Phosphorus II type anhydrous gypsum-based self-leveling mortar and preparation method thereof
By using specific components and processes in phosphorus II type anhydrous gypsum-based self-leveling mortar, the hydration process and crystal growth rate are adjusted to solve the problem of difficulty in balancing early strength and slurry viscosity, and achieve high-performance gypsum-based green Building materials.
Patent Information
- Application Number
- CN202410805231.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-21
- Publication Date
- 2024-10-11
AI Technical Summary
The existing phosphorus II type anhydrous gypsum-based self-leveling mortar is difficult to balance the early strength and slurry viscosity requirements, and there are problems such as the consistency of the finished product being difficult to control or the later quality being difficult to ensure.
Using phosphorus II type anhydrous gypsum, mineral powder, fly ash, cement, water reducing agent, retardant, defoaming agent, suspension stabilizer, calcined potassium aluminum sulfate, calcined potassium sulfate, building gypsum, calcium sulfoaluminate cement materials, calcium formate, etc. The appropriate proportion of components, through the use of ball milling modification and high-temperature calcined sulfate activator, adjusts the hydration process and crystal growth rate to form a self-leveling mortar with good fluidity, high strength, wear resistance and water resistance.
The phosphorus II type anhydrous gypsum-based self-leveling mortar has the advantages of good fluidity, high strength, good wear resistance and water resistance, low slurry viscosity, superior construction performance, strong product quality controllability, and good volume stability. , which solves the problem of resource utilization of phosphogypsum and coordinated and integrated utilization of solid waste resources.
Smart Images

Figure FDA0004904478730000011 
Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of building materials, and in particular to a phosphorus II type anhydrous gypsum-based self-leveling mortar and a preparation method thereof. Background Art
[0002] As a typical industrial solid waste in my country, phosphogypsum produces about 7000wt per year. Its large-scale storage has brought about the waste of land resources and the risk of environmental pollution. The chemical composition of phosphogypsum is similar to that of natural gypsum. The mass fraction of the main component calcium sulfate dihydrate is generally 85% to 90%. It has the potential to be used as a gypsum-based building material. Phosphogypsum can be used as a green building material in gypsum building materials. Among them, the gypsum-based self-leveling prepared with calcined phosphogypsum as raw material has the advantages of good fluidity, high early strength, fast construction speed, no cracking or hollowing, and no need for maintenance in the later stage. It overcomes the defects of traditional cement-based self-leveling, which has slow setting speed and easy cracking.
[0003] At present, most of the gypsum self-leveling mortars on the market are made of β-type semi-hydrated gypsum as the main cementing material and admixtures. However, β-type semi-hydrated gypsum-based self-leveling mortars have the following problems: 1. Low strength and surface hardness, poor water resistance and wear resistance; 2. The production of β-type semi-hydrated gypsum powder is volatile, and the mortar formula has poor adaptability, and the formula must be adjusted accordingly according to the fluctuations at any time; 3. Due to the front-end phosphogypsum purification or insufficient purification, the back-end self-leveling mortar has problems such as mold and cracking. Although α-type semi-hydrated gypsum-based self-leveling mortar has better strength, the production and preparation conditions of α-type semi-hydrated gypsum are harsh, the product stability is poor, and the cost is high, making it difficult to achieve large-scale promotion and application. Therefore, it has become a development trend to use phosphorus II anhydrous gypsum as the main cementing material for gypsum self-leveling mortar.
[0004] Since the chemical potential of the thermodynamic spontaneous process of type II anhydrous gypsum is small, the Ca 2+ and SO4 2- The concentration is low, the supersaturation of dihydrate gypsum crystallization is very low, and it is difficult for the crystal nucleus to grow above the critical size. Therefore, the reaction rate of the hydration process is slow and the setting time is long, resulting in low early strength of the self-leveling mortar prepared with Type II anhydrous gypsum.
[0005] Therefore, in order to meet the early strength of the self-leveling mortar, it is necessary to stimulate the hydration activity of type II anhydrous gypsum by physical, chemical and other methods. CN113773038A discloses a type II anhydrous gypsum-based self-leveling mortar, wherein the sulfate activator is aluminum sulfate. In the self-leveling mortar, since aluminum sulfate will cause irreversible damage to the gypsum matrix structure in the later stage, there is a great risk of long-term volume stability.
[0006] In order to further improve the early strength of self-leveling mortar, most researchers will add hydraulic inorganic gelling materials such as cement and mineral powder. However, the addition amount of cement and mineral powder should not be too large, especially the addition amount of cement is too large. Although it will form strength in the early stage, it will hinder the crystal growth space during the hydration process of type II anhydrous gypsum, resulting in cracking of the hardened body of self-leveling mortar. CN114644501A discloses an anhydrous gypsum self-leveling material and a preparation method thereof, wherein the cement addition amount is 5%-15%, and the water-retaining thickener includes any one of hydroxypropyl methyl cellulose ether, hydroxyethyl methyl cellulose ether or carboxymethyl cellulose ether or a combination of at least two. When the cement addition amount exceeds 10% in the type II anhydrous gypsum-based self-leveling mortar system, it is easy to cause the risk of cracking in the later stage. Since the viscosity of the type II anhydrous gypsum slurry prepared by calcining phosphogypsum is relatively large, the viscosity of the self-leveling mortar slurry prepared after adding the cellulose ether water-retaining thickener is further increased, resulting in the self-leveling mortar not having construction properties during actual use.
[0007] CN113603447A discloses an anhydrous gypsum self-leveling material and its preparation method and use. The admixture includes 2000-3000 parts of α-type hemihydrate gypsum and / or β-type hemihydrate gypsum, and the aggregate includes river sand and machine-made sand. In the anhydrous gypsum-based system, the amount of hemihydrate gypsum added should not be too large. Since the hydration rate of hemihydrate gypsum is relatively fast and the fluidity loss is relatively large, the addition of protein retarders can prolong the setting rate of hemihydrate gypsum to a certain extent, but it will also inhibit the hydration of anhydrous gypsum. Although the introduced machine-made sand can improve the compressive strength, the machine-made sand is a bulk raw material, some of which contain a large amount of mud and have poor controllability, which is difficult to control for industrial production.
[0008] In summary, it is difficult to take into account both the early strength and slurry viscosity requirements in the existing self-leveling mortar system, and there are problems such as difficulty in controlling the consistency of the finished product or difficulty in ensuring the quality in the later stage. Therefore, it is urgent to develop a gypsum-based self-leveling mortar that can meet the fluidity and strength requirements as well as the requirements of low slurry viscosity, good construction performance and strong quality controllability. Summary of the invention
[0009] The purpose of the present invention is to provide a phosphorus II anhydrous gypsum-based self-leveling mortar and a preparation method thereof, so as to solve the problems that the existing self-leveling mortar is difficult to take into account both the early strength and slurry viscosity requirements, and there is a problem that the consistency of the finished product is difficult to control or the later quality is difficult to ensure.
[0010] In order to solve the above technical problems, the present invention adopts the following technical solution: a phosphorus II type anhydrous gypsum-based self-leveling mortar, characterized in that the components included are as follows in parts by weight:
[0011]
[0012]
[0013] A further technical solution is that the phosphorus II anhydrous gypsum is prepared by calcining the phosphogypsum at 750-850°C for 1-2 hours, and then ball-milling the phosphogypsum to a surface area of 500-600 m 2 / kg prepared.
[0014] A further technical solution is that the cement is ordinary Portland cement P·O 42.5, the fly ash grade is ≥ grade II, and grade I is better; the mineral powder grade is ≥ grade S95, and grade S105 is better.
[0015] A further technical solution is that the water reducer is a polycarboxylic acid water reducer having a phosphate group linked to the side chain.
[0016] A further technical solution is that the retarder is sodium gluconate.
[0017] A further technical solution is that the defoamer is an organosilicon defoamer.
[0018] A further technical solution is that the suspension stabilizer is modified sodium bentonite with a mesh size of 300 meshes.
[0019] A further technical solution is that the calcium sulphoaluminate binder is graded at 62.5 MPa.
[0020] A further technical solution is that the calcined potassium aluminum sulfate and calcined potassium sulfate are prepared by calcining potassium aluminum sulfate dodecahydrate and potassium sulfate at 500-800° C. for 30-60 minutes, respectively, and crushing them to less than 75 microns after cooling.
[0021] A further technical solution is that the building gypsum is β-type building gypsum or α-type building gypsum prepared by calcining phosphogypsum or desulfurized gypsum, with an initial setting time of ≥6 minutes, a semi-aqueous phase and a type III anhydrous phase content of less than 3%, and a strength performance of Grade 3.0 or above as specified in GB / T 9776-2022.
[0022] A further technical solution is that the preparation method of the gypsum-based self-leveling mortar is as follows: phosphorus II type anhydrous gypsum, mineral powder, fly ash, cement, water reducer, retarder, defoamer, suspension stabilizer, calcined potassium aluminum sulfate, calcined potassium sulfate, building gypsum, calcium sulfoaluminate binder, and calcium formate are mixed in a dry powder mixer according to the metered amount for 10 to 15 minutes, and then added into water and stirred for 4 to 8 minutes to prepare a phosphorus II type anhydrous gypsum-based self-leveling mortar slurry.
[0023] For strength:
[0024] The main strength of the self-leveling mortar is provided by the formation of dihydrate gypsum with a certain spatial network structure during the hydration process of phosphorus II anhydrous gypsum. The early strength sources: the hydration of tricalcium silicate and dicalcium silicate in the cement silicon phase to form calcium silicate gel and the dissolution of sulfate and tricalcium aluminate in the aluminum phase and then precipitation to form high-sulfur type hydrated calcium aluminate to produce strength; part of phosphorus II anhydrous gypsum hydrated under the action of activator to produce strength; building gypsum powder hydrated to produce strength. In the middle and late stages, the strength is mainly provided by the further hydration of phosphorus II anhydrous gypsum, and cement and dihydrate gypsum stimulate the activity of mineral powder and fly ash to form calcium silicate gel and calcium aluminate attached to the surface of gypsum crystals. The hydration products are densely stacked in the unit space, which improves the density of the hardened body and thus improves the strength. Mineral powder and phosphorus type II anhydrous gypsum can promote each other's hydration. Phosphorus type II anhydrous gypsum reacts with the active silicon and aluminum components in the mineral powder to promote the hydration of the mineral powder. The hydration of the mineral powder can drive the dissolution and hydration of phosphorus type II anhydrous gypsum, and finally form hydraulic minerals such as calcium aluminate and hydrated calcium silicate, thereby improving the strength and water resistance of the hardened self-leveling mortar.
[0025] For liquidity:
[0026] Since the viscosity of phosphorus II anhydrous gypsum slurry itself is relatively high, the proportion of phosphorus II anhydrous gypsum in self-leveling mortar is reduced by adding mineral powder and fly ash, and the fluidity is improved by using the ball effect generated by adding fly ash in the self-leveling slurry, thereby reducing the viscosity of the slurry. After ball milling modification, phosphorus II anhydrous gypsum can increase the hydration rate and change the appearance of the particles. Ball milling can remove the water chestnuts of anhydrous gypsum particles, changing them from irregular flakes to nearly elliptical shapes, thereby improving the fluidity of the slurry. On the other hand, the hydration activity and rheology of phosphorus II anhydrous gypsum are affected by calcination temperature and time. As the calcination temperature increases and the calcination time prolongs, the hydration activity of phosphorus II anhydrous gypsum increases and the slurry viscosity decreases.
[0027] For calcined aluminum potassium sulfate, calcined potassium sulfate:
[0028] Sulfate activators are added to change the hydration and hardening mode of anhydrous gypsum, adjust the crystallization habit of dihydrate gypsum at low supersaturation, concentrate the hydration exotherm, shorten the setting time, and accelerate the hydration process of phosphorus type II anhydrous gypsum. According to the double salt theory, sulfate first dissolves and adsorbs on the surface of type II anhydrous gypsum, then complexes with water to form unstable double salts, and finally, because the double salts are thermodynamically unstable, they will immediately decompose into dihydrate gypsum and metal cations. However, the metal cation ions formed by sulfate will undergo adsorption and coagulation with the negatively charged functional groups of the water reducer itself, reducing the adsorption and dispersion effect of the water reducer on the gypsum particles, resulting in a decrease in the fluidity of the mortar. In the present invention, the sulfate activator is calcined at a certain temperature and time to reduce the solubility of sulfuric acid in the early stage, thereby weakening its effect on the fluidity of the self-leveling mortar. At the same time, excessive addition of sulfate activator and too small radius of metal cations in sulfate are likely to cause frosting and volume stability problems in the late stage of mortar. Therefore, in the present invention, the addition amount of the sulfate activator is controlled to be below 1.5%, and calcined potassium aluminum sulfate and calcined potassium sulfate with a larger metal cation radius are selected as the sulfate activator.
[0029] For building plaster:
[0030] The difference in solubility between building gypsum and phosphorus type II anhydrous gypsum is used to change the nucleation and crystal growth rate of each other, thereby accelerating the hydration of phosphorus type II anhydrous gypsum. Building gypsum dissolves to form a saturated solution of calcium sulfate, which accelerates the nucleation and crystal growth rate of dihydrate gypsum and promotes the hydration of phosphorus type II anhydrous gypsum. The hydration of phosphorus type II anhydrous gypsum slows down the coagulation and hardening rate of building gypsum and reduces its hydration heat release. The hydration of building gypsum can make up for the insufficient early excitation of type II anhydrous gypsum, which leads to surface exudation of self-leveling slurry and improves the early strength of self-leveling mortar. Therefore, the addition amount of building gypsum and the control of hydration rate are particularly critical. Excessive addition will lead to excessive loss of fluidity of self-leveling mortar in 30 minutes. The structure formed by hydration hinders the crystal growth during the hydration process of phosphorus type II anhydrous gypsum, which ultimately reduces the overall strength of self-leveling mortar.
[0031] For admixtures:
[0032] Because the hydration speed of building gypsum is too fast under normal circumstances, it is easy to cause the slurry to lose fluidity and the strength of the self-leveling mortar system to decrease. The calcium formate added to this formula system dissolves faster than the semi-aqueous phase in the building gypsum in the early stage. 2+ The concentration slows down the dissolution of the semi-aqueous phase. At the same time, calcium formate dissolves in the HCOO in the liquid phase. -Adsorbed on the surface of gypsum crystals, it reduces the early hydration rate of building gypsum in the system. The retarding effect of calcium formate on the early stage of building gypsum powder not only provides sufficient time and space for the growth of hydration crystals of phosphorus type II anhydrous gypsum, but also reduces the viscosity of self-leveling slurry and the thickening speed of slurry, ensuring the initial fluidity and 30min fluidity loss.
[0033] In order to further reduce the fluidity loss of the self-leveling mortar in 30 minutes, a retarder is introduced into the present formula system, but the retarding effect of the traditional protein retarder is too strong, which not only produces a retarding effect on the building gypsum, but also inhibits the hydration rate of the phosphorus II anhydrous gypsum, prolongs the water absorption time of the mortar and causes water bleeding. Therefore, in the present invention, sodium gluconate with a weaker retarding effect is selected as a retarder, and sodium gluconate can also produce a retarding effect on the cement and building gypsum in the formula, prolong the setting time, and provide sufficient time for the hydration of the phosphorus II anhydrous gypsum.
[0034] Water reducers adsorb on the surface of phosphorus II anhydrous gypsum, change the interface structure and electrochemical properties of the powder particles, generate electrostatic repulsion and steric hindrance dispersion effects, and can ensure the fluidity of self-leveling mortar while reducing the water demand of self-leveling materials to improve strength. The water reduction efficiency of polycarboxylic acid-based water reducers is much better than that of sulfonated melamine-based and naphthalene-based water reducers. However, the -COO - With SO4 in liquid phase 2- There is competitive adsorption, which easily leads to excessive use of polycarboxylic acid water reducer, thus causing water seepage in the later stage of slurry. Therefore, the polycarboxylic acid water reducer used in the present invention has a phosphate group on the side chain. 2- The adsorption capacity of phosphate groups on phosphorus II anhydrous gypsum in the system is much stronger than that of -COO - , thereby reducing the amount of polycarboxylic acid water reducer in phosphorus II type anhydrous gypsum-based self-leveling mortar and the possibility of mortar bleeding while ensuring fluidity.
[0035] Suspension stabilizers are used to solve the problem of bleeding and sedimentation of self-leveling mortar slurry, but cellulose-type suspension stabilizers will increase the viscosity of the self-leveling mortar slurry and affect the construction performance of the self-leveling mortar. Therefore, the suspension stabilizer selected in the present invention is a modified sodium bentonite with a mesh size of 300, which not only solves the bleeding of the slurry but also minimizes the increase in the viscosity of the slurry.
[0036] The main sources of bubbles on the surface of gypsum self-leveling mortar are the interstitial air between the particles of phosphorus type II anhydrous gypsum powder, the air wrapped by the slurry during the mixing process, and the bubbles generated by the floating of the covering air during the slurry pouring process. The silicone defoamer is introduced into the formula system of the present invention. On the one hand, it can quickly diffuse and expand on the surface of the slurry bubbles by utilizing the low surface tension of the defoamer, reducing the surface tension of the bubble wall and causing the bubbles to burst. On the other hand, the defoamer causes the liquid film of the bubbles generated by the slurry to have poor cohesion, and the local viscosity decreases, causing the foam to burst. The introduction of the defoamer improves the surface smoothness and flatness of the gypsum self-leveling slurry, and suppresses the problem of water seepage on the slurry surface caused by the floating of bubbles.
[0037] In order to improve the early strength of the phosphorus II anhydrous gypsum-based self-leveling mortar, an early strength agent is added to the system of the present invention, and the early strength agent is calcium formate and calcium sulfoaluminate binder. On the one hand, by increasing the concentration of calcium ions and sulfate ions in the early liquid phase of the self-leveling slurry hydration, the time required for the two ions in the liquid phase to reach supersaturation is shortened, and the growth rate of calcium sulfate dihydrate crystals is accelerated to form early strength. On the other hand, the calcium sulfoaluminate binder is self-hydrated to form hydrated calcium sulfoaluminate to produce early strength.
[0038] Compared with the prior art, the present invention has the following beneficial effects:
[0039] 1. Phosphorus II anhydrous gypsum, mineral powder, fly ash, cement, water reducer, retarder, defoamer, suspension stabilizer, calcined potassium aluminum sulfate, calcined potassium sulfate, building gypsum, calcium sulfoaluminate binder and calcium formate are prepared into gypsum-based self-leveling mortar through appropriate proportions. Through the synergistic influence of the components, the phosphorus II anhydrous gypsum-based self-leveling mortar with good fluidity, high strength, good wear resistance and water resistance, low slurry viscosity, excellent construction performance, strong product quality controllability and good volume stability is obtained, which not only solves the resource utilization of phosphogypsum, but also introduces fly ash and mineral powder, realizes the synergistic and integrated utilization of solid waste resources, and obtains high-performance gypsum-based green building materials.
[0040] 2. Compared with traditional building gypsum-based self-leveling mortar, there is no need to carry out front-end purification and impurity removal process for the phosphogypsum raw materials when calcining phosphorus type II anhydrous gypsum at high temperature, thereby indirectly reducing the production cost of phosphorus type II anhydrous gypsum-based self-leveling mortar and the possibility of long-term mold. DETAILED DESCRIPTION
[0041] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0042] Example 1
[0043] This embodiment provides a phosphorus II anhydrous gypsum-based self-leveling mortar and a preparation method thereof, and the experimental and curing conditions are respectively a temperature of 20±5°C and a relative humidity of 55±10%. The specific steps are as follows:
[0044] (1) Preparation of phosphogypsum II: 92% phosphogypsum was fluidized and calcined at 800°C for 90 min, and then ball-milled to a specific surface area of 550 m 2 / kg.
[0045] Preparation of activator: Industrial grade potassium aluminum sulfate dodecahydrate and potassium sulfate were calcined at 750°C for 40 minutes and then crushed to less than 75 microns.
[0046] (2) The following raw materials were weighed in parts by weight: 700 parts of phosphorus type II anhydrous gypsum, 100 parts of mineral powder (grade S95), 50 parts of fly ash (grade I), 90 parts of cement (PO 42.5), 1.4 parts of water reducer (polycarboxylic acid water reducer with phosphate groups on the side chain, PC-301 water reducer produced by Shandong Haoyu Building Materials Technology Co., Ltd.), 0.5 parts of retarder (sodium gluconate), 0.5 parts of organosilicon defoamer, 0.55 parts of suspension stabilizer (300 mesh sodium bentonite produced by Renshou Hongruitai Bentonite Technology Co., Ltd.), 10 parts of calcined potassium aluminum sulfate, 3.5 parts of calcined potassium sulfate, α-type building gypsum (initial setting time ≥ 6 min, semi-aqueous phase and type III anhydrous phase contents are both less than 3%, strength properties reach GB / T 9776-2022 (grade 3.0 and above), 50 parts, 5 parts of calcium formate, and 5 parts of calcium sulphoaluminate binder (labeled as 62.5MPa).
[0047] (3) The above-mentioned phosphorus II anhydrous gypsum, mineral powder, fly ash, cement, water reducer, retarder, defoamer, suspension stabilizer, α-type building gypsum, calcium formate, and calcium sulfoaluminate binder are mixed in a dry powder mixer according to the measured weight for 10 minutes, then added into 400 parts of water, and stirred for 5 minutes to prepare phosphorus II anhydrous gypsum-based self-leveling mortar.
[0048] Comparative Example 1:
[0049] This comparative example provides a phosphorus II anhydrous gypsum-based self-leveling mortar and a preparation method thereof. The weight proportions of the components of the self-leveling mortar refer to those of Example 1, with the only difference being that the weight proportions of phosphorus II anhydrous gypsum are 850 parts, i.e., the amount of phosphorus II anhydrous gypsum added is too much.
[0050] Comparative Example 2:
[0051] This comparative example provides a phosphorus II anhydrous gypsum-based self-leveling mortar and a preparation method thereof. The weight proportions of the components of the self-leveling mortar refer to those of Example 1, with the only difference being that the weight proportions of the phosphorus II anhydrous gypsum are 500 parts, i.e., the amount of phosphorus II anhydrous gypsum added is too small.
[0052] Comparative Example 3: This comparative example provides a phosphorus II anhydrous gypsum-based self-leveling mortar and a preparation method thereof. The weight proportions of the components of the self-leveling mortar refer to those of Example 1, with the only difference being that the water reducer used is the PCE-8300 polycarboxylic acid-based water reducer produced by Jiangsu Zhaojia Building Materials Technology Co., Ltd., which does not contain a phosphate group on the side chain, and the weight proportion of the water reducer is 1.4 parts.
[0053] Comparative Example 4: This comparative example provides a phosphorus II anhydrous gypsum-based self-leveling mortar and a preparation method thereof. The weight proportions of the components of the self-leveling mortar refer to those of Example 1, with the only difference being that the water reducer used is the PC-3000 polycarboxylic acid water reducer produced by Zhaojia, which does not contain a phosphate group on the side chain, and the weight proportion of the water reducer is 2.0 parts.
[0054] The physical and mechanical properties of the phosphorus II type anhydrous gypsum-based self-leveling mortars prepared in Example 1 and Comparative Examples 1-4 were tested respectively. The test results are shown in Table 1.
[0055] Table 1
[0056] Performance Indicators Example 1 Comparative Example 1 Comparative Example 2 Comparative Example 3 Comparative Example 4 Initial fluidity / mm 155 135 160 130 155 30min fluidity / mm 155 125 164 126 158 Slurry state No water seepage No water seepage Bleeding No water seepage Bleeding Initial setting time / h 4 3.8 4.5 3.7 5 Final setting time / h 11 10 12 11 12.5 2d flexural strength / MPa 2.8 2.9 2.1 2.8 2.3 2d compressive strength / MPa 9.4 9.6 7.0 9.8 8.2 28d absolute dry flexural strength / MPa 11.7 9.1 8.7 10.3 9.4 28d absolute dry compressive strength / MPa 32.4 27.3 23.0 28.5 26.0
[0057] In Comparative Example 1, due to the excessive addition of phosphorus II anhydrous gypsum, the viscosity of the self-leveling slurry increased, and the excessive phosphorus II anhydrous gypsum hydrated and lost the plasticity of the slurry, resulting in a decrease in the initial fluidity and 30min fluidity of the slurry, and normal construction could not be guaranteed. At the same time, part of the phosphorus II anhydrous gypsum cannot be fully hydrated. After hardening, the phosphorus II anhydrous gypsum acts as a filler component in the self-leveling material, and the 28d absolute dry strength is reduced. In addition, this part of the unhydrated phosphorus II anhydrous gypsum hydrates in a high humidity environment to produce volume expansion, and the risk of cracking of the hardened body in the later stage increases. In Comparative Example 2, due to the small amount of phosphorus II anhydrous gypsum added, the setting time is prolonged, the self-leveling slurry exudes water, and the early and late strengths of the hardened body are greatly reduced. In Comparative Example 3, the -COO in the ordinary polycarboxylic acid water reducer - With SO4 in liquid phase 2- The competitive adsorption caused the water reducing agent to have a poor dispersion effect, reduced initial fluidity, uneven dispersion of powder particles in the slurry, and reduced compactness formed by hydration and hardening, resulting in reduced strength in the later stage. In Comparative Example 4, although increasing the amount of ordinary polycarboxylate water reducing agent can ensure fluidity, it will cause the setting time to be prolonged, the slurry to bleed, and the early and late strength of the hardened body to be reduced.
[0058] Example 2
[0059] This embodiment provides a phosphorus II anhydrous gypsum-based self-leveling mortar and a preparation method thereof, and the experimental and curing conditions are respectively a temperature of 20±5°C and a relative humidity of 55±10%. The specific steps are as follows:
[0060] (1) Preparation of phospho-type II anhydrous gypsum: 90% phosphogypsum was fluidized and calcined at 750°C for 100 min, and then ball-milled to a specific surface area of 525 m 2 / kg.
[0061] Preparation of activator: Industrial grade potassium aluminum sulfate dodecahydrate and potassium sulfate are calcined at 700°C for 30 minutes and then crushed to less than 75 microns.
[0062] (2) The following raw materials were weighed in parts by weight: 650 parts of phosphorus II anhydrous gypsum, 140 parts of mineral powder (grade S95), 50 parts of fly ash (grade I), 100 parts of cement (PO 42.5), 1.4 parts of water reducer (polycarboxylic acid water reducer with phosphate groups on the side chain, PC-301 water reducer produced by Shandong Haoyu Building Materials Technology Co., Ltd.), 0.6 parts of retarder (sodium gluconate), 0.5 parts of organosilicon defoamer, 0.65 parts of suspension stabilizer (300 mesh sodium bentonite produced by Renshou Hongruitai Bentonite Technology Co., Ltd.), 10 parts of calcined potassium aluminum sulfate, 3 parts of calcined potassium sulfate, β-type building gypsum (initial setting time ≥ 6 min, semi-aqueous phase and type III anhydrous phase contents are both less than 3%, strength properties reach GB / T 9776-2022 (grade 3.0 and above), 50 parts, 5 parts of calcium formate, and 5 parts of calcium sulphoaluminate binder (labeled as 62.5MPa).
[0063] (3) The above-mentioned phosphorus II anhydrous gypsum, mineral powder, fly ash, cement, water reducer, retarder, defoamer, suspension stabilizer, β-type building gypsum, calcium formate, and calcium sulfoaluminate binder are mixed in a dry powder mixer according to the measured amount for 10 minutes, then added into 400 parts of water, and stirred for 5 minutes to prepare a phosphorus II anhydrous gypsum-based self-leveling mortar.
[0064] Comparative Example 5:
[0065] This comparative example provides a phosphorus II anhydrous gypsum-based self-leveling mortar and a preparation method thereof. The weight proportions of the components of the self-leveling mortar refer to those of Example 2, with the only difference being that β-type building gypsum is 120 parts, i.e., the amount of β-type building gypsum added is too much.
[0066] Comparative Example 6:
[0067] This comparative example provides a phosphorus II anhydrous gypsum-based self-leveling mortar and a preparation method thereof. The weight proportions of the components of the self-leveling mortar refer to those of Example 2, with the only difference being that β-type building gypsum is 15 parts, i.e., the amount of β-type building gypsum added is too small.
[0068] Comparative Example 7:
[0069] This comparative example provides a phosphorus II anhydrous gypsum-based self-leveling mortar and a preparation method thereof. The weight proportions of the components of the self-leveling mortar refer to those of Example 2, with the only difference being that the retarder used is the 7602T protein retarder produced by Beijing Bernuo.
[0070] Comparative Example 8:
[0071] This comparative example provides a phosphorus II type anhydrous gypsum-based self-leveling mortar and a preparation method thereof. The weight proportions of the components of the self-leveling mortar refer to those of Example 2, with the only difference being that the suspension stabilizer used is hydroxypropyl methylcellulose with a viscosity of 4000.
[0072] The physical and mechanical properties of the phosphorus II type anhydrous gypsum-based self-leveling mortars prepared in Example 2 and Comparative Examples 5-8 were tested respectively. The test results are shown in Table 2.
[0073] Table 2
[0074] Performance Indicators Example 2 Comparative Example 5 Comparative Example 6 Comparative Example 7 Comparative Example 8 Initial fluidity / mm 160 145 168 170 142 30min fluidity / mm 163 125 170 174 125 Slurry state No water seepage No water seepage Bleeding Bleeding No water seepage Initial setting time / h 4.5 4.3 4.8 5 4.3 Final setting time / h 13 12.5 14 14.5 12.5 2d flexural strength / MPa 2.7 2.8 2.2 1.9 2.9 2d compressive strength / MPa 9.2 9.4 8.4 7.3 9.3 28d absolute dry flexural strength / MPa 11.0 7.5 8.5 8.7 9.4 28d absolute dry compressive strength / MPa 30.8 22.4 25.5 24.0 28.1
[0075] In this self-leveling system, building gypsum is mainly used to adjust the setting time of the slurry, adjust the surface water absorption time, and avoid the problem of water seepage and segregation in the slurry. Self-hydration and the stimulation of hydration of phosphorus type II anhydrous gypsum provide a certain early strength. In comparative example 5, when too much β-type building gypsum is added, the slurry will thicken and the 30min slurry thickening rate will be accelerated due to its own hydration rate being too fast, resulting in a decrease in initial fluidity and a large loss in 30min fluidity. The hardened body formed by the hydration of β-type building gypsum hinders the hydration growth space of phosphorus type II anhydrous gypsum, and the hydration sufficiency becomes poor, resulting in a decrease in the 28d absolute dry strength and an increase in the risk of cracking of the hardened body in the later stage.
[0076] In Comparative Example 6, when too little β-type building gypsum is added, the setting time and surface water absorption time of the slurry are prolonged, and the slurry bleeds. The self-hydration and the hydration stimulation effect on the phosphorus type II anhydrous gypsum are weakened, and the hydration ratio of the early phosphorus type II anhydrous gypsum is reduced, resulting in a decrease in the 2d strength. Due to the loss of water caused by bleeding and the increase in the content ratio of unhydrated phosphorus type II anhydrous gypsum in the later stage, the hydration process of the phosphorus type II anhydrous gypsum in the later stage is affected, resulting in a decrease in the 28d absolute dry flexural strength.
[0077] In Comparative Example 7, 7602T protein retarder was used. Due to the strong retarding effect, the early hydration of building gypsum and phosphorus II anhydrous gypsum was delayed, the surface water absorption time was prolonged, resulting in severe bleeding of the slurry and reduced 2d strength. The surface moisture formed by bleeding evaporated too quickly, resulting in reduced 28d absolute dry strength.
[0078] In Comparative Example 8, hydroxypropyl methylcellulose with a viscosity of 4000 was used as a suspension stabilizer. Since the viscosity of the type II anhydrous gypsum slurry itself is high, the viscosity of the self-leveling slurry is further increased after the addition of hydroxypropyl methylcellulose, the construction performance deteriorates, and the fluidity decreases.
[0079] Example 3
[0080] This embodiment provides a phosphorus II anhydrous gypsum-based self-leveling mortar and a preparation method thereof, and the experimental and curing conditions are respectively a temperature of 20±5°C and a relative humidity of 55±10%. The specific steps are as follows:
[0081] (1) Preparation of phospho-type II anhydrous gypsum: 90% phosphogypsum was fluidized and calcined at 775°C for 100 min, cooled and then ball-milled to a specific surface area of 550 m 2 / kg.
[0082] Preparation of activator: Industrial grade potassium aluminum sulfate dodecahydrate and potassium sulfate are calcined at 600°C for 50 minutes and then crushed to less than 75 microns.
[0083] (2) The following raw materials were weighed in parts by weight: 600 parts of phosphorus II anhydrous gypsum, 165 parts of mineral powder (grade S95), 55 parts of fly ash (grade I), 100 parts of cement (PO 42.5), 1.2 parts of water reducer (polycarboxylic acid water reducer with phosphate groups on the side chain, PC-301 water reducer produced by Shandong Haoyu Building Materials Technology Co., Ltd.), 0.5 parts of retarder (sodium gluconate), 0.4 parts of organosilicon defoamer, 0.3 parts of suspension stabilizer (300 mesh sodium bentonite produced by Renshou Hongruitai Bentonite Technology Co., Ltd.), 8 parts of calcined potassium aluminum sulfate, 3.5 parts of calcined potassium sulfate, α-type building gypsum (initial setting time ≥ 6 min, semi-aqueous phase and type III anhydrous phase contents are both less than 3%, strength properties reach GB / T 9776-2022 (grade 3.0 and above), 40 parts, calcium formate, and 15 parts of calcium sulphoaluminate binder (labeled as 62.5MPa).
[0084] (3) The above-mentioned phosphorus II anhydrous gypsum, mineral powder, fly ash, cement, water reducer, retarder, defoamer, suspension stabilizer, α-type building gypsum, calcium formate, and calcium sulfoaluminate binder are mixed in a dry powder mixer for 12 minutes, added to 400 parts of water, and stirred for 6 minutes to prepare a phosphorus II anhydrous gypsum-based self-leveling mortar.
[0085] Comparative Example 9:
[0086] This comparative example provides a phosphorus II anhydrous gypsum-based self-leveling mortar and a preparation method thereof. The weight proportions of the components of the self-leveling mortar refer to those of Example 3, with the only difference being that the amount of calcium formate is 50 parts, i.e., the amount of calcium formate added is too much.
[0087] Comparative Example 10:
[0088] This comparative example provides a phosphorus II type anhydrous gypsum-based self-leveling mortar and a preparation method thereof. The weight proportions of the components of the self-leveling mortar refer to those of Example 3, with the only difference being that the calcium formate is 2 parts, i.e., the amount of calcium formate added is too small.
[0089] Comparative Example 11:
[0090] This comparative example provides a phosphorus II anhydrous gypsum-based self-leveling mortar and a preparation method thereof. The weight proportions of the components of the self-leveling mortar refer to those of Example 3, with the only difference being that the calcium sulfoaluminate binder is 40 parts, i.e., the amount of calcium sulfoaluminate binder added is too much.
[0091] The physical and mechanical properties of the phosphorus II anhydrous gypsum-based self-leveling mortars prepared in Example 3 and Comparative Examples 9-11 were tested respectively. The test results are shown in Table 3.
[0092] Table 3
[0093] Performance Indicators Example 3 Comparative Example 9 Comparative Example 10 Comparative Example 11 Initial fluidity / mm 150 145 154 140 30min fluidity / mm 150 130 155 110 Slurry state No water seepage No water seepage Bleeding No water seepage Initial setting time / h 4.5 4 5 3.8 Final setting time / h 14 13 14.6 12 2d flexural strength / MPa 2.7 3.2 2.4 3.5 2d compressive strength / MPa 9.1 9.8 8.0 10.8 28d absolute dry flexural strength / MPa 10.8 9.0 8.7 7.2 28d absolute dry compressive strength / MPa 31.2 27.3 27.0 22.5
[0094] In Comparative Example 9, the amount of calcium formate added was too much, and the Ca dissolved in the liquid phase 2+ The concentration increases, forming a supersaturated solution too quickly, thereby accelerating the hydration and crystallization rate of phosphorus type II anhydrous gypsum, compressing the growth space of hydraulic minerals formed by the later gypsum, mineral powder and fly ash, resulting in a decrease in initial fluidity and 30min fluidity, a decrease in absolute dry strength, a deterioration in the long-term volume stability of the hardened body, and an increase in the risk of cracking. In Comparative Example 10, the amount of calcium formate added is too small, and the Ca dissolved in the liquid phase 2+ The concentration decreased, the early hydration rate of building gypsum and phosphorus II anhydrous gypsum decreased, the setting time and surface water absorption time were prolonged, resulting in mild bleeding and reduced strength of the slurry. In Comparative Example 11, the amount of calcium sulfoaluminate binder added was too much. Although the 2d strength was improved, the hydration rate of the calcium sulfoaluminate binder was too fast, resulting in a decrease in initial fluidity and a large loss of 30min fluidity. The large amount of calcium sulfoaluminate hydrate formed by the early hydration of the calcium sulfoaluminate binder seriously hindered the hydration crystal growth space of phosphorus II anhydrous gypsum, resulting in a decrease in the 28d absolute dry strength, a deterioration in the long-term volume stability of the hardened body, and a significant increase in the risk of cracking.
[0095] Example 4
[0096] This embodiment provides a phosphorus II anhydrous gypsum-based self-leveling mortar and a preparation method thereof, and the experimental and curing conditions are respectively a temperature of 20±5°C and a relative humidity of 55±10%. The specific steps are as follows:
[0097] (1) Preparation of phosphorus type II anhydrous gypsum: 85% phosphogypsum was subjected to fluidized calcination at 750°C for 80 min, and then ball-milled to a specific surface area of 520 m 2 / kg.
[0098] Preparation of activator: Industrial grade potassium aluminum sulfate dodecahydrate and potassium sulfate are calcined at 500°C for 1 hour and then crushed to less than 75 microns.
[0099] (2) The following raw materials were weighed in parts by weight: 650 parts of phosphorus II anhydrous gypsum, 145 parts of mineral powder (grade S95), 40 parts of fly ash (grade I), 80 parts of cement (PO 42.5), 1.65 parts of water reducer (polycarboxylic acid water reducer with phosphate groups on the side chain, PC-301 water reducer produced by Shandong Haoyu Building Materials Technology Co., Ltd.), 0.6 parts of retarder (sodium gluconate), 0.5 parts of organosilicon defoamer, 0.65 parts of suspension stabilizer (300 mesh sodium bentonite produced by Renshou Hongruitai Bentonite Technology Co., Ltd.), 12 parts of calcined potassium aluminum sulfate, 3.5 parts of calcined potassium sulfate, β-type building gypsum (initial setting time ≥ 6 min, semi-aqueous phase and type III anhydrous phase contents are both less than 3%, strength properties reach GB / T 9776-2022 Grade 3.0 and above) 30 parts, calcium formate 20 parts, calcium sulphoaluminate binder 15 parts (labeled 62.5MPa).
[0100] (3) The above-mentioned phosphorus II anhydrous gypsum, mineral powder, fly ash, cement, water reducer, retarder, defoamer, suspension stabilizer, β-type building gypsum, calcium formate, and calcium sulfoaluminate binder are mixed in a dry powder mixer according to the measured amount for 12 minutes, then added to 410 parts of water, and stirred for 6 minutes to prepare a phosphorus II anhydrous gypsum-based self-leveling mortar.
[0101] Comparative Example 12:
[0102] This comparative example provides a phosphorus II anhydrous gypsum-based self-leveling mortar and a preparation method thereof. The weight proportions of the components of the self-leveling mortar refer to those of Example 4, with the only difference being that the weight proportion of calcined potassium aluminum sulfate is 25 parts, i.e., the amount of calcined potassium aluminum sulfate added is too large.
[0103] Comparative Example 13:
[0104] This comparative example provides a phosphorus II anhydrous gypsum-based self-leveling mortar and a preparation method thereof. The weight proportions of the components of the self-leveling mortar refer to those of Example 4, with the only difference being that the weight proportion of calcined potassium aluminum sulfate is 3 parts, i.e., the amount of calcined potassium aluminum sulfate added is too small.
[0105] Comparative Example 14:
[0106] This comparative example provides a phosphorus II anhydrous gypsum-based self-leveling mortar and a preparation method thereof. The weight proportions of the components of the self-leveling mortar refer to those of Example 4, with the only difference being that the added industrial-grade potassium aluminum sulfate dodecahydrate is not subjected to calcination and crushing treatment.
[0107] The physical and mechanical properties of the phosphorus II type anhydrous gypsum-based self-leveling mortars prepared in Example 4 and Comparative Examples 12-14 were tested, and the test results are shown in Table 4.
[0108] Table 4
[0109]
[0110]
[0111] In Comparative Example 12, the amount of calcined aluminum potassium sulfate added is too large, and phosphorus type II anhydrous gypsum and calcined aluminum potassium sulfate form a complex salt in the liquid phase system, and then the complex salt decomposes to accelerate the hydration process of phosphorus type II anhydrous gypsum. The proportion of phosphorus type II anhydrous gypsum hydrated in the early stage increases significantly, forming a dense spatial structure. There is not enough space for the hydraulic minerals generated by the hydration of fly ash and mineral powder in the later stage, resulting in a decrease in absolute dry strength and an increase in the risk of cracking. The potassium ions formed by the dissolution of excessive calcined aluminum potassium sulfate are easy to migrate to the surface along the pores of the hardened body in a high humidity environment, causing the occurrence of frosting.
[0112] In Comparative Example 13, the amount of calcined potassium aluminum sulfate added is too small, the proportion of early hydrated phosphorus type II anhydrous gypsum is reduced, the setting time is prolonged, and due to insufficient hydration excitation, the proportion of unhydrated phosphorus type II anhydrous gypsum in the later hardened body increases, and the absolute dry strength is significantly reduced. This part of unhydrated phosphorus type II anhydrous gypsum undergoes hydration in a high humidity environment to produce volume expansion, and the risk of cracking of the hardened body in the later stage is increased.
[0113] In Comparative Example 14, the added industrial-grade potassium aluminum sulfate was not subjected to calcination and crushing treatment. Compared with the calcined dodecahydrate and potassium aluminum sulfate, the lack of calcination resulted in an increase in the solubility of dodecahydrate and potassium aluminum sulfate in the liquid phase in the early stage, an increase in the content of metal cation ions in the liquid phase, and an adsorption and coagulation effect with the negatively charged functional groups of the water reducer itself, which reduced the adsorption and dispersion effect of the water reducer on the gypsum particles, resulting in a decrease in the initial fluidity of the slurry, an increase in viscosity, and a deterioration in workability.
[0114] The present invention illustrates the detailed products and methods of the present invention through the above embodiments, but the present invention is not limited to the above detailed products and methods, that is, it does not mean that the present invention must rely on the above detailed products and methods to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of the product of the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.
Claims
1. A phosphorus II anhydrous gypsum-based self-leveling mortar, characterized in that: The components included are as follows by weight:
2. The phosphorus II type anhydrous gypsum-based self-leveling mortar according to claim 1, characterized in that: The phosphorus II anhydrous gypsum is prepared by calcining phosphogypsum at 750-850°C for 1-2 hours, cooling it, and then ball-milling it to a surface area of 500-600m 2 / kg prepared.
3. The phosphorus II type anhydrous gypsum-based self-leveling mortar according to claim 1, characterized in that: The cement is ordinary Portland cement P·O 42.5, the fly ash grade is ≥ grade II, and the mineral powder grade is ≥ grade S95.
4. The phosphorus II type anhydrous gypsum-based self-leveling mortar according to claim 1, characterized in that: The retarder is sodium gluconate, and the water reducer is a polycarboxylic acid-based water reducer with a phosphate group linked to the side chain.
5. The phosphorus II type anhydrous gypsum-based self-leveling mortar according to claim 1, characterized in that: The defoamer is an organosilicon defoamer.
6. The phosphorus II type anhydrous gypsum-based self-leveling mortar according to claim 1, characterized in that: The suspension stabilizer is sodium bentonite prepared through modification.
7. The phosphorus II type anhydrous gypsum-based self-leveling mortar according to claim 1, characterized in that: The calcium sulphoaluminate binder is labeled as 62.5MPa.
8. The phosphorus II type anhydrous gypsum-based self-leveling mortar according to claim 1, characterized in that: The calcined potassium aluminum sulfate and calcined potassium sulfate are prepared by calcining potassium aluminum sulfate dodecahydrate and potassium sulfate at 500-800° C. for 30-60 minutes, respectively, and crushing them to less than 75 microns after cooling.
9. The phosphorus II type anhydrous gypsum-based self-leveling mortar according to claim 1, characterized in that: The building gypsum is β-type building gypsum or α-type building gypsum prepared by calcining phosphogypsum or desulfurized gypsum, with an initial setting time of ≥6 minutes, a semi-aqueous phase and a type III anhydrous phase content of less than 3%, and a strength performance of grade 3.0 or above as specified in GB / T 9776-2022.
10. A phosphorus II type anhydrous gypsum-based self-leveling mortar according to any one of claims 1 to 9, characterized in that: The preparation method of the gypsum-based self-leveling mortar is as follows: Phosphorus II anhydrous gypsum, mineral powder, fly ash, cement, water reducer, retarder, defoamer, suspension stabilizer, calcined potassium aluminum sulfate, calcined potassium sulfate, building gypsum, calcium sulfoaluminate binder and calcium formate are mixed in a dry powder mixer according to the measured amount for 10 to 15 minutes, and then added into water and stirred for 4 to 8 minutes to prepare a phosphorus II anhydrous gypsum-based self-leveling mortar slurry.
Citation Information
Patent Citations
Anhydrous gypsum self-leveling material and preparation method thereof
CN114644501A
Gypsum-based polycarboxylate superplasticizer and preparation method thereof
CN115850605A
Cited By
Activation method of anhydrite II and gypsum product
CN121292924A