Environment-friendly antiskid material for ice and snow pavements and preparation method of environment-friendly antiskid material

Porous anti-skid materials made from coal gasification fine ash, oil shale tailings, dry sludge, waste glass and waste building ceramic tiles have solved the problems of limited use and safety hazards of traditional anti-skid materials on ice and snow roads, and achieved It achieves efficient anti-slip effect and resource reuse, which is superior to traditional slag materials.

CN118754602APending Publication Date: 2024-10-11JILIN INST OF ARCHITECTURE & TECH
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410750742.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-12
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

On ice and snow roads, existing anti-skid materials such as slag and gravel have limited use or safety hazards. Especially on roads far away from urban centers, it is difficult to quickly solve traffic safety problems caused by snow and frozen ice.

Method used

It is made of environmentally friendly anti-slip materials made from coal gasification fine ash, oil shale tailings, dry sludge, waste glass and waste building ceramic tiles, and is prepared through drying, grinding, mixing, granulation and sintering processes to form Spherical porous anti-skid material increases the friction coefficient between the road and the vehicle and reduces bulk density and hardness to avoid splashing and blowing.

Benefits of technology

It improves the safe passage of vehicles on ice and snow roads, has good anti-skid performance and resource utilization effect, is superior to traditional slag materials, and reduces energy consumption and environmental impact.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention provides an environment-friendly antiskid material for ice and snow pavements and a preparation method of the environment-friendly antiskid material. The environment-friendly antiskid material comprises the following components in parts by weight: 100 parts of coal gasification fine ash, 50-100 parts of oil shale tailings, 40-80 parts of dry sludge, 20-40 parts of waste glass, 20-40 parts of waste building ceramic tiles and 30-50 parts of water. The raw materials are ground, sieved, weighed, mixed, granulated, dried and calcined to prepare the composite material. When the anti-skid material is used for ice and snow pavements, the friction coefficient between the road and a vehicle tire is increased, so that the anti-skid effect is achieved. The antiskid material is ground and crushed by a vehicle, and the crushed porous antiskid material increases the contact area with ice and snow and the ground, is tightly combined with the ice and snow, is not easy to blow away under the condition of wind, and can still play an antiskid role. Various solid wastes are used as raw materials, and a new way for resource utilization of the solid wastes is opened up. And the environment-friendly anti-skid material for ice and snow pavements can be prepared, and has better social and economic benefits.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of solid waste resource utilization and road materials, and relates to an environmentally friendly anti-skid material for ice and snow roads. Background Art

[0002] A considerable part of my country's land area is located in the northern high latitudes or even high latitudes. These areas have a certain period of low temperature and snowy weather every year. Especially in Northeast my country, the period of low temperature and snow is as long as half a year. Low temperature and snowy weather brings many inconveniences to people's lives and production. Since travel and transportation are important parts of daily life and production, snow and ice on the roads have a great negative impact. Snow and ice will significantly reduce the friction coefficient of the road surface. Vehicles are very easy to slip when driving on icy and snowy roads, which seriously affects the road driving and the personal and property safety of drivers and passengers.

[0003] At present, the snow and ice removal of municipal roads in cities adopts a combination of manual snow removal and mechanical snow removal, which can basically quickly eliminate the traffic hazards caused by ice and snow. However, the snow and ice removal work on provincial highways, county highways, expressways and other roads far away from the city center is often not solved quickly. Long-term traffic closures seriously affect people's travel and economic development. Therefore, it is crucial to achieve safe passage of vehicles when there is snow and ice on the road, and vehicle anti-skid on icy and snowy roads has become an important task of highway management. At present, throwing anti-skid materials on the road surface is an effective way to solve this problem. According to actual conditions, commonly used anti-skid materials for the road surface are slag and gravel. Slag generally comes from thermal power plants. Due to source restrictions, areas far away from thermal power plants cannot use slag as anti-skid materials for the road surface. Although gravel materials are easy to obtain, there are often large particles in the gravel. These large particles are easily rolled up by vehicles during driving, seriously affecting the safety of the following vehicles. Summary of the invention

[0004] The purpose of the present invention is to provide an environmentally friendly anti-skid material for icy and snowy roads and a preparation method thereof. The anti-skid material provided by the present invention can be used on icy and snowy roads to increase the friction coefficient between the road surface and the vehicle to play an anti-skid role and improve road driving safety.

[0005] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0006] An environmentally friendly anti-skid material for icy and snowy roads, comprising the following components in parts by weight:

[0007] 100 parts of coal gasification fine ash, 50-100 parts of oil shale tailings, 40-80 parts of dry sludge, 20-40 parts of waste glass, 20-40 parts of waste building ceramic tiles, and 30-50 parts of water.

[0008] Preferably, the coal gasification fine ash is fine ash with a particle size of less than 50 μm produced in the coal gasification process, wherein SiO 2 Mass fraction greater than 40%, Al 2 O 3 The mass fraction is greater than 15% and the loss on ignition is greater than 20%.

[0009] Preferably, the oil shale tailings are small particles of oil shale with a particle size of less than 2 cm remaining when oil shale is distilled to produce shale oil, wherein SiO 2 Mass fraction greater than 50%, Al 2 O 3 The mass fraction is greater than 12%, and the high calorific value (dry basis) is greater than 3.0MJ / Kg.

[0010] Preferably, the dry sludge is solid sediment material produced in the sewage treatment process, and after drying, the dry sludge has a moisture content of less than 1% and a loss on ignition of more than 40%.

[0011] Preferably, the waste glass is waste soda-lime glass products used in daily life, wherein SiO 2 Mass fraction greater than 60%, Na 2 The mass fraction of O is greater than 10%.

[0012] Preferably, the waste building ceramic tiles are derived from building roof tiles.

[0013] The present invention also provides a method for preparing the environmentally friendly anti-slip material according to the above technical solution, comprising the following steps:

[0014] The coal gasification fine ash is dried at 105°C for 24 hours until the moisture content is less than 1%, and then passed through a 200-mesh square hole sieve, and the coal gasification fine ash with a particle size of less than 300 mesh is taken as the raw material;

[0015] The oil shale tailings are ground by a ball mill for a certain period of time, passed through a 200-mesh square-hole sieve, and the oil shale tailings with a particle size less than 200 mesh are taken as raw materials;

[0016] The dry sludge is crushed by a crusher and passed through a 200-mesh square hole sieve, and the sludge with a particle size less than 200 mesh is taken as the raw material;

[0017] Grind the waste glass with a ball mill for a certain period of time, pass it through a 200-mesh square hole sieve, and take the waste glass powder with a particle size less than 200 mesh as raw material;

[0018] Grind the discarded building ceramic tiles with a ball mill for a certain period of time, pass through a 200-mesh square hole sieve, and take the discarded building tile powder with a particle size less than 200 mesh as raw material;

[0019] The coal gasification fine ash, oil shale tailings, dry sludge, waste glass powder, and waste building ceramic tile powder are mixed in a certain proportion and poured into a three-dimensional mixer for mixing for 10 minutes to obtain a mixed dry material;

[0020] Pour the mixed dry materials into a granulator, add water according to a certain ratio and granulate, control the particle size of the granulation to be 1.0cm-1.5cm, and obtain spherical raw material balls;

[0021] Place the raw material balls in a drying oven and dry them at 105°C for 8 hours;

[0022] The dried raw material balls are placed in a box-type high-temperature furnace, heated from room temperature to 750°C at a heating rate of 10°C / min, kept warm for 20 minutes, and then continued to be heated to 1050°C-1100°C at a heating rate of 10°C / min. After keeping warm for 1 hour, the balls are naturally cooled to room temperature to obtain a spherical environmentally friendly anti-slip material.

[0023] Beneficial effects: coal gasification fine ash, oil shale tailings, sludge, discarded glass, and discarded building ceramic tiles are all solid wastes. The present invention uses the above solid wastes as raw materials after simple preliminary treatment, and prepares anti-skid materials for icy and snowy roads through mixing, granulation, drying, and sintering. The silicon-aluminum chemical components contained in coal gasification fine ash, oil shale tailings, and discarded building tiles provide a certain strength to the anti-skid material after reaction under high temperature conditions, and the unburned carbon contained in the coal gasification fine ash, the organic matter contained in the oil shale tailings, and the organic matter contained in the sludge provide heat for high-temperature sintering, which can reduce energy consumption in the preparation process. At the same time, certain pores are formed in the anti-skid material after sintering. The presence of pores reduces the bulk density and hardness of the anti-skid material. When the anti-skid material is used on icy and snowy roads, even if the anti-skid material splashes due to vehicle driving, it will not cause harm to the passing vehicles behind. When the anti-skid material is thrown on the icy and snowy road, the friction coefficient between the road surface and the vehicle tires is increased, thereby playing an anti-skid role. On the other hand, the anti-skid material is crushed by the vehicle, and the crushed anti-skid material is porous, which increases the contact area between the anti-skid material and the ice and snow and the ground, and is closely combined with the ice and snow. It is not easy to be blown away in the wind, and can still play an anti-skid role. The present invention uses a variety of solid wastes as raw materials, opening up a new way to recycle solid waste resources. In addition, an environmentally friendly anti-skid material for ice and snow roads can be prepared, which has good social and economic benefits. The results of the embodiments show that the environmentally friendly anti-skid material prepared by the present invention has good anti-skid performance compared with the commonly used anti-skid material slag. DETAILED DESCRIPTION

[0024] The present invention provides an environmentally friendly anti-skid material for icy and snowy roads, comprising the following components in parts by weight:

[0025] 100 parts of coal gasification fine ash, 50-100 parts of oil shale tailings, 40-80 parts of dry sludge, 20-40 parts of waste glass, 20-40 parts of waste building ceramic tiles, and 30-50 parts of water.

[0026] The present invention also provides a method for preparing the environmentally friendly anti-slip material according to the above technical solution, comprising the following steps:

[0027] Step 1: Dry the coal gasification fine ash at 105°C for 24 hours until the moisture content is less than 1%, then pass it through a 200-mesh square hole sieve, and take the coal gasification fine ash with a particle size of less than 300 mesh as raw material;

[0028] Step 2: Grind the oil shale tailings with a ball mill for a certain period of time, pass through a 200-mesh square hole sieve, and take the oil shale tailings with a particle size less than 200 mesh as raw material;

[0029] Step 3: The dry sludge is crushed by a crusher and passed through a 200-mesh square hole sieve, and the sludge with a particle size less than 200 mesh is taken as the raw material;

[0030] Step 4: Grind the waste glass with a ball mill for a certain period of time, pass it through a 200-mesh square hole sieve, and take the waste glass powder with a particle size less than 200 mesh as raw material;

[0031] Step 5: Grind the waste building ceramic tiles with a ball mill for a certain period of time, pass through a 200-mesh square hole sieve, and take the waste building tile powder with a particle size less than 200 mesh as the raw material;

[0032] Step 6: Mix the coal gasification fine ash, oil shale tailings, dry sludge, waste glass powder, and waste building ceramic tile powder according to a certain proportion, pour them into a three-dimensional mixer and mix them for 10 minutes to obtain a mixed dry material;

[0033] Step 7: Pour the mixed dry materials into a granulator, slowly add water according to a certain ratio while stirring to granulate, control the particle size of the granulation to 1.0cm-1.5cm, and obtain spherical raw material balls;

[0034] Step 8: Place the raw material balls in a drying oven and dry them at 105°C for 8 hours;

[0035] Step 9: Place the dried raw material ball in a box-type high-temperature furnace, heat it from room temperature to 750°C at a heating rate of 10°C / min, keep it warm for 20 minutes, continue to heat it to 1050°C-1100°C at a heating rate of 10°C / min, keep it warm for 1 hour, and then naturally cool it to room temperature to obtain a spherical environmentally friendly anti-slip material.

[0036] The following is a detailed description of an environmentally friendly anti-skid material for icy and snowy roads and a preparation method thereof provided by the present invention in conjunction with embodiments, but they should not be construed as limiting the scope of protection of the present invention.

[0037] Example 1

[0038] Step 1: Dry 300 kg of coal gasification fine ash at 105°C for 24 hours until the moisture content is less than 1%, then pass through a 200-mesh square hole sieve, and take the coal gasification fine ash with a particle size of less than 300 mesh as raw material;

[0039] Step 2: Grind 300 kg of oil shale tailings with a ball mill for a certain period of time, pass through a 200-mesh square hole sieve, and take the oil shale tailings with a particle size less than 200 mesh as raw material;

[0040] Step 3: 300 kg of dry sludge is crushed by a crusher and passed through a 200-mesh square hole sieve, and the sludge with a particle size less than 200 mesh is taken as the raw material;

[0041] Step 4: Grind 300 kg of waste glass with a ball mill for a certain period of time, pass through a 200-mesh square hole sieve, and take the waste glass powder with a particle size less than 200 mesh as the raw material;

[0042] Step 5: Grind 300 kg of waste building ceramic tiles with a ball mill for a certain period of time, pass through a 200-mesh square hole sieve, and take the waste building tile powder with a particle size less than 200 mesh as the raw material;

[0043] Step 6: Weigh 100 kg of coal gasification fine ash, 50 kg of oil shale tailings, 40 kg of dry sludge, 20 kg of waste glass powder, and 20 kg of waste building ceramic tile powder, mix them according to a certain ratio, pour them into a three-dimensional mixer and mix them for 10 minutes to obtain a mixed dry material;

[0044] Step 7: Pour the mixed dry materials into a granulator, slowly add 30 kg of water while stirring to granulate, control the particle size of the granulation to 1.0 cm-1.5 cm, and obtain spherical raw material balls;

[0045] Step 8: Place the raw material balls in a drying oven and dry them at 105°C for 8 hours;

[0046] Step 9: Place the dried raw material ball in a box-type high-temperature furnace, heat it from room temperature to 750°C at a heating rate of 10°C / min, keep it warm for 20 minutes, continue to heat it to 1100°C at a heating rate of 10°C / min, keep it warm for 1 hour, and then naturally cool it to room temperature to obtain a spherical environmentally friendly anti-slip material.

[0047] The performance of the anti-skid material of the present invention is compared with that of the commonly used slag anti-skid material. The test conditions are as follows: road ice layer thickness: 2mm; spreading amount: 200g / m 2; Vehicle speed: 60km / h; Ambient temperature -20°C. After evenly spreading the slag and the anti-skid material of the present invention, the braking distance was measured to determine the anti-skid effect of the product and the slag anti-skid material. The test results are shown in Table 1.

[0048] Table 1 Comparative experimental results of the anti-skid effect of this product and slag

[0049] Test Project Slag This product Braking distance / m 25.6 22.4

[0050] Judging from the test results, the anti-slip effect of this product is better than slag and has good anti-slip performance.

[0051] Example 2

[0052] Step 1: Dry 300 kg of coal gasification fine ash at 105°C for 24 hours until the moisture content is less than 1%, then pass through a 200-mesh square hole sieve, and take the coal gasification fine ash with a particle size of less than 300 mesh as raw material;

[0053] Step 2: Grind 300 kg of oil shale tailings with a ball mill for a certain period of time, pass through a 200-mesh square hole sieve, and take the oil shale tailings with a particle size less than 200 mesh as raw material;

[0054] Step 3: 300 kg of dry sludge is crushed by a crusher and passed through a 200-mesh square hole sieve, and the sludge with a particle size less than 200 mesh is taken as the raw material;

[0055] Step 4: Grind 300 kg of waste glass with a ball mill for a certain period of time, pass through a 200-mesh square hole sieve, and take the waste glass powder with a particle size less than 200 mesh as the raw material;

[0056] Step 5: Grind 300 kg of waste building ceramic tiles with a ball mill for a certain period of time, pass through a 200-mesh square hole sieve, and take the waste building tile powder with a particle size less than 200 mesh as the raw material;

[0057] Step 6: Weigh 100 kg of coal gasification fine ash, 75 kg of oil shale tailings, 60 kg of dry sludge, 30 kg of waste glass powder, and 30 kg of waste building ceramic tile powder, mix them according to a certain ratio, pour them into a three-dimensional mixer and mix them for 10 minutes to obtain a mixed dry material;

[0058] Step 7: Pour the mixed dry materials into a granulator, slowly add 40 kg of water while stirring to granulate, control the particle size of the granulation to 1.0 cm-1.5 cm, and obtain spherical raw material balls;

[0059] Step 8: Place the raw material balls in a drying oven and dry them at 105°C for 8 hours;

[0060] Step 9: Place the dried raw material ball in a box-type high-temperature furnace, heat it from room temperature to 750°C at a heating rate of 10°C / min, keep it warm for 20 minutes, continue to heat it to 1075°C at a heating rate of 10°C / min, keep it warm for 1 hour, and then naturally cool it to room temperature to obtain a spherical environmentally friendly anti-slip material.

[0061] The performance of the anti-skid material of the present invention is compared with that of the commonly used slag anti-skid material. The test conditions are as follows: road ice layer thickness: 2mm; spreading amount: 200g / m 2 ; Vehicle speed: 60km / h; Ambient temperature -20°C. After evenly spreading the slag and the anti-skid material of the present invention, the braking distance was measured to determine the anti-skid effect of the product and the slag anti-skid material. The test results are shown in Table 2.

[0062] Table 2 Comparison test results of the anti-skid effect of this product and slag

[0063] Test Project Slag This product Braking distance / m 25.6 20.4

[0064] Judging from the test results, the anti-slip effect of this product is better than slag and has good anti-slip performance.

[0065] Example 3

[0066] Step 1: Dry 300 kg of coal gasification fine ash at 105°C for 24 hours until the moisture content is less than 1%, then pass through a 200-mesh square hole sieve, and take the coal gasification fine ash with a particle size of less than 300 mesh as raw material;

[0067] Step 2: Grind 300 kg of oil shale tailings with a ball mill for a certain period of time, pass through a 200-mesh square hole sieve, and take the oil shale tailings with a particle size less than 200 mesh as raw material;

[0068] Step 3: 300 kg of dry sludge is crushed by a crusher and passed through a 200-mesh square hole sieve, and the sludge with a particle size less than 200 mesh is taken as the raw material;

[0069] Step 4: Grind 300 kg of waste glass with a ball mill for a certain period of time, pass through a 200-mesh square hole sieve, and take the waste glass powder with a particle size less than 200 mesh as the raw material;

[0070] Step 5: Grind 300 kg of waste building ceramic tiles with a ball mill for a certain period of time, pass through a 200-mesh square hole sieve, and take the waste building tile powder with a particle size less than 200 mesh as the raw material;

[0071] Step 6: Weigh 100 kg of coal gasification fine ash, 100 kg of oil shale tailings, 80 kg of dry sludge, 40 kg of waste glass powder, and 40 kg of waste building ceramic tile powder, mix them according to a certain ratio, pour them into a three-dimensional mixer and mix them for 10 minutes to obtain a mixed dry material;

[0072] Step 7: Pour the mixed dry materials into a granulator, slowly add 50 kg of water while stirring to granulate, control the particle size of the granulation to 1.0 cm-1.5 cm, and obtain spherical raw material balls;

[0073] Step 8: Place the raw material balls in a drying oven and dry them at 105°C for 8 hours;

[0074] Step 9: Place the dried raw material ball in a box-type high-temperature furnace, heat it from room temperature to 750°C at a heating rate of 10°C / min, keep it warm for 20 minutes, continue to heat it to 1050°C at a heating rate of 10°C / min, keep it warm for 1 hour, and then naturally cool it to room temperature to obtain a spherical environmentally friendly anti-slip material.

[0075] The performance of the anti-skid material of the present invention is compared with that of the commonly used slag anti-skid material. The test conditions are as follows: road ice layer thickness: 2mm; spreading amount: 200g / m 2 ; Vehicle speed: 60km / h; Ambient temperature -20°C. After evenly spreading the slag and the anti-skid material of the present invention, the braking distance was measured to determine the anti-skid effect of the product and the slag anti-skid material. The test results are shown in Table 3.

[0076] Table 3 Comparative experimental results of the anti-skid effect of this product and slag

[0077] Test Project Slag This product Braking distance / m 25.6 21.4

[0078] Judging from the test results, the anti-slip effect of this product is better than slag and has good anti-slip performance.

[0079] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. An environmentally friendly anti-skid material for icy and snowy roads, characterized by: The environmentally friendly anti-slip material is composed of the following components by weight: 100 parts of coal gasification fine ash, 50-100 parts of oil shale tailings, 40-80 parts of dry sludge, 20-40 parts of waste glass, 20-40 parts of waste building ceramic tiles, and 30-50 parts of water; The coal gasification fine ash is fine ash with a particle size of less than 50 μm produced in the coal gasification process, wherein the mass fraction of SiO2 in the chemical composition is greater than 40%, the mass fraction of Al2O3 is greater than 15%, and the loss on ignition is greater than 20%; The oil shale tailings are small particles of oil shale with a particle size of less than 2 cm remaining when shale oil is produced by dry distillation of oil shale, wherein the mass fraction of SiO2 in the chemical composition is greater than 50%, the mass fraction of Al2O3 is greater than 12%, and the high calorific value (dry basis) is greater than 3.0 MJ / Kg; The dry sludge is solid sediment produced in the sewage treatment process, and after drying, the moisture content of the dry sludge is less than 1%, and the loss on ignition is greater than 40%; The waste glass is waste soda-lime glass products used in daily life, wherein the mass fraction of SiO2 in the chemical composition is greater than 60%, and the mass fraction of Na2O is greater than 10%; The waste building ceramic tiles come from building roof tiles.

2. The method for preparing an environmentally friendly anti-skid material for icy and snowy roads according to claim 1, characterized in that: The following steps are involved: The coal gasification fine ash is dried at 105°C for 24 hours until the moisture content is less than 1%, and then passed through a 200-mesh square hole sieve, and the coal gasification fine ash with a particle size of less than 300 mesh is taken as the raw material; The oil shale tailings are ground by a ball mill for a certain period of time, passed through a 200-mesh square-hole sieve, and the oil shale tailings with a particle size less than 200 mesh are taken as raw materials; The dry sludge is crushed by a crusher and passed through a 200-mesh square hole sieve, and the sludge with a particle size less than 200 mesh is taken as the raw material; Grind the waste glass with a ball mill for a certain period of time, pass it through a 200-mesh square hole sieve, and take the waste glass powder with a particle size less than 200 mesh as raw material; Grind the discarded building ceramic tiles with a ball mill for a certain period of time, pass through a 200-mesh square hole sieve, and take the discarded building tile powder with a particle size less than 200 mesh as raw material; The coal gasification fine ash, oil shale tailings, dry sludge, waste glass powder, and waste building ceramic tile powder are mixed in a certain proportion and poured into a three-dimensional mixer for mixing for 10 minutes to obtain a mixed dry material; Pour the mixed dry materials into a granulator, add water according to a certain ratio and granulate, control the particle size of the granulation to be 1.0cm-1.5cm, and obtain spherical raw material balls; Place the raw material balls in a drying oven and dry them at 105°C for 8 hours; The dried raw material balls are placed in a box-type high-temperature furnace, heated from room temperature to 750°C at a heating rate of 10°C / min, kept warm for 20 minutes, and then continued to be heated to 1050°C-1100°C at a heating rate of 10°C / min. After keeping warm for 1 hour, the balls are naturally cooled to room temperature to obtain a spherical environmentally friendly anti-slip material.

Citation Information

Patent Citations

  • Method for burning haydite by solid castoff

    CN101215150A

  • Pavement self icebreaking anti-slip pavement layer mixed material and preparation method thereof

    CN102432228A

  • Novel ceramic particle composite resin-based heat-resistance recession friction material and preparation method thereof

    CN106928649A

  • Sludge-based high-strength ceramsite and preparation method thereof

    CN110963783A

  • Antislip material spinkled over frozen road

    JP1994145651A