Iron-manganese-zinc ferrite material as well as preparation method and application thereof
By optimizing the composition and preparation process of iron-manganese-zinc ferrite materials, the problem of reduced inductance of existing materials under stress has been solved, and iron-manganese-zinc ferrites with low stress sensitivity, high magnetic permeability and broadband high impedance have been achieved. Material, suitable for signal transmission and anti-electromagnetic interference.
Patent Information
- Application Number
- CN202410824343.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-25
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2044-06-25
AI Technical Summary
The existing iron-manganese-zinc ferrite material has the problem of reduced inductance under stress, and it is difficult to have low stress sensitivity, high magnetic permeability and broadband high impedance at the same time.
Fe-manganese-zinc ferrite material with a specific composition is used, including 68-71wt% Fe2O3, 11-15wt% ZnO and Mn3O4 as the main components, supplemented by auxiliary components such as CaCO3, Bi2O3, TiO2 or MoO3, through pre-sintering and sintering Process preparation, optimizing the material's microstructure to reduce stress sensitivity and improve magnetic permeability and impedance.
It has realized an iron-manganese-zinc ferrite material with a smaller inductance drop ratio under the same stress. It has low stress sensitivity, high initial magnetic permeability and broadband high impedance, and is suitable for signal transmission and anti-electromagnetic interference.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of ferrite materials, and relates to an iron-manganese-zinc ferrite material, and in particular to an iron-manganese-zinc ferrite material and a preparation method and application thereof. Background Art
[0002] In recent years, as humans gradually enter the electronic information age, electronic products have become indispensable for human work, office, leisure, entertainment, study, video conferencing, etc. While electronic products bring convenience to humans, they also bring certain environmental pollution, namely electromagnetic interference. High magnetic permeability manganese zinc ferrite is widely used in signal transmission and anti-electromagnetic interference technology. High magnetic permeability manganese zinc ferrite materials have been favored by customers due to their high magnetic permeability, low price and product miniaturization. However, due to the low resistivity of high-conductivity manganese zinc ferrite materials, it is difficult to meet the withstand voltage requirements. Spraying treatment, as well as assembly and winding treatment by downstream customers are required. The subsequent operations of the above cores will produce certain stress on the cores, resulting in a decrease in the inductance of the cores.
[0003] CN101870578A discloses a high magnetic permeability 12000μi wide temperature manganese-zinc ferrite material, which achieves high magnetic permeability and wide temperature performance of the manganese-zinc ferrite material with a magnetic permeability μi=12000 by limiting the content of iron oxide to 53-58mol%, the content of zinc oxide to 20-28mol%, and the rest being manganese oxide. However, the stress sensitivity of the high magnetic permeability 12000μi wide temperature manganese-zinc ferrite material disclosed in the patent is too high.
[0004] CN103011791A discloses a high magnetic permeability manganese-zinc ferrite material, which achieves high magnetic permeability by limiting the content of iron oxide to 51-54 mol%, the content of zinc oxide to 23-27 mol%, and the rest being manganese oxide; similarly, the stress sensitivity of the high magnetic permeability manganese-zinc ferrite material is too high.
[0005] CN105541316A discloses an anti-EMI manganese-zinc ferrite material and a preparation method thereof, which achieves the preparation of an anti-EMI manganese-zinc ferrite material with a magnetic permeability greater than 12000 by limiting the content of iron oxide to 50.5-52.5 mol%, the content of zinc oxide to 18.5-20.5 mol%, and the rest being manganese oxide. Similarly, the stress sensitivity of the anti-EMI manganese-zinc ferrite material is too high.
[0006] The currently disclosed iron-manganese-zinc ferrite materials all have certain defects, and there is a problem that they cannot have low stress sensitivity, high magnetic permeability and broadband high impedance at the same time. Therefore, it is very important to develop and design a new type of iron-manganese-zinc ferrite material and its preparation method. Summary of the invention
[0007] In view of the shortcomings of the prior art, the object of the present invention is to provide an iron-manganese-zinc ferrite material and a preparation method and application thereof. The iron-manganese-zinc ferrite material provided by the present invention has low stress sensitivity, high initial magnetic permeability and broadband high impedance, so that the proportion of inductance drop of the magnetic core made of the iron-manganese-zinc ferrite material is smaller when subjected to the same stress.
[0008] To achieve this object, the present invention adopts the following technical solutions:
[0009] In a first aspect, the present invention provides an iron-manganese-zinc ferrite material, wherein the iron-manganese-zinc ferrite material comprises a main component and an auxiliary component;
[0010] Taking the mass of the main component as 100%, the main component includes 68-71wt% of Fe2O3, 11-15wt% of ZnO, and the remainder of Mn3O4;
[0011] The auxiliary components include any one of CaCO3, Bi2O3, TiO2 or MoO3, or a combination of at least two thereof.
[0012] In the present invention, the mass of the main component is taken as percentage, and the main component includes Fe2O3 with a mass fraction of 68 to 71wt%, for example, it can be 68wt%, 68.5wt%, 69wt%, 69.5wt%, 70wt%, 70.5wt% or 71wt%, but it is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0013] In the present invention, the mass of the main component is expressed as 100%, and the main component includes ZnO with a mass fraction of 11 to 15 wt%, for example, 11 wt%, 11.5 wt%, 12 wt%, 12.5 wt%, 13 wt%, 13.5 wt%, 14 wt%, 14.5 wt% or 15 wt%, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0014] The auxiliary components in the present invention include any one of CaCO3, Bi2O3, TiO2 or MoO3 or a combination of at least two of them. Typical but non-limiting combinations include a combination of CaCO3 and Bi2O3, a combination of Bi2O3 and TiO2, a combination of TiO2 and MoO3, or a combination of CaCO3, Bi2O3 and TiO2.
[0015] The iron-manganese-zinc ferrite material provided by the present invention has low stress sensitivity, high initial magnetic permeability and broadband high impedance, so that the proportion of inductance drop of the magnetic core made of the iron-manganese-zinc ferrite material is small under the condition of the same stress.
[0016] Preferably, based on the mass of the main component as the total mass, the auxiliary components include CaCO3 with a mass fraction of 200 to 2000 ppm, Bi2O3 with a mass fraction of 200 to 2000 ppm, TiO2 with a mass fraction of 200 to 2000 ppm, and MoO3 with a mass fraction of 200 to 2000 ppm.
[0017] In the present invention, the mass of the main component is taken as the total mass, and the auxiliary component includes CaCO3 with a mass fraction of 200 to 2000 ppm, for example, it can be 200 ppm, 300 ppm, 400 ppm, 500 ppm, 600 ppm, 700 ppm, 800 ppm, 900 ppm, 1000 ppm, 1100 ppm, 1200 ppm, 1300 ppm, 1400 ppm, 1500 ppm, 1600 ppm, 1700 ppm, 1800 ppm, 1900 ppm or 2000 ppm, but it is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0018] In the present invention, the mass of the main component is taken as the total mass, and the auxiliary component includes Bi2O3 with a mass fraction of 200 to 2000 ppm, for example, it can be 200 ppm, 300 ppm, 400 ppm, 500 ppm, 600 ppm, 700 ppm, 800 ppm, 900 ppm, 1000 ppm, 1100 ppm, 1200 ppm, 1300 ppm, 1400 ppm, 1500 ppm, 1600 ppm, 1700 ppm, 1800 ppm, 1900 ppm or 2000 ppm, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0019] In the present invention, the mass of the main component is taken as the total mass, and the auxiliary component includes TiO2 with a mass fraction of 200 to 2000 ppm, for example, it can be 200 ppm, 300 ppm, 400 ppm, 500 ppm, 600 ppm, 700 ppm, 800 ppm, 900 ppm, 1000 ppm, 1100 ppm, 1200 ppm, 1300 ppm, 1400 ppm, 1500 ppm, 1600 ppm, 1700 ppm, 1800 ppm, 1900 ppm or 2000 ppm, but it is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0020] In the present invention, the mass of the main component is taken as the total mass, and the auxiliary component includes MoO3 with a mass fraction of 200 to 2000 ppm, for example, it can be 200 ppm, 300 ppm, 400 ppm, 500 ppm, 600 ppm, 700 ppm, 800 ppm, 900 ppm, 1000 ppm, 1100 ppm, 1200 ppm, 1300 ppm, 1400 ppm, 1500 ppm, 1600 ppm, 1700 ppm, 1800 ppm, 1900 ppm or 2000 ppm, but it is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0021] Preferably, based on the mass of the main component as percentage, the main component includes 69-70wt% of Fe2O3, 12.5-13.5wt% of ZnO, and the remainder is Mn3O4.
[0022] In the present invention, the mass of the main component is taken as percentage, and the main component includes Fe2O3 with a mass fraction of 69 to 70wt%, for example, it can be 69wt%, 69.1wt%, 69.2wt%, 69.3wt%, 69.4wt%, 69.5wt%, 69.6wt%, 69.7wt%, 69.8wt%, 69.9wt% or 70wt%, but it is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0023] In the present invention, the mass of the main component is taken as percentage, and the main component includes ZnO with a mass fraction of 12.5 to 13.5wt%, for example, it can be 12.5wt%, 12.6wt%, 12.7wt%, 12.8wt%, 12.9wt%, 13wt%, 13.1wt%, 13.2wt%, 13.3wt%, 13.4wt% or 13.5wt%, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0024] Preferably, based on the mass of the main component as the total mass, the auxiliary components include CaCO3 with a mass fraction of 200 to 1000 ppm, Bi2O3 with a mass fraction of 200 to 1000 ppm, TiO2 with a mass fraction of 200 to 1000 ppm, and MoO3 with a mass fraction of 200 to 1000 ppm.
[0025] In the present invention, the mass of the main component is taken as the total mass, and the auxiliary component includes CaCO3 with a mass fraction of 200 to 1000 ppm, for example, it can be 200 ppm, 250 ppm, 300 ppm, 350 ppm, 400 ppm, 450 ppm, 500 ppm, 550 ppm, 600 ppm, 650 ppm, 700 ppm, 750 ppm, 800 ppm, 850 ppm, 900 ppm, 950 ppm or 1000 ppm, but it is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0026] In the present invention, the mass of the main component is taken as the total mass, and the auxiliary component includes Bi2O3 with a mass fraction of 200 to 1000 ppm, for example, it can be 200 ppm, 250 ppm, 300 ppm, 350 ppm, 400 ppm, 450 ppm, 500 ppm, 550 ppm, 600 ppm, 650 ppm, 700 ppm, 750 ppm, 800 ppm, 850 ppm, 900 ppm, 950 ppm or 1000 ppm, but it is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0027] In the present invention, the mass of the main component is taken as the total mass, and the auxiliary component includes TiO2 with a mass fraction of 200 to 1000 ppm, for example, it can be 200 ppm, 250 ppm, 300 ppm, 350 ppm, 400 ppm, 450 ppm, 500 ppm, 550 ppm, 600 ppm, 650 ppm, 700 ppm, 750 ppm, 800 ppm, 850 ppm, 900 ppm, 950 ppm or 1000 ppm, but it is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0028] In the present invention, the mass of the main component is taken as the total mass, and the auxiliary component includes MoO3 with a mass fraction of 200 to 1000 ppm, for example, it can be 200 ppm, 250 ppm, 300 ppm, 350 ppm, 400 ppm, 450 ppm, 500 ppm, 550 ppm, 600 ppm, 650 ppm, 700 ppm, 750 ppm, 800 ppm, 850 ppm, 900 ppm, 950 ppm or 1000 ppm, but it is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0029] In a second aspect, the present invention provides a method for preparing the iron-manganese-zinc ferrite material according to the first aspect, the preparation method comprising:
[0030] (1) mixing a main component and a solvent to obtain a slurry and then pre-calcining to obtain a pre-calcined material, wherein the main component includes Fe2O3, ZnO and Mn3O4;
[0031] (2) mixing the pre-sintered material obtained in step (1) with auxiliary components to obtain a mixed material;
[0032] (3) Sintering the mixture obtained in step (2) in a protective atmosphere to obtain an iron-manganese-zinc ferrite material.
[0033] Preferably, the mixing method in step (1) includes a first ball milling, and the ball milling time is 20 to 80 min, for example, it can be 20 min, 25 min, 30 min, 35 min, 40 min, 45 min, 50 min, 55 min, 60 min, 65 min, 70 min, 75 min or 80 min, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0034] Preferably, during the first ball milling process, the mass ratio of the main component, the grinding balls and the solvent is (0.5-1.5):(3.5-4.5):(0.5-1.5).
[0035] The mass ratio of the main component to the grinding ball in the present invention is 0.5:3.5, 0.6:3.5, 0.9:3.5, 1.1:3.5, 1.3:3.5, 1.5:3.5, 0.5:4, 0.6:4, 0.9:4, 1.1:4, 1.3:4, 1.5:4, 0.5:4.5, 0.6:4.5, 1.1:4.5 or 1.3:4.5, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0036] The mass ratio of the grinding balls to the solvent in the present invention is 3.5:0.5, 3.5:0.6, 3.5:0.9, 3.5:1.1, 3.5:1.3, 3.5:1.5, 4:0.5, 4:0.6, 4:0.9, 4:1.1, 4:1.3, 4:1.5, 4.5:0.5, 4.5:0.6, 4.5:1.1 or 4.5:1.3, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0037] Preferably, the solvent in step (1) comprises water.
[0038] Preferably, the pre-burning temperature in step (1) is 980-1035° C., the pre-burning is carried out in a rotary kiln, and the speed at which the slurry enters the rotary kiln is 400-500 kg / h.
[0039] The pre-calcining temperature in step (1) of the present invention is 980-1035°C, for example, it can be 980°C, 985°C, 990°C, 995°C, 1000°C, 1005°C, 1010°C, 1015°C, 1020°C, 1025°C, 1030°C or 1035°C, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0040] In the present invention, the speed at which the slurry enters the rotary kiln is 400-500kg / h, for example, it can be 400kg / h, 410kg / h, 420kg / h, 430kg / h, 440kg / h, 450kg / h, 460kg / h, 470kg / h, 480kg / h, 490kg / h or 500kg / h, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0041] Preferably, the mixing in step (2) also includes mixing of a dispersant and a binder.
[0042] Preferably, the mixing method in step (2) includes a second ball milling, and the time of the second ball milling is 120 to 150 minutes, for example, it can be 120 minutes, 125 minutes, 130 minutes, 135 minutes, 140 minutes, 145 minutes or 150 minutes, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0043] Preferably, during the second ball milling process, the mass ratio of the pre-sintered material, the dispersant, the binder and the grinding balls is (0.5-1.5):(0.005-0.015):(0.05-0.15):(3-5).
[0044] The mass ratio of the pre-sintered material to the dispersant in the second ball milling process of the present invention is (0.5-1.5):(0.005-0.015), for example, it can be 0.5:0.005, 0.7:0.005, 0.9:0.005, 1.1:0.005, 1.3:0.005, 1.5:0.005, 0.5:0.007, 0.9:007, 1.1: 0.007, 1.3:0.007, 1.5:0.007, 0.5:0.009, 0.7:0.009, 1.1:0.009, 1.3:0.009, 0.5:0.015, 0.7:0.015, 1.1:0.015 or 1.3:0.015, but are not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0045] The mass ratio of the pre-sintered material to the binder in the second ball milling process of the present invention is (0.5-1.5):(0.05-0.15), for example, it can be 0.5:0.05, 0.7:0.05, 0.9:0.05, 1.1:0.05, 1.3:0.05, 1.5:0.05, 0.5:0.07, 0.9:0.07, 1.1:0.07, 1.3:0.07, 1.5:0.07, 0.5:0.09, 0.7:0.09, 1.1:0.09, 1.3:0.09, 0.5:0.15, 0.7:0.15, 1.1:0.15 or 1.3:0.15, but is not limited to the listed values, and other unlisted values within the numerical range are equally applicable.
[0046] The mass ratio of the pre-sintered material to the grinding balls in the second ball milling process of the present invention is (0.5-1.5):(3-5), for example, it can be 0.5:3, 0.7:3, 0.8:3, 1.1:3, 1.3:3, 1.5:3, 0.5:4, 0.7:4, 0.8:4, 1.1:4, 1.3:4, 1.5:4, 0.5:5, 0.7:5, 0.8:5, 1.1:5, 1.3:5 or 1.5:5, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0047] Preferably, the dispersant comprises citric acid.
[0048] Preferably, the adhesive comprises PVA.
[0049] Preferably, spray granulation is further included between step (2) and step (3).
[0050] Preferably, embryo pressing is further included between the spray granulation and step (3).
[0051] Preferably, the oxygen content in the protective atmosphere in step (3) is 0 to 21 vol%, for example, it can be 0 vol%, 1 vol%, 3 vol%, 5 vol%, 7 vol%, 9 vol%, 11 vol%, 13 vol%, 15 vol%, 17 vol%, 19 vol% or 21 vol%, but is not limited to the listed values. Other values not listed within the numerical range are also applicable, preferably 0 to 10 vol%.
[0052] Preferably, the sintering temperature in step (3) is 1200-1400° C. and the sintering time is 4-10 hours.
[0053] The sintering temperature in step (3) of the present invention is 1200-1400°C, for example, it can be 1200°C, 1210°C, 1220°C, 1230°C, 1240°C, 1250°C, 1260°C, 1270°C, 1280°C, 1290°C, 1300°C, 1310°C, 1320°C, 1330°C, 1340°C, 1350°C, 1360°C, 1370°C, 1380°C, 1390°C or 1400°C, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0054] The sintering time in step (3) of the present invention is 4 to 10 hours, for example, 4 hours, 5 hours, 6 hours, 7 hours, 8 hours, 9 hours or 10 hours, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0055] Preferably, the sintering in step (3) is carried out in three stages; the temperature of the first stage is 1350-1400° C., and the time is 7-9 hours; the temperature of the second stage is 1350-1400° C., and the time is 0.5-1.5 hours; the temperature of the third stage is 1300-1350° C., and the time is 0.5-1.5 hours;
[0056] The temperature of the first stage in the present invention is 1350-1400°C, for example, it can be 1350°C, 1360°C, 1370°C, 1380°C, 1390°C or 1400°C, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0057] The time of the first section in the present invention is 7 to 9 hours, for example, it can be 7h, 7.2h, 7.4h, 7.6h, 7.8h, 8h, 8.2h, 8.4h, 8.6h, 8.8h or 9h, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0058] The temperature of the second stage in the present invention is 1350-1400°C, for example, it can be 1350°C, 1360°C, 1370°C, 1380°C, 1390°C or 1400°C, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0059] The time of the second segment in the present invention is 0.5 to 1.5 h, for example, it can be 0.5 h, 0.6 h, 0.7 h, 0.8 h, 0.9 h, 1 h, 1.1 h, 1.2 h, 1.35 h, 1.4 h or 1.5 h, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0060] The temperature of the third stage in the present invention is 1300-1350°C, for example, it can be 1300°C, 1310°C, 1320°C, 1330°C, 1340°C or 1350°C, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0061] The time of the third section in the present invention is 0.5 to 1.5 hours, for example, it can be 0.5 hours, 0.6 hours, 0.7 hours, 0.8 hours, 0.9 hours, 1 hour, 1.1 hours, 1.2 hours, 1.35 hours, 1.4 hours or 1.5 hours, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0062] Preferably, step (3) further includes cooling after the sintering, and the cooling is performed under a balanced oxygen partial pressure.
[0063] As a preferred technical solution of the preparation method of the present invention, the preparation method comprises:
[0064] (1) mixing the main component and water by ball milling for 20 to 80 minutes to obtain a slurry, wherein the mass ratio of the main component, the grinding ball and the solvent is (0.5 to 1.5):(3.5 to 4.5):(0.5 to 1.5), and then pre-calcining in a rotary kiln at a temperature of 980 to 1035° C., and the slurry enters the rotary kiln at a speed of 400 to 500 kg / h to obtain a pre-calcined material, wherein the main component includes Fe2O3, ZnO and Mn3O4;
[0065] (2) mixing the pre-sintered material obtained in step (1) with auxiliary components, a dispersant and a binder by ball milling, wherein the mass ratio of the pre-sintered material, the dispersant, the binder and the grinding balls during the ball milling is (0.5-1.5):(0.005-0.015):(0.05-0.15):(3-5) to obtain a mixed material;
[0066] (3) The mixture obtained in step (2) is spray granulated and then pressed to obtain an embryo body, and the obtained embryo body is sintered, and the sintering is carried out in three stages; the temperature of the first stage is 1350-1400°C and the time is 7-9 hours; the temperature of the second stage is 1350-1400°C and the time is 0.5-1.5 hours; the temperature of the third stage is 1200-1350°C and the time is 0.5-1.5 hours, and then the temperature is lowered under a balanced oxygen partial pressure to obtain an iron-manganese-zinc ferrite material.
[0067] In a third aspect, the present invention provides an application of the iron-manganese-zinc ferrite material described in the first aspect, wherein the iron-manganese-zinc ferrite material is used for signal transmission or anti-electromagnetic interference.
[0068] Compared with the prior art, the present invention has the following beneficial effects:
[0069] The iron-manganese-zinc ferrite material provided by the present invention has low stress sensitivity, high initial magnetic permeability and broadband high impedance, so that the proportion of inductance drop of the magnetic core made of the iron-manganese-zinc ferrite material is small under the condition of the same stress. DETAILED DESCRIPTION
[0070] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.
[0071] Example 1
[0072] This embodiment provides an iron-manganese-zinc ferrite material, wherein the iron-manganese-zinc ferrite material includes a main component and an auxiliary component;
[0073] Taking the mass of the main component as 100%, the main component includes 69.08wt% of Fe2O3, 12.23wt% of ZnO, and the remainder is Mn3O4.
[0074] Taking the mass of the main component as the total mass, the auxiliary components include CaCO3 with a mass fraction of 400 ppm, Bi2O3 with a mass fraction of 500 ppm, TiO2 with a mass fraction of 300 ppm, and MoO3 with a mass fraction of 200 ppm.
[0075] The preparation method of the iron-manganese-zinc ferrite material is:
[0076] (1) mixing the main component and water by ball milling for 30 minutes to obtain a slurry, wherein the mass ratio of the main component, grinding balls and water during the ball milling process is 1:4:1, and then pre-calcining in a rotary kiln at a temperature of 1020° C., and the slurry enters the rotary kiln at a speed of 450 kg / h to obtain a pre-calcined material, wherein the main component includes Fe2O3, ZnO and Mn3O4;
[0077] (2) mixing the pre-burned material obtained in step (1) with auxiliary components, citric acid and PVA by ball milling, wherein the mass ratio of the pre-burned material, citric acid, PVA and grinding balls during the ball milling is 1:0.01:0.1:4 to obtain a mixed material, wherein the auxiliary components include CaCO3, Bi2O3, TiO2 and MoO3;
[0078] (3) The mixture obtained in step (2) is spray granulated and then pressed to obtain an embryo body, and the obtained embryo body is sintered at 1385° C. for 8 h in a nitrogen atmosphere with an oxygen content of 21 vol%, and then sintered at 1385° C. for 1 h in a nitrogen atmosphere with an oxygen content of 8 vol%, and then sintered at 1260° C. for 1 h in a nitrogen atmosphere with an oxygen content of 6 vol%, and then cooled under a balanced oxygen partial pressure, and the cooling is carried out in a nitrogen atmosphere with an oxygen content of 0 vol%, to obtain an iron-manganese-zinc ferrite material.
[0079] Example 2
[0080] This embodiment provides an iron-manganese-zinc ferrite material, wherein the iron-manganese-zinc ferrite material includes a main component and an auxiliary component;
[0081] Taking the mass of the main component as 100%, the main component includes 69.24wt% of Fe2O3, 12.41wt% of ZnO, and the remainder is Mn3O4.
[0082] Taking the mass of the main component as the total mass, the auxiliary components include CaCO3 with a mass fraction of 400 ppm, Bi2O3 with a mass fraction of 500 ppm, TiO2 with a mass fraction of 300 ppm, and MoO3 with a mass fraction of 200 ppm.
[0083] The preparation method of the iron-manganese-zinc ferrite material is:
[0084] (1) mixing the main component and water by ball milling for 30 minutes to obtain a slurry, wherein the mass ratio of the main component, the grinding ball and the solvent is 1:4:1 during the ball milling process, and then pre-calcining in a rotary kiln at a temperature of 1020° C., and the slurry enters the rotary kiln at a speed of 450 kg / h to obtain a pre-calcined material, wherein the main component includes Fe2O3, ZnO and Mn3O4;
[0085] (2) mixing the pre-burned material obtained in step (1) with auxiliary components, citric acid and PVA by ball milling, wherein the mass ratio of the pre-burned material, citric acid, PVA and grinding balls during the ball milling is 1:0.01:0.1:4 to obtain a mixed material, wherein the auxiliary components include CaCO3, Bi2O3, TiO2 and MoO3;
[0086] (3) The mixture obtained in step (2) is spray granulated and then pressed to obtain an embryo body, and the obtained embryo body is sintered at 1385° C. for 8 h in a protective atmosphere with an oxygen content of 21 vol%, and then sintered at 1385° C. for 1 h in a nitrogen atmosphere with an oxygen content of 8 vol%, and then sintered at 1260° C. for 1 h in a nitrogen atmosphere with an oxygen content of 6 vol%, and then cooled under a balanced oxygen partial pressure, and the cooling is carried out in a nitrogen atmosphere with an oxygen content of 0 vol%, to obtain an iron-manganese-zinc ferrite material.
[0087] Example 3
[0088] This embodiment provides an iron-manganese-zinc ferrite material, wherein the iron-manganese-zinc ferrite material includes a main component and an auxiliary component;
[0089] Taking the mass of the main component as 100%, the main component includes 69.4wt% of Fe2O3, 12.6wt% of ZnO, and the remainder is Mn3O4.
[0090] Taking the mass of the main component as the total mass, the auxiliary components include CaCO3 with a mass fraction of 400 ppm, Bi2O3 with a mass fraction of 500 ppm, TiO2 with a mass fraction of 300 ppm, and MoO3 with a mass fraction of 200 ppm.
[0091] The preparation method of the iron-manganese-zinc ferrite material is:
[0092] (1) mixing the main component and water by ball milling for 30 minutes to obtain a slurry, wherein the mass ratio of the main component, the grinding ball and the solvent is 1:4:1 during the ball milling process, and then pre-calcining in a rotary kiln at a temperature of 1020° C., and the slurry enters the rotary kiln at a speed of 450 kg / h to obtain a pre-calcined material, wherein the main component includes Fe2O3, ZnO and Mn3O4;
[0093] (2) mixing the pre-burned material obtained in step (1) with auxiliary components, citric acid and PVA by ball milling, wherein the mass ratio of the pre-burned material, citric acid, PVA and grinding balls during the ball milling is 1:0.01:0.1:4 to obtain a mixed material, wherein the auxiliary components include CaCO3, Bi2O3, TiO2 and MoO3;
[0094] (3) The mixture obtained in step (2) is spray granulated and then pressed to obtain an embryo body, and the obtained embryo body is sintered at 1385° C. for 8 h in a nitrogen atmosphere with an oxygen content of 21 vol%, and then sintered at 1385° C. for 1 h in a nitrogen atmosphere with an oxygen content of 8 vol%, and then sintered at 1260° C. for 1 h in a nitrogen atmosphere with an oxygen content of 6 vol%, and then cooled under a balanced oxygen partial pressure, and the cooling is carried out in a nitrogen atmosphere with an oxygen content of 0 vol%, to obtain an iron-manganese-zinc ferrite material.
[0095] Example 4
[0096] This embodiment provides an iron-manganese-zinc ferrite material, wherein the iron-manganese-zinc ferrite material includes a main component and an auxiliary component;
[0097] Taking the mass of the main component as 100%, the main component includes 69.56wt% of Fe2O3, 12.78wt% of ZnO, and the remainder is Mn3O4.
[0098] Taking the mass of the main component as the total mass, the auxiliary components include CaCO3 with a mass fraction of 400 ppm, Bi2O3 with a mass fraction of 500 ppm, TiO2 with a mass fraction of 300 ppm, and MoO3 with a mass fraction of 200 ppm.
[0099] The preparation method of the iron-manganese-zinc ferrite material is:
[0100] (1) mixing the main component and water by ball milling for 30 minutes to obtain a slurry, wherein the mass ratio of the main component, the grinding ball and the solvent is 1:4:1 during the ball milling process, and then pre-calcining in a rotary kiln at a temperature of 1020° C., and the slurry enters the rotary kiln at a speed of 450 kg / h to obtain a pre-calcined material, wherein the main component includes Fe2O3, ZnO and Mn3O4;
[0101] (2) mixing the pre-burned material obtained in step (1) with auxiliary components, citric acid and PVA by ball milling, wherein the mass ratio of the pre-burned material, citric acid, PVA and grinding balls during the ball milling is 1:0.01:0.1:4 to obtain a mixed material, wherein the auxiliary components include CaCO3, Bi2O3, TiO2 and MoO3;
[0102] (3) The mixture obtained in step (2) is spray granulated and then pressed to obtain an embryo body, and the obtained embryo body is sintered at 1385° C. for 8 h in a nitrogen atmosphere with an oxygen content of 21 vol%, and then sintered at 1385° C. for 1 h in a nitrogen atmosphere with an oxygen content of 8 vol%, and then sintered at 1260° C. for 1 h in a nitrogen atmosphere with an oxygen content of 6 vol%, and then cooled under a balanced oxygen partial pressure, and the cooling is carried out in a nitrogen atmosphere with an oxygen content of 0 vol%, to obtain an iron-manganese-zinc ferrite material.
[0103] Example 5
[0104] This embodiment provides an iron-manganese-zinc ferrite material, which is the same as that of Embodiment 1 except that the mass fraction of CaCO3 in the auxiliary component is 100 ppm.
[0105] Example 6
[0106] This embodiment provides an iron-manganese-zinc ferrite material, which is the same as that of Embodiment 1 except that the mass fraction of CaCO3 in the auxiliary component is 2500ppm.
[0107] Example 7
[0108] This embodiment provides an iron-manganese-zinc ferrite material, which is the same as that of Embodiment 1 except that the mass fraction of Bi2O3 in the auxiliary component is 2500ppm.
[0109] Example 8
[0110] This embodiment provides an iron-manganese-zinc ferrite material, which is the same as that of Embodiment 1 except that the mass fraction of TiO2 in the auxiliary component is 100 ppm.
[0111] Example 9
[0112] This embodiment provides an iron-manganese-zinc ferrite material, which is the same as that of Embodiment 1 except that the mass fraction of TiO2 in the auxiliary component is 2500ppm.
[0113] Example 10
[0114] This embodiment provides an iron-manganese-zinc ferrite material, which is the same as that of Embodiment 1 except that the mass fraction of MoO3 in the auxiliary component is 2500ppm.
[0115] Embodiment 11
[0116] The present embodiment provides an iron-manganese-zinc ferrite material, which is the same as Example 1 except that the step (3) of "sintering the obtained embryo at 1385°C for 8 hours in a nitrogen atmosphere with an oxygen content of 21 vol%, sintering it at 1385°C for 1 hour in a nitrogen atmosphere with an oxygen content of 8 vol%, and then sintering it at 1260°C for 1 hour in a nitrogen atmosphere with an oxygen content of 6 vol%" is replaced by "sintering the obtained embryo at 1385°C for 10 hours in a nitrogen atmosphere with an oxygen content of 21 vol%.
[0117] Example 12
[0118] The present embodiment provides an iron-manganese-zinc ferrite material, which is the same as Example 1 except that in step (3), "the obtained embryo is sintered at 1385°C for 8 hours in a nitrogen atmosphere with an oxygen content of 21 vol%" is replaced by "the obtained embryo is sintered at 1500°C for 8 hours in a nitrogen atmosphere with an oxygen content of 21 vol%".
[0119] Embodiment 13
[0120] The present embodiment provides an iron-manganese-zinc ferrite material, which is the same as Example 1 except that in step (3), "sintering at 1260°C for 1 hour in a nitrogen atmosphere with an oxygen content of 6 vol%" is replaced by "sintering at 1100°C for 1 hour in a nitrogen atmosphere with an oxygen content of 6 vol%.
[0121] Comparative Example 1
[0122] This comparative example provides an iron-manganese-zinc ferrite material, which is the same as Example 1 except that the mass fraction of Fe2O3 in the main component is 65wt% and the mass fraction of Mn3O4 is increased accordingly.
[0123] Comparative Example 2
[0124] This comparative example provides an iron-manganese-zinc ferrite material, which is the same as Example 1 except that the mass fraction of Fe2O3 in the main component is 73wt% and the mass fraction of Mn3O4 is reduced accordingly.
[0125] Comparative Example 3
[0126] This comparative example provides an iron-manganese-zinc ferrite material, which is the same as Example 1 except that the mass fraction of ZnO in the main component is 9wt% and the mass fraction of Mn3O4 is increased accordingly.
[0127] Comparative Example 4
[0128] This comparative example provides an iron-manganese-zinc ferrite material, which is the same as Example 1 except that the mass fraction of ZnO in the main component is 17wt% and the mass fraction of Mn3O4 is reduced accordingly.
[0129] Comparative Example 5
[0130] This comparative example provides an iron-manganese-zinc ferrite material, which is the same as Example 1 except that the auxiliary components in the iron-manganese-zinc ferrite material are omitted.
[0131] The iron-manganese-zinc ferrite materials in the above-mentioned embodiments and comparative examples were subjected to stress sensitivity test, initial magnetic permeability test and broadband impedance test respectively;
[0132] The stress sensitivity test method is the oil pressure method, and the magnetic permeability ratio at 10MPa relative to the magnetic permeability at 0MPa is shown in Table 1;
[0133] The method for testing the initial magnetic permeability is: winding 10Ts, testing the inductance, and then testing and obtaining the initial magnetic permeability μi at 0.25V, 25°C and 10KHz according to the calculation formula of inductance and magnetic permeability as shown in Table 1;
[0134] The method for broadband impedance testing is: winding 1Ts, and using an impedance analyzer to test the impedance Z at a frequency of 1MHz as shown in Table 1.
[0135] Table 1
[0136]
[0137] From Table 1, we can get:
[0138] (1) The iron-manganese-zinc ferrite materials prepared in Examples 1 to 4 have a relatively high magnetic permeability, indicating that the obtained iron-manganese-zinc ferrite materials have a low stress sensitivity. At the same time, the obtained iron-manganese-zinc ferrite materials also have a high initial magnetic permeability and a wide-band high impedance;
[0139] (2) By comparing Example 1 with Examples 5 and 6, it can be seen that the mass fraction of CaCO3 in the auxiliary component of the present invention affects the performance of the iron-manganese-zinc ferrite material; when the mass fraction of CaCO3 is low, the impedance R of the iron-manganese-zinc ferrite material becomes smaller, because the resistivity becomes smaller due to the low calcium carbonate; when the mass fraction of CaCO3 is high, the magnetic permeability ratio of the iron-manganese-zinc ferrite material remains unchanged and the initial magnetic permeability μi becomes smaller;
[0140] (3) By comparing Examples 1 and 7, it can be seen that the mass fraction of Bi2O3 in the auxiliary component of the present invention affects the performance of the iron-manganese-zinc ferrite material; when the mass fraction of Bi2O3 is high, the magnetic permeability ratio of the iron-manganese-zinc ferrite material becomes larger, the initial magnetic permeability μi becomes smaller, and the impedance R becomes smaller. This is because the low Bi2O3 content makes the grain size larger;
[0141] (4) By comparing Example 1 with Examples 8 and 9, it can be seen that the mass fraction of TiO2 in the auxiliary component of the present invention will affect the performance of the iron-manganese-zinc ferrite material; when the mass fraction of TiO2 is low, the magnetic permeability ratio of the iron-manganese-zinc ferrite material remains unchanged, the initial magnetic permeability μi becomes smaller, and the impedance R remains unchanged. This is because the change of TiO2 will change the position of the two peaks; when the mass fraction of TiO2 is high, the magnetic permeability ratio of the iron-manganese-zinc ferrite material remains unchanged, the initial magnetic permeability μi becomes smaller, and the impedance R remains unchanged. This is because the change of TiO2 will change the position of the two peaks.
[0142] (5) By comparing Examples 1 and 10, it can be seen that the mass fraction of MoO3 in the auxiliary component of the present invention affects the performance of the iron-manganese-zinc ferrite material; when the mass fraction of MoO3 is high, the magnetic permeability ratio of the iron-manganese-zinc ferrite material becomes larger, the initial magnetic permeability μi becomes smaller, and the impedance R becomes smaller. This is because the low MoO3 content makes the grain size larger;
[0143] (6) By comparing Example 1 with Example 11, it can be seen that the sintering in three stages in step (3) of the present invention will affect the performance of the iron-manganese-zinc ferrite material; when the three-stage sintering is replaced by one-stage sintering, the magnetic permeability ratio of the iron-manganese-zinc ferrite material will become larger or smaller, the initial magnetic permeability μi will become smaller, and the impedance R will become smaller or larger, which is due to the change in the grain size;
[0144] (7) By comparing Example 1 with Examples 12 and 13, it can be seen that the sintering temperature in step (3) of the present invention affects the performance of the iron-manganese-zinc ferrite material; when the sintering temperature is low, the initial magnetic permeability μi of the iron-manganese-zinc ferrite material will become smaller; when the sintering temperature is high, the magnetic permeability ratio of the iron-manganese-zinc ferrite material will become larger, the initial magnetic permeability μi will become smaller, and the impedance R will become smaller. This is because the grain size becomes larger and more zinc oxide volatilizes;
[0145] (8) By comparing Example 1 with Comparative Examples 1 and 2, it can be seen that the mass fraction of Fe2O3 in the main component of the present invention affects the performance of the iron-manganese-zinc ferrite material; when the mass fraction of Fe2O3 in the main component is low, the magnetic permeability ratio of the iron-manganese-zinc ferrite material remains unchanged, the initial magnetic permeability μi decreases, and the impedance R remains unchanged, which is due to the movement of the two peaks; when the mass fraction of Fe2O3 in the main component is high, the magnetic permeability ratio of the iron-manganese-zinc ferrite material remains unchanged, the initial magnetic permeability μi decreases, and the impedance R remains unchanged, which is due to the movement of the two peaks;
[0146] (9) By comparing Example 1 with Comparative Examples 3 and 4, it can be seen that the mass fraction of ZnO in the main component of the present invention affects the performance of the iron-manganese-zinc ferrite material; when the mass fraction of ZnO in the main component is low, the magnetic permeability ratio of the iron-manganese-zinc ferrite material remains unchanged, the initial magnetic permeability μi decreases, and the impedance R remains unchanged, which is due to the movement of the two peaks; when the mass fraction of ZnO in the main component is high, the magnetic permeability ratio of the iron-manganese-zinc ferrite material remains unchanged, the initial magnetic permeability μi decreases, and the impedance R remains unchanged, which is due to the movement of the two peaks;
[0147] (9) By comparing Example 1 with Comparative Example 5, it can be seen that the auxiliary components in the iron-manganese-zinc ferrite material of the present invention will affect the performance of the iron-manganese-zinc ferrite material; when the auxiliary components are omitted, the magnetic permeability ratio of the iron-manganese-zinc ferrite material remains unchanged, the initial magnetic permeability μi becomes smaller, and the impedance R remains unchanged, which is due to the abnormal growth of grains.
[0148] In summary, the iron-manganese-zinc ferrite material provided by the present invention has low stress sensitivity, high initial magnetic permeability and broadband high impedance, so that the proportion of inductance drop of the magnetic core made of the iron-manganese-zinc ferrite material is relatively small when subjected to the same stress.
[0149] The above description is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention are within the protection scope and disclosure scope of the present invention.
Claims
1. An iron-manganese-zinc ferrite material, characterized in that: The iron-manganese-zinc ferrite material comprises a main component and an auxiliary component; Based on the mass of the main component as 100%, the main component includes 68-71wt% of Fe2O3, 11-15wt% of ZnO, and the remainder is Mn3O4; The auxiliary components include any one of CaCO3, Bi2O3, TiO2 or MoO3, or a combination of at least two thereof.
2. The iron-manganese-zinc ferrite material according to claim 1, characterized in that: Taking the mass of the main component as the total mass, the auxiliary components include CaCO3 with a mass fraction of 200 to 2000 ppm, Bi2O3 with a mass fraction of 200 to 2000 ppm, TiO2 with a mass fraction of 200 to 2000 ppm, and MoO3 with a mass fraction of 200 to 2000 ppm.
3. The iron-manganese-zinc ferrite material according to claim 1 or 2, characterized in that: Based on the mass of the main component as 100%, the main component includes 69-70wt% of Fe2O3, 12.5-13.5wt% of ZnO, and the remainder is Mn3O4; Preferably, based on the mass of the main component as the total mass, the auxiliary components include CaCO3 with a mass fraction of 200 to 1000 ppm, Bi2O3 with a mass fraction of 200 to 1000 ppm, TiO2 with a mass fraction of 200 to 1000 ppm, and MoO3 with a mass fraction of 200 to 1000 ppm.
4. A method for preparing the iron-manganese-zinc ferrite material according to any one of claims 1 to 3, characterized in that: The preparation method comprises: (1) mixing a main component and a solvent to obtain a slurry and then pre-calcining to obtain a pre-calcined material, wherein the main component includes Fe2O3, ZnO and Mn3O4; (2) mixing the pre-sintered material obtained in step (1) with auxiliary components to obtain a mixed material; (3) Sintering the mixture obtained in step (2) in a protective atmosphere to obtain an iron-manganese-zinc ferrite material.
5. The preparation method according to claim 4, characterized in that: The mixing method in step (1) includes a first ball milling, and the ball milling time is 20 to 80 minutes; Preferably, the mass ratio of the main component, the grinding balls and the solvent during the first ball milling process is (0.5-1.5):(3.5-4.5):(0.5-1.5); Preferably, the pre-burning temperature in step (1) is 980-1035° C., the pre-burning is carried out in a rotary kiln, and the speed at which the slurry enters the rotary kiln is 400-500 kg / h.
6. The preparation method according to claim 4 or 5, characterized in that: The mixing in step (2) also includes mixing of a dispersant and a binder; Preferably, the mixing method in step (2) includes a second ball milling, and the time of the second ball milling is 120 to 150 minutes; Preferably, during the second ball milling process, the mass ratio of the pre-sintered material, the dispersant, the binder and the grinding balls is (0.5-1.5):(0.005-0.015):(0.05-0.15):(3-5).
7. The preparation method according to any one of claims 4 to 6, characterized in that: The step (2) and the step (3) further include spray granulation; Preferably, embryo pressing is further included between the spray granulation and step (3).
8. The preparation method according to any one of claims 4 to 7, characterized in that: The oxygen content in the protective atmosphere in step (3) is 0 to 21 vol%, preferably 0 to 10 vol%; Preferably, the sintering temperature in step (3) is 1200-1400° C. and the sintering time is 4-10 h; Preferably, the sintering in step (3) is carried out in three stages; the temperature of the first stage is 1350-1400° C., and the time is 7-9 hours; the temperature of the second stage is 1350-1400° C., and the time is 0.5-1.5 hours; the temperature of the third stage is 1200-1350° C., and the time is 0.5-1.5 hours; Preferably, step (3) further includes cooling after the sintering, and the cooling is performed under a balanced oxygen partial pressure.
9. The preparation method according to any one of claims 4 to 8, characterized in that: The preparation method comprises: (1) mixing the main component and water by ball milling for 20 to 80 minutes to obtain a slurry, wherein the mass ratio of the main component, the grinding ball and the solvent is (0.5 to 1.5):(3.5 to 4.5):(0.5 to 1.5), and then pre-calcining in a rotary kiln at a temperature of 980 to 1035° C., and the slurry enters the rotary kiln at a speed of 400 to 500 kg / h to obtain a pre-calcined material, wherein the main component includes Fe2O3, ZnO and Mn3O4; (2) mixing the pre-sintered material obtained in step (1) with auxiliary components, a dispersant and a binder by ball milling, wherein the mass ratio of the pre-sintered material, the dispersant, the binder and the grinding balls during the ball milling is (0.5-1.5):(0.005-0.015):(0.05-0.15):(3-5) to obtain a mixed material; (3) The mixture obtained in step (2) is spray granulated and then pressed to obtain an embryo body, and the obtained embryo body is sintered, and the sintering is carried out in three stages; the temperature of the first stage is 1350-1400°C and the time is 7-9 hours; the temperature of the second stage is 1350-1400°C and the time is 0.5-1.5 hours; the temperature of the third stage is 1200-1350°C and the time is 0.5-1.5 hours, and then the temperature is lowered under a balanced oxygen partial pressure to obtain an iron-manganese-zinc ferrite material.
10. An application of the iron-manganese-zinc ferrite material according to any one of claims 1 to 3, characterized in that: The iron-manganese-zinc ferrite material is used for signal transmission or anti-electromagnetic interference.
Citation Information
Patent Citations
Manganese zinc soft magnetic ferrite material and preparation method thereof
CN104628371A
MnZn ferrite material with high Bs and high ui and preparation method thereof
CN105819847A
Manganese-zinc ferrite with high BS, High ZN and excellent ultra-wide-band characteristic and preparation method thereof