Annular boron carbide-aluminum oxide pellet as well as near-net-size forming preparation method and application thereof

Through wet ball milling and dry isostatic pressing combined with gradient temperature sintering process, the complexity and shrinkage unevenness problems in the preparation of cyclic boron carbide-alumina core blocks are solved, and high precision, low grinding volume and High-strength pellet molding promotes the industrial production of nuclear fuel components.

CN118754622APending Publication Date: 2024-10-11GRINM RESOURCES & ENVIRONMENT TECH CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202410915907.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-09
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

It is difficult to effectively prepare cyclic boron carbide-alumina pellets that meet the high-precision requirements of nuclear fuel elements with existing technology. The preparation process is complex and difficult to industrialize, and it is difficult to achieve uniform shrinkage and high strength of the pellets.

Method used

Use wet ball milling to mix B4C, Al2O3 and sintering aids, add surface modifiers to form a modulated slurry, prepare spherical composite powder through spray granulation, use dry isostatic pressing to press thin-walled tube green bodies, and pass through gradient The temperature-raising sintering process controls the shrinkage and density of the core blocks to achieve near-net size molding.

Benefits of technology

It achieves high-precision molding of cyclic boron carbide-alumina pellets, reduces processing margin and difficulty, meets the size, composition and strength requirements of nuclear fuel elements, simplifies the preparation process, and is suitable for industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118754622A_ABST
    Figure CN118754622A_ABST
Patent Text Reader

Abstract

The invention provides an annular boron carbide-aluminum oxide pellet and a near-net-size forming preparation method and application thereof.The annular boron carbide-aluminum oxide pellet is prepared by the steps that B4C, Al2O3 and a sintering aid are mixed to be uniform through wet ball milling, then a surface modifier is added for further ball milling to form prepared slurry, the prepared slurry is subjected to spray granulation to form spherical composite powder, and the spherical composite powder is prepared into the annular boron carbide-aluminum oxide pellet. Performing dry isostatic pressing on the spherical composite powder to form a thin-walled tube green body; gradient heating sintering and surface finish machining are conducted on the thin-walled tube green body, and finally the annular boron carbide-aluminum oxide pellet is obtained; due to the addition of the surface modifier, the uniformity of the prepared slurry and the flowability of spherical composite powder formed by spray granulation can be improved; during high-temperature sintering, it is ensured that a surface modifier is completely removed by setting a reasonable heat preservation point, in the sintering densification process, medium-temperature section (1200 DEG C) heat preservation is preferably conducted in a micro-positive-pressure argon atmosphere, then the temperature is increased to 1400-1600 DEG C for sintering, and changes of deformation, density and inner diameter shrinkage of the pellet are accurately controlled.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of nuclear industry combustible poison pellet materials, and in particular to a ring-shaped boron carbide-alumina pellet and a near-net-size molding preparation method and application. Background Art

[0002] In nuclear fuel elements, burnable poison assemblies are used to compensate for part of the residual reactivity of the core, reduce the boron concentration in the coolant to maintain the negative temperature coefficient of the reactor moderator, flatten the core neutron flux distribution, extend the refueling cycle, and improve the fuel cycle economy.

[0003] The water-permeable annular combustible poison boron carbide-alumina pellets are used in the first nuclear fuel elements of AP1000 and CAP1400, which can improve the effectiveness of combustible poisons and reduce fuel cycle costs. The length of the alumina-boron carbide pellets is 10-51mm, the wall thickness is only about 0.5mm, and the preparation process is complicated. Existing molding methods such as extrusion molding, gel injection molding, stamping molding, injection molding, etc. have complex powder slurry or mud preparation processes and high difficulty in controlling the concentricity / straightness of the pellet green body, making it difficult to industrialize. In addition, the pellets need to shrink evenly during the sintering process to reduce internal stress and meet the requirements of low deformation and high strength. This places high requirements on the matching of powder uniformity and fluidity, the inner and outer diameter design of the molding mold, and the sintering process parameters.

[0004] Due to the high-precision size, composition, strength and other technical requirements of the annular alumina-boron carbide pellets, the engineering difficulty of its preparation is relatively high, and there is no engineering preparation technology and commercial products in China. Therefore, it is urgent to develop a new near-net-size molding preparation method for annular boron carbide-alumina pellets to promote the technology towards engineering and industrialization, so as to achieve the strategic goal of mass production of nuclear fuel elements. Summary of the invention

[0005] In view of the above problems existing in the prior art, the present invention provides a ring-shaped boron carbide-alumina pellet and a near-net-size molding preparation method and application, so as to obtain a ring-shaped boron carbide-alumina pellet that meets the high-precision requirements of nuclear fuel combustible poisons in terms of size, composition and strength.

[0006] The specific content of the invention is as follows:

[0007] In a first aspect, the present invention provides a near-net-size molding preparation method for annular boron carbide-alumina pellets, the preparation method comprising the following steps:

[0008] S1. After mixing B4C, Al2O3 and a sintering aid, deionized water is added at a water-to-material ratio of 1-3:1, and wet ball milling is performed for 2-3 hours to obtain a premixed slurry; among the B4C, Al2O3 and the sintering aid, the mass proportion of B4C is 13-15%, the mass proportion of Al2O3 is 82-84%, and the mass proportion of the sintering aid is 1-4%;

[0009] S2, adding a surface modifier to the premixed slurry, continuing ball milling for 1-3 hours, and mixing evenly to form a modulated slurry with a solid content of 40-50%;

[0010] S3, preparing the prepared slurry into spherical composite powder with a particle size of 20-50 μm by spray granulation;

[0011] S4, using dry isostatic pressing method to press the spherical composite powder to obtain a spherical composite powder with an inner diameter of 7.3-7.4 mm, a wall thickness of 1.6 mm, and a bulk density of 2.05-2.20 g / cm 3 Thin-walled tube green body;

[0012] S5, performing gradient temperature sintering on the thin-walled tube green body to obtain a crude pellet;

[0013] S6, performing surface finishing on the crude pellets to obtain annular boron carbide-alumina pellets;

[0014] The gradient temperature sintering includes a first sintering and a second sintering. The first sintering includes: in a vacuum atmosphere, heating to 650°C at 2-3°C / min, keeping warm for 2-3 hours, and continuing to heat to 950°C at 2-3°C / min, and keeping warm for 2-3 hours; the second sintering includes: in an argon atmosphere, heating to 1200°C at 1-2°C / min, keeping warm for 2-3 hours, and continuing to heat to 1400-1600°C at 1-3°C / min, and keeping warm for 1-3 hours.

[0015] Optionally, the surface modifier includes a wetting agent, a dispersant and a binder;

[0016] The moisturizing agent is polyethylene glycol;

[0017] The dispersant is polyethylene glycol tert-octylphenyl ether;

[0018] The binder is polyvinyl alcohol;

[0019] The sintering aid is SiO2 or MgSiO3.

[0020] Optionally, the ball-to-material ratio of the wet ball milling is 1 to 3:1.

[0021] Optionally, the spherical composite powder is pressed by dry isostatic pressing at a pressure of 110-140 MPa.

[0022] Optionally, the second sintering is performed in an argon atmosphere at a pressure of 0.1-0.2 MPa.

[0023] Optionally, the gradient temperature rising sintering is performed by buried firing or vertical firing.

[0024] Optionally, the surface finishing method includes: centerless grinder and / or surface grinder and / or wire cutting, deionized water ultrasonic cleaning and drying treatment.

[0025] In a second aspect, the present invention provides an annular boron carbide-alumina pellet block, wherein the annular boron carbide-alumina pellet block is obtained by the preparation method described in the first aspect.

[0026] Optionally, the volume density of the annular boron carbide-alumina pellet is 2.27-2.47 g / cm 3 , the compressive strength is not less than 69Mpa.

[0027] In a third aspect, the present invention provides an application of an annular boron carbide-alumina pellet, wherein the annular boron carbide-alumina pellet obtained by the preparation method described in the first aspect is used as a burnable poison for nuclear fuel assemblies, or as other neutron absorbers.

[0028] Compared with the prior art, the present invention has the following advantages:

[0029] The invention provides a near-net-size molding preparation method for an annular boron carbide-alumina core block. The method comprises the following steps: using wet ball milling to uniformly mix B4C, Al2O3 and a sintering aid, and then adding a surface modifier for further ball milling, so that the B4C and Al2O3 in the slurry are fully mixed with the sintering aid and the surface modifier to form a modulated slurry. The modulated slurry is subjected to spray granulation to form a spherical composite powder. The spherical composite powder is subjected to dry isostatic pressing to form a thin-walled tube green body with an inner diameter of 7.3 to 7.4 mm and a wall thickness of 1.6 mm. The shrinkage rate of the thin-walled tube green body is further controlled by reasonably designing a sintering path. The obtained core block crude product has an inner diameter that does not require processing and can directly meet the requirements of the inner diameter and roughness of the core block. The inner diameter roughness is less than 0.8 μm and the outer diameter is less than 1.6 μm. The diameter machining allowance is less than 3mm, which reduces the processing amount of the core block. The rough core block only needs surface finishing to obtain the annular boron carbide-alumina core block; during the ball milling process, the addition of surface modifier is beneficial to improve the uniformity of the prepared slurry and the fluidity of the spherical composite powder formed by spray granulation; the preparation of spherical composite powder solves the problems of complex preparation process of the original B4C / Al2O3 powder slurry or mud, poor fluidity of fine-particle powder during charging, uneven powder composition, and uneven shrinkage of the green body; further combined with the dry isostatic pressing method, the principle of matching the design of the charging end cover of the forming mold with the required inner and outer diameter design of the green body is adopted to press the spherical composite powder into a thin-walled tube green body, so as to achieve uniform and rapid charging and good control of the concentricity of the green body. Compared with other forming methods, the core block green body prepared by the dry isostatic pressing method has better concentricity and straightness; before high-temperature sintering, a reasonable holding point is set to ensure that the surface modifier is completely removed, and during the sintering densification process, it is preferably kept in a medium temperature section (1200°C) in a slightly positive pressure argon atmosphere, and then the temperature is raised to 1400-1600°C for sintering, so that the core block shrinks uniformly during the sintering process, and the changes in the deformation, density, and inner diameter shrinkage rate of the core block are accurately controlled to meet the requirements of low grinding amount and high strength, so as to obtain annular boron carbide-alumina core blocks with performance indicators that meet the requirements.

[0030] The present invention realizes the near-net-size forming preparation of annular boron carbide-alumina (WABA) core blocks by combining the preparation method of spherical composite powders and the coordinated control of performance regulation, molding process parameters, green body size and gradient sintering process parameters, thereby reducing the processing allowance and processing difficulty of the core blocks; the preparation process is simple and can be directly used for industrialization. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0032] Figure 1 A flow chart of a method for preparing an annular boron carbide-alumina pellet provided in an embodiment of the present invention is shown;

[0033] Figure 2 The SEM morphology of the B4C / Al2O3 spherical composite powder provided by the embodiment of the present invention is shown;

[0034] Figure 3 A particle size statistical diagram of the B4C / Al2O3 spherical composite powder provided by an embodiment of the present invention is shown;

[0035] Figure 4 A physical picture of a ring-shaped boron carbide-alumina pellet provided in an embodiment of the present invention is shown;

[0036] Figure 5 The SEM morphology of the annular boron carbide-alumina pellet provided by the embodiment of the present invention is shown;

[0037] Figure 6 The metallographic morphology of the annular boron carbide-alumina core block provided by the embodiment of the present invention is shown;

[0038] Figure 7 The figure shows the density distribution diagram of the thin-walled tube green body provided by the embodiment of the present invention. DETAILED DESCRIPTION

[0039] The technical solutions in the embodiments of the present invention will be described clearly and completely below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only a part of the embodiments of the present invention, not all of the embodiments. The following description of at least one exemplary embodiment is actually only illustrative and is by no means a limitation on the present invention and its application or use. Based on the embodiments of the present invention, any product identical or similar to the present invention obtained by anyone under the inspiration of the present invention or by combining the features of the present invention with other prior arts falls within the scope of protection of the present invention. In addition, all other embodiments obtained by ordinary technicians in this field without carrying out creative work belong to the scope of protection of the present invention.

[0040] In the embodiment, no specific experimental steps or conditions are indicated, and the operation or conditions of the conventional experimental steps described in the prior art in this field can be carried out. The reagents used and other instruments that do not indicate the manufacturer are conventional reagent products that can be obtained commercially. In addition, the accompanying drawings are only schematic diagrams of the embodiments of the present invention and are not necessarily drawn to scale. The same reference numerals in the figures represent the same or similar parts, and thus their repeated description will be omitted. Some block diagrams shown in the accompanying drawings are functional entities and do not necessarily correspond to physically or logically independent entities.

[0041] Technologies, methods, and equipment known to ordinary technicians in the relevant field may not be discussed in detail, but where appropriate, the technologies, methods, and equipment should be considered as part of the description of the present invention.

[0042] In the description of the present invention, it should be understood that the use of terms such as "first" and "second" to limit components is only for the convenience of distinguishing the corresponding components. Unless otherwise stated, the above terms have no special meaning and therefore cannot be understood as limiting the scope of protection of the present invention.

[0043] In addition, the technical features involved in the different embodiments of the present invention described below can be combined with each other as long as they do not conflict with each other.

[0044] In a first aspect, the present invention provides a method for preparing a near-net-size annular boron carbide-alumina pellet. Figure 1 The flowchart of the method for preparing the annular boron carbide-alumina pellet provided in the embodiment of the present invention is shown as follows: Figure 1 As shown, the preparation method comprises the following steps:

[0045] S1. After mixing B4C, Al2O3 and a sintering aid, deionized water is added at a water-to-material ratio of 1-3:1, and wet ball milling is performed for 2-3 hours to obtain a premixed slurry; among the B4C, Al2O3 and the sintering aid, the mass proportion of B4C is 13-15%, the mass proportion of Al2O3 is 82-84%, and the mass proportion of the sintering aid is 1-4%;

[0046] S2, adding a surface modifier to the premixed slurry, continuing ball milling for 1-3 hours, and mixing evenly to form a modulated slurry with a solid content of 40-50%;

[0047] S3, preparing the prepared slurry into spherical composite powder with a particle size of 20-50 μm by spray granulation;

[0048] S4, using dry isostatic pressing to press the spherical composite powder to obtain a bulk density of 2.05-2.2 g / cm 3 Thin-walled tube green body;

[0049] S5, performing gradient temperature sintering on the thin-walled tube green body to obtain a crude pellet;

[0050] S6, performing surface finishing on the crude pellet to obtain the annular boron carbide-alumina pellet;

[0051] The gradient temperature sintering includes a first sintering and a second sintering. The first sintering includes: in a vacuum atmosphere, heating to 650°C at 2-3°C / min, keeping warm for 2-3 hours, and continuing to heat to 950°C at 2-3°C / min, and keeping warm for 2-3 hours; the second sintering includes: in an argon atmosphere, heating to 1200°C at 1-2°C / min, keeping warm for 2-3 hours, and continuing to heat to 1400-1600°C at 1-3°C / min, and keeping warm for 1-3 hours.

[0052] In the specific implementation, there are particle size requirements for B4C in the preparation of the core block, and its particle size distribution cannot be significantly changed during the ball milling mixing process. If the ball milling mixing time is too long, the B4C particle size will change to a certain extent. Therefore, it is necessary to control the appropriate ball milling time while ensuring the uniformity of the raw material powder. Therefore, this embodiment adopts wet ball milling for step-by-step ball milling, that is, firstly, B4C, Al2O3, and sintering aid are mixed evenly, and then a surface modifier is added for further ball milling, so that B4C, Al2O3 in the slurry are fully mixed with the sintering aid and the surface modifier to form a modulated slurry, and the sintering aid (SiO2 or MgSiO3) is a useful component that can remain in the core block and is regarded as a part of the core block raw material; after the raw materials (B4C, Al2O3 and sintering aid) are mixed evenly in deionized water in advance to improve the mixing uniformity of the three raw material powders, when the surface modifier is further added for mixing, the ball milling mixing time of the surface modifier and the raw material powder is shortened, and the fluidity of the resulting slurry is also better.

[0053] In the specific implementation, the powder raw material aluminum oxide is submicron grade Al2O3, and the powder particle size D50 is 0.3um to 3um; the boron carbide powder particle size is 5 to 35um; the powder particle size D50 of the sintering aid is 30 to 100nm. In order to control wear, the ball-to-material ratio of wet ball milling is (1 to 3): 1; the water-to-material ratio is (1 to 3): 1; the slurry is prepared and sprayed to form a spherical composite powder, and the spherical composite powder is pressed by dry isostatic pressing to form a thin-walled tube green body. By controlling the pressing pressure to 110-140Mpa, the volume density of the formed thin-walled tube green body is 2.05-2.2g / cm 3; The thin-walled tube green body is subjected to gradient temperature sintering to obtain a core block crude product; the core block crude product is subjected to surface finishing to finally obtain a ring-shaped boron carbide-alumina core block; during the ball milling process, the addition of a surface modifier is beneficial to improving the uniformity of the prepared slurry and the fluidity of the spherical composite powder formed by spray granulation; the preparation of the spherical composite powder solves the problems of the original B4C / Al2O3 powder slurry or mud preparation process being complicated, the fine-particle powder having poor fluidity during loading, the uneven powder composition, and the uneven shrinkage of the green body; further combined with the dry isostatic pressing method, the spherical composite powder is pressed into a thin-walled tube green body in accordance with the principle that the design of the molding die loading end cover matches the design of the required green body inner and outer diameters, and uniform and rapid loading and good control of the green body concentricity are achieved. Compared with other molding methods, the green body core block prepared by the dry isostatic pressing method has better concentricity and straightness.

[0054] Furthermore, in order to avoid the unreasonable setting of the high-temperature sintering path, which may lead to uneven shrinkage and excessive deformation of the green body, the present embodiment selects a gradient temperature rise sintering method. Before high-temperature sintering, the surface modifier is completely removed (first sintering). The present embodiment has conducted a large number of experimental investigations on the selection of the holding point in the process. It was found that the surface modifier in the annular boron carbide-alumina core block can be completely removed by slowly heating the temperature to 650°C at 2-3°C / min and keeping it for 2-3h, and then continuing to slowly heat the temperature to 950°C at 2-3°C / min and keeping it for another 2-3h. Compared with setting one holding point at 650°C for long-term surface modifier removal, this path setting adopts two holding points (650°C and 950°C) in this embodiment, which effectively shortens the processing time for surface modifier removal; and compared with setting one holding point at 950°C for high-temperature rapid surface modifier removal, this embodiment adopts two holding points (650°C and 950°C) to effectively avoid the problems of uneven shrinkage and excessive deformation of the blank caused by too long a temperature rise route. In the subsequent sintering and densification process (second sintering), it is preferred to keep the temperature in a medium temperature section (1200°C) in a slightly positive pressure argon atmosphere, and then heat it to 1400-1600°C for sintering and densification, so that the core block from which the surface modifier has been removed shrinks evenly during the sintering process, thereby accurately controlling the changes in the deformation, density, and inner diameter shrinkage rate of the core block to meet the requirements of low grinding amount and high strength, and obtaining an annular boron carbide-alumina core block with performance indicators that meet the requirements; more preferably, in order to effectively reduce the hydrogen content in the core block, the high-temperature sintering temperature needs to be between 1500°C and 1600°C, and the average density of the obtained core block is 2.41-2.43 g / cm 3The preparation process is simple and can be directly used for industrialization. It should be noted that the gradient heating process is a continuous process, that is, the first sintering and the second sintering are continuous operations. After the first sintering is completed and kept at 950℃ for 2-3h, argon is introduced into the vacuum sintering furnace body, and the furnace body is adjusted to continue to heat up to 1200℃ at 1-2℃ / min for the subsequent second sintering.

[0055] In some embodiments, the surface modifier includes a wetting agent, a dispersant and a binder; the wetting agent is selected from polyethylene glycol; the dispersant is selected from polyethylene glycol tert-octylphenyl ether; the binder is selected from polyvinyl alcohol; the sintering aid is SiO2 or MgSiO3. Experiments have shown that using SiO2 as a sintering aid can effectively reduce the water absorption properties of the core blocks obtained by sintering while lowering the melting point of the sintering system.

[0056] In some embodiments, the gradient temperature sintering is performed by buried firing or vertical firing, and the slightly positive pressure provided by the argon atmosphere is 0.1-0.2 MPa.

[0057] The embodiment of the present invention uses submicron alumina powder as a sintering skeleton and nano silicon dioxide as a sintering aid. The present invention can coordinately control the B content of the mixed raw materials (the mass proportion of B4C is 13-15%), the core block processing size and the core block density. 10 The B line density is controlled within the range of ±0.0005g / cm.

[0058] In addition, the hydrogen content of the pellet is related to the particle size of the raw material powder, the high-temperature sintering temperature and the post-processing process after the pellet processing. The present invention reasonably controls the raw material powder performance in the early stage, regulates the sintering activity of the raw material powder, appropriately increases the sintering temperature during the high-temperature sintering process, and coordinately controls the post-processing process to achieve the control of the hydrogen content of the pellet below 30ppm. The hydrogen content in the annular boron carbide-alumina pellet is greatly reduced, and its anti-water absorption performance is enhanced, meeting the requirements of nuclear fuel elements for low hydrogen content and high axial compressive strength of water-permeable annular combustible poison.

[0059] In a second aspect, the present invention provides an annular boron carbide-alumina pellet, which is obtained by the preparation method described in the first aspect. The volume density of the obtained annular boron carbide-alumina pellet is 2.27-2.47 g / cm 3 , the compressive strength is not less than 69Mpa.

[0060] In a third aspect, the present invention provides an application of an annular boron carbide-alumina pellet block, wherein the annular boron carbide-alumina pellet block obtained by the preparation method described in the first aspect is used as a combustible poison for nuclear fuel, or as a neutron absorber.

[0061] In order to enable those skilled in the art to more clearly understand the present invention, the annular boron carbide-alumina core block and the near-net-size molding preparation method and application of the present invention are now described in detail through the following examples.

[0062] Example 1

[0063] According to the component ratio, B4C:Al2O3:SiO2=14:83.5:2.5wt% were weighed and mixed evenly, and then deionized water was added with a water-to-material ratio of 1.5:1 and ball-milled for 3h; then polyethylene glycol (0.4wt%), polyethylene glycol tert-octylphenyl ether (1wt%), and polyvinyl alcohol (1.5wt%) were added and ball-milled for 2h to obtain a slurry;

[0064] The prepared slurry was then spray granulated to prepare B4C / Al2O3 spherical composite powder with a fluidity of 65S / 50g and a morphology of Figure 2 As shown in Figure 2, the particle size statistics of B4C / Al2O3 spherical composite powders are as follows: Figure 3 As shown, the particle size is concentrated in the range of 20-50um, and the particle fluidity is good, which can achieve uniform and fast loading. The B4C / Al2O3 composite powder is loaded into a pressing mold and pressed under a dry bag isostatic press of 120Mpa to obtain several thin-walled tube green bodies with a wall thickness of 1.6mm and an inner diameter of 7.3mm. The average (volume) density of the green body is about 2.116g / cm 3 ;

[0065] The obtained green body is placed in a vacuum carbon tube furnace, and alumina particles are used as buried particles. High-temperature sintering is carried out at 1550°C to obtain boron carbide-alumina core blocks. The specific sintering process is as follows: under a vacuum atmosphere, the temperature in the furnace body is raised to 650°C in 4 hours and kept warm for 2 hours, and then the temperature is further raised to 950°C in 2 hours and kept warm for 2 hours; after the insulation at 950°C is completed, argon gas is filled into the furnace body to maintain the pressure in the furnace body at a slight positive pressure of 0.2Mpa; and the temperature in the furnace body is raised to 1200°C in 3 hours, and kept warm for 3 hours; and the temperature is further raised to 1550°C in 3 hours and kept warm for 1 hour.

[0066] The core block is finely processed by a centerless grinder and a yarn cutter to obtain a finished annular boron carbide-alumina core block.

[0067] Figure 4 The actual picture of the annular boron carbide-alumina pellet provided by the embodiment of the present invention is shown. Figure 5 The SEM morphology of the annular boron carbide-alumina pellet provided in the embodiment of the present invention is shown. Figure 6 The metallographic morphology of the annular boron carbide-alumina pellet provided by the embodiment of the present invention is shown; after testing, the average (volume) density of the annular boron carbide-alumina pellet is 2.43 g / cm 3The core block compressive strength is 106Mpa and the H2O content is 76.82ppm, which meets the application requirements of annular wet combustible poison absorbers for nuclear fuel elements.

[0068] Example 2

[0069] According to the component ratio, B4C:Al2O3:SiO2=14:83.5:2.5wt% were weighed and mixed evenly, and then deionized water was added with a water-to-material ratio of 1.5:1 and ball-milled for 3h; then polyethylene glycol (0.4wt%), polyethylene glycol tert-octylphenyl ether (1wt%), and polyvinyl alcohol (1.5wt%) were added and ball-milled for 2h to obtain a slurry;

[0070] Subsequently, the prepared slurry was prepared into B4C / Al2O3 spherical composite powder by spray granulation, and the B4C / Al2O3 spherical composite powder was pressed into a number of core blocks with a wall thickness of 1.6 mm and an inner diameter of 7.4 mm by dry bag isostatic pressing at 130 MPa. The average (volume) density of the green blocks was about 2.15 g / cm 3 .

[0071] The obtained green body was placed in a vacuum carbon tube furnace and sintered at 1400°C in a vertical firing manner to obtain a boron carbide-alumina core block. The specific sintering process was as follows: under a vacuum atmosphere, the temperature in the furnace body was raised to 650°C in 4 hours and kept for 2 hours, then the temperature was further raised to 950°C in 2 hours and kept for 2 hours. After the insulation at 950°C, argon was filled into the furnace body to maintain the pressure in the furnace body at a slight positive pressure of 0.1 MPa; and the temperature in the furnace body was raised to 1200°C in 3 hours and kept for 3 hours; then the temperature was further raised to 1450°C in 2 hours and kept for 1 hour.

[0072] The core block was finely processed by a centerless grinder and a yarn cutter to obtain a finished annular boron carbide-alumina core block; after testing, the average (volume) density of the core block was 2.41 g / cm 3 The core block has a compressive strength of 86Mpa and a H2O content of 160ppm, which meets the application requirements of annular wet combustible poison absorbers for nuclear fuel elements.

[0073] Figure 7 FIG. 4 shows a density distribution diagram of a thin-walled tube green body provided by an embodiment of the present invention. Figure 7 As shown, the average density of the green body prepared in Example 1-2 is about 2.133 g / cm 3 .

[0074] The SEM morphology image and particle size statistical graph results of the B4C / Al2O3 spherical composite powder obtained in this embodiment are similar or close to those in Example 1, and are not repeated here; the physical image, SEM morphology image and metallographic morphology image results of the finished annular boron carbide-alumina core block obtained in this embodiment are similar or close to those in Example 1, and are not repeated here.

[0075] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification.

[0076] For the method embodiments, for the sake of simplicity, they are all described as a series of action combinations, but those skilled in the art should know that the present invention is not limited by the order of the actions described, because according to the present invention, some steps can be performed in other orders or simultaneously. Secondly, those skilled in the art should also know that the embodiments described in the specification are all preferred embodiments, and the actions and components involved are not necessarily required by the present invention.

[0077] The above is a detailed introduction to a ring-shaped boron carbide-alumina core block and a near-net size molding preparation method and application provided by the present invention. Specific examples are used in this article to illustrate the principles and implementation methods of the present invention. The description of the above embodiments is only used to help understand the method of the present invention and its core idea; at the same time, for general technicians in this field, according to the ideas of the present invention, there will be changes in the specific implementation methods and application scopes. In summary, the content of this specification should not be understood as a limitation on the present invention.

Claims

1. A near-net-size forming method for preparing annular boron carbide-alumina pellets, characterized in that: The preparation method comprises the following steps: S1. After mixing B4C, Al2O3 and a sintering aid, deionized water is added at a water-to-material ratio of 1-3:1, and wet ball milling is performed for 2-3 hours to obtain a premixed slurry; among the B4C, Al2O3 and the sintering aid, the mass proportion of B4C is 13-15%, the mass proportion of Al2O3 is 82-84%, and the mass proportion of the sintering aid is 1-4%; S2, adding a surface modifier to the premixed slurry, continuing ball milling for 1-3 hours, and mixing evenly to form a modulated slurry with a solid content of 40-50%; S3, preparing the prepared slurry into spherical composite powder with a particle size of 20-50 μm by spray granulation; S4, using dry isostatic pressing method to press the spherical composite powder to obtain a spherical composite powder with an inner diameter of 7.3-7.4 mm, a wall thickness of 1.6 mm, and a bulk density of 2.05-2.20 g / cm 3 Thin-walled tube green body; S5, performing gradient temperature sintering on the thin-walled tube green body to obtain a crude pellet; S6, performing surface finishing on the crude pellets to obtain annular boron carbide-alumina pellets; The gradient temperature sintering includes a first sintering and a second sintering. The first sintering includes: in a vacuum atmosphere, heating to 650°C at 2-3°C / min, keeping warm for 2-3 hours, and continuing to heat to 950°C at 2-3°C / min, and keeping warm for 2-3 hours; the second sintering includes: in an argon atmosphere, heating to 1200°C at 1-2°C / min, keeping warm for 2-3 hours, and continuing to heat to 1400-1600°C at 1-3°C / min, and keeping warm for 1-3 hours.

2. The near-net-size forming preparation method of the annular boron carbide-alumina pellet according to claim 1, characterized in that: The surface modifier includes a wetting agent, a dispersant and a binder; The moisturizing agent is polyethylene glycol; The dispersant is polyethylene glycol tert-octylphenyl ether; The binder is polyvinyl alcohol; The sintering aid is SiO2 or MgSiO3.

3. The near-net-size forming preparation method of the annular boron carbide-alumina pellet according to claim 1 or 2, characterized in that: The ball-to-material ratio of the wet ball milling is 1 to 3:

1.

4. The near-net-size forming preparation method of annular boron carbide-alumina pellets according to claim 1, characterized in that: The dry isostatic pressing method is used, and the pressure for pressing the spherical composite powder is 110-140 MPa.

5. The near-net-size forming preparation method of annular boron carbide-alumina pellets according to claim 1, characterized in that: The second sintering is carried out in an argon atmosphere with a pressure of 0.1-0.2 Mpa.

6. The method for preparing the annular boron carbide-alumina pellet according to claim 1, characterized in that: The gradient temperature rising sintering is carried out by buried sintering or vertical sintering.

7. The near-net-size forming preparation method of annular boron carbide-alumina pellets according to claim 1, characterized in that: The surface finishing methods include: centerless grinder and / or surface grinder and / or wire cutting, deionized water ultrasonic cleaning and drying treatment.

8. A ring-shaped boron carbide-alumina pellet, characterized in that: The annular boron carbide-alumina core block is obtained by the preparation method described in any one of claims 1 to 7.

9. The annular boron carbide-alumina pellet according to claim 8, characterized in that: The volume density of the annular boron carbide-alumina pellet is 2.27-2.47 g / cm 3 , the compressive strength is not less than 69Mpa.

10. An application of an annular boron carbide-alumina pellet, characterized in that: The annular boron carbide-alumina pellet obtained by the preparation method according to any one of claims 1 to 7 is used as a burnable poison for nuclear fuel assemblies or as other neutron absorbers.

Citation Information

Patent Citations

  • Preparation method of nuclear grade boron carbide core block for high-temperature gas cooling pile control rod

    CN105913888A

  • Porous boron carbide ceramic material for neutron shielding material and preparation method of porous boron carbide ceramic material

    CN116655383A

  • Preparation method of B4C composite ceramic material

    CN117263691A

  • Alumina ceramic bracket as well as preparation method and application thereof

    CN118271069A

  • Neutron absorber pellets with modified microstructure

    US4474728A