Reinforced material, preparation method and application thereof, and preparation method of fiber reinforced concrete
By fixing fiber bundle nails and fiber layers with ice, the problems of agglomeration and high void ratio of fiber concrete during the mixing process are solved, the density and strength of fiber-reinforced concrete are improved, and the stability and durability of the structure are ensured.
Patent Information
- Application Number
- CN202410772530.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-14
- Publication Date
- 2024-10-11
AI Technical Summary
During the mixing and vibrating process of existing fiber concrete, the fibers are easy to agglomerate and the dispersion is difficult to maintain, resulting in voids and high void ratio, which hinders the development of heavy-duty, long-span and better performance structures.
Ice is used to fix the fiber bundle nail pins and fiber layers, and the water-soluble load-bearing components are frozen to form reinforcement materials to avoid fiber aggregation and fill in the concrete as fine aggregate to reduce the void ratio.
Maintain the initial dispersion state of fibers, reduce the void ratio of fiber-reinforced concrete, improve strength and durability, ensure normal hydration reaction, and alleviate the problem of chaotic fiber length distribution.
Smart Images

Figure CN118754477A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of building materials, and in particular to a reinforcing material and a preparation method and application thereof, and a preparation method of fiber reinforced concrete. Background Art
[0002] With the gradual shift of my country's industrialization from "high speed" to "high quality" and the proposal of the concept of sustainable development, the volume and quality requirements of concrete have also gradually increased. In the early days, the strength of concrete was improved by adding water reducers and high-activity admixtures to concrete. However, the poor bonding performance, poor toughness and high brittleness between aggregates and cementitious materials in the ordinary high-strength concrete matrix have hindered the development of structures towards heavy, large spans and better structural performance.
[0003] At present, the use of fiber concrete is an important means to improve the brittle characteristics and durability of ordinary concrete, but the fiber distribution has an important influence on fiber concrete. 1. Fibers are prone to agglomeration due to electrostatic adsorption during mixing and vibration; 2. Dispersion is difficult to maintain: some fibers are difficult to maintain a good dispersion state during concrete mixing. During the pouring construction process, the fibers are displaced and redistributed, resulting in voids in the concrete or fiber distribution is different from the design; 3. Higher void ratio: long cut fibers are randomly distributed inside the concrete and interconnected, resulting in more voids. Summary of the invention
[0004] The purpose of the present invention is to provide a reinforcing material and a preparation method and application thereof, and a preparation method of fiber reinforced concrete. The reinforcing material of the present invention avoids agglomeration caused by electrostatic adsorption, can maintain the initial dispersion state in the fiber reinforced concrete and reduce the porosity of the fiber reinforced concrete.
[0005] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0006] The present invention provides a reinforcing material, comprising ice, fiber bundle nails and fiber layers fixed together by ice;
[0007] The mass content of ice in the reinforcing material is 1 to 5%;
[0008] The preparation method of the fiber bundle nail needle comprises the following steps:
[0009] The fiber bundle is formed into a target shape and then fixed with an adhesive to obtain the fiber bundle nail.
[0010] Preferably, the shape of the fiber bundle staple includes one or more of U-shape, T-shape and L-shape.
[0011] Preferably, the shape of the reinforcement material includes a cuboid, and the length of the reinforcement material is 40 to 100 mm, the width is 20 to 200 mm, and the thickness is 0.1 to 1 mm.
[0012] Preferably, the volume content of the fiber layer in the reinforcing material is 1-3%.
[0013] Preferably, the fibers in the fiber bundle staples and the fibers in the fiber layer include silica-modified fibers;
[0014] The length of the fibers in the fiber bundle nails is greater than 6 mm; the length of the fibers in the fiber layer is less than 6 mm.
[0015] The present invention also provides a method for preparing the reinforcing material described in the above technical solution, comprising the following steps:
[0016] The water-soluble load-bearing component with the fiber bundle nails fixed thereon is placed in the fiber dispersion liquid, so that the water-soluble load-bearing component with the fiber bundle nails fixed thereon floats on the surface of the dispersion liquid or is immersed in the dispersion liquid, and then is frozen to obtain the reinforcing material.
[0017] Preferably, the water-soluble supporting component comprises water-soluble paper.
[0018] Preferably, the freezing temperature is -5 to 0°C.
[0019] The present invention also provides the use of the reinforcing material described in the above technical solution or the reinforcing material prepared by the preparation method described in the above technical solution in fiber reinforced concrete.
[0020] The present invention also provides a method for preparing fiber reinforced concrete, comprising the following steps:
[0021] The reinforcing material is laid in the component on which part of the cement mortar has been poured, and the remaining cement mortar is cured after casting to obtain the fiber-reinforced concrete;
[0022] The reinforcing material is the reinforcing material described in the above technical solution or the reinforcing material prepared by the preparation method described in the above technical solution.
[0023] The present invention provides a reinforcing material, comprising ice, fiber bundle nails and fiber layers fixed together by ice;
[0024] The mass content of ice in the reinforcing material is 1 to 5%;
[0025] The preparation method of the fiber bundle nail needle comprises the following steps:
[0026] The fiber bundle is formed into a target shape and then fixed with an adhesive to obtain the fiber bundle nail.
[0027] The present invention fixes the fibers in ice by making fiber bundle nails and fiber layers, without stirring and vibrating with other raw materials of concrete, which not only solves the "clumping" phenomenon of fibers in the matrix caused by the stirring and vibrating process, but also avoids the problem of changes in the dispersion state; and the fiber layer in the ice can also be used as "fine aggregate" to fill the pores of the matrix during the pouring of fiber-reinforced concrete, thereby alleviating the problem of high porosity of fiber-reinforced concrete, increasing the density of the fiber-reinforced concrete matrix, and improving the strength and durability of the fiber-reinforced concrete; in addition, the ice acts as a "water reservoir" inside the fiber-reinforced concrete, ensuring the normal hydration reaction inside the fiber-reinforced concrete, forming an internal curing environment, and at the same time reducing the influence of water generated during the melting of the fiber ice plate on the strength of the fiber-reinforced concrete.
[0028] The invention is not only applicable to regenerated fibers with disordered fiber length distribution, but also applicable to magnetic and non-magnetic fibers.
[0029] Different from the roughening treatment of fiber surface in the existing patents, the fiber bundle nails of the present invention can be "nailed" in the fiber reinforced concrete along the vertical direction, avoiding the problem of easy pulling out of the fibers during the longitudinal tension process.
[0030] The invention utilizes recycled fibers to prepare reinforcing materials, which can promote the reuse of solid waste and achieve sustainable development of resources and environment.
[0031] The layered pouring and laying of fiber bundle nails of the present invention transforms the three-dimensional random distribution of fibers into a two-dimensional surface distribution, which greatly changes the current disorderly status of fibers in fiber-reinforced concrete and makes the distribution of fibers in fiber-reinforced concrete artificially controllable, thereby maximizing the mechanical properties of fibers and maximizing the value of fibers in fiber-reinforced concrete. At the same time, it provides a method for subsequent scientific researchers to study the distribution direction of fibers and their application in large-volume fiber-reinforced concrete. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 is a process flow chart for preparing fiber reinforced concrete in an embodiment of the present invention;
[0033] Figure 2 This is a schematic diagram of a T-shaped regenerated fiber bundle nail needle;
[0034] Figure 3 This is a schematic diagram of an L-shaped regenerated fiber bundle nail needle;
[0035] Figure 4 This is a schematic diagram of a U-shaped regenerated fiber bundle nail needle;
[0036] Figure 5 It is a schematic diagram of the structure of the reinforcement material;
[0037] Figure 6 is the SEM image of the fiber of Comparative Example 1;
[0038] Figure 7 is the SEM image of the fiber of Example 1;
[0039] Figure 8 The infrared spectrum analysis diagram of the fibers of Examples 1 to 9 and Comparative Example 1;
[0040] Fig. 9 It is the force direction diagram of the shear member in Application Example 1 and the schematic diagram of the arrangement of the reinforcement material in the shear member;
[0041] Fig.10 It is the force direction diagram of the bending member in application example 2 and the schematic diagram of the arrangement of the reinforcement material in the bending member;
[0042] Fig.11 It is the force direction diagram of the compressive member in Application Example 3 and the schematic diagram of the arrangement of the reinforcing material in the compressive member. DETAILED DESCRIPTION
[0043] The present invention provides a reinforcing material, comprising ice, fiber bundle nails and fiber layers fixed together by ice;
[0044] The mass content of ice in the reinforcing material is 1 to 5%;
[0045] The preparation method of the fiber bundle nail needle comprises the following steps:
[0046] The fiber bundle is formed into a target shape and then fixed with an adhesive to obtain the fiber bundle nail.
[0047] In the present invention, the shape of the reinforcing material preferably includes a rectangular parallelepiped; the length of the reinforcing material is preferably 40 to 100 mm, more preferably 50 to 90 mm, and further preferably 60 to 80 mm; the width is preferably 20 to 200 mm, more preferably 50 to 150 mm, and further preferably 80 to 120 mm; the thickness is preferably 0.1 to 1 mm, more preferably 0.5 to 0.8 mm; the volume content of the fiber layer is preferably 1 to 3%, more preferably 1.5%.
[0048] In the present invention, the shapes of the fiber bundle nails in one reinforcement material are preferably consistent; the directions of all the fiber bundle nails are preferably consistent; and the spacing between adjacent fiber bundle nails along the length direction of the ice plate is preferably 3 to 5 mm.
[0049] In the present invention, the shape of the fiber bundle nail needle preferably includes one or more of U-type, T-type and L-type. The U-type structure is composed of a curved portion connected by two relatively long parallel side arms, has good lateral and longitudinal stability and uniform force distribution, and has a relatively complex preparation process; the L-type structure has a relatively short side arm, which makes its lateral force stability lower, the force is mainly concentrated in a certain direction, and the preparation process is simple; the T-type structure adds a crossbeam at the other end of the L-type structure, so that it has good lateral and longitudinal stability and a more uniform force distribution.
[0050] In the present invention, the method for preparing the fiber bundle staple needle comprises the following steps:
[0051] The preparation method of the fiber bundle nail needle comprises the following steps:
[0052] The fiber bundle is formed into a target shape and then fixed with an adhesive to obtain the fiber bundle nail.
[0053] In the present invention, the adhesive preferably includes epoxy resin.
[0054] In the present invention, the length of the fibers in the fiber bundle staple is preferably greater than 6 mm; and the length of the fibers in the fiber layer is preferably less than 6 mm.
[0055] In the present invention, the fiber length in the fiber bundle staple and the fiber in the fiber layer preferably include silica-modified fibers; the silica-modified fibers preferably include silica-modified regenerated fibers;
[0056] When the fiber length in the fiber bundle nail and the fiber in the fiber layer are silica-modified regenerated fibers, the method for preparing the fiber length in the fiber bundle nail and the fiber in the fiber layer preferably comprises the following steps:
[0057] removing the epoxy resin on the surface of the regenerated fiber bundle to obtain a regenerated fiber bundle after removal;
[0058] The fiber bundle after removal is mixed with water, a monohydric alcohol solvent, and a ethyl orthosilicate solution, and the pH value of the obtained mixture is adjusted to 9 to 10 for hydrolysis reaction to obtain a modified regenerated fiber bundle;
[0059] The modified fiber bundle is sieved to obtain the fiber bundle and fibers.
[0060] In the present invention, the removal agent preferably includes dichloromethane, formic acid, phenol and sulfuric acid. In the present invention, the volume ratio of dichloromethane, formic acid, phenol and sulfuric acid is preferably 60:25:10:5; the concentration of sulfuric acid is preferably 4 mol / L.
[0061] After the removal, the present invention preferably washes and dries the obtained fiber bundle to obtain the regenerated fiber bundle after the removal.
[0062] In the present invention, the water preferably includes deionized water, which can avoid the influence of ions on the fiber surface and reduce the influence of ions on the fiber surface and the modifier; the monohydric alcohol preferably includes ethanol, and the volume ratio of the water to the tetraethyl orthosilicate solution is preferably 1 to 6:1, more preferably 2 to 5:1, and further preferably 3 to 4:1; the volume ratio of the ethanol to the tetraethyl orthosilicate solution is preferably 50:1. The monohydric alcohol acts as a reaction medium to help the modifier react with the fiber.
[0063] The mass ratio of the removed fiber bundle to TEOS in the tetraethyl orthosilicate solution is preferably 1 to 5:1; the concentration of the tetraethyl orthosilicate solution is preferably 2 to 6 mol / L, more preferably 3 to 5 mol / L.
[0064] In the present invention, the compound for adjusting the pH preferably includes aqueous ammonia.
[0065] In the present invention, the temperature of the hydrolysis reaction is preferably 20-60°C, more preferably 30-50°C; the time is preferably 2-6 hours, more preferably 3-5 hours. The nano-SiO2 particles generated by the hydrolysis reaction are loaded on the regenerated fiber. The nano-SiO2 particles can not only increase the roughness of the regenerated fiber, but also repair the weak points of the regenerated fiber, thereby achieving the purpose of improving the mechanical strength of the regenerated fiber.
[0066] In the present invention, the reinforcing material preferably further comprises a water-soluble load-bearing component, and the fiber bundle nail needle is preferably further fixed on the water-soluble load-bearing component. The fixing is preferably achieved by bonding with a water-soluble glue.
[0067] In the present invention, the fiber bundle staples are preferably fixed to the surface of the water-soluble paper.
[0068] In the present invention, the dissolution time of the water-soluble supporting member is preferably 2 to 3 minutes.
[0069] In the present invention, the water-soluble supporting component preferably includes water-soluble paper; when the water-soluble supporting component is water-soluble paper, the fiber layer is preferably located at the bottom of the water-soluble paper; and the fiber bundle pins are preferably fixed to the upper surface of the water-soluble paper.
[0070] The present invention also provides a method for preparing the reinforcing material described in the above technical solution, comprising the following steps:
[0071] The water-soluble load-bearing component with the fiber bundle nails fixed thereon is placed in the fiber dispersion liquid, so that it floats on the surface of the dispersion liquid or is immersed in the dispersion liquid, and then is frozen to obtain the reinforcing material.
[0072] In the present invention, the method for preparing the fiber dispersion preferably comprises the following steps:
[0073] The fibers are mixed with a phenol-tetrachloroethane fiber dispersion solution for pre-dispersion, and the pre-dispersed fibers are mixed with water.
[0074] In the present invention, the mass ratio of the fiber to the phenol-tetrachloroethane fiber dispersion solution is preferably 2:1; the mass ratio of phenol to tetrachloroethane in the phenol-tetrachloroethane fiber dispersion solution is preferably 3:7.
[0075] Prior to said mixing, the obtained fibers are preferably separated and washed.
[0076] In the present invention, the freezing temperature is preferably -5 to 0°C.
[0077] The preparation process flow chart of the reinforcing material and fiber reinforced concrete according to the embodiment of the present invention is as follows: Figure 1 shown.
[0078] The structure of the reinforcing material of the present invention is as follows Figure 5 Shown: 3-fiber nail needle; 4-water-soluble paper; 5-ice; 6-chopped fiber; 7-reinforcement material.
[0079] The present invention also provides the use of the reinforcing material described in the above technical solution or the reinforcing material prepared by the preparation method described in the above technical solution in fiber reinforced concrete.
[0080] The present invention also provides a method for preparing fiber reinforced concrete, comprising the following steps:
[0081] Laying the reinforcing material in the component where part of the cement mortar has been cast, and curing the remaining cement mortar after casting, to obtain the fiber-reinforced concrete;
[0082] The reinforcing material is the reinforcing material described in the above technical solution or the reinforcing material prepared by the preparation method described in the above technical solution.
[0083] In the present invention, the fluidity of the cement mortar is preferably 200±10 mm. The present invention ensures that the position of the fiber bundle nail pins will not be dislocated when the slurry is poured on the fiber bundle nail pins by adjusting the fluidity of the cement mortar.
[0084] The reinforcing material provided by the present invention, its preparation method and application, and the preparation method of fiber reinforced concrete are described in detail below in conjunction with the embodiments, but they should not be understood as limiting the scope of protection of the present invention.
[0085] Example 1
[0086] The epoxy resin in the regenerated fiber is removed by a remover, washed and then dried; the remover is dichloromethane, formic acid, phenol and sulfuric acid; the volume ratio of dichloromethane, formic acid, phenol and sulfuric acid is 60:25:10:5; the concentration of sulfuric acid is 4 mol / L;
[0087] Put 12mL of deionized water and 100mL of anhydrous ethanol into a three-necked flask containing dried fibers and stir evenly with a high-speed stirrer, then add 2mL of 6mol / L tetraethyl orthosilicate solution, the mass ratio of fiber to tetraethyl orthosilicate in the tetraethyl orthosilicate solution is 3:1, then add ammonia solution dropwise, adjust the pH value to 9-10, and finally stir with a stirring rod for 15min. At a reaction temperature of 20℃, the reaction time is 2h.
[0088] Example 2
[0089] The difference from Example 1 is that the volume of the ethyl orthosilicate solution is 6 mL; the reaction time is 4 h; and the other conditions are the same.
[0090] Example 3
[0091] The difference from Example 1 is that the volume of the ethyl orthosilicate solution is 10 mL; the reaction time is 6 h; and the other conditions are the same.
[0092] Example 4
[0093] The difference from Example 1 is that the reaction temperature is 40° C., the volume of the ethyl orthosilicate solution is 6 mL, the reaction time is 2 h, and the other conditions are the same.
[0094] Example 5
[0095] The difference from Example 1 is that the reaction temperature is 40° C., the volume of the ethyl orthosilicate solution is 10 mL, the reaction time is 4 h, and the other conditions are the same.
[0096] Example 6
[0097] The difference from Example 1 is that the reaction temperature is 40° C., the volume of the ethyl orthosilicate solution is 2 mL, the reaction time is 6 h, and the other conditions are the same.
[0098] Example 7
[0099] The difference from Example 1 is that the reaction temperature is 60° C., the volume of the ethyl orthosilicate solution is 10 mL, the reaction time is 2 h, and the other conditions are the same.
[0100] Example 8
[0101] The difference from Example 1 is that the reaction temperature is 60° C., the volume of the ethyl orthosilicate solution is 2 mL, the reaction time is 4 h, and the other conditions are the same.
[0102] Example 9
[0103] The difference from Example 1 is that the reaction temperature is 60° C., the volume of the ethyl orthosilicate solution is 6 mL, the reaction time is 6 h, and the other conditions are the same.
[0104] Comparative Example 1
[0105] The fiber from which epoxy resin was removed in Example 1.
[0106] Concrete
[0107] 1. Raw materials for concrete preparation: water 180kg / m 3 Maanshan Conch brand P.O32.5 ordinary Portland cement 375kg / m 3 , river sand 738kg / m 3 , stone (continuous grading of 5-10mm melon seed pieces) 1107kg / m 3 , one of the modified fibers of Examples 1 to 9 and the fiber from which epoxy resin is removed in Comparative Example 1;
[0108] Table 1 Parameters of river sand
[0109]
[0110] 2. Compressive strength: The size of concrete is 100mm×100mm×100mm;
[0111] Flexural strength: The dimensions of the concrete are 40mm×40mm×160mm;
[0112] 3. The preparation method of concrete is
[0113] (1) Pour cement, river sand and gravel into a mixing drum with a moist surface and no obvious water accumulation, and stir for 1 minute to uniformly mix the materials in the mixing drum; and quickly add water during the stirring process, and stir for another 3 minutes to fully and uniformly mix the various components of the slurry, and then add 0.3% of the slurry volume of the modified fibers of Examples 1 to 9 and the fibers from which the epoxy resin is removed in Comparative Example 1 (the densities of the modified fibers of Examples 1 to 9 and the fibers from which the epoxy resin is removed in Comparative Example 1 are both 0.036 g / cm 3 );
[0114] (2) After completing the above steps, observe the properties and dryness and wetness of the concrete. If it meets the pouring requirements, the pouring of test blocks can be carried out. The flexural strength and compressive strength of the concrete are measured on the 28th day after the pouring is completed.
[0115] Table 2 Test results of mechanical properties of SiO2 fiber reinforced concrete with recycled fiber surface components
[0116]
[0117] As shown in Table 1, the fiber treated with the reaction temperature of 20°C, the reaction time of 4h and the TEOS volume of 6 mol / L in Example 2 has the best compressive strength and flexural strength.
[0118] The fibers of Comparative Example 1 and Example 1 were subjected to SEM analysis, and the results were as follows: Figures 6-7 As shown. Figures 6-7 It can be seen that the SEM analysis of comparative example 1 shows that there are some obvious microcracks on the fiber surface, which will continue to expand with the increase of temperature, thereby reducing the mechanical strength of the fiber; these microcracks will further reduce the bonding strength of the interface, resulting in an insignificant fiber reinforcement effect. However, the SEM analysis of Example 1 shows that under the catalytic action of ammonia water, TEOS first undergoes a hydrolysis reaction in an aqueous solution. The generated silicic acid and TEOS undergo a condensation reaction to generate siloxane ring oligomers. When the oligomer reaches a certain concentration, nano-SiO2 particles will be generated through a polycondensation reaction; finally, the crystal nucleus continues to grow to form a nano-SiO2 with a three-dimensional network structure, which has the characteristics of small size and uniform particle size distribution. The formed nanoparticles help to repair the microcracks on the fiber surface, thereby significantly improving the fiber reinforcement effect.
[0119] The fibers of Examples 1 to 9 and Comparative Example 1 were analyzed by infrared spectroscopy. The results are as follows: Figure 8 In the figure, N1-9 are examples 1-9, and N0 is comparative example 1.
[0120] Depend on Figure 8 It can be seen that the strength of the Si-O-Si bond functional groups on the surface of the modified regenerated fiber is enhanced, indicating that nano-SiO2 particles have been successfully attached to the surface of the regenerated fiber. With the increase of reaction time, the number and volume of nano-SiO2 particles also increase. These nano-SiO2 particles can not only increase the roughness of the regenerated fiber, but also repair the weak points of the regenerated fiber, thereby achieving the purpose of improving the mechanical strength of the regenerated fiber.
[0121] Preparation of ice plates:
[0122] 1. Preparation of short fiber dispersion:
[0123] The fibers prepared in Example 1 were sieved to obtain long fiber bundles with a length of 10 to 15 mm and short fiber bundles with a length of 0.2 to 0.6 mm;
[0124] The short fibers were mixed with phenol-tetrachloroethane (the mass ratio of phenol to tetrachloroethane fiber was 3:7) for pre-dispersion, and the pre-dispersed fibers were separated, washed with water, and then mixed with water; the mass ratio of the short fibers to the phenol-tetrachloroethane fiber was 2:1; and the volume ratio of the short fibers to water was 1.5%.
[0125] 2. Preparation of fiber nails:
[0126] The long fiber bundle was bent into a U shape (the ratio of the distance between the two arms to the length of the two arms was 1:2) and then fixed with an aqueous epoxy resin to obtain a fiber nail needle.
[0127] The fiber pins were fixed on water-soluble paper using aqueous epoxy resin; the spacing between adjacent fiber bundle pins along the length of the ice plate was 3 mm.
[0128] The obtained water-soluble paper is laid on the fiber dispersion and then frozen to obtain an ice plate.
[0129] Application Example 1
[0130] Under the action of four-point bending, the shear member 9, the longitudinal tensile steel bars 8 are arranged in the tensile zone of the member, and the arrangement of the reinforcing material 7 is as follows Fig. 9 As shown. The U-shaped fiber bundle nails in the reinforcing material are arranged along the pure bending section of the shear member 9 along the beam span direction and parallel to the beam bottom; 2 In the bending shear section of the shear member 9, the arrangement along the plane where the line connecting the loading point and the support is located can reduce the number of stirrups arranged and even eliminate the need to arrange stirrups at equal intervals.
[0131] Application Example 2
[0132] Under the action of uniformly distributed load, the bending member 11 (the member has a distributed load on the entire cross section), the longitudinal stress reinforcement 8 arranged on the entire cross section, the distribution reinforcement 10 and the arrangement of the reinforcement material 7 are as follows: Fig.10 As shown, the U-shaped fiber bundle nails in the reinforcing material are arranged along the span direction of the bending member 11 and parallel to the board surface.
[0133] Application Example 3
[0134] Under the action of axial pressure, the arrangement of the compression member 13 (the member is stressed along the long axis direction), the reinforcing material 7, the longitudinal stress-bearing steel bars 8 arranged inside and the stirrups 12 is as follows: Fig.11 As shown, the U-shaped fiber bundle nails in the reinforcing material are arranged along the height direction of the compression member 13 and parallel to the side.
[0135] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A reinforcing material, characterized in that: including ice, fiber bundles, staples, and fiber layers held together by the ice; The mass content of ice in the reinforcing material is 1 to 5%; The method for preparing the fiber bundle nail needle comprises the following steps: The fiber bundle is formed into a target shape and then fixed with an adhesive to obtain the fiber bundle nail.
2. The reinforcing material according to claim 1, characterized in that The shape of the fiber bundle staple needle includes one or more of U-shape, T-shape and L-shape.
3. The reinforcing material according to claim 1, characterized in that The shape of the reinforcing material includes a rectangular parallelepiped, and the length of the reinforcing material is 40 to 100 mm, the width is 20 to 200 mm, and the thickness is 0.1 to 1 mm.
4. The reinforcing material according to claim 1, characterized in that The volume content of the fiber layer in the reinforcing material is 1-3%.
5. The reinforcing material according to claim 1, characterized in that The fibers in the fiber bundle staples and the fibers in the fiber layer include silica-modified fibers; The length of the fibers in the fiber bundle nails is greater than 6 mm; the length of the fibers in the fiber layer is less than 6 mm.
6. The method for preparing the reinforcing material according to any one of claims 1 to 5, characterized in that: The following steps are involved: The water-soluble load-bearing component with the fiber bundle nails fixed thereon is placed in the fiber dispersion liquid, so that the water-soluble load-bearing component with the fiber bundle nails fixed thereon floats on the surface of the dispersion liquid or is immersed in the dispersion liquid, and then is frozen to obtain the reinforcing material.
7. The preparation method according to claim 6, characterized in that: The water-soluble supporting member includes water-soluble paper.
8. The preparation method according to claim 6, characterized in that: The freezing temperature is -5 to 0°C.
9. Use of the reinforcing material according to any one of claims 1 to 5 or the reinforcing material prepared by the preparation method according to any one of claims 6 to 8 in fiber reinforced concrete.
10. A method for preparing fiber reinforced concrete, characterized in that: The following steps are involved: Laying the reinforcing material in the component that has been partially poured with cement mortar, and curing the remaining cement mortar after pouring, to obtain the fiber-reinforced concrete; The reinforcing material is the reinforcing material according to any one of claims 1 to 5 or the reinforcing material prepared by the preparation method according to any one of claims 6 to 8.
Citation Information
Cited By
Method for improving performance of concrete member by using freezing enhancement unit and prepared concrete member
CN119897938A
A method for improving the performance of a concrete member using a freeze enhancement unit and a concrete member produced thereby
CN119897938B