Hollow brick prepared based on recycled foundry waste sand and preparation method thereof

By distinguishing the foundry waste sand and treating it with specific processes, highly efficient hollow bricks are prepared, which solves the limitations of different types of waste sand treatment in the existing technology and achieves efficient recovery of resources and high performance of the finished product.

CN118754606AInactive Publication Date: 2024-10-11MAANSHAN LVKE ENVIRONMENTAL PROTECTION TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410756889.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-13
Publication Date
2024-10-11
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing technology cannot effectively handle different types of foundry waste sand, resulting in greater limitations in the production line and difficulty in realizing resource utilization.

Method used

By distinguishing the foundry waste sand and using specific reuse technology, regeneration technology and resource utilization technology, we can prepare a mixture of foundry waste sand, Portland cement, glass fiber, fly ash, aluminum oxide, aluminum hydroxide, The hollow bricks composed of quicklime and colorant use plasticizer to improve the plasticity and bonding ability of the raw materials, and are formed into shaped hollow bricks through multi-stage crushing, aging, mixing and vacuum extrusion processes.

Benefits of technology

It achieves the effective reuse and resource utilization of different types of foundry waste sand, improves the regeneration rate of waste sand and the compressive strength of finished products, and meets the needs for efficient resource utilization.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a hollow brick prepared based on recycled foundry waste sand and a preparation method of the hollow brick, and belongs to the technical field of foundry waste sand recycling. The invention discloses a hollow brick prepared based on recycled foundry waste sand and a preparation method thereof, and the hollow brick is prepared from the following raw materials in parts by weight: 35-55 parts of foundry waste sand, 20-35 parts of silicate cement, 10-15 parts of glass fiber, 10-12 parts of fly ash, 9-12 parts of aluminum oxide, 5-6 parts of aluminum hydroxide, 5-6 parts of quick lime and 3-6 parts of a coloring agent. In order to solve the problem that the whole production line is greatly limited due to the facts that existing casting waste sand is various in variety, and different types of waste sand cannot be effectively treated at the same time through a single recycling process, the types of the casting waste sand are distinguished; corresponding recycling technology, regeneration technology and resource utilization technology can be provided for different types of casting waste sand and dedusting ash.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of foundry waste sand recovery, in particular to hollow bricks prepared based on recovered foundry waste sand and a preparation method thereof. Background Art

[0002] Foundry sand is the most important auxiliary material in foundry production. Its life cycle generally begins from leaving nature to being completely discarded.

[0003] At present, there are three types of molding sand processes commonly used in casting production, namely clay sand, resin sand and water glass sand. According to the different components added during sand mixing, the main components that the waste sand may contain, and the properties of various types of waste sand, the composition and properties of casting waste sand directly determine the required subsequent treatment, possible disposal methods and the possibility of resource utilization. The composition of clay sand waste sand is relatively simple. The main difference from new sand is that the particles are fine and the particle size distribution is uneven, and the ash content is high. Therefore, when the requirements for particle size distribution and ash content are not high, it is feasible to use some clay sand waste sand to replace natural sand. Due to the addition of chemical binders (water glass or resin) to water glass sand and resin sand, the waste sand has a more complex composition on the one hand, and on the other hand, most of them are still in agglomerate form after falling sand and have high mechanical strength. Generally, it is difficult to restore the performance of the waste sand by mechanical crushing alone (water glass sand is washed and resin sand is roasted at high temperature to obtain a better regeneration effect). Therefore, it is quite different from natural sand and more difficult to utilize as a resource.

[0004] There are many types of existing foundry waste sand, and a single recycling process cannot effectively process different types of waste sand at the same time, which leads to great limitations in the entire production line. Summary of the invention

[0005] The purpose of the present invention is to provide hollow bricks prepared based on recycled foundry waste sand and a preparation method thereof. By distinguishing the types of foundry waste sand, different types of foundry waste sand and dust ash can have corresponding recycling technology, regeneration technology and resource utilization technology, which can solve the problems in the prior art.

[0006] To achieve the above-mentioned purpose, the present invention provides the following technical solution: a hollow brick prepared based on recycled foundry waste sand, which is made of the following raw materials in parts by weight: 35-55 parts of foundry waste sand, 20-35 parts of silicate cement, 10-15 parts of glass fiber, 10-12 parts of fly ash, 9-12 parts of alumina, 5-6 parts of aluminum hydroxide, 5-6 parts of quicklime and 3-6 parts of colorant.

[0007] A method for preparing hollow bricks based on recycled foundry waste sand comprises the following steps:

[0008] Step 1: Weigh the foundry waste sand, silicate cement, glass fiber and other raw materials accurately according to a certain proportion, and then put them into the batching tank. During the batching process, it is necessary to adjust according to the strength and other characteristics of the brick body. Then put the raw materials with good proportion into the mixer and mix them fully to form a uniform mortar. The mixing time is 3-5 minutes;

[0009] Step 2: The pulverized, mixed, and properly watered mud is piled up and stored in a material warehouse for more than 72 hours to allow the water to fully penetrate, the mud to be loosened, and homogenized. The aging mixture is sent to a box feeder by a bucket excavator for buffering, and then evenly fed to a double-shaft mixer for proper water addition and stirring to ensure that its moisture content does not exceed 16%;

[0010] Step 3: After the secondary water addition and stirring, the raw materials are sent to a double-stage vacuum brick extruder for extrusion and molding, and then the molded mud strips are injected into the hollow brick mold, and a press is used to pressurize the raw materials in the hollow brick mold to form it;

[0011] Step 4: Stack the formed wet billets on the kiln car and park them on the static parking line for a period of time to reduce the moisture content of the wet billets, increase the uniformity of moisture in the wet billets, and improve the strength of the wet billets;

[0012] Step 5: The bricks are sent to the drying kiln for drying by the kiln car. The drying time is 24-26 hours. The heat source of the drying kiln comes from the waste heat of the roasting kiln. The dried bricks enter the roasting kiln with the kiln car. The firing temperature is 700-780℃ and the firing cycle is 27-28 hours.

[0013] Preferably, in step one, the raw materials are crushed by roller crushing equipment before proportioning, forming a three-level crushing process of coarse, medium and fine, and the maximum particle size is controlled below 2 mm. The crushed raw materials are evenly fed and stirred with water before being sent to an aging warehouse for aging.

[0014] Preferably, the cage-shaped crusher is used to finely crush various shales that are relatively hard and have a relatively high natural water content;

[0015] Roller mills are used to crush soft shales with high natural water content;

[0016] Dry ball mill is used to grind hard coal gangue or shale with natural moisture content less than 3%;

[0017] Jaw crusher or larger impact crusher to crush medium hardness or above coal gangue or shale;

[0018] Roller mills are used to crush soft shales and clays.

[0019] Preferably, in the step 1, a wheel mill is used to grind the clay material after it is crushed.

[0020] Preferably, in step one, a plasticizing material is used as an additive material to improve the plasticity, bonding ability and fluidity of the raw materials.

[0021] Compared with the prior art, the present invention has the following beneficial effects:

[0022] 1. The present invention distinguishes the types of foundry waste sand, and different types of foundry waste sand and dust removal ash can have corresponding recycling technology, regeneration technology and resource utilization technology;

[0023] 2. The present invention uses plasticizers as additives to improve the plasticity, binding capacity and fluidity of raw materials. Most inorganic plasticizers are plasticized by changing the pH value and the adsorbed cations on the surface of raw material particles, thereby affecting the thickness of the hydration film. The molecules of organic plasticizers can generate a hydration film in an aqueous solution and are firmly adsorbed on the surface of raw material particles, so that a layer of hydration film and a highly viscous polymer are formed on the surface of the particles, thereby effectively improving the plasticity and binding capacity of the raw materials.

[0024] 3. According to the present invention, for raw materials with too high plasticity index, coal ash, slag, fly ash or waste brick powder can be appropriately added to thin them. For raw materials with poor plasticity index, they should be mined in advance, naturally weathered, appropriately increased in fineness, watered to loosen, and improved by mechanical methods such as stirring, rolling, aging, mixing, and extrusion. Clay and shale powder with high plasticity index can also be appropriately added to adjust the overall plasticity index of the mixture. When producing fly ash bricks, bentonite can also be appropriately added as a binder so that a thin layer of bentonite is adhered to the surface of each fly ash particle. The plasticity is improved by mixing, homogenizing, and extruding to meet the molding requirements. DETAILED DESCRIPTION

[0025] Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in the field without making any creative work shall fall within the scope of protection of the present invention.

[0026] Embodiment 1:

[0027] A hollow brick prepared based on recycled foundry waste sand is made of the following raw materials in parts by weight: 35 parts of foundry waste sand, 20 parts of silicate cement, 10 parts of glass fiber, 10 parts of fly ash, 9 parts of aluminum oxide, 5 parts of aluminum hydroxide, 5 parts of quicklime and 3 parts of colorant.

[0028] The thermal regeneration method of foundry waste sand adopts the following steps:

[0029] S1: The waste sand is first crushed by a crusher, and then put into a screening and magnetic separation device for screening. The screened sand is calcined at 550-650℃, and then cooled and screened to obtain regenerated sand with a particle diameter of less than 2mm;

[0030] S2: During the high-temperature roasting process of self-hardening alkali phenolic resin sand casting waste sand regeneration, chemical additives should be added to neutralize the influence of residual alkali.

[0031] A method for preparing hollow bricks based on recycled foundry waste sand comprises the following steps:

[0032] Step 1: Weigh the foundry waste sand, silicate cement, glass fiber and other raw materials accurately according to a certain proportion, and then put them into the batching tank. During the batching process, it is necessary to adjust according to the strength and other characteristics of the brick body. Then put the raw materials with good proportion into the mixer and mix them fully to form a uniform mortar. The mixing time is 3-5 minutes;

[0033] The wheel mill is used to grind the mud after it is crushed;

[0034] The raw materials are crushed by roller crushing equipment before proportioning, forming a three-level crushing process of coarse, medium and fine. The maximum particle size is controlled below 2mm. The crushed raw materials are evenly fed and stirred with water before being sent to the aging warehouse for aging.

[0035] Cage crusher is used to crush various hard shales with high natural water content;

[0036] Roller mills are used to crush soft shales with high natural water content;

[0037] Dry ball mill is used to grind hard coal gangue or shale with natural moisture content less than 3%;

[0038] Jaw crusher or larger impact crusher to crush medium hardness or above coal gangue or shale;

[0039] Toothed roller mill to crush soft shale and clay;

[0040] Plasticizers are additives that improve the plasticity, binding ability and fluidity of raw materials. Inorganic plasticizers are mostly plasticized by changing the pH value and the adsorbed cations on the surface of raw material particles, thereby affecting the thickness of the hydration film. The molecules of organic plasticizers can form a hydration film in aqueous solution and are firmly adsorbed on the surface of raw material particles, so that there is a layer of hydration film and highly viscous polymers on the surface of the particles, thereby effectively improving the plasticity and binding ability of the raw materials;

[0041] Step 2: The pulverized, mixed, and properly watered mud is piled up and stored in a material warehouse for more than 72 hours to allow the water to fully penetrate, the mud to be loosened, and homogenized. The aging mixture is sent to a box feeder by a bucket excavator for buffering, and then evenly fed to a double-shaft mixer for proper water addition and stirring to ensure that its moisture content does not exceed 16%;

[0042] The plasticity of the powder is achieved by the full mixing and penetration of water. The main function of adding water and stirring is to fully mix the water and powder, and try to make the water fully penetrate into the interior of each powder to form the plasticity required for molding;

[0043] According to the test, for the same raw materials, the drying cracks of the extruded bricks are as high as 4% after stirring for only two minutes, while when stirred for more than 3 minutes, under the same conditions, the drying cracks are only 1%. The powerful mixer stirs the mud and then forces it to extrude through the double-screw mud cylinder, so that the water can penetrate better in the mud particles and the effect is better.

[0044] Step 3: After the secondary water addition and stirring, the raw materials are sent to a double-stage vacuum brick extruder for extrusion and molding, and then the molded mud strips are injected into the hollow brick mold, and a press is used to pressurize the raw materials in the hollow brick mold to form it;

[0045] Step 4: Stack the formed wet billets on the kiln car and park them on the static parking line for a period of time to reduce the moisture content of the wet billets, increase the uniformity of moisture in the wet billets, and improve the strength of the wet billets;

[0046] Step 5: The bricks are sent to the drying kiln for drying by the kiln car. The drying time is 24-26 hours. The heat source of the drying kiln comes from the waste heat of the roasting kiln. The dried bricks enter the roasting kiln with the kiln car. The firing temperature is 700-780℃ and the firing cycle is 27-28 hours.

[0047] Embodiment 2:

[0048] A hollow brick prepared based on recycled foundry waste sand is made of the following raw materials in parts by weight: 35 parts of foundry waste sand, 20 parts of silicate cement, 10 parts of glass fiber, 10 parts of fly ash, 9 parts of aluminum oxide, 5 parts of aluminum hydroxide, 5 parts of quicklime and 3 parts of colorant.

[0049] The thermal regeneration method of foundry waste sand adopts the following steps:

[0050] S1: After the foundry waste sand is roughly crushed by a vibrating bed, the larger metal blocks are magnetically selected; the second time, it is finely crushed by a drum crusher to less than 8mm, and fine iron sand is selected;

[0051] S2: calcining at 650-700°C, cooling in a cooling flow tank and then mechanically grinding;

[0052] S3: After dust removal by wind, the regenerated sand with suitable particle size is screened out, cooled in a cooler and then stored.

[0053] A method for preparing hollow bricks based on recycled foundry waste sand comprises the following steps:

[0054] Step 1: Weigh the foundry waste sand, silicate cement, glass fiber and other raw materials accurately according to a certain proportion, and then put them into the batching tank. During the batching process, it is necessary to adjust according to the strength and other characteristics of the brick body. Then put the raw materials with good proportion into the mixer and mix them fully to form a uniform mortar. The mixing time is 3-5 minutes;

[0055] The wheel mill is used to grind the mud after it is crushed;

[0056] The raw materials are crushed by roller crushing equipment before proportioning, forming a three-level crushing process of coarse, medium and fine. The maximum particle size is controlled below 2mm. The crushed raw materials are evenly fed and stirred with water before being sent to the aging warehouse for aging.

[0057] Cage crusher is used to crush various hard shales with high natural water content;

[0058] Roller mills are used to crush soft shales with high natural water content;

[0059] Dry ball mill is used to grind hard coal gangue or shale with natural moisture content less than 3%;

[0060] Jaw crusher or larger impact crusher to crush medium hardness or above coal gangue or shale;

[0061] Toothed roller mill to crush soft shale and clay;

[0062] Plasticizers are additives that improve the plasticity, binding ability and fluidity of raw materials. Inorganic plasticizers are mostly plasticized by changing the pH value and the adsorbed cations on the surface of raw material particles, thereby affecting the thickness of the hydration film. The molecules of organic plasticizers can form a hydration film in aqueous solution and are firmly adsorbed on the surface of raw material particles, so that there is a layer of hydration film and highly viscous polymers on the surface of the particles, thereby effectively improving the plasticity and binding ability of the raw materials;

[0063] Step 2: The pulverized, mixed, and properly watered mud is piled up and stored in a material warehouse for more than 72 hours to allow the water to fully penetrate, the mud to be loosened, and homogenized. The aging mixture is sent to a box feeder by a bucket excavator for buffering, and then evenly fed to a double-shaft mixer for proper water addition and stirring to ensure that its moisture content does not exceed 16%;

[0064] The plasticity of the powder is achieved by the full mixing and penetration of water. The main function of adding water and stirring is to fully mix the water and powder, and try to make the water fully penetrate into the interior of each powder to form the plasticity required for molding;

[0065] According to the test, for the same raw materials, the drying cracks of the extruded bricks are as high as 4% after stirring for only two minutes, while when stirred for more than 3 minutes, under the same conditions, the drying cracks are only 1%. The powerful mixer stirs the mud and then forces it to extrude through the double-screw mud cylinder, so that the water can penetrate better in the mud particles and the effect is better.

[0066] Step 3: After the secondary water addition and stirring, the raw materials are sent to a double-stage vacuum brick extruder for extrusion and molding, and then the molded mud strips are injected into the hollow brick mold, and a press is used to pressurize the raw materials in the hollow brick mold to form it;

[0067] Step 4: Stack the formed wet billets on the kiln car and park them on the static parking line for a period of time to reduce the moisture content of the wet billets, increase the uniformity of moisture in the wet billets, and improve the strength of the wet billets;

[0068] Step 5: The bricks are sent to the drying kiln for drying by the kiln car. The drying time is 24-26 hours. The heat source of the drying kiln comes from the waste heat of the roasting kiln. The dried bricks enter the roasting kiln with the kiln car. The firing temperature is 700-780℃ and the firing cycle is 27-28 hours.

[0069] Embodiment 3:

[0070] A hollow brick prepared based on recycled foundry waste sand is made of the following raw materials in parts by weight: 35 parts of foundry waste sand, 20 parts of silicate cement, 10 parts of glass fiber, 10 parts of fly ash, 9 parts of aluminum oxide, 5 parts of aluminum hydroxide, 5 parts of quicklime and 3 parts of colorant.

[0071] The thermal regeneration method of foundry waste sand adopts the following steps:

[0072] S1: After the inorganic casting waste sand is crushed, it is passed through a screening machine to remove metal blocks; then it is passed through a fine screen to remove metal chips, and the waste sand is heated to above 150-220℃, and the inorganic binder film on the surface of the waste sand is removed by mechanical grinding or impact;

[0073] S2: calcined at 650-700℃ to remove the residual inorganic binder activity;

[0074] S3: Remove the residual activity of inorganic binder, cool it through cooling flow trough, and then sieve it to obtain regenerated sand.

[0075] A method for preparing hollow bricks based on recycled foundry waste sand comprises the following steps:

[0076] Step 1: Weigh the foundry waste sand, silicate cement, glass fiber and other raw materials accurately according to a certain proportion, and then put them into the batching tank. During the batching process, it is necessary to adjust according to the strength and other characteristics of the brick body. Then put the raw materials with good proportion into the mixer and mix them fully to form a uniform mortar. The mixing time is 3-5 minutes;

[0077] The wheel mill is used to grind the mud after it is crushed;

[0078] The raw materials are crushed by roller crushing equipment before proportioning, forming a three-level crushing process of coarse, medium and fine. The maximum particle size is controlled below 2mm. The crushed raw materials are evenly fed and stirred with water before being sent to the aging warehouse for aging.

[0079] Cage crusher is used to crush various hard shales with high natural water content;

[0080] Roller mills are used to crush soft shales with high natural water content;

[0081] Dry ball mill is used to grind hard coal gangue or shale with natural moisture content less than 3%;

[0082] Jaw crusher or larger impact crusher to crush medium hardness or above coal gangue or shale;

[0083] Toothed roller mill to crush soft shale and clay;

[0084] Plasticizers are additives that improve the plasticity, binding ability and fluidity of raw materials. Inorganic plasticizers are mostly plasticized by changing the pH value and the adsorbed cations on the surface of raw material particles, thereby affecting the thickness of the hydration film. The molecules of organic plasticizers can form a hydration film in aqueous solution and are firmly adsorbed on the surface of raw material particles, so that there is a layer of hydration film and highly viscous polymers on the surface of the particles, thereby effectively improving the plasticity and binding ability of the raw materials;

[0085] Step 2: The pulverized, mixed, and properly watered mud is piled up and stored in a material warehouse for more than 72 hours to allow the water to fully penetrate, the mud to be loosened, and homogenized. The aging mixture is sent to a box feeder by a bucket excavator for buffering, and then evenly fed to a double-shaft mixer for proper water addition and stirring to ensure that its moisture content does not exceed 16%;

[0086] The plasticity of the powder is achieved by the full mixing and penetration of water. The main function of adding water and stirring is to fully mix the water and powder, and try to make the water fully penetrate into the interior of each powder to form the plasticity required for molding;

[0087] According to the test, for the same raw materials, the drying cracks of the extruded bricks are as high as 4% after stirring for only two minutes, while when stirred for more than 3 minutes, under the same conditions, the drying cracks are only 1%. The powerful mixer stirs the mud and then forces it to extrude through the double-screw mud cylinder, so that the water can penetrate better in the mud particles and the effect is better.

[0088] Step 3: After the secondary water addition and stirring, the raw materials are sent to a double-stage vacuum brick extruder for extrusion and molding, and then the molded mud strips are injected into the hollow brick mold, and a press is used to pressurize the raw materials in the hollow brick mold to form it;

[0089] Step 4: Stack the formed wet billets on the kiln car and park them on the static parking line for a period of time to reduce the moisture content of the wet billets, increase the uniformity of moisture in the wet billets, and improve the strength of the wet billets;

[0090] Step 5: The bricks are sent to the drying kiln for drying by the kiln car. The drying time is 24-26 hours. The heat source of the drying kiln comes from the waste heat of the roasting kiln. The dried bricks enter the roasting kiln with the kiln car. The firing temperature is 700-780℃ and the firing cycle is 27-28 hours.

[0091] Waste sand recovery rate Reproduction rate Compressive strength Example 1 56% 96% 5.36 Example 2 77% 96% 6.17 Example 3 71% 98% 5.84

[0092] It can be seen from the above table that by distinguishing the types of foundry waste sand, it can be divided into clay sand, resin sand, inorganic metal sand and glass sand. Different types of foundry waste sand and dust ash can have corresponding reuse technology, regeneration technology and resource utilization technology.

[0093] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.

[0094] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A hollow brick prepared based on recycled foundry waste sand, characterized in that: The invention is prepared from the following raw materials in parts by weight: 35-55 parts of foundry waste sand, 20-35 parts of silicate cement, 10-15 parts of glass fiber, 10-12 parts of fly ash, 9-12 parts of aluminum oxide, 5-6 parts of aluminum hydroxide, 5-6 parts of quicklime and 3-6 parts of colorant.

2. A method for preparing hollow bricks based on recycled foundry waste sand, characterized in that: The method for preparing the hollow bricks prepared based on recycled foundry waste sand according to claim 1 comprises the following steps: Step 1: Weigh the foundry waste sand, silicate cement, glass fiber and other raw materials accurately according to a certain proportion, and then put them into the batching tank. During the batching process, it is necessary to adjust according to the strength and other characteristics of the brick body. Then put the raw materials with good proportion into the mixer and mix them fully to form a uniform mortar. The mixing time is 3-5 minutes; Step 2: The pulverized, mixed, and properly watered mud is piled up and stored in a material warehouse for more than 72 hours to allow the water to fully penetrate, the mud to be loosened, and homogenized. The aging mixture is sent to a box feeder by a bucket excavator for buffering, and then evenly fed to a double-shaft mixer for proper water addition and stirring to ensure that its moisture content does not exceed 16%; Step 3: After the secondary water addition and stirring, the raw materials are sent to a double-stage vacuum brick extruder for extrusion and molding, and then the molded mud strips are injected into the hollow brick mold, and a press is used to pressurize the raw materials in the hollow brick mold to form it; Step 4: Stack the formed wet billets on the kiln car and park them on the static parking line for a period of time to reduce the moisture content of the wet billets, increase the uniformity of moisture in the wet billets, and improve the strength of the wet billets; Step 5: The bricks are sent to the drying kiln for drying by the kiln car. The drying time is 24-26 hours. The heat source of the drying kiln comes from the waste heat of the roasting kiln. The dried bricks enter the roasting kiln with the kiln car. The firing temperature is 700-780℃ and the firing cycle is 27-28 hours.

3. The method for preparing hollow bricks based on recycled foundry waste sand according to claim 2, characterized in that: In the step 1, the raw materials are crushed by roller crushing equipment before proportioning, forming a three-level crushing process of coarse, medium and fine, and the maximum particle size is controlled below 2 mm. The crushed raw materials are evenly fed and stirred with water before being sent to the aging warehouse for aging.

4. The method for preparing hollow bricks based on recycled foundry waste sand according to claim 3, characterized in that: The cage crusher is used to crush various shales that are relatively hard and have a high natural water content; Roller mills are used to crush soft shales with high natural water content; Dry ball mill is used to grind hard coal gangue or shale with natural moisture content less than 3%; Jaw crusher or larger impact crusher to crush medium hardness or above coal gangue or shale; Toothed roller mill is used to crush soft shale and clay.

5. The method for preparing hollow bricks based on recycled foundry waste sand according to claim 2, characterized in that: In the step 1, a wheel mill is used to grind the mud material after it is crushed.

6. The method for preparing hollow bricks based on recycled foundry waste sand according to claim 2, characterized in that: In the step 1, a plasticizing material is used as an additive material to improve the plasticity, bonding ability and fluidity of the raw materials.