P-type bismuth telluride-based thermoelectric material and macro preparation method thereof
The discharge plasma SPS technology is used to sinter p-type bismuth telluride-based thermoelectric materials, which solves the problem of low production efficiency of thermoelectric materials and achieves efficient and energy-saving thermoelectric material preparation. The thermoelectric performance reaches the level of hot-press sintering.
Patent Information
- Application Number
- CN202410907526.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-08
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2044-07-08
AI Technical Summary
The existing production process of thermoelectric materials has problems such as high energy consumption, long production cycle and low production efficiency. In particular, commercial p-type Bi2-xSbxTe3 thermoelectric materials mainly use hot-press sintering technology.
Discharge plasma SPS technology is used for sintering. By weighing Bi, Zn, Sb and Te respectively according to the stoichiometric ratio of p-type bismuth telluride-based thermoelectric materials, smelting, ball milling and discharge plasma sintering are performed to obtain dense thermoelectric materials.
It realizes the sintering of high-quality thermoelectric materials in a short time, saving time and cost. The quality of a single finished product can be as high as 1000g, which improves production efficiency and saves energy consumption. The thermoelectric performance is comparable to hot press sintering.
Smart Images

Figure CN118754664A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of thermoelectric materials, and in particular to a p-type bismuth telluride-based thermoelectric material and a method for preparing the same in large quantities. Background Art
[0002] Thermoelectric materials are a type of functional materials that achieve direct coupling and mutual conversion between thermal energy and electrical energy through the Seebeck effect and Peltier effect of semiconductor materials. Due to their own advantages such as no pollution, no noise, small size, long life, and high reliability, they are widely used in waste heat power generation, aerospace, military equipment, household appliances and other fields.
[0003] Currently, commercial p-type Bi 2-x Sb x Te3 thermoelectric materials are mainly produced by hot pressing (HP) technology, which is to process powder or granular materials under high temperature, high pressure and oxygen-free environment to cause chemical reaction or physical change between particles, thus forming a dense bulk material. However, hot pressing has the disadvantages of high energy consumption, long production cycle and low production efficiency.
[0004] Therefore, how to improve the production efficiency of thermoelectric materials is a problem that needs to be solved urgently. Summary of the invention
[0005] The main purpose of the present application is to provide a p-type bismuth telluride-based thermoelectric material and a method for mass production thereof, aiming to solve the technical problem of how to improve the production efficiency of thermoelectric materials.
[0006] To achieve the above object, the present application provides a p-type bismuth telluride-based thermoelectric material, wherein the p-type bismuth telluride-based thermoelectric material has the following chemical formula:
[0007] Bi 2-x-y Zn y Sb x Te3; wherein, 1.5≤x≤1.6, 0.01≤y≤0.05.
[0008] Furthermore, in one embodiment, the value of x is 1.55, and the value of y is 0.03.
[0009] In addition, to achieve the above-mentioned purpose, the present application also provides a method for preparing a large amount of p-type bismuth telluride-based thermoelectric material, comprising the following steps:
[0010] Step 1, weighing Bi, Zn, Sb and Te respectively according to the stoichiometric ratio of the p-type bismuth telluride-based thermoelectric material;
[0011] Step 2, placing the weighed material into a quartz tube for smelting to obtain a smelted material ingot;
[0012] Step 3, ball milling the smelted material ingot with a ball mill;
[0013] Step 4: Place the ball-milled powder into a graphite mold and perform discharge plasma sintering to obtain a p-type bismuth telluride-based thermoelectric material.
[0014] Furthermore, in one embodiment, in the step 2, when smelting, the temperature is first raised to 650° C. and kept warm, then raised to 800° C. and kept warm, and finally cooled.
[0015] Furthermore, in one embodiment, the first heating duration is 2.5h to 3.5h, the second heating duration is 0.5h to 1.5h, the cooling duration is 3.5h to 4.5h, the first insulation duration is 1.5h to 2.5h, and the second insulation duration is 9.5h to 10.5h.
[0016] Furthermore, in one embodiment, in the step three, the rotation speed of the ball mill is 800 r / min to 1000 r / min, and the time of the ball mill is 20 min to 30 min.
[0017] Furthermore, in one embodiment, in the step 4, when spark plasma sintering is performed, the temperature is first raised to 450° C., then raised to 500° C. and kept at that temperature, and finally lowered.
[0018] Furthermore, in one embodiment, the diameter of the graphite mold is 30-100 mm, and the pressure corresponding to the spark plasma sintering is 30 MPa-40 MPa.
[0019] Furthermore, in one embodiment, the first heating period lasts for 8 to 12 minutes, the second heating period lasts for 2 to 4 minutes, and the heat preservation period lasts for 10 to 15 minutes.
[0020] Further, in one embodiment, in step 1, according to the chemical formula Bi 2-x-y Zn y Sb x The stoichiometric ratio of Te3 is to weigh Bi, Zn, Sb and Te respectively, and the weight of the material after weighing is 100g-1000g.
[0021] The present application comprises the following steps: weighing Bi, Zn, Sb and Te respectively according to the stoichiometric ratio of a p-type bismuth telluride-based thermoelectric material; then placing the weighed materials into a quartz tube for smelting to obtain a smelted material ingot; then ball-milling the smelted material ingot with a ball mill; then placing the ball-milled powder into a graphite mold, and performing discharge plasma sintering to obtain a p-type bismuth telluride-based thermoelectric material. The discharge plasma SPS technology is used for sintering, and a dense thermoelectric material can be sintered in a short time, saving time and cost. The thermoelectric performance of the sintered finished product is comparable to that of hot pressing sintering, and the mass of a single finished product can be as high as 1000g, thereby effectively improving production efficiency and saving energy consumption. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate embodiments consistent with the present application and, together with the description, serve to explain the principles of the present application.
[0023] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative labor.
[0024] Figure 1 A schematic diagram of a process flow diagram provided for Example 1 of a method for mass production of p-type bismuth telluride-based thermoelectric materials of the present application;
[0025] Figure 2 The test results of the thermoelectric performance of the p-type bismuth telluride-based thermoelectric material of this application.
[0026] The realization of the purpose, functional features and advantages of this application will be further explained in conjunction with embodiments and with reference to the accompanying drawings. DETAILED DESCRIPTION
[0027] It should be understood that the specific embodiments described herein are only used to explain the present application and are not used to limit the present application.
[0028] In order to better understand the technical solution of the present application, a detailed description will be given below in conjunction with the accompanying drawings and specific implementation methods.
[0029] The main solution of the present application is: step 1, weighing Bi, Zn, Sb and Te respectively according to the stoichiometric ratio of p-type bismuth telluride-based thermoelectric material; step 2, placing the weighed materials into a quartz tube for smelting to obtain a smelted material ingot; step 3, ball milling the smelted material ingot with a ball mill; step 4, placing the ball-milled powder into a graphite mold, and performing discharge plasma sintering to obtain a p-type bismuth telluride-based thermoelectric material.
[0030] At present, thermoelectric materials are a type of functional materials that realize direct coupling and mutual conversion of thermal energy and electrical energy through the Seebeck effect and Peltier effect of semiconductor materials. Due to its own advantages such as no pollution, no noise, small size, long life, and high reliability, it is widely used in waste heat power generation, aerospace, military equipment, household appliances and other fields. 2-x Sb x Te3 thermoelectric materials are mainly produced by hot pressing (HP) technology, which is to process powder or granular materials under high temperature, high pressure and oxygen-free environment to cause chemical reaction or physical change between particles, thereby forming a dense bulk material. However, hot pressing has the disadvantages of high energy consumption, long production cycle and low production efficiency. Therefore, how to improve the production efficiency of thermoelectric materials is a problem that needs to be solved urgently.
[0031] This application adopts discharge plasma SPS technology for sintering. Since the discharge plasma sintering time is short, the heating rate is fast and the sintering process is easy to control, dense thermoelectric materials can be sintered in a short time, saving time and cost. The thermoelectric performance of the sintered product is comparable to that of hot pressing sintering. The weight of a single finished product can be as high as 1000g, which can effectively improve production efficiency and save energy consumption.
[0032] An embodiment of the present application provides a p-type bismuth telluride-based thermoelectric material, which has the following chemical formula: Bi 2-x-y Zn y Sb x Te3; wherein, 1.5≤x≤1.6, 0.01≤y≤0.05.
[0033] Furthermore, the value of x is 1.55, and the value of y is 0.03, that is, the chemical formula of the p-type bismuth telluride-based thermoelectric material is Bi 0.42 Zn 0.03 Sb 1.55 Te3.
[0034] Furthermore, the present application proposes a first embodiment of a method for preparing a large amount of p-type bismuth telluride-based thermoelectric material, please refer to Figure 1 The method for preparing a large amount of p-type bismuth telluride-based thermoelectric material comprises:
[0035] Step 1, weighing Bi, Zn, Sb and Te respectively according to the stoichiometric ratio of the p-type bismuth telluride-based thermoelectric material;
[0036] In this embodiment, Bi, Zn, Sb and Te are weighed respectively according to the stoichiometric ratio of the p-type bismuth telluride-based thermoelectric material to obtain the weighed material. Preferably, the weighed material can be obtained according to the chemical formula Bi 2-x-y Zn y Sb xThe stoichiometric ratio of Te3 is obtained by weighing Bi, Zn, Sb and Te respectively to obtain a weighed material, the weight of the weighed material is 100g-1000g, preferably, the weight of the weighed material is 1000g, specifically, according to the chemical formula Bi 0.42 Zn 0.03 Sb 1.55 The stoichiometric ratio of Te3 is weighed separately for Bi, Zn, Sb and Te.
[0037] Among them, Bi, Zn, Sb and Te can all be powders or particles.
[0038] Step 2, placing the weighed material into a quartz tube for smelting to obtain a smelted material ingot;
[0039] In this embodiment, the weighed material is first placed in a quartz tube, and the weighed material in the quartz tube is smelted to obtain a smelted material ingot.
[0040] Specifically, during smelting, the temperature is first raised to 650° C. and maintained, then raised to 800° C. and maintained, and finally cooled to room temperature (eg, 30° C.) to obtain a smelted material ingot.
[0041] Further, the duration of the first heating is 2.5h to 3.5h, the duration of the second heating is 0.5h to 1.5h, the duration of cooling is 3.5h to 4.5h, the duration of the first insulation is 1.5h to 2.5h, and the duration of the second insulation is 9.5h to 10.5h. Preferably, the duration of the first heating is 3h, the duration of the second heating is 1h, the duration of cooling is 4h, the duration of the first insulation is 2h, and the duration of the second insulation is 10h. That is, the smelting process is: heating from room temperature (e.g., 30°C) to 650°C for 3h, then maintaining 650°C for 2h, then heating to 800°C for 1h, maintaining 800°C for 10h, and finally cooling to room temperature (e.g., 30°C) for 4h.
[0042] Step 3, ball milling the smelted material ingot with a ball mill;
[0043] In this embodiment, after obtaining the smelted material ingot, the smelted material ingot is ball-milled and crushed using a ball mill to obtain ball-milled powder, wherein the ball milling speed is 800r / min~1000r / min, and the ball milling time is 20min~30min. Preferably, the ball milling speed is 900r / min, and the ball milling time is 25min.
[0044] Step 4: Place the ball-milled powder into a graphite mold and perform discharge plasma sintering to obtain a p-type bismuth telluride-based thermoelectric material.
[0045] In this embodiment, after obtaining the ball-milled powder, the ball-milled powder is placed in a graphite mold. Specifically, the ball-milled powder can be sieved to obtain the sieved powder, and the sieved powder is placed in the graphite mold. During the process of placing the powder in the graphite mold, a certain amount of powder is placed each time and compacted, and then a certain amount of powder is continued to be placed and compacted again until 1 kg of the material is completely placed in the graphite mold. The diameter of the graphite mold is 30-100 mm, and preferably, the diameter of the graphite mold is 80 mm.
[0046] In this embodiment, after the ball-milled powder is placed in a graphite mold, it is sintered using a spark plasma sintering (SPS) technique to obtain a p-type bismuth telluride-based thermoelectric material. Specifically, during the spark plasma sintering process, the temperature is first raised to 450°C, then raised to 500°C for insulation, and finally cooled. Among them, the duration of the first heating is 8min to 12min, the duration of the second heating is 2min to 4min, the duration of insulation is 10min to 15min, and the pressure corresponding to the spark plasma sintering is 30MPa to 40MPa. Preferably, the duration of the first heating is 10min, the duration of the second heating is 3min, the duration of insulation is 12min, and the pressure corresponding to the spark plasma sintering is 35MPa. The specific sintering process can be: heating from room temperature (for example, 30°C) to 450°C through 10min, then heating from 450°C to 500°C through 3min, maintaining 500°C for 10min to 15min, and then cooling to room temperature (for example, 30°C).
[0047] Bi 0.42 Zn 0.03 Sb 1.55 For example, Te3 Figure 2 , Figure 2 The test results of the thermoelectric performance of the p-type bismuth telluride-based thermoelectric material of this application.
[0048] The prepared 1kg p-type bismuth telluride-based thermoelectric material was cut and tested. The electrical and thermal properties of the kilogram-level thermoelectric material were tested by cutting in different regions and its thermoelectric figure of merit zT was calculated. In order to characterize whether the performance of each region of the sintered finished product is relatively uniform, the relative standard deviation (RSD) is introduced to characterize the uniformity of the performance parameters of each part. The smaller it is, the lower the degree of discreteness and the better the uniformity. Generally, RSD less than 10% is considered to have good uniformity. The calculation formula is as follows:
[0049] RSD = standard deviation / mean value*100%.
[0050] like Figure 2 As shown in a, the conductivity of different regions is basically between 8.8 and 10.3×10 4Near S / m, RSD is less than 6.5%.
[0051] like Figure 2 b shows Bi 0.42 Zn 0.03 Sb 1.55 The curve of the Seebeck coefficient of Te3 alloy changing with temperature shows that the Seebeck coefficient of each area of the sample is relatively uniform overall, among which the Seebeck coefficient of the edge3 area is slightly higher than that of other areas, but the RSD is less than 2.4%.
[0052] like Figure 2 c shows Bi 0.42 Zn 0.03 Sb 1.55 The power factor of different areas of Te3 sample varies with temperature. The power factor is between 3587.2Wm -1 K -2 and 3875.6Wm -1 K -2 The RSD is less than 3.2%, and the power factor is basically uniform overall.
[0053] like Figure 2 d is Bi 0.42 Zn 0.03 Sb 1.55 The thermal conductivity of different areas of Te3 alloy cutting varies with temperature. It can be seen from the figure that the thermal conductivity of the sample decreases first and then increases with the increase of temperature. The total thermal conductivity of different areas of the sample fluctuates slightly, basically between 1.06Wm -1 K -1 and 1.14Wm -1 K -1 The RSD was less than 6.0%.
[0054] like Figure 2 e is the κ of the sample total -κ e The relationship curve with temperature has an RSD of less than 7.5%. The overall thermal performance is relatively uniform.
[0055] like Figure 2 f shows Bi 0.42 Zn 0.03 Sb 1.55 The relationship between the thermoelectric figure of merit zT value of Te3 alloy and temperature. Since the power factor calculated in each region is relatively uniform, while maintaining a low and uniform thermal conductivity. The average zT of different regions is finally obtained. ave It is 1.1@300-425K, and the RSD is less than 5.0%.
[0056] The large-scale preparation method of p-type bismuth telluride-based thermoelectric material proposed in this embodiment is as follows: Bi, Zn, Sb and Te are weighed respectively according to the stoichiometric ratio of the p-type bismuth telluride-based thermoelectric material; the weighed materials are then placed in a quartz tube for smelting to obtain a smelted material ingot; the smelted material ingot is then ball-milled and crushed using a ball mill; the ball-milled powder is then placed in a graphite mold and subjected to discharge plasma sintering to obtain a p-type bismuth telluride-based thermoelectric material. The discharge plasma SPS technology is used for sintering, which can sinter dense thermoelectric materials in a short time, saving time and cost. The thermoelectric performance of the sintered finished product is comparable to that of hot pressing sintering, and the mass of a single finished product can be as high as 1000g, which can effectively improve production efficiency and save energy consumption.
[0057] The above are only preferred embodiments of the present application, and are not intended to limit the patent scope of the present application. Any equivalent structure or equivalent process transformation made using the contents of the present application specification and drawings, or directly or indirectly applied in other related technical fields, are also included in the patent protection scope of the present application.
Claims
1. A p-type bismuth telluride-based thermoelectric material, characterized in that: The p-type bismuth telluride-based thermoelectric material has the following chemical formula: Bi 2-x-y Zinc y Sb x Te3; Among them, 1.5≤x≤1.6, 0.01≤y≤0.
05.
2. The p-type bismuth telluride-based thermoelectric material according to claim 1, characterized in that: The value of x is 1.55 and the value of y is 0.
03.
3. A method for mass production of p-type bismuth telluride-based thermoelectric materials, characterized in that: The following steps are involved: Step 1, weighing Bi, Zn, Sb and Te respectively according to the stoichiometric ratio of the p-type bismuth telluride-based thermoelectric material; Step 2, placing the weighed material into a quartz tube for smelting to obtain a smelted material ingot; Step 3, ball milling the smelted material ingot with a ball mill; Step 4: Place the ball-milled powder into a graphite mold and perform discharge plasma sintering to obtain a p-type bismuth telluride-based thermoelectric material.
4. The method for mass production of p-type bismuth telluride-based thermoelectric materials according to claim 3, characterized in that: In the step 2, when smelting, the temperature is first raised to 650° C. and kept warm, then raised to 800° C. and kept warm, and finally cooled.
5. The method for mass production of p-type bismuth telluride-based thermoelectric materials according to claim 4, characterized in that: The first heating period lasts for 2.5h to 3.5h, the second heating period lasts for 0.5h to 1.5h, the cooling period lasts for 3.5h to 4.5h, the first heat preservation period lasts for 1.5h to 2.5h, and the second heat preservation period lasts for 9.5h to 10.5h.
6. The method for mass production of p-type bismuth telluride-based thermoelectric materials according to claim 3, characterized in that: In the step 3, the rotation speed of the ball mill is 800 r / min to 1000 r / min, and the time of the ball mill is 20 min to 30 min.
7. The method for mass production of p-type bismuth telluride-based thermoelectric materials according to claim 3, characterized in that: In the step 4, when spark plasma sintering is performed, the temperature is first raised to 450° C., then raised to 500° C. and kept at that temperature, and finally lowered.
8. The method for mass production of p-type bismuth telluride-based thermoelectric materials according to claim 7, characterized in that: The diameter of the graphite mold is 30-100 mm, and the pressure corresponding to the spark plasma sintering is 30 MPa-40 MPa.
9. The method for mass production of p-type bismuth telluride-based thermoelectric materials according to claim 7, characterized in that: The first heating period lasts for 8 to 12 minutes, the second heating period lasts for 2 to 4 minutes, and the insulation period lasts for 10 to 15 minutes.
10. The method for mass production of p-type bismuth telluride-based thermoelectric materials according to any one of claims 3 to 9, characterized in that: In the step 1, according to the chemical formula Bi 2-x-y Zn y Sb x The stoichiometric ratio of Te3 is to weigh Bi, Zn, Sb and Te respectively, and the weight of the material after weighing is 100g-1000g.
Citation Information
Patent Citations
A making for nano thermal electric material with nucleus shell structure
CN101237020A
P-type bismuth telluride thermoelectric material and preparation method thereof
CN111848165A
N-type bismuth telluride-based room-temperature thermoelectric material and preparation method thereof
CN113421959A
Perovskite solar cell-thermoelectric refrigerating unit combined device
CN114824089A
Method for manufacturing bi-te based thermoelectric materials
KR100727391B1