Microbial mineralized steel slag brick wrapped by organic-geopolymer and preparation method of microbial mineralized steel slag brick

By soaking steel slag in microbial liquid to generate CaCO3 and wrapping it with an organic-geopolymer network, the problem of uneven expansion and strength reduction of steel slag is solved, and microbial mineralized steel slag bricks with high stability and excellent mechanical properties are achieved. Suitable for the field of building materials.

CN118754533APending Publication Date: 2024-10-11WUHAN UNIV OF TECH +1
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411001043.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-25
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

During the treatment process, steel slag causes uneven expansion due to hydration reaction, which affects its resource utilization. Existing methods such as natural aging take a long time or increase energy consumption, and cannot effectively suppress expansion and improve strength.

Method used

The steel slag is soaked in a microbial liquid that can induce calcium precipitation to generate CaCO3, which is wrapped with an organic-geopolymer three-dimensional network to prevent moisture reaction, enhance the compactness and strength of the brick, reduce cracks, and improve mechanical properties.

Benefits of technology

It significantly inhibits the uneven expansion of steel slag bricks, improves the stability and mechanical properties, and forms microbial mineralized steel slag bricks with excellent properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004961568760000091
    Figure BDA0004961568760000091
Patent Text Reader

Abstract

The invention provides an organic-geopolymer coated microorganism mineralized steel slag brick and a preparation method thereof, the preparation method comprises the following steps: S1, soaking steel slag in a microorganism bacterium solution with a calcium precipitation inducing effect for a certain time, and then taking out the steel slag; s2, dissolving an organic polymer or a monomer thereof in an aqueous solution of an alkali activator, then adding a silicon-aluminum raw material and the steel slag soaked in the step S1, and uniformly mixing to obtain slurry; and S3, carrying out static pressure molding on the slurry obtained in the step S2, and curing to obtain the organic-geopolymer wrapped microorganism mineralized steel slag brick. The non-uniform expansion of the organic-geopolymer coated microorganism mineralized steel slag brick prepared by the method is obviously inhibited, and the organic-geopolymer coated microorganism mineralized steel slag brick is high in stability and excellent in mechanical property.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of building materials, and in particular to an organic-geopolymer-coated microbial mineralized steel slag brick and a preparation method thereof. Background Art

[0002] Steel slag is a byproduct of the steelmaking process. In my country, the recycling rate of steel slag is only about 30%. Most of the steel slag is disposed of by landfill or pile-up, which has caused many problems such as land occupation and ecological environment pollution. At present, how to deal with steel slag and make resource utilization of steel slag has become an urgent problem to be solved.

[0003] Steel slag contains the main minerals in cement clinker and can be used as aggregate in bricks. However, the f-CaO in steel slag is highly active and will react with water to generate Ca(OH)2, causing local uneven volume expansion and cracking and collapse of the brick body. At present, the main methods to improve the stability of steel slag are natural aging and autoclaving. The natural aging method refers to the natural accumulation of steel slag produced by steelmaking for a period of time after cooling, so that the f-CaO in the steel slag can react with moisture in the air to hydrate, resulting in a decrease in the f-CaO content, thereby solving the problem of uneven expansion of steel slag. However, the natural aging method is time-consuming and ineffective, and cannot be the best choice. The autoclaving method uses steam to accelerate the hydration of f-CaO, which can reduce the expansion rate of steel slag. However, under autoclaving conditions, iron will be in an active state and oxidized to generate Fe2O3 and FeO, which will also cause volume expansion. In addition, the autoclaving method will increase energy consumption and increase production costs. The shortcomings of these methods have restricted the resource utilization of steel slag to varying degrees.

[0004] Therefore, it is necessary to develop a slag converter that can suppress the uneven expansion of slag and improve the strength to a certain extent in order to solve the above problems. Summary of the invention

[0005] In order to solve the problems existing in the background technology, the present invention provides an organic-geopolymer coated microbial mineralized steel slag brick and a preparation method thereof. The uneven expansion of the organic-geopolymer coated microbial mineralized steel slag brick is significantly suppressed, and it has high stability and excellent mechanical properties.

[0006] The technical solution of the present invention to solve the above technical problems is as follows:

[0007] In a first aspect, the present invention provides a method for preparing an organic-geopolymer coated microbial mineralized slag brick, characterized in that it comprises the following steps:

[0008] S1. Soak the steel slag in a microbial solution that induces calcium precipitation, and take it out after soaking for a certain period of time;

[0009] S2. The organic polymer or its monomer is dissolved in an aqueous solution of an alkaline activator, and then the silicon-aluminum raw material and the steel slag soaked in step S1 are added and mixed to obtain a slurry;

[0010] S3. The slurry obtained in step S2 is statically pressed and cured to obtain the organic-geopolymer-coated microbial mineralized steel slag brick.

[0011] The beneficial effects of the present invention are:

[0012] 1) Calcifying microorganisms enter the steel slag and generate CaCO3, which can make the brick more compact and increase the strength of the brick. At the same time, it can also isolate the entry of moisture, thereby inhibiting the uneven expansion of the steel slag;

[0013] 2) The three-dimensional network of organic-geopolymer wrapped around the steel slag. The organic polymer can isolate the steel slag from contact with water and prevent the free calcium oxide from reacting, thereby suppressing the problem of uneven expansion of the steel slag brick. It can also serve as a culture medium for microorganisms, so that the microorganisms can carry out mineralization reactions more fully and lastingly. The introduced geopolymer can play a synergistic role with the organic film. The geopolymer can strengthen the interface strength of the steel slag and solve the problem of reduced strength of the steel slag caused by organic coating. At the same time, the organic matter can be dispersed in the geopolymer to significantly reduce the number and length of microcracks in the geopolymer. The organic matter is bonded to the geopolymer to form a Ca-O-Si bond, which simultaneously improves the performance of the organic matter and the geopolymer, significantly reduces the number and length of cracks in the organic-geopolymer, thereby improving its mechanical properties and increasing fracture toughness.

[0014] According to the above scheme, the microbial bacterial liquid is a Bacillus pasteurianus bacterial liquid, and the microbial bacterial liquid contains urea with a concentration of 1 to 4 mol / L.

[0015] According to the above scheme, the microbial liquid is obtained by inoculating the microbial seed liquid into a new liquid culture medium at a volume fraction of 2% to 10%, and culturing it at 20 to 30° C. and 110 to 150 r / min for 12 to 36 hours.

[0016] According to the above scheme, the microbial culture liquid is a denitrifying bacterial culture liquid, and the microbial culture liquid contains sodium formate and calcium nitrate, and the concentrations thereof are 400-600 g / L and 6-9 g / L, respectively.

[0017] Although the mechanisms of action are different, both Bacillus pasteurianus and denitrifying bacteria can produce CO2 for calcium precipitation with excellent results.

[0018] According to the above scheme, the soaking time in step S1 is 24 to 72 hours, and the soaking temperature is 20 to 40°C.

[0019] Optionally, in step S1, the steel slag is first soaked in an acetic acid solution for pretreatment before being soaked in the microbial solution.

[0020] According to the above scheme, the pretreatment conditions are: the concentration of acetic acid solution is 0.2-2 mol / L, the solid-liquid ratio is 1 g:8-20 ml, the immersion temperature is 40-70°C, and the immersion time is 0.5-2.5 h.

[0021] By soaking the steel slag in an acidic solution, part of the Fe element is dissolved, which can expand the porosity in the steel slag and increase the amount of microorganisms that enter the steel slag during the subsequent microbial soaking process.

[0022] According to the above scheme, in step S2, the organic polymer or its monomer is one or more of sodium polyacrylate, epoxy resin, chitosan or propylamine.

[0023] The alkaline activator is one or more of sodium hydroxide, water glass, potassium hydroxide and sodium aluminate.

[0024] The silicon-alumina raw material is one or more of kaolin, fly ash and slag powder.

[0025] According to the above scheme, in step S2, the mass ratio of the organic polymer or its monomer, the alkali activator, the silicoaluminous raw material, the steel slag and the water is (2-10):(1-5):(10-20):(90-110):(10-20).

[0026] In a second aspect, the present invention provides an organic-geopolymer coated microbial mineralized steel slag brick prepared by the above preparation method.

[0027] The microbial mineralized steel slag brick coated with organic-geopolymer of the present invention has excellent mechanical properties, significantly suppressed uneven expansion and high stability. DETAILED DESCRIPTION

[0028] The principles and features of the present invention are described below in conjunction with specific embodiments. The examples given are only used to explain the present invention and are not used to limit the scope of the present invention.

[0029] It should be noted that in the description of the embodiments of the present application, the description of the term "some specific embodiments" means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same implementation or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.

[0030] In a first aspect, the present invention provides a method for preparing an organic-geopolymer coated microbial mineralized steel slag brick, characterized in that it comprises the following steps:

[0031] S1. Soak the steel slag in a microbial solution that induces calcium precipitation, and take it out after soaking for a certain period of time;

[0032] S2. The organic polymer or its monomer is dissolved in an aqueous solution of an alkaline activator, and then the silicon-aluminum raw material and the steel slag soaked in step S1 are added and mixed to obtain a slurry;

[0033] S3. The slurry obtained in step S2 is statically pressed and cured to obtain the organic-geopolymer-coated microbial mineralized steel slag brick.

[0034] Since the f-CaO in steel slag has high activity and content, it will react with water to generate Ca(OH)2, and the use of steel slag to make bricks will result in uneven volume expansion. The present invention soaks the steel slag in a microbial bacterial solution that has the effect of inducing calcium precipitation, allowing the microorganisms to enter the steel slag. During the soaking and subsequent brick preparation and curing process, the microorganisms can induce the CaO in the steel slag to undergo a mineralization reaction to generate CaCO3; at the same time, the organic polymer or its monomer reacts with the alkali activator and the silicon-aluminum raw material to generate an organic-geopolymer three-dimensional network structure, which is wrapped around the steel slag to form an organic-geopolymer-wrapped microbial mineralized steel slag, which is statically pressed and cured to obtain an organic-geopolymer-wrapped microbial mineralized steel slag brick.

[0035] The beneficial effects of the present invention are:

[0036] 1) Calcifying microorganisms enter the steel slag and generate CaCO3, which can make the brick more compact and increase the strength of the brick. At the same time, it can also isolate moisture from entering, thereby inhibiting the uneven expansion of steel slag bricks;

[0037] 2) The three-dimensional network of organic-geopolymer wrapped around the steel slag. The organic polymer can isolate the steel slag from contact with water and prevent the free calcium oxide from reacting, thereby further suppressing the problem of uneven expansion of the steel slag. It can also serve as a culture medium for microorganisms, so that the microorganisms can carry out mineralization reactions more fully and lastingly. However, due to the low surface strength of the organic film, a flexible layer will be formed on the outside of the steel slag, resulting in a decrease in the surface strength of the material. The introduced geopolymer can play a synergistic role with the organic film. The geopolymer can strengthen the interface strength of the steel slag and solve the problem of reduced strength of the steel slag caused by organic wrapping. At the same time, the organic matter can be dispersed in the geopolymer to significantly reduce the number and length of microcracks in the geopolymer. The organic matter is bonded to the geopolymer to form a Ca-O-Si bond, which simultaneously improves the improvement effect of the organic matter and the geopolymer, significantly reducing the number and length of cracks in the organic-geopolymer, thereby improving its mechanical properties and increasing fracture toughness.

[0038] In some specific embodiments, the microbial culture liquid is a Bacillus pasteurianus culture liquid, and the microbial culture liquid contains urea at a concentration of 1 to 4 mol / L.

[0039] Bacillus pasteurianus uses urea to decompose carbon dioxide and produce CO3 2- , and the free Ca in the slag 2+ Combine to form CaCO3 precipitate.

[0040] Furthermore, the microbial liquid is obtained by inoculating activated Bacillus pasteurianus seed liquid into a new liquid culture medium at a volume fraction of 2% to 10%, and culturing at 20 to 30° C. and 110 to 150 r / min for 12 to 36 hours.

[0041] According to the above scheme, the liquid culture medium of Bacillus pasteurianus is M9 medium, and 1-4 mol / L urea is added.

[0042] In other specific embodiments, the microbial culture liquid is a denitrifying bacterial culture liquid, and sodium formate and calcium nitrate are added to the microbial culture liquid to provide necessary ions for the reaction, the concentration of sodium formate is 400-600 g / L, and the concentration of calcium nitrate is 6-9 g / L.

[0043] The whole reaction process of denitrifying bacteria is mainly divided into five stages. In each stage of the reaction, new substances are generated, which serve as the reaction substrate for the next stage: In the first stage, formate ions (HCOO - )、NO3 - , H + The reaction produces nitrite ions (NO2 - ), H2O, CO2; the second stage, HCOO - With NO2 - , H + React to generate nitric oxide (NO) and CO2; in the third stage, NO combines with HCOO - Produce nitrous oxide (N2O) and CO2; in the fourth stage, N2O continues to react with HCOO - The reaction generates nitrogen (N2) and CO2; the fifth stage is carried out simultaneously with the first four stages. The CO2 generated in the first four stages induces Ca 2+ A precipitate formed.

[0044] According to the above scheme, the microbial liquid is obtained by inoculating the activated denitrifying bacteria seed liquid into a new liquid culture medium at a volume fraction of 2% to 10%, and culturing it at 20 to 30° C. and 110 to 150 r / min for 12 to 36 hours.

[0045] According to the above scheme, the liquid culture medium for denitrifying bacteria is M9 culture medium, and 400-600 g / L sodium formate and 6-9 g / L calcium nitrate are added.

[0046] The above-mentioned denitrifying bacteria include but are not limited to Pseudomonas denitrificans, Paracoccus denitrificans, and Pseudomonas aeruginosa.

[0047] In some specific embodiments, the soaking time in step S1 is 24 to 72 hours, and the soaking temperature is 20 to 40°C.

[0048] In some specific embodiments, the steel slag is pre-treated by being immersed in an acetic acid solution before being immersed in the microbial solution in step S1.

[0049] The pretreatment conditions are as follows: the concentration of the acetic acid solution is 0.2-2 mol / L, the solid-liquid ratio is 1 g:8-20 ml, the soaking temperature is 40-70°C, and the soaking time is 0.5-2.5 h.

[0050] The steel slag is soaked in an acidic solution to dissolve part of the Fe element, expand the porosity in the steel slag, and increase the amount of subsequent microorganisms that can enter.

[0051] In some specific embodiments, in step S2, the organic polymer or its monomer is one or more of sodium polyacrylate, epoxy resin, chitosan or propylamine;

[0052] The alkaline activator is one or more of sodium hydroxide, water glass, potassium hydroxide, and sodium aluminate;

[0053] The silicon-alumina raw material is one or more of kaolin, fly ash and slag powder.

[0054] In some specific embodiments, in step S2, the mass ratio of the organic polymer or its monomer, the alkali activator, the silicoaluminous raw material, the steel slag and the water is (2-10):(1-5):(10-20):(90-110):(10-20).

[0055] In a second aspect, the present invention provides an organic-geopolymer coated microbial mineralized steel slag brick prepared by the above preparation method.

[0056] On the basis of the above-mentioned embodiments, the present invention provides the following specific examples to further illustrate the present invention. It should be understood that these examples are only used to illustrate the present invention and are not intended to limit the scope of the present invention. The experimental methods in the following examples that do not specify specific conditions are usually based on the conditions recommended by the manufacturer. Unless otherwise stated, percentages and parts are calculated by mass. The materials used in the examples can all be purchased through conventional commercial channels.

[0057] Example 1

[0058] The activated Bacillus pasteurianus was inoculated into a liquid culture medium containing 2 mol / L urea at an inoculum amount of 2%, and cultured in a constant temperature culture shaking box at 25°C and 130 r / min for 24 hours to obtain a microbial culture solution. Steel slag with a particle range of 4.75 to 9.5 mm was soaked in a 1 mol / L acetic acid solution with a solid-liquid ratio of 1:10, a soaking temperature of 40 to 70°C, and a soaking time of 0.5 to 2.5 hours, then taken out and soaked in the microbial culture solution for 72 hours, so that the microbial culture solution completely submerged the steel slag and was 2 to 3 cm higher than the steel slag. Add 1 part of chitosan by weight into 5 parts of sodium hydroxide, 10 parts of water glass and 20 parts of water to prepare an alkaline activator, then add 50 parts of mineral powder and 250 parts of soaked steel slag to mix, use a 200mm×100mm×60mm mold, static press molding after 2h demoulding, put it in a sealed bag for curing for 6d, 27d, then remove the sealed bag, immerse it in water for curing for 1d to obtain the treated steel slag brick.

[0059] Stability test method: The above-mentioned steel slag bricks are subjected to an autoclave test to measure the strength loss rate after autoclave.

[0060] Mechanical properties test method: After immersing in water for 1 day, wipe off the water on the surface of the specimen and conduct compressive strength test.

[0061] The 7d and 28d compressive strengths of the steel slag bricks produced in this case are 38.2MPa and 46.5MPa, respectively, and the pressure steam strength loss rate is 9.5%.

[0062] Example 2

[0063] This implementation case is the same as Example 1, except that the slag soaking time is 24 hours.

[0064] The 7d and 28d compressive strengths of the steel slag bricks produced in this case are 33.2MPa and 39.4MPa, respectively, and the pressure steam strength loss rate is 16.2%.

[0065] Example 3

[0066] This embodiment is the same as embodiment 1, except that the microorganism used is Pseudomonas denitrificans, which is a denitrifying bacterium.

[0067] The 7d and 28d compressive strengths of the steel slag bricks produced in this case are 32.4MPa and 37.6MPa, respectively, and the pressure steam strength loss rate is 18.3%.

[0068] Example 4

[0069] This embodiment is the same as Embodiment 1, except that acetic acid is not used to soak the steel slag.

[0070] The 7d and 28d compressive strengths of the steel slag bricks produced in this case are 31.8MPa and 36.7MPa, respectively, and the pressure steam strength loss rate is 12.6%.

[0071] Comparative Example 1

[0072] Instead of using microbial liquid to treat the steel slag, 1 part of chitosan by weight is added to 5 parts of sodium hydroxide, 10 parts of water glass and 20 parts of water to prepare an alkali activator, and then 50 parts of mineral powder are added to mix with 250 parts of steel slag. A 200mm×100mm×60mm mold is used, and the mold is demolded 2 hours after static pressure molding. The brick is placed in a sealed bag and cured for 6 days and 27 days, and the sealed bag is removed. The brick is immersed in water and cured for 1 day to obtain the treated steel slag brick.

[0073] The 7d and 28d compressive strengths of the steel slag bricks prepared in this comparative example are 20.3MPa and 27.9MPa, respectively, and the autoclave strength loss rate is 27.4%.

[0074] Comparative Example 2:

[0075] The activated Bacillus pasteurianus was inoculated in a buffer solution containing 2 mol / L urea at an inoculation rate of 2%, and cultured in a constant temperature culture shaker at 25°C and 130 r / min for 24 hours to obtain a microbial culture solution, and steel slag with a particle range of 4.75 to 9.5 mm was immersed in the steel slag microbial culture solution for 72 hours, so that the microbial culture solution completely submerged the steel slag and was 2 to 3 cm higher than the steel slag. 86 parts of cement were mixed with 250 parts of the soaked steel slag, and a 200mm×100mm×60mm mold was used. After static pressure molding, the mold was demoulded 2 hours later, and the steel slag brick was placed in a sealed bag for curing for 6 days, and the sealed bag was removed after 27 days, and the steel slag brick was immersed in water for curing for 1 day to obtain the treated steel slag brick.

[0076] The 7d and 28d compressive strengths of the steel slag bricks prepared in this comparative example are 23.6MPa and 28.4MPa, respectively, and the autoclave strength loss rate is 26.3%.

[0077] Comparative Example 3:

[0078] The activated Bacillus pasteurianus was inoculated in a buffer solution containing 2 mol / L urea at an inoculation rate of 2%, and cultured in a constant temperature culture shaker at 25°C and 130 r / min for 24 hours to obtain a microbial culture solution, and steel slag with a particle range of 4.75 to 9.5 mm was immersed in the microbial culture solution for 72 hours, so that the microbial culture solution completely submerged the steel slag and was 2 to 3 cm higher than the steel slag. 5 parts of sodium hydroxide, 10 parts of water glass and 20 parts of water were mixed to form an alkali activator, and then 50 parts of mineral powder and 250 parts of steel slag were added to mix, and a mold of 200mm×100mm×60mm was used. After static pressure molding, the mold was demoulded 2 hours later, and the steel slag brick was placed in a sealed bag for curing for 6 days and 27 days, and then the sealed bag was removed, and the steel slag brick was immersed in water for curing for 1 day to obtain the treated steel slag brick.

[0079] The 7d and 28d compressive strengths of the steel slag bricks prepared in this comparative example are 27.6MPa and 35.9MPa, respectively, and the autoclave strength loss rate is 24.4%.

[0080] Comparative Example 4:

[0081] Mix 86 parts of cement with 250 parts of steel slag, use a 200mm×100mm×60mm mold, demould 2 hours after static pressure molding, put it in a sealed bag and cure for 6 days, remove the sealed bag after 27 days, immerse it in water and cure for 1 day to obtain the treated steel slag brick.

[0082] The 7d and 28d compressive strengths of the steel slag bricks prepared in this comparative example are 19.6MPa and 26.9MPa, respectively, and the autoclave strength loss rate is 31.5%.

[0083] The experimental results of the embodiments and comparative examples are shown in Table 1:

[0084]

[0085] It can be seen from the test results in Table 1 that the steel slag bricks prepared by this method can not only solve the problem of uneven expansion of steel slag bricks, but also have a short molding time and can improve the mechanical properties of steel slag bricks. Compared with traditional steel slag bricks, they have the characteristics of high stability and excellent mechanical properties, and have broad application prospects in the field of building materials.

[0086] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing organic-geopolymer coated microbial mineralized slag brick, characterized in that: The steps include: S1. Soak the steel slag in a microbial solution that can induce calcium precipitation, and take it out after soaking for a certain period of time; S2. The organic polymer or its monomer is dissolved in an aqueous solution of an alkaline activator, and then the silicon-aluminum raw material and the steel slag soaked in step S1 are added and mixed to obtain a slurry; S3. The slurry obtained in step S2 is statically pressed and cured to obtain the organic-geopolymer-coated microbial mineralized steel slag brick.

2. The preparation method according to claim 1, characterized in that: In step S1, the microbial culture liquid is a Bacillus pasteurianus culture liquid, and the microbial culture liquid contains urea at a concentration of 1 to 4 mol / L.

3. The preparation method according to claim 2, characterized in that: The microbial bacterial liquid is obtained by inoculating microbial seed liquid into a new liquid culture medium at a volume fraction of 2% to 10%, and culturing at 20 to 30° C. and 110 to 150 r / min for 12 to 36 hours.

4. The preparation method according to claim 1, characterized in that: The microorganisms are denitrifying bacteria, and the microbial bacterial solution contains sodium formate and calcium nitrate, and the concentrations thereof are 400-600 g / L and 6-9 g / L respectively.

5. The preparation method according to any one of claims 1 to 4, characterized in that: The soaking time in step S1 is 24 to 72 hours, and the soaking temperature is 20 to 40°C.

6. The preparation method according to any one of claims 1 to 4, characterized in that: Step S1: Before being immersed in the microbial solution, the steel slag is immersed in an acetic acid solution for pretreatment.

7. The preparation method according to claim 6, characterized in that: The pretreatment conditions are as follows: the concentration of the acetic acid solution is 0.2-2 mol / L, the solid-liquid ratio is 1 g:8-20 ml, the soaking temperature is 40-70°C, and the soaking time is 0.5-2.5 h.

8. The preparation method according to claim 1, characterized in that: In step S2, the organic polymer or its monomer is one or more of sodium polyacrylate, epoxy resin, chitosan or propylamine; The alkaline activator is one or more of sodium hydroxide, water glass, potassium hydroxide, and sodium aluminate; The silicon-alumina raw material is one or more of kaolin, fly ash and slag powder.

9. The preparation method according to claim 1, characterized in that: In step S2, the mass ratio of the organic polymer or its monomer, the alkali activator, the silicon-aluminum raw material, the steel slag and the water is (2-10):(1-5):(10-20):(90-110):(10-20).

10. An organic-geopolymer coated microbial mineralized steel slag brick, characterized in that: The compound is prepared by the preparation method according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Method for making microorganism-slag carbon-fixed water permeable brick

    CN110183194A

  • Method for strengthening recycled aggregate concrete by utilizing microbial denitrification phenomenon and recycled aggregate concrete

    CN112851170A

  • Geopolymer coated carbonated steel slag aggregate as well as preparation method and application thereof

    CN116354636A

  • Method for inhibiting uneven expansion of steel slag for pavement base course coarse aggregate

    CN116354637A