Slow-release air entraining agent based on nano material and preparation method and application of slow-release air entraining agent

By using a combination of nano-calcium carbonate and polyethylene glycol-b-polyaspartic acid in concrete to form nanomicelles or nanoparticles, the problem of uneven pore distribution caused by air-entraining agents is solved, and the mechanical properties of concrete are improved. Strength and freeze-thaw durability, achieving uniform and stable pore distribution and reducing production costs.

CN118754499AActive Publication Date: 2024-10-11SHIJIAZHUANG CHANGAN YUCAI BUILDING MATERIALS +1
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411253062.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-09
Publication Date
2024-10-11
Estimated Expiration
2044-09-09

AI Technical Summary

Technical Problem

Existing air-entraining agents cause uneven distribution of pores in concrete, affecting the mechanical properties and durability of concrete, and generate too many or uneven bubbles, affecting the freeze-thaw durability of concrete.

Method used

A slow-release air-entraining agent based on nanomaterials is used to form nanomicelles or nanoparticles through the combination of nanometer calcium carbonate particles and polyethylene glycol-b-polyaspartic acid, which promotes the cement hydration reaction and releases surfactants. , to achieve uniform and stable pore distribution.

Benefits of technology

It achieves uniform, fine and stable pore distribution in concrete, improves the mechanical strength and freeze-thaw durability of concrete, and at the same time reduces production costs and preparation complexity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention provides a slow-release air entraining agent based on a nano material as well as a preparation method and application of the slow-release air entraining agent, and belongs to the technical field of building materials. The slow-release air entraining agent based on the nanometer material comprises the following raw materials in parts by weight: 10-40 parts of carbonate, 10-20 parts of calcium salt, 2-3 parts of a dispersing agent, 2-3 parts of a surfactant and 0.02-0.05 part of a stabilizer, calcium carbonate in the slow-release air entraining agent exists in a nanometer size, and the air entraining agent is uniformly dispersed in fresh concrete cement mortar. According to the present invention, the effective time of the stable bubbles in the cement mortar is maximized, the uniform, fine and stable pores can be introduced, the nano calcium carbonate is gradually etched in the concrete, the cement hydration reaction is promoted, the mechanical strength of the hardened cement mortar is improved, the cost is low, and the preparation process is simple.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of building materials, and in particular relates to a slow-release air-entraining agent based on nanomaterials and a preparation method and application thereof. Background Art

[0002] In recent years, the durability of concrete has received considerable attention in the construction industry. Introducing uniform, small, and stable pores into fresh concrete can effectively improve the freeze-thaw durability of concrete. Air-entraining agent is an important concrete admixture that can intentionally create some effective voids in concrete and is also beneficial to concrete in other ways, such as reducing air permeability and improving the workability of fresh concrete.

[0003] Air-entraining agent is a surfactant with an amphiphilic structure. It has a strong tendency to aggregate around the water-air interface, which can enhance the stability of the liquid film and improve the foaming ability of the solution. There are many factors that lead to the inability of air-entraining agent to entrain bubbles in new concrete, such as the adsorption of high-valent metal cations and air-entraining agent on inorganic materials, or the bubbles generated by the air-entraining agent cannot be evenly dispersed in the concrete, resulting in uneven distribution of pores inside the concrete, affecting the mechanical properties and durability of the concrete, or the air-entraining agent generates bubbles too quickly, resulting in too many bubbles, thus affecting various aspects of the concrete performance. Summary of the invention

[0004] In order to solve the above technical problems, the present invention proposes a slow-release air-entraining agent based on nanomaterials and a preparation method and application thereof. The present invention has low cost and simple preparation process. The slow-release air-entraining agent has opened up a new strategy for the use of carbonates in concrete at the nanoscale, which can not only introduce uniform, small and stable pores into fresh concrete, but also gradually etch nano calcium carbonate in the concrete, thereby promoting cement hydration reaction and improving the mechanical strength of hardened cement mortar.

[0005] To achieve the above object, the present invention provides the following technical solutions: A slow-release air-entraining agent based on nanomaterials, comprising the following raw materials in parts by weight: 10-40 parts of carbonate, 10-20 parts of calcium salt, 2-3 parts of dispersant and 0.02-0.05 parts of stabilizer; The dispersant is polyethylene glycol-b-polyaspartic acid.

[0006] Furthermore, the preparation method of polyethylene glycol-b-polyaspartic acid comprises the following steps: The initiator and the ring-opening polymerization agent are dissolved in anhydrous dimethylformamide under nitrogen conditions, polymerized at 30-50°C for 80-120 minutes, the mixture is precipitated into ether, vacuum dried at room temperature and then placed in trifluoroacetic acid, HBr is then added and stirred at 30-40°C, and precipitated into excess ether, the precipitate is dissolved with anhydrous dimethylformamide, and dialyzed with deionized water to remove small molecular impurities, and then the crude product in the dialysis bag is collected, the pH of the crude product is adjusted to 7-8 with sodium hydroxide, and freeze-dried to obtain a white powder, namely polyethylene glycol-b-polyaspartic acid.

[0007] As an amphiphilic polymer, polyethylene glycol-b-polyaspartic acid has both the hydrophilicity of polyethylene glycol and the dispersibility of aspartic acid. This amphiphilicity enables polyethylene glycol-b-polyaspartic acid to form nano micelles or nanoparticles in aqueous solution. These nanostructures can be used as dispersants for nano calcium carbonate particles. The synergistic effect of polyethylene glycol and polyaspartic acid in the polyethylene glycol-b-polyaspartic acid molecular chain can significantly enhance the dispersibility of nano calcium carbonate particles. Polyethylene glycol provides steric hindrance and hydrophilicity, while polyaspartic acid provides dispersibility and chelation. The two work together to enable nano calcium carbonate particles to remain highly dispersed and stable in aqueous solution.

[0008] Furthermore, in the preparation method of polyethylene glycol-b-polyaspartic acid, the initiator is one of alkynyl-polyethylene glycol-amino and methoxy polyethylene glycol amine. The ring-opening polymer is γ-benzyl-L-glutamic acid-N-carboxylic anhydride.

[0009] Furthermore, in the preparation method of polyethylene glycol-b-polyaspartic acid, the molar ratio of the initiator to the ring-opening polymerization agent is 1: (30-40).

[0010] Furthermore, the carbonate is one or more of sodium carbonate, potassium carbonate and ammonium carbonate.

[0011] Furthermore, the calcium salt is calcium nitrate tetrahydrate or calcium chloride.

[0012] Furthermore, the stabilizer is one or more of guar gum, xanthan gum and weinberg gum.

[0013] The stabilizer molecular chain contains a large number of hydrophilic groups such as hydroxyl groups. During the self-assembly process of nano-calcium carbonate, the stabilizer molecules can interact with calcium ions or other active sites on the surface of nano-calcium carbonate particles through these hydrophilic groups, such as hydrogen bonds, electrostatic attraction, etc., and thus adsorb on the surface of nano-calcium carbonate particles. This adsorption allows the stabilizer to form a uniform coating on the surface of nano-calcium carbonate particles, occupying a certain spatial position, thereby maintaining the appropriate distance and orderly arrangement between the particles. These small nanoparticles are stacked in an orderly manner, forming a rich mesoporous structure along the surface of the ball, making it an ideal choice for surfactant carriers.

[0014] Furthermore, the raw material also includes 2-3 parts of a surfactant.

[0015] Furthermore, the surfactant is one or more of sodium dodecylbenzene sulfonate, sodium dodecyl sulfate and sodium fatty acid.

[0016] The second technical solution of the present invention: A method for preparing the nanomaterial-based slow-release air-entraining agent comprises the following steps: Weigh each raw material by weight, mix carbonate and deionized water to obtain a carbonate solution, dissolve a dispersant, a surfactant and a calcium salt in deionized water, stir evenly and then add a stabilizer, then continue stirring, then drop the carbonate solution, adjust the pH of the solution to 7-10 during the dropping process, and obtain a nanomaterial-based slow-release air-entraining agent solution after the dropping is completed, vacuum filter the nanomaterial-based slow-release air-entraining agent solution, wash with ethanol, and then dry the solid product overnight to obtain the nanomaterial-based slow-release air-entraining agent powder.

[0017] Furthermore, the pH of the solution is adjusted to 7-10 using 30 wt % dilute hydrochloric acid or 30 wt % calcium hydroxide solution.

[0018] Furthermore, the carbonate solution is prepared by mixing 10-40 parts of carbonate and 60-90 parts of deionized water by weight.

[0019] The third technical solution of the present invention: Application of the nanomaterial-based slow-release air-entraining agent in the preparation of concrete.

[0020] Furthermore, the dosage of the nano-material-based slow-release air-entraining agent is 0.01% of the rubber material.

[0021] Compared with the prior art, the present invention has the following advantages and technical effects: (1) The slow-release air-entraining agent of the present invention has low cost, simple preparation process and requires less production equipment.

[0022] (2) In the present invention, the raw materials carbonate and calcium salt react to generate nano-calcium carbonate. The nano-calcium carbonate air-entraining agent with a certain dispersion stability is uniformly dispersed in the cement mortar of fresh concrete. The nano-calcium carbonate is gradually etched in the concrete, which promotes the cement hydration reaction while continuously releasing the surfactant in the mesopores of the nano-calcium carbonate self-assembly body, thereby maximizing the effectiveness time of stable bubbles in the cement mortar, thereby introducing uniform, small and stable pores into the fresh concrete. DETAILED DESCRIPTION

[0023] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.

[0024] It should be understood that the terms described in the present invention are only for describing special embodiments and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. Each smaller range between the intermediate value in any stated value or stated range and any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.

[0025] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.

[0026] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to those skilled in the art. The present invention description and examples are exemplary only.

[0027] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.

[0028] The embodiment of the present invention provides a slow-release air-entraining agent based on nanomaterials, comprising the following raw materials in parts by weight: 10-40 parts of carbonate, 10-20 parts of calcium salt, 2-3 parts of dispersant, 2-3 parts of surfactant and 0.02-0.05 parts of stabilizer.

[0029] In a preferred embodiment of the present invention, the carbonate is one or more of sodium carbonate, potassium carbonate and ammonium carbonate.

[0030] In a preferred embodiment of the present invention, the calcium salt is calcium nitrate tetrahydrate or calcium chloride.

[0031] In a preferred embodiment of the present invention, the dispersant is polyethylene glycol-b-polyaspartic acid.

[0032] In a preferred embodiment of the present invention, the method for preparing polyethylene glycol-b-polyaspartic acid comprises the following steps: The initiator and the ring-opening polymerization agent are dissolved in anhydrous dimethylformamide under nitrogen conditions, polymerized at 30-50°C for 80-120 minutes, the mixture is precipitated into ether, vacuum dried at room temperature for 24 hours, and then placed in trifluoroacetic acid, and then HBr is added and stirred at 30-40°C for 4-6 hours, and precipitated into excess ether. The precipitate is dissolved with anhydrous dimethylformamide and dialyzed with deionized water for 24 hours to remove small molecular impurities, and then the crude product in the dialysis bag is collected, the pH is adjusted to 7-8 with sodium hydroxide, and freeze-dried to obtain a white powder, which is polyethylene glycol-b-polyaspartic acid.

[0033] Preferably, in the preparation method of polyethylene glycol-b-polyaspartic acid, the initiator is one of alkynyl-polyethylene glycol-amino and methoxy polyethylene glycol amine, and the ring-opening polymer is γ-benzyl-L-glutamic acid-N-carboxylic anhydride.

[0034] Preferably, in the method for preparing polyethylene glycol-b-polyaspartic acid, the molar ratio of the initiator to the ring-opening polymerization agent is 1:(30-40).

[0035] In a preferred embodiment of the present invention, the surfactant is one or more of sodium dodecylbenzene sulfonate, sodium dodecyl sulfate and sodium fatty acid.

[0036] In a preferred embodiment of the present invention, the stabilizer is one or more of guar gum, xanthan gum and weinensis gum.

[0037] The embodiment of the present invention further proposes a method for preparing the nanomaterial-based slow-release air-entraining agent, comprising the following steps: Weigh each raw material by weight, mix carbonate and deionized water to obtain a carbonate solution, dissolve a dispersant, a surfactant and a calcium salt in deionized water, stir evenly and then add a stabilizer, then continue stirring, then drop the carbonate solution, during the dropping process, adjust the pH of the solution to be weakly alkaline, and after the dropping is completed, obtain a nanomaterial-based slow-release air-entraining agent solution, vacuum filter the nanomaterial-based slow-release air-entraining agent solution, wash with ethanol, and then dry the solid product overnight to obtain the nanomaterial-based slow-release air-entraining agent powder.

[0038] In a preferred embodiment of the present invention, the pH of the solution is regulated to 7-10 using 30 wt % dilute hydrochloric acid or 30 wt % calcium hydroxide solution.

[0039] In a preferred embodiment of the present invention, the carbonate solution is prepared by mixing 10-40 parts of carbonate and 60-90 parts of deionized water by weight.

[0040] The raw materials used in the embodiments of the present invention are all commercially available.

[0041] In the embodiments of the present invention, "parts" represent "parts by weight" unless otherwise specified.

[0042] The technical solution of the present invention is further illustrated by the following embodiments.

[0043] Example 1 S1. 2mmol methoxypolyethylene glycol amine and 60mmol γ-benzyl-L-glutamic acid-N-carboxylic anhydride were dissolved in 60mL anhydrous dimethylformamide under nitrogen conditions, polymerized at 40°C for 90min, the mixture was precipitated into diethyl ether, vacuum dried at room temperature for 24h, then placed in 30mL trifluoroacetic acid, and then 30mL HBr was added. The solution was stirred at 40°C for 6h, and then precipitated into excess diethyl ether. The precipitate was dissolved with anhydrous dimethylformamide and dialyzed with deionized water for 24h to remove small molecular impurities, and then the crude product in the dialysis bag was collected, the pH of the crude product was adjusted to 7 with sodium hydroxide solution, and finally freeze-dried to obtain a white powder, namely polyethylene glycol-b-polyaspartic acid; S2. 2 parts of polyethylene glycol-b-polyaspartic acid, 2 parts of sodium lauryl sulfate, and 10 parts of calcium chloride were dissolved in 900 parts of deionized water, dispersed at a speed of 3000 rpm for 10 min, and then 0.02 parts of xanthan gum were added, followed by high-speed dispersion at a speed of 3000 rpm for 30 min, and then a sodium carbonate solution was added dropwise, wherein the sodium carbonate solution was mixed with 20 parts of sodium carbonate and 80 parts of water, and the addition time was 10 min. During the addition process, the pH of the solution was adjusted to 7 with dilute hydrochloric acid, and after the addition was completed, a slow-release air-entraining agent solution based on nanomaterials was obtained; S3. The slow-release air-entraining agent solution obtained in S2 is vacuum filtered, washed with ethanol, and then the solid product is dried at 70°C overnight to obtain a slow-release air-entraining agent powder based on nanomaterials.

[0044] Example 2 S1. 2mmol methoxypolyethylene glycol amine and 60mmol γ-benzyl-L-glutamic acid-N-carboxylic anhydride were dissolved in 60mL anhydrous dimethylformamide under nitrogen conditions, polymerized at 40°C for 90min, the mixture was precipitated into diethyl ether, vacuum dried at room temperature for 24h, then placed in 30mL trifluoroacetic acid, and then 30mL HBr was added. The solution was stirred at 40°C for 6h, and then precipitated into excess diethyl ether. The precipitate was dissolved with anhydrous dimethylformamide and dialyzed with deionized water for 24h to remove small molecular impurities. The crude product in the dialysis bag was then collected, the pH was adjusted to 7 with sodium hydroxide solution, and finally freeze-dried to obtain a white powder, namely polyethylene glycol-b-polyaspartic acid; S2. 2 parts of polyethylene glycol-b-polyaspartic acid, 1 part of sodium dodecyl sulfate, 1 part of sodium dodecylbenzene sulfonate, and 10 parts of calcium chloride were dissolved in 900 parts of deionized water, dispersed at a speed of 3000 rpm for 10 minutes, and then 0.02 parts of xanthan gum were added, followed by high-speed dispersion at a speed of 3000 rpm for 30 minutes, and then a sodium carbonate solution was added dropwise, wherein the sodium carbonate solution was mixed with 20 parts of sodium carbonate and 80 parts of water, and the addition time was 10 minutes. During the addition process, the pH of the solution was adjusted to 7 with dilute hydrochloric acid, and after the addition was completed, a slow-release air-entraining agent solution based on nanomaterials was obtained; S3. The slow-release air-entraining agent solution obtained in S2 is vacuum filtered, washed with ethanol, and then the solid product is dried at 70°C overnight to obtain a slow-release air-entraining agent powder based on nanomaterials.

[0045] Example 3 S1. 2mmol methoxypolyethylene glycol amine and 60mmol γ-benzyl-L-glutamic acid-N-carboxylic anhydride were dissolved in 60mL anhydrous dimethylformamide under nitrogen conditions, polymerized at 40°C for 90min, the mixture was precipitated into diethyl ether, vacuum dried at room temperature for 24h, then placed in 30mL trifluoroacetic acid, and then 30mL HBr was added. The solution was stirred at 40°C for 6h, and then precipitated into excess diethyl ether. The precipitate was dissolved with anhydrous dimethylformamide and dialyzed with deionized water for 24h to remove small molecular impurities. The crude product in the dialysis bag was then collected, the pH was adjusted to 7 with sodium hydroxide solution, and finally freeze-dried to obtain a white powder, namely polyethylene glycol-b-polyaspartic acid; S2. 2 parts of polyethylene glycol-b-polyaspartic acid, 3 parts of sodium lauryl sulfate, and 10 parts of calcium chloride were dissolved in 900 parts of deionized water, dispersed at a speed of 3000 rpm for 10 min, and then 0.02 parts of xanthan gum were added, followed by high-speed dispersion at a speed of 3000 rpm for 30 min, and then a sodium carbonate solution was added dropwise, wherein the sodium carbonate solution was mixed with 20 parts of sodium carbonate and 80 parts of water, and the addition time was 10 min. During the addition process, the pH of the solution was adjusted to 7 with dilute hydrochloric acid, and after the addition was completed, a slow-release air-entraining agent solution based on nanomaterials was obtained; S3. The slow-release air-entraining agent solution obtained in S2 is vacuum filtered, washed with ethanol, and then the solid product is dried at 70°C overnight to obtain a slow-release air-entraining agent powder based on nanomaterials.

[0046] Example 4 S1. 2mmol methoxypolyethylene glycol amine and 60mmol γ-benzyl-L-glutamic acid-N-carboxylic anhydride were dissolved in 60mL anhydrous dimethylformamide under nitrogen conditions, polymerized at 40°C for 120min, the mixture was precipitated into diethyl ether, vacuum dried at room temperature for 24h, then placed in 40mL trifluoroacetic acid, and then 40mL HBr was added. The solution was stirred at 40°C for 6h, and then precipitated into excess diethyl ether. The precipitate was dissolved with anhydrous dimethylformamide and dialyzed with deionized water for 24h to remove small molecular impurities. The crude product in the dialysis bag was then collected, the pH was adjusted to 7 with sodium hydroxide solution, and finally freeze-dried to obtain a white powder, namely polyethylene glycol-b-polyaspartic acid; S2. 2 parts of polyethylene glycol-b-polyaspartic acid, 2 parts of sodium lauryl sulfate, and 10 parts of calcium chloride were dissolved in 900 parts of deionized water, dispersed at a speed of 3000 rpm for 10 min, and then 0.02 parts of xanthan gum were added, followed by high-speed dispersion at a speed of 3000 rpm for 30 min, and then a sodium carbonate solution was added dropwise, wherein the sodium carbonate solution was mixed with 20 parts of sodium carbonate and 80 parts of water, and the addition time was 10 min. During the addition process, the pH of the solution was adjusted to 7 with dilute hydrochloric acid, and after the addition was completed, a slow-release air-entraining agent solution based on nanomaterials was obtained; S3. The slow-release air-entraining agent solution obtained in S2 is vacuum filtered, washed with ethanol, and then the solid product is dried at 70°C overnight to obtain a slow-release air-entraining agent powder based on nanomaterials.

[0047] Example 5 S1. 2mmol methoxypolyethylene glycol amine and 60mmol γ-benzyl-L-glutamic acid-N-carboxylic anhydride were dissolved in 60mL anhydrous dimethylformamide under nitrogen conditions, polymerized at 40°C for 120min, the mixture was precipitated into diethyl ether, vacuum dried at room temperature for 24h, then placed in 40mL trifluoroacetic acid, and then 40mL HBr was added. The solution was stirred at 40°C for 6h, and then precipitated into excess diethyl ether. The precipitate was dissolved with anhydrous dimethylformamide and dialyzed with deionized water for 24h to remove small molecular impurities. The crude product in the dialysis bag was then collected, the pH was adjusted to 7 with sodium hydroxide solution, and finally freeze-dried to obtain a white powder, namely polyethylene glycol-b-polyaspartic acid; S2. 2 parts of polyethylene glycol-b-polyaspartic acid, 2 parts of sodium fatty acid, and 20 parts of calcium nitrate tetrahydrate were dissolved in 900 parts of deionized water, dispersed at a speed of 3000 rpm for 10 min, and then 0.05 parts of guar gum were added, followed by high-speed dispersion at a speed of 3000 rpm for 30 min, and then an ammonium carbonate solution was added dropwise, wherein the ammonium carbonate solution was mixed with 40 parts of ammonium carbonate and 60 parts of water, and the addition time was 10 min. During the addition process, the pH of the solution was regulated to 7 with dilute hydrochloric acid, and a slow-release air-entraining agent solution based on nanomaterials was obtained after the addition was completed; S3. The slow-release air-entraining agent solution obtained in S2 is vacuum filtered, washed with ethanol, and then the solid product is dried at 70°C overnight to obtain a slow-release air-entraining agent powder based on nanomaterials.

[0048] Example 6 S1. 2mmol methoxypolyethylene glycol amine and 60mmol γ-benzyl-L-glutamic acid-N-carboxylic anhydride were dissolved in 60mL anhydrous dimethylformamide under nitrogen conditions, polymerized at 40°C for 120min, the mixture was precipitated into diethyl ether, vacuum dried at room temperature for 24h, then placed in 40mL trifluoroacetic acid, and then 40mL HBr was added. The solution was stirred at 40°C for 6h, and then precipitated into excess diethyl ether. The precipitate was dissolved with anhydrous dimethylformamide and dialyzed with deionized water for 24h to remove small molecular impurities. The crude product in the dialysis bag was then collected, the pH was adjusted to 7 with sodium hydroxide solution, and finally freeze-dried to obtain a white powder, namely polyethylene glycol-b-polyaspartic acid; S2. 2 parts of polyethylene glycol-b-polyaspartic acid, 2 parts of sodium dodecylbenzene sulfonate, and 20 parts of calcium nitrate tetrahydrate were dissolved in 900 parts of deionized water, dispersed at a speed of 3000 rpm for 10 min, and then 0.04 parts of guar gum were added, followed by high-speed dispersion at a speed of 3000 rpm for 30 min, and then potassium carbonate solution was added dropwise, wherein the potassium carbonate solution was mixed with 10 parts of potassium carbonate and 90 parts of deionized water, and the addition time was 10 min. During the addition process, the pH of the solution was adjusted to 7 with dilute hydrochloric acid, and after the addition was completed, a slow-release air-entraining agent solution based on nanomaterials was obtained; S3. The slow-release air-entraining agent solution obtained in S2 is vacuum filtered, washed with ethanol, and then the solid product is dried at 70°C overnight to obtain a slow-release air-entraining agent powder based on nanomaterials.

[0049] Comparative Example 1 The same as Example 1, except that the dispersant polyethylene glycol-b-polyaspartic acid is not added, and the preparation steps are as follows: 2 parts of sodium dodecyl sulfate and 10 parts of calcium chloride are dissolved in 900 parts of deionized water, dispersed at a high speed of 3000 rpm for 10 minutes, and then 0.02 parts of xanthan gum are added, followed by high-speed dispersion at a rotation speed of 3000 rpm for 30 minutes, and then a sodium carbonate solution is added dropwise, wherein the sodium carbonate solution is a mixture of 20 parts of sodium carbonate and 85 parts of water, and the dropping time is 10 minutes. During the dropping process, the pH value of the solution is adjusted to 7 with dilute hydrochloric acid. After the dropping is completed, the solution is vacuum filtered, washed with ethanol, and then the solid product is dried at 70°C overnight to obtain a slow-release air-entraining agent powder.

[0050] Comparative Example 2 The same as Example 1, except that no stabilizer xanthan gum is added, and the preparation steps are as follows: S1. 2mmol methoxypolyethylene glycol amine and 60mmol γ-benzyl-L-glutamic acid-N-carboxylic anhydride were dissolved in 60mL anhydrous dimethylformamide under nitrogen conditions, polymerized at 40°C for 90min, the mixture was precipitated into diethyl ether, vacuum dried at room temperature for 24h, then placed in 30mL trifluoroacetic acid, and then 30mL HBr was added. The solution was stirred at 40°C for 6h, and then precipitated into excess diethyl ether. The precipitate was dissolved with anhydrous dimethylformamide and dialyzed with deionized water for 24h to remove small molecular impurities. The crude product in the dialysis bag was then collected, the pH was adjusted to 7 with sodium hydroxide solution, and finally freeze-dried to obtain a white powder, namely polyethylene glycol-b-polyaspartic acid; S2. 2 parts of polyethylene glycol-b-polyaspartic acid, 2 parts of sodium lauryl sulfate, and 10 parts of calcium chloride were dissolved in 900 parts of deionized water, dispersed at a high speed of 3000 rpm for 10 minutes, and then a sodium carbonate solution was added dropwise, wherein the sodium carbonate solution was mixed with 20 parts of sodium carbonate and 80 parts of water, and the addition time was 10 minutes. During the addition process, the pH of the solution was adjusted to 7 with dilute hydrochloric acid, and after the addition was completed, a slow-release air-entraining agent solution based on nanomaterials was obtained; S3. The slow-release air-entraining agent solution obtained in S2 is vacuum filtered, washed with ethanol, and then the solid product is dried at 70°C overnight to obtain a slow-release air-entraining agent powder based on nanomaterials.

[0051] Comparative Example 3 The same as Example 1, except that the pH of the solution in S2 is regulated to 10.

[0052] Comparative Example 4 Commercially available alkylbenzene sulfonate air-entraining agent (purchased from Henan Kuntai Chemical Products Co., Ltd.).

[0053] Comparative Example 5 The same as Example 1, except that in step S2, 5 parts of polyethylene glycol-b-polyaspartic acid, 2 parts of sodium lauryl sulfate, and 10 parts of calcium chloride are dissolved in 900 parts of deionized water.

[0054] Comparative Example 6 Same as Example 1, except that the same mass of polyethylene glycol-b-polyaspartic acid is replaced by polyaspartic acid.

[0055] Performance Testing 1. Particle size analysis The particle sizes of the sustained-release air-entraining agent powders prepared in Examples 1-6 were measured using a laser particle size analyzer. The results are shown in Table 1.

[0056] Table 1 Particle size of slow-release air-entraining agent powder (nm)

[0057] It can be seen from Table 1 that the slow-release air-entraining agent powders prepared in the embodiments of the present invention are all nanometer-grade and can be evenly dispersed in fresh concrete cement mortar.

[0058] 2. Foam performance analysis The foam height and bubble size of Examples 1-6 and Comparative Examples 1-6 were tested using a dynamic foam analyzer. During the test, the mass concentration of the air entraining agent was 0.1%, the solution was a calcium hydroxide aqueous solution (50 mL, pH = 10), the gas flow rate was 0.2 L / min, the bubbling time was 1.5 min, and the foam heights at the initial, 10 min and 20 min were tested, which were recorded as H0, H1 and H2, respectively. The specific results are shown in Table 2.

[0059] Table 2 Foam performance test results

[0060] As can be seen from Table 2, compared with Comparative Examples 1-6, Examples 1-6 have lower initial foam heights and slower bubble loss rates, which is attributed to the fact that nano-calcium carbonate with a certain dispersion stability can effectively disperse gas molecules and make them evenly distributed in the liquid. This dispersion effect helps to reduce the aggregation and rupture phenomena between bubbles. Comparative Example 1 did not effectively disperse the nano-calcium carbonate because no dispersant was added, causing the nano-calcium carbonate to agglomerate and the surfactant could not be effectively adsorbed. Comparative Example 2 did not add a stabilizer, which caused the nano-calcium carbonate to weaken its dispersibility and disorderly agglomerate, causing the surfactant to be unable to effectively adsorb. Comparative Example 3 caused the solution pH to be too high, causing hydroxide ions to attack the carbonyl carbon atoms in the ester bond or amide bond in polyethylene glycol-b-polyaspartic acid, initiating a hydrolysis reaction, which weakened the dispersibility of nano-calcium carbonate. Comparative Example 5 caused the original dispersion system balance to be destroyed due to the addition of excessive dispersant, resulting in a decrease in the stability of nano-calcium carbonate. In Comparative Example 6, the dispersant was polyaspartic acid, and the poor dispersion effect caused the nano-calcium carbonate to have poor dispersion stability. In Comparative Example 4, conventional alkylbenzene sulfonate air-entraining agent was used instead. Compared with the examples, the slow-release air-entraining agent prepared by the present invention produces more uniform, smaller and more stable bubbles than the commercially available alkylbenzene sulfonate air-entraining agent.

[0061] 2. Mortar air content test The air content of cement mortars of Examples 1-6 and Comparative Examples 1-6 was tested using the method of Standard JGJ / T70 2009 "Standard for Test Methods of Basic Properties of Building Mortars". The water reducer used in the test was polycarboxylic acid water reducer D4, the dosage of which was 0.2% of the adhesive, and the dosage of air entraining agent was 0.01% of the adhesive. The cement used in the test was P•O42.5R cement produced by Esheng Cement Plant, and the sand used was ISO standard sand produced by Xiamen Aisiou Standard Sand Co., Ltd. The mortar mix ratio was: 900g cement, 1450g sand and 324g water. The specific results are shown in Table 3.

[0062] Table 3 Test results of mortar air content

[0063] It can be seen from Table 3 that, compared with Comparative Examples 1-6, Examples 1-6 have finer and more stable bubbles, and the gas content loss in 2 hours does not exceed 0.2%, which indicates that the slow-release air-entraining agent prepared by the present invention has excellent foaming and bubble stabilization capabilities.

[0064] Compared with Example 1, Comparative Examples 1, 3 and 6 have the largest initial bubbles and the fastest 2h gas content loss, exceeding 64%. This is attributed to the failure of nano calcium carbonate to disperse stably under the action of the dispersant, which promotes the disordered agglomeration of nano calcium carbonate and affects the effective adsorption of the surfactant. In Comparative Example 2, no stabilizer xanthan gum was added, and the initial gas content of the prepared mortar was high. After two hours, the gas content loss exceeded 47%, indicating that the stabilizer plays an important role in stabilizing the bubbles and maintaining the stability of the mortar; in Comparative Example 5, excessive dispersant was added, and the gas content loss of the prepared mortar exceeded 40% in 2h, indicating that excessive dispersant cannot improve the stability of the bubbles. In Comparative Example 4, conventional alkylbenzene sulfonate air entraining agent was replaced, and the sustained release effect and stability were inferior to those of the embodiment, indicating that the sustained release air entraining agent powder based on nanomaterials prepared by the present invention has good air entraining capacity and sustained release effect.

[0065] 3. Cement mortar strength test According to the "Test Method for Strength of Cement Mortar" GB / T 17671-2021, the slow-release air-entraining agents obtained in Examples 1-6 and Comparative Examples 1-6 were respectively added as additives to cement mortar, and cubic test blocks were prepared. The blocks were cured for 8h, 1d and 28d under standard curing conditions, and mechanical properties were tested.

[0066] The cement mortar formula is: 900g cement, 1450g sand, 324g water, 1.8g water reducer D4, 0.01% of the air entraining agent, and 72g of accelerator, wherein the accelerator is prepared according to the method in Example 1 of the patent with the authorization announcement number CN 113603384 B.

[0067] The mechanical property test results of cement mortar test blocks prepared using the slow-release air-entraining agents obtained in Examples 1-6 and Comparative Examples 1-6 are shown in Table 4.

[0068] Table 4 Mechanical properties test of cement mortar

[0069] It can be seen from Table 4 that, compared with Comparative Examples 1-6, Examples 1-6 have higher strengths at 8h, 1d and 28d, indicating that the slow-release air-entraining agent prepared by the present invention can also improve the mechanical strength of cement mortar.

[0070] Compared with Example 1, both the early strength and the 28d compressive strength of Comparative Examples 1-2 are significantly reduced, indicating that the dispersant polyethylene glycol-b-polyaspartic acid and the stabilizer affect the air entraining agent by stabilizing the dispersion of nano-calcium carbonate, and play an important role in improving the mechanical properties of cement mortar; the pH of the air entraining agent in Comparative Example 3 was changed during the preparation of the air entraining agent to cause the dispersant to decompose, and the nano-calcium carbonate in Comparative Examples 5 and 6 also had poor dispersibility, causing the air entraining agent to seriously affect the mechanical properties of the cement mortar. In Comparative Example 4, the commercially available air entraining agent used, after being finally applied to the cement mortar, had significantly lower mechanical properties than Example 1, indicating that the quality of the slow-release air entraining agent has a great influence on the mechanical properties of the prepared cement mortar.

[0071] The above are only preferred specific implementations of the present application, but the protection scope of the present application is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed in the present application should be included in the protection scope of the present application. Therefore, the protection scope of the present application should be based on the protection scope of the claims.

Claims

1. A slow-release air-entraining agent based on nanomaterials, It is characterized in that The raw materials include the following parts by weight: 10-40 parts of carbonate, 10-20 parts of calcium salt, 2-3 parts of dispersant and 0.02-0.05 parts of stabilizer; The dispersant is polyethylene glycol-b-polyaspartic acid.

2. The nanomaterial-based slow-release air-entraining agent according to claim 1, It is characterized in that The carbonate is one or more of sodium carbonate, potassium carbonate and ammonium carbonate.

3. The slow-release air-entraining agent based on nanomaterials according to claim 1, It is characterized in that The calcium salt is calcium nitrate tetrahydrate or calcium chloride.

4. The nanomaterial-based slow-release air-entraining agent according to claim 1, It is characterized in that The stabilizer is one or more of guar gum, xanthan gum and weinberg gum.

5. The slow-release air-entraining agent based on nanomaterials according to claim 1, It is characterized in that The raw materials also include 2-3 parts of surfactant.

6. The nanomaterial-based slow-release air-entraining agent according to claim 5, It is characterized in that The surfactant is one or more of sodium dodecylbenzene sulfonate, sodium dodecyl sulfate and sodium fatty acid.

7. A method for preparing the nanomaterial-based slow-release air-entraining agent according to any one of claims 1 to 6, It is characterized in that The following steps are involved: Weigh each raw material by weight, mix carbonate and deionized water to obtain a carbonate solution, dissolve a dispersant, a surfactant and a calcium salt in deionized water, stir evenly and then add a stabilizer, then continue stirring, then drop the carbonate solution, adjust the pH of the solution to 7-10 during the dropping process, and obtain a nanomaterial-based slow-release air-entraining agent solution after the dropping is completed, vacuum filter the nanomaterial-based slow-release air-entraining agent solution, wash with ethanol, and then dry the solid product overnight to obtain the nanomaterial-based slow-release air-entraining agent powder.

8. The method for preparing the slow-release air-entraining agent based on nanomaterials according to claim 7, It is characterized in that The carbonate solution is prepared by mixing 10-40 parts of carbonate and 60-90 parts of deionized water by weight.

9. Use of the nanomaterial-based slow-release air-entraining agent according to any one of claims 1 to 6 in the preparation of concrete.

10. Use of the nanomaterial-based slow-release air-entraining agent in preparing concrete according to claim 9, It is characterized in that The dosage of the nano material-based slow-release air entraining agent is 0.01% of the rubber material.

Citation Information

Patent Citations

  • An ultra-early strength, fluorine-free, alkali-free liquid accelerator and its preparation method

    CN113603384B

  • Triblock PEG-PBLA-PAAPBA polymer and preparation method and application thereof

    CN107446095A

  • Concrete air entraining agent as well as preparation and application thereof

    CN112062500A

  • Slow-release air entraining agent, preparation method thereof and concrete state retaining agent

    CN114873949A