Preparation process of high-strength ceramic product
By adding modified materials such as alumina and silicon carbide to high-strength ceramic products to form composite materials, the problem of insufficient corrosion resistance of ceramic products in high-temperature and strong-acid environments is solved, and their high-temperature resistance and corrosion resistance are significantly improved. And provide catalytic function under high temperature conditions.
Patent Information
- Application Number
- CN202410824168.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-25
- Publication Date
- 2024-10-11
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing high-strength ceramic products have insufficient corrosion resistance in high-temperature and strong-acid environments, resulting in shortened service life.
By adding modified materials, such as alumina and silicon carbide, and forming uniform composite materials through physical mixing and chemical treatment, combined with binders and fluxes, ceramic powders are prepared, and high-strength ceramic products are made using pressing and sintering processes.
It significantly improves the high temperature resistance and corrosion resistance of ceramic products, enhances their chemical stability and thermal shock resistance in high temperature acid and alkali environments, and provides catalytic functions to extend their service life.
Smart Images

Figure CN118754632A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of ceramic materials, in particular to a preparation process of a high-strength ceramic product. Background Art
[0002] As an outstanding representative of modern material science, high-strength ceramic products have won high praise from the industry for their excellent physical properties and wide application fields. These ceramic products not only have the delicate texture and artistic beauty of traditional ceramics, but also have achieved a qualitative leap in strength and hardness.
[0003] High-strength ceramic products undergo precise manufacturing processes and strict quality control to ensure that they can maintain stable and reliable performance in extreme environments. Whether in high temperature, high pressure, high wear or high corrosion situations, these ceramic products can show amazing durability and compressive strength, greatly extending their service life;
[0004] In the industrial field, high-strength ceramic products are widely used in a variety of industries such as aerospace, automobile manufacturing, medical equipment, and advanced mechanical equipment. They can bear complex mechanical loads and resist erosion in various harsh environments, providing a solid material foundation for the development of modern industry.
[0005] Application No. 201410329975.9 discloses a new type of ceramic product, which is composed of the following raw material components: 15-20 parts of nano kaolin, 5-10 parts of activated clay, 3-5 parts of clay, 3-5 parts of silicate cement, 2-5 parts of limestone, 4-5 parts of carbon black, 5-10 parts of phenolic resin, 2-3 parts of sodium carbonate, 2-5 parts of talcum powder, 3-4 parts of silicon powder, and 10-15 parts of deionized water. The new type of ceramic product does not require kiln firing, but is made by coagulation, and the raw material source is abundant and economical. The finished product has the characteristics of high strength, corrosion resistance, acid and alkali resistance, not easy to weather, and not easy to deform.
[0006] Existing high-strength ceramic products face severe challenges in high-temperature and strong-acid environments. High temperature intensifies the corrosion of strong acids, leading to faster corrosion of ceramic products and shortening the service life of ceramic products. Therefore, how to improve the corrosion resistance of high-strength ceramic products under high-temperature conditions has become a technical problem that urgently needs to be overcome. Summary of the invention
[0007] 1. Technical issues to be solved
[0008] In view of the deficiencies in the prior art, the present invention provides a process for preparing high-strength ceramic products, which significantly improves the corrosion resistance of ceramic products under high temperature conditions by adding modified materials.
[0009] (II) Technical solution
[0010] To achieve the above object, the present invention provides the following technical solution: a preparation process of a high-strength ceramic product, comprising the following steps:
[0011] S1. Raw material preparation: ceramic powder, modified material, binder, flux;
[0012] S2. Preparation of modified materials: combining specific inorganic substances with organic substances to obtain modified materials through physical mixing and chemical treatment;
[0013] S3, raw material mixing: ceramic powder is mixed with modified material, binder and flux in proportion to prepare a uniform mixture;
[0014] S4, molding: pressing the mixture into a molding die;
[0015] S5. Sintering: Sinter the formed green body at 1200-1400°C for 2-4 hours to obtain a high-strength ceramic product.
[0016] Preferably, the modified material includes aluminum oxide and silicon carbide, which are mixed in a weight ratio of 1:1. Polyvinyl alcohol can also be replaced by other organic substances with the same effect, such as polypropylene alcohol, polyethylene glycol or polylactic acid. Aluminum oxide and silicon carbide can also be replaced by other inorganic substances with the same effect, such as zirconium oxide, cerium oxide, silicon nitride or silicon boron nitride.
[0017] Preferably, the binder is polyvinyl alcohol, and its content is 5%-10% by weight of the mixture.
[0018] Preferably, the flux is borate, and its content is 3%-7% by weight of the mixture.
[0019] Preferably, the sintering temperature is 1300°C.
[0020] Preferably, the sintering holding time is 3 hours.
[0021] Preferably, the particle size of the ceramic powder is 1-10 microns.
[0022] Preferably, the molding pressure is 100-200 MPa.
[0023] Preferably, the molding pressure is 100-200 MPa.
[0024] Preferably, the method for preparing the modified material comprises the following steps:
[0025] a) preparing the required raw materials: alumina, silicon carbide and polyvinyl alcohol;
[0026] b) Mix inorganic matter and organic matter in proportion: the specific proportion can be:
[0027] Alumina: 10 parts by weight;
[0028] Silicon carbide: 10 parts by weight;
[0029] Polyvinyl alcohol: 5 parts by weight;
[0030] c) placing the mixture in a mechanical stirrer and stirring it uniformly for 2 hours at a speed of 2000 rpm to ensure that the inorganic and organic substances are fully mixed to form a uniform mixture;
[0031] d) chemically treating the mechanically stirred mixture, the specific method is as follows:
[0032] dS1) placing the mixture in a reaction kettle and adding an appropriate amount of distilled water, the amount of water being 50% of the weight of the mixture;
[0033] dS2) slowly adding 5% sodium hydroxide solution to the reactor, controlling the addition speed to prevent excessive reaction, the amount of sodium hydroxide solution used is 10% of the weight of the mixture;
[0034] dS3) maintaining the reaction temperature at 80° C. for 2 hours to ensure that the inorganic and organic substances undergo sufficient chemical reactions to form a stable composite material;
[0035] e) filtering the mixture after chemical treatment to remove excess solution and impurities, and then washing with distilled water for 3 times, with the amount of water used each time being 2 times the weight of the mixture, to ensure that the residual chemical reagents are completely removed;
[0036] f) placing the washed mixture in an oven for drying at a temperature of 100° C. for 12 hours to ensure that the mixture is completely dried to obtain a solid composite material;
[0037] e) crushing the dried solid composite material using a ball mill for 3 hours to obtain a fine powdered modified material;
[0038] f) Screening the pulverized modified material using a 100-500 mesh screen to ensure that the particle size of the modified material is uniform, thereby obtaining the final modified material.
[0039] (III) Beneficial effects
[0040] Compared with the prior art, the present invention provides a preparation process for high-strength ceramic products, which has the following beneficial effects:
[0041] 1. By adding modified materials, the high temperature resistance of ceramic products can be significantly improved. These materials have a high melting point and thermal stability and can maintain structural stability in high temperature environments.
[0042] 2. The corrosion resistance of ceramic products has been significantly improved by the introduction of modified materials. These modified materials not only give ceramics excellent chemical stability in high-temperature acid-base environments, but also significantly slow down the rate of corrosion by strong acids under extreme conditions. This chemical inertness enables ceramic products to maintain long-term stability and reliability in harsh environments such as high temperature, high humidity, and strong acid.
[0043] The addition of modified materials optimizes the microstructure of ceramic products and enhances the density and uniformity of their surface layer, thereby effectively preventing the penetration and erosion of acid and alkali solutions into the ceramic matrix. Under high temperature conditions, the modified materials can also effectively disperse and absorb the thermal stress inside the ceramic products, further improving their thermal shock resistance and corrosion resistance.
[0044] 3. Through the addition of modified materials, although the modified materials themselves do not have the direct function of catalytic reaction, in a specific strong acid environment, the modified materials can effectively activate the surface structure of the ceramics through interaction with the ceramic surface under strong acid conditions, thereby giving the originally strong and durable ceramic products the ability to accelerate chemical reactions in a strong acid environment;
[0045] This activation process not only improves the chemical stability of ceramic products in strong acid environments, but also gives it a unique catalytic function. While maintaining its original high-strength characteristics, it can also act as a catalyst under strong acid conditions, significantly promoting the rate of chemical reactions. This high-strength ceramic product with catalytic function has shown broad applications in many fields such as chemical industry, environmental protection treatment, and catalyst carriers.
[0046] 4. Through reasonable raw material mixing and homogenization treatment, modified materials and ceramic powders can be evenly distributed in ceramic products, thereby improving the overall performance of the material. BRIEF DESCRIPTION OF THE DRAWINGS
[0047] Figure 1 The present invention is a flowchart of a preparation process of a high-strength ceramic product. DETAILED DESCRIPTION
[0048] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0049] Alumina is used as a raw material in the present invention. Alumina is an important inorganic material with excellent physical and chemical properties. Its melting point is as high as 2054°C, which makes it extremely resistant to high temperatures. In addition, alumina has high hardness and strength and is widely used in wear-resistant materials and structural ceramics. The chemical stability of alumina is also very good, and it can remain stable in most acidic and alkaline environments, which makes it an important component for improving the corrosion resistance of ceramic products. Alumina has excellent electrical insulation properties, which makes it also have important application value in the electronics industry.
[0050] Silicon carbide (SiC) is a ceramic material with high hardness, high thermal conductivity and excellent corrosion resistance. Its Mohs hardness is close to that of diamond and it is widely used in cutting tools and abrasives. Silicon carbide has high thermal conductivity, can dissipate heat quickly, and can maintain excellent mechanical properties even in high temperature environments. In addition, silicon carbide has excellent chemical stability and can withstand the erosion of strong acids and alkalis, which makes it an important material for improving the corrosion resistance of ceramic products. Silicon carbide also has good electrical properties and is often used to make electronic devices and high-frequency components.
[0051] Polyvinyl alcohol (PVA) is used as raw material. Polyvinyl alcohol (PVA) is a synthetic polymer material with excellent film-forming properties, adhesion and chemical stability. It can form a transparent and tough film after dissolving in water and is widely used in coatings, adhesives and textile processing. The molecular structure of polyvinyl alcohol contains a large number of hydroxyl groups, which can form a good combination with inorganic materials such as alumina and silicon carbide, improving the mechanical properties and corrosion resistance of the composite material. In addition, polyvinyl alcohol has good biocompatibility and environmental protection characteristics, and is widely used in the fields of medicine and food packaging.
[0052] Embodiment 1:
[0053] A preparation process of a high-strength ceramic product specifically comprises the following steps:
[0054] S1. Raw material preparation: Take ceramic powder (50 parts of silicon oxide, 20 parts of zinc oxide), 10 parts of aluminum oxide, 10 parts of silicon carbide, 5 parts of polyvinyl alcohol, and 5 parts of borate by weight.
[0055] S2. Preparation of modified materials: Aluminum oxide, silicon carbide and polyvinyl alcohol are mixed in proportion, and a uniform composite material is formed by mechanical stirring and chemical treatment, and then dried and crushed to obtain a modified material.
[0056] S3. Raw material mixing: ceramic powder, modified material, polyvinyl alcohol and borate are mixed and stirred evenly to prepare a uniform mixture.
[0057] S4, molding: fill the mixture into a mold and apply a pressure of 150MPa to press and mold.
[0058] S5. Sintering: Sinter at 1300°C for 3 hours to obtain a high-strength ceramic product.
[0059] Embodiment 2:
[0060] A preparation process of a high-strength ceramic product specifically comprises the following steps:
[0061] S1. Raw material preparation: Take ceramic powder (55 parts of silicon oxide, 25 parts of zinc oxide), 15 parts of aluminum oxide, 15 parts of silicon carbide, 6 parts of polyvinyl alcohol, and 6 parts of borate by weight.
[0062] S2. Preparation of modified materials: same as Example 1.
[0063] S3. Raw material mixing: Mix according to the above proportions to prepare a uniform mixture.
[0064] S4, molding: applying a pressure of 160 MPa to press molding.
[0065] S5. Sintering: Sinter at 1350°C for 4 hours to obtain a high-strength ceramic product.
[0066] Embodiment three:
[0067] A preparation process of a high-strength ceramic product specifically comprises the following steps:
[0068] S1. Raw material preparation: Take ceramic powder (60 parts of silicon oxide, 30 parts of zinc oxide), 20 parts of aluminum oxide, 20 parts of silicon carbide, 7 parts of polyvinyl alcohol, and 7 parts of borate by weight.
[0069] S2. Preparation of modified materials: same as Example 1.
[0070] S3. Raw material mixing: Mix according to the above proportions to prepare a uniform mixture.
[0071] S4, molding: applying a pressure of 170 MPa to press molding.
[0072] S5. Sintering: Sinter at 1400°C for 4 hours to obtain a high-strength ceramic product.
[0073] Embodiment 4:
[0074] A preparation process of a high-strength ceramic product specifically comprises the following steps:
[0075] S1. Raw material preparation: by weight, take ceramic powder (52 parts of silicon oxide, 22 parts of zinc oxide), 12 parts of aluminum oxide, 12 parts of silicon carbide, 5.5 parts of polyvinyl alcohol, and 5.5 parts of borate.
[0076] S2. Preparation of modified materials: same as Example 1.
[0077] S3. Raw material mixing: Mix according to the above proportions to prepare a uniform mixture.
[0078] S4, molding: applying a pressure of 155 MPa to press molding.
[0079] S5. Sintering: Sinter at 1320° C. for 3.5 hours to obtain a high-strength ceramic product.
[0080] Embodiment five:
[0081] A preparation process of a high-strength ceramic product specifically comprises the following steps:
[0082] S1. Raw material preparation: Take ceramic powder (54 parts of silicon oxide, 24 parts of zinc oxide), 14 parts of aluminum oxide, 14 parts of silicon carbide, 6.5 parts of polyvinyl alcohol, and 6.5 parts of borate by weight.
[0083] S2. Preparation of modified materials: same as Example 1.
[0084] S3. Raw material mixing: Mix according to the above proportions to prepare a uniform mixture.
[0085] S4, molding: applying a pressure of 160 MPa to press molding.
[0086] S5. Sintering: Sinter at 1350°C for 4 hours to obtain a high-strength ceramic product.
[0087] Comparative Example 1:
[0088] S1. Raw material preparation: Take ceramic powder (50 parts of silicon oxide, 20 parts of zinc oxide), 5 parts of polyvinyl alcohol, and 5 parts of borate by weight.
[0089] S2. Raw material mixing: without adding any modifying materials, mix in the above proportions to prepare a uniform mixture.
[0090] S3, molding: applying a pressure of 150 MPa to press molding.
[0091] S4. Sintering: Sinter at 1300° C. for 3 hours to obtain a ceramic product.
[0092] Comparative Example 2:
[0093] S1. Raw material preparation: Take ceramic powder (55 parts of silicon oxide, 25 parts of zinc oxide), 6 parts of polyvinyl alcohol, and 6 parts of borate by weight.
[0094] S2. Raw material mixing: without adding any modifying materials, mix in the above proportions to prepare a uniform mixture.
[0095] S3, molding: applying a pressure of 160 MPa to press molding.
[0096] S4. Sintering: Sinter at 1350° C. for 4 hours to obtain a ceramic product.
[0097] Five portions of the ceramic products prepared in Examples 1, 2, 3, 4, 5 and Comparative Examples 1 and 2 were taken for compressive performance test under high temperature conditions, and the five ceramic products were respectively tested for compressive performance using the GB / T 3810.4 standard. The higher the compressive strength value, the better the compressive strength. Conversely, the lower the compressive strength value, the worse the compressive strength. The test results are shown in Table 1.
[0098] Table 1. Compressive performance test results under high temperature conditions of Examples 1-5 and Comparative Examples 1-2
[0099]
[0100]
[0101] Therefore, it can be seen from the test results in Table 1 that the compressive strength of the ceramic material prepared in the embodiment of the present invention at high temperature is significantly better than the compressive strength of the ceramic material prepared in the comparative example.
[0102] Five portions of the ceramic products prepared in Examples 1, 2, 3, 4, 5 and Comparative Examples 1 and 2 were taken for bending strength test, and the national standard for ceramic three-point bending test (GB / T 3810.3-2016) was used for the five ceramic products. The higher the bending strength value, the better the bending resistance. Conversely, the lower the bending strength value, the worse the bending resistance. The test results are shown in Table 2.
[0103] Table 2. Bending strength test results of Examples 1-5 and Comparative Examples 1-2
[0104] Test samples Bending strength(MPa) Example 1 156 Example 2 168 Example 3 171 Example 4 155 Example 5 164 Comparative Example 1 126 Comparative Example 2 132
[0105] Therefore, it can be seen from the test results in Table 2 that the bending strength of the ceramic material prepared in the embodiment of the present invention is significantly better than the bending strength of the ceramic material prepared in the comparative example.
[0106] Five portions of the ceramic products prepared in Examples 1, 2, 3, 4, 5 and Comparative Examples 1 and 2 were taken for corrosion resistance test under high temperature and strong acid conditions. The specific test method was as follows: a strong acid of the same concentration was heated to the same temperature, and each portion of the ceramic product was placed in the heated strong acid conditions for the same reaction time, the mass loss before and after the reaction was tested, and the corrosion rate was calculated. The specific corrosion rate calculation method adopts a known calculation method, which is not described in detail here. The larger the corrosion rate value of the calculated test, the worse the corrosion resistance under high temperature and strong acid conditions, and vice versa. The test results are shown in Table 3.
[0107] Table 3. Corrosion resistance test results of Examples 1-5 and Comparative Examples 1-2
[0108] Test samples Strong acid environment <![CDATA[Corrosion rate (mg / cm 2 ·h)]]> Example 1 Concentrated sulfuric acid 0.05 Example 2 Concentrated nitric acid 0.04 Example 3 Concentrated sulfuric acid 0.03 Example 4 Concentrated nitric acid 0.06 Example 5 Concentrated sulfuric acid 0.05 Comparative Example 1 Concentrated sulfuric acid 0.15 Comparative Example 2 Concentrated nitric acid 0.12
[0109] Therefore, it can be seen from the test results in Table 3 that the corrosion resistance of the ceramic material prepared in the embodiment of the present invention is significantly better than the corrosion resistance of the ceramic material prepared in the comparative example.
[0110] Five portions of the ceramic products prepared in Examples 1, 2, 3, 4, 5 and Comparative Examples 1 and 2 were taken respectively to test the reaction speed under high temperature resistance and strong acid conditions. High temperature resistance test method: The high temperature resistance test was carried out using conventional test methods in the art, which will not be described in detail here. The reaction speed test method under strong acid conditions: A chemical reaction under strong acid conditions was carried out in a reaction vessel prepared in each embodiment and comparative example, and solid reactants of the same material, shape and mass were placed in the container, and the reaction time was recorded (the chemical reaction time under strong acid conditions in the same manner in conventional reaction vessels in the art is 16 minutes, and conventional reaction vessels do not have the catalytic ability of chemical reactions under strong acid conditions). The shorter the reaction time, the better the catalytic effect, and vice versa. The test results are shown in Table 4.
[0111] Table 4. Test results of high temperature resistance and catalytic effect of raw materials of Examples 1-5 and Comparative Examples 1-2
[0112]
[0113]
[0114] Therefore, it can be seen from the test results in Table 4 that the ceramic material prepared in the embodiment of the present invention has an obvious catalytic effect on strong acid reactions, and the high temperature resistance of the ceramic material prepared in the embodiment of the present invention is significantly better than the high temperature resistance of the ceramic material prepared in the comparative example.
[0115] In summary, the high-strength ceramic product of the present invention is significantly better than the control example in terms of compressive strength, flexural strength, high temperature resistance, corrosion resistance and catalytic effect, which verifies that the modified material improves the performance of the ceramic material.
[0116] The above are only specific embodiments of the present invention, but the technical features of the present invention are not limited thereto. Any simple changes, equivalent replacements or modifications made based on the present invention to solve basically the same technical problems and achieve basically the same technical effects are all included in the protection scope of the present invention.
Claims
1. A process for preparing a high-strength ceramic product, characterized in that: The specific steps include: S1. Raw material preparation: ceramic powder, modified material, binder, flux; S2. Preparation of modified materials: combining specific inorganic substances with organic substances to obtain modified materials through physical mixing and chemical treatment; S3, raw material mixing: ceramic powder is mixed with modified material, binder and flux in proportion to prepare a uniform mixture; S4, molding: pressing the mixture into a molding die; S5. Sintering: Sinter the formed green body at 1200-1400°C for 2-4 hours to obtain a high-strength ceramic product.
2. The process for preparing the high-strength ceramic product according to claim 1, characterized in that: The modified material includes aluminum oxide and silicon carbide, which are mixed in a weight ratio of 1:
1.
3. The preparation process of the high-strength ceramic product according to claim 1, characterized in that: The binder is polyvinyl alcohol, and its content is 5%-10% of the weight of the mixture.
4. The process for preparing the high-strength ceramic product according to claim 1, characterized in that: The flux is borate, and its content is 3%-7% of the weight of the mixture.
5. The process for preparing the high-strength ceramic product according to claim 1, characterized in that: The sintering temperature is 1300°C.
6. The process for preparing a high-strength ceramic product according to claim 1, characterized in that: The sintering holding time is 3 hours.
7. The process for preparing a high-strength ceramic product according to claim 1, characterized in that: The particle size of the ceramic powder is 1-10 microns.
8. The process for preparing a high-strength ceramic product according to claim 1, characterized in that: The molding pressure is 100-200 MPa.
9. The process for preparing a high-strength ceramic product according to claim 1, characterized in that: The forming mold is made of stainless steel.
10. The process for preparing a high-strength ceramic product according to claim 1, characterized in that: The preparation method of the modified material comprises the following steps: a) preparing the required raw materials: alumina, silicon carbide and polyvinyl alcohol; b) Mix inorganic matter and organic matter in proportion: the specific proportion can be: Alumina: 10 parts by weight; Silicon carbide: 10 parts by weight; Polyvinyl alcohol: 5 parts by weight; c) placing the mixture in a mechanical stirrer and stirring it uniformly for 2 hours at a speed of 2000 rpm to ensure that the inorganic and organic substances are fully mixed to form a uniform mixture; d) chemically treating the mechanically stirred mixture, the specific method is as follows: dS1) placing the mixture in a reaction kettle and adding an appropriate amount of distilled water, the amount of water being 50% of the weight of the mixture; dS2) slowly adding 5% sodium hydroxide solution to the reactor, controlling the addition speed to prevent excessive reaction, the amount of sodium hydroxide solution used is 10% of the weight of the mixture; dS3) maintaining the reaction temperature at 80° C. for 2 hours to ensure that the inorganic and organic substances undergo sufficient chemical reactions to form a stable composite material; e) filtering the mixture after chemical treatment to remove excess solution and impurities, and then washing with distilled water for 3 times, with the amount of water used each time being 2 times the weight of the mixture, to ensure that the residual chemical reagents are completely removed; f) placing the washed mixture in an oven for drying at a temperature of 100° C. for 12 hours to ensure that the mixture is completely dried to obtain a solid composite material; e) crushing the dried solid composite material using a ball mill for 3 hours to obtain a fine powdered modified material; f) Screening the pulverized modified material using a 100-500 mesh screen to ensure that the particle size of the modified material is uniform, thereby obtaining the final modified material.
Citation Information
Patent Citations
Preparation method of silicon carbide ceramic high-temperature corrosion-resistant part
CN104649675A
Manufacturing method of ceramic cooker with high thermal shock resistance
CN105645925A
Preparation method of flat plate type nano ceramic film
CN108101549A
High-temperature-resistant heat-insulation ceramic processing technology
CN108298968A
High-temperature-resistant ceramic and preparation method thereof
CN111454052A
Cited By
High-strength ceramic and forming process thereof
CN120309315A
Ceramic piece and manufacturing method thereof
CN120664865A