitted into an XRD spectrum comparison chart, as shown in FIG. Figures 1-2 . Figures 1-2 The main purpose is to show the structural changes of the ion sieve after a long period of high-temperature salt bath. In order to more intuitively compare the structural changes of the ion sieve before and after absorbing lithium ions, the XRD spectra before and after absorption are placed on the same chart after longitudinal translation. Figures 1-2 The vertical axis in the figure is magnified and does not correspond to a specific value, and does not directly display the crystalline phase content in the ion sieve.

[0172] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the technical solution. Those skilled in the art should understand that those modifications or equivalent substitutions of the technical solution of the present invention that do not depart from the purpose and scope of the technical solution should be included in the scope of the claims of the present invention.

Claims

1. A crystallized ion sieve, characterized in that: The crystallized ion sieve contains SiO2, Al2O3 and alkali metal oxides in terms of oxides; the crystallized ion sieve contains nepheline crystal phase, and the content of the nepheline crystal phase in the crystallized ion sieve is not less than 45.00wt% based on the total mass of the ion sieve; The crystallized ion sieve has a thermogravimetric weight loss of less than or equal to 1.60% by weight in the range of 30°C to 500°C; Calculated by molar percentage of oxides, the crystallized ion sieve includes the following components: 28.00mol%~60.00mol% SiO2, 8.00mol%~28.00mol% Al2O3, 30.00mol%~55.00mol% Na2O, 0~6.00mol% K2O, 0~8.00mol% TiO2, 0~12.00mol% ZrO2, 0~5.00mol% P2O5, 0~4.90mol% B2O3.

2. The crystallized ion sieve according to claim 1, characterized in that: The nepheline crystal phase includes sodium nepheline crystal phase and / or potassium nepheline crystal phase.

3. The crystallized ion sieve according to claim 2, characterized in that: The nepheline crystal phase includes a sodium nepheline crystal phase, or the nepheline crystal phase includes a sodium nepheline crystal phase and a potassium nepheline crystal phase.

4. The crystallized ion sieve according to claim 2, characterized in that: The content of the nepheline crystal phase is not less than 50.00wt%.

5. The crystallized ion sieve according to claim 4, characterized in that: The content of the nepheline crystal phase is not less than 60.00wt%.

6. The crystallized ion sieve according to claim 4, characterized in that: The content of the nepheline crystal phase is not less than 70.00wt%.

7. The crystallized ion sieve according to any one of claims 1 to 6, characterized in that: The crystallized ion sieve has a thermogravimetric weight loss of less than or equal to 1.50% by weight in the range of 30° C. to 500° C.

8. The crystallized ion sieve according to claim 7, characterized in that: The crystallized ion sieve has a thermogravimetric weight loss of 0.30% to 1.50% by weight in the range of 30 to 500° C.

9. The crystallized ion sieve according to any one of claims 1 to 6, characterized in that: Calculated by molar percentage of oxides, the crystallized ion sieve includes the following components: 30.00mol% to 55.00mol% SiO2; and / or, 8.00mol% to 25.00mol% Al2O3; and / or, 30.00mol% to 50.00mol% Na2O; and / or, 0-3.00 mol% K2O; and / or, 0-7.00 mol% TiO2; and / or, 0-7.00 mol% ZrO2; and / or, 0-3.00 mol% P2O5; and / or, 0~2.50mol% B2O3.

10. The crystallized ion sieve according to any one of claims 1 to 6, characterized in that: In the crystallized ion sieve, the molar percentage of Na2O is 39.32mol%~41.1mol%.

11. The crystallized ion sieve according to claim 10, characterized in that: In the crystallized ion sieve, the molar percentage of Na2O is 41.1 mol%, 39.32 mol%, 40.32 mol% or 39.5 mol%.

12. The crystallized ion sieve according to claim 9, characterized in that: In the crystallized ion sieve, the molar percentage of SiO2 is 35.00mol% to 45.00mol%; and / or, The molar percentage of Al2O3 is 10.00mol% to 20.00mol%; and / or, The molar percentage of Na2O is 35.00mol%~50.00mol%.

13. The crystallized ion sieve according to claim 12, characterized in that: In the crystallized ion sieve, the molar percentage of Al2O3 is 10.00mol% to 18.00mol%; and / or, The molar percentage of Na2O is 35.00mol%~45.00mol%.

14. The crystallized ion sieve according to any one of claims 1 to 6, characterized in that: The alkali metal oxide does not contain lithium oxide.

15. The crystallized ion sieve according to any one of claims 1 to 6, characterized in that: In the crystallized ion sieve, the molar percentage of SiO2 is 37.5mol%~40.2mol%.

16. The crystallized ion sieve according to claim 15, characterized in that: In the crystallized ion sieve, the molar percentage of SiO2 is 40.2 mol%, 37.5 mol%, 39.32 mol% or 38.5 mol%.

17. The crystallized ion sieve according to any one of claims 1 to 6, characterized in that: In the crystallized ion sieve, the molar percentage of Al2O3 is 14.7mol%~15.36mol%.

18. The crystallized ion sieve according to claim 17, characterized in that: In the crystallized ion sieve, the molar percentage of Al2O3 is 14.7 mol%, 15.36 mol% or 15 mol%.

19. The crystallized ion sieve according to any one of claims 1 to 6, characterized in that: In the crystallized ion sieve, the sum of the molar percentages of TiO2 and ZrO2 is 2.00 mol% to 16.00 mol%.

20. The crystallized ion sieve according to any one of claims 1 to 6, characterized in that: Calculated by molar percentage of oxides, the crystallized ion sieve includes the following components: 35.00mol% to 45.00mol% SiO2, 10.00mol% to 18.00mol% Al2O3, 35.00mol% to 45.00mol% Na2O, 0 to 2.00mol% P2O5, 0 to 1.50mol% B2O3, 0 to 6.00mol% ZrO2 and 0 to 6.00mol% TiO2; In the crystallized ion sieve, the sum of the molar percentages of TiO2 and ZrO2 is 2.00 mol% to 8.00 mol%.

21. The crystallized ion sieve according to any one of claims 1 to 6, characterized in that: The crystallized ion sieve is in a granular, sheet or porous form.

22. The crystallized ion sieve according to claim 21, characterized in that The crystallized ion sieve is in a granular form.

23. The crystallized ion sieve according to claim 22, characterized in that: The particle size of granular crystallized ion sieve is 1 mm ~10 mm.

24. The crystallized ion sieve according to any one of claims 1 to 6, characterized in that: Calculated based on the mass of the salt bath, 1 wt% of the crystallized ion sieve is added to a 500° C. salt bath containing 90 ppm to 120 ppm of impurity lithium ions and reacted for 24 hours, and the growth rate of the salt bath pH is ≤40.00%.

25. The crystallized ion sieve according to any one of claims 1 to 6, characterized in that: Calculated based on the mass of the salt bath, the crystallized ion sieve with a mass share of 1wt% is added to a 500°C salt bath containing 90ppm~120ppm of impurity lithium ions and reacted for 24 hours. The absorption rate of the crystallized ion sieve to lithium ions is ≥50.00%.

26. A method for preparing a crystallized ion sieve according to any one of claims 1 to 25, characterized in that: The steps include: (1) taking the raw materials of the components according to the proportion of the ion sieve components and mixing them evenly, melting the obtained mixture, and then shaping and cooling the obtained molten liquid to prepare the ion sieve substrate; (2) The ion sieve substrate is heat-treated to obtain a crystallized ion sieve; the crystallized ion sieve contains a nepheline crystal phase, and the content of the nepheline crystal phase in the crystallized ion sieve is not less than 45.00wt% calculated based on the total mass of the ion sieve; the crystallized ion sieve has a thermogravimetric weight loss of less than or equal to 1.60% by weight in the range of 30°C to 500°C.

27. The preparation method according to claim 26, characterized in that: In step (2), when heat treatment is performed, the heat treatment temperature is 500°C to 900°C, and the heat treatment time is 1h to 6h; and / or, when heat treatment is performed, the heating rate is controlled to be 5°C / min to 15°C / min.

28. The preparation method according to claim 27, characterized in that: The heating rate is 10°C / min.

29. The preparation method according to claim 26 or 27, characterized in that: In the step (1), the molten liquid is rolled or drawn by external force into a sheet-like ion sieve substrate; or, the molten liquid is poured into water for quenching to obtain a granular ion sieve substrate; or, a foaming agent is added to the molten liquid to obtain a porous ion sieve substrate.

30. A use of the crystallized ion sieve according to any one of claims 1 to 25, characterized in that: The crystallized ion sieve is added to a molten salt bath for strengthening glass to adsorb impurity ions in the salt bath.

31. The use of the crystallized ion sieve according to claim 30, characterized in that: The salt bath contains potassium ions and / or sodium ions and / or lithium ions; the temperature of the salt bath is 350°C to 600°C.

32. The use of the crystallized ion sieve according to claim 30, characterized in that: The temperature of the salt bath is 450℃~600℃.

33. The use of the crystallized ion sieve according to claim 30 or 31, characterized in that: The amount of the crystallized ion sieve used is 0.3 wt % to 5.0 wt % of the salt bath.

34. The use of the crystallized ion sieve according to claim 33, characterized in that: The amount of the crystallized ion sieve used is 0.5wt% to 3.0wt% of the salt bath.

35. A method for producing chemically strengthened glass, characterized in that: include: The step of adding the crystallized ion sieve according to any one of claims 1 to 25 to a salt bath; and A step of bringing the lithium-containing glass into contact with the salt bath to perform ion exchange.

36. The method for producing chemically strengthened glass according to claim 35, wherein: The amount of the crystallized ion sieve used is 0.3 wt % to 5.0 wt % of the salt bath.

Citation Information

Cited By

  • Sodium ion adsorption material with high stability as well as preparation method and application thereof

    CN122321787A