Preparation method of large-size silicon nitride ceramic
Through the process of spray granulation and cold isostatic pressing combined with hot isostatic pressing, the problems of densification and performance consistency of large-sized silicon nitride ceramics in the existing technology are solved, and large-sized nitrogen with high density and uniformity is achieved. Preparation of silicon ceramics, suitable for mass production.
Patent Information
- Application Number
- CN202410934632.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-12
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2044-07-12
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of ceramic products and relates to a method for preparing a ceramic product, in particular to a method for preparing a large-size silicon nitride ceramic. Background Art
[0002] Silicon nitride ceramics have excellent properties such as high temperature resistance, wear resistance, high strength, high toughness, corrosion resistance, high hardness and light specific gravity. They have broad applications and development prospects in aerospace, chemical metallurgy, mechanical processing, nuclear industry and other fields.
[0003] In the prior art, the preparation process of silicon nitride ceramics includes but is not limited to tape casting, dry pressing and injection molding. Among them, tape casting is suitable for the preparation of thin plate ceramics, which is widely used in the preparation of heat dissipation and packaging materials; injection molding is mainly used to prepare small-sized and complex-structured silicon nitride ceramic parts; dry pressing is suitable for small and medium-sized plate-shaped or disc-shaped ceramic parts; therefore, tape casting, dry pressing and injection molding are not conducive to the preparation of large-sized silicon nitride ceramics.
[0004] The sintering methods mainly include normal pressure sintering, gas pressure sintering, hot pressing and hot isostatic pressing. Normal pressure sintering, also known as pressureless sintering, is to sinter the silicon nitride blank at 1700-1800℃ under normal pressure N2. The density of the sintered product is poor, and it is difficult to prepare high-performance products; gas pressure sintering generally uses high-pressure N2 sintering not exceeding 10MPa. Due to the poor penetration of N2, when preparing large-sized products, the N2 in the core is difficult to completely remove to form an internal porous structure, resulting in poor consistency of internal and external performance of large-sized materials; hot isostatic pressing applies pressure during the sintering process to promote the densification of the material with the help of high temperature and high pressure, but the existing technology has not conducted research on the preparation of large-sized silicon nitride ceramics by hot pressing sintering.
[0005] Therefore, it is necessary to provide a method for preparing high-performance large-size silicon nitride ceramics to achieve the smooth preparation of large-size silicon nitride ceramics. Summary of the invention
[0006] The object of the present invention is to provide a method for preparing large-sized silicon nitride ceramics. The preparation method can realize the preparation of large-sized silicon nitride ceramics, and the process is simple and easy to mass produce. The obtained large-sized silicon nitride ceramics have high density, good uniformity and excellent performance.
[0007] In order to achieve the purpose of the invention, the present invention adopts the following technical solutions:
[0008] The present invention provides a method for preparing large-size silicon nitride ceramics, characterized in that the preparation method comprises the following steps:
[0009] (1) first mixing a sintering aid and a dispersant to obtain a first mixed powder;
[0010] (2) mixing a second silicon nitride powder with the first mixed powder to obtain a second mixed powder;
[0011] (3) mixing the third binder solution with the second mixed powder to obtain silicon nitride slurry;
[0012] (4) using silicon nitride slurry for spray granulation to obtain spherical powder;
[0013] (5) After the spherical powder is filled into a mold, it is cold isostatically pressed to obtain a silicon nitride green body;
[0014] (6) The silicon nitride green body is degreased and hot isostatically pressed to obtain the large-sized silicon nitride ceramic.
[0015] The preparation method provided by the present invention can realize the preparation of large-sized silicon nitride ceramics, and the process is simple and easy to mass produce, and the obtained large-sized silicon nitride ceramics have high density, good uniformity and excellent performance; the preparation method provided by the present invention realizes uniform mixing of silicon nitride powder, sintering aid, dispersant and binder through the first mixing, second mixing and third mixing performed in sequence, so that the composition of silicon nitride slurry is uniform, so that the size and composition of the obtained spherical powder are uniform; and then by strictly controlling the conditions of cold isostatic pressing, degreasing and hot isostatic pressing, large-sized silicon nitride ceramics with high density, good uniformity and excellent performance are obtained.
[0016] The "large size" in the present invention refers to a length of more than 1.5 meters.
[0017] Preferably, the first mixing in step (1) is carried out in anhydrous ethanol.
[0018] Preferably, the sintering aid in step (1) includes any one of Y2O3, CaF2 or MgO or a combination of at least two of them. Typical but non-limiting combinations include a combination of Y2O3 and CaF2, a combination of CaF2 and MgO, a combination of Y2O3 and MgO, or a combination of Y2O3, CaF2 and MgO, preferably a combination of Y2O3 and CaF2.
[0019] Preferably, the sintering aid in step (1) is a combination of Y2O3 and CaF2, and the mass ratio of Y2O3 to CaF2 is (2-4):1, for example, it can be 2:1, 2.5:1, 3:1, 3.5:1 or 4:1, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0020] Preferably, the amount of the sintering aid in step (1) is 1-5wt% of the silicon nitride powder, for example, it can be 1wt%, 2wt%, 3wt%, 4wt% or 5wt%, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0021] Preferably, the dispersant in step (1) comprises any one of herring oil, castor oil or triolein, or a combination of at least two of them. Typical but non-limiting combinations include a combination of herring oil and castor oil, a combination of castor oil and triolein, a combination of herring oil and triolein, or a combination of herring oil, castor oil and triolein.
[0022] Preferably, the amount of the dispersant in step (1) is 0.5-3wt% of the silicon nitride powder, for example, it can be 0.5wt%, 1wt%, 1.5wt%, 2wt%, 2.5wt% or 3wt%, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0023] Preferably, the second mixing in step (2) is carried out in anhydrous ethanol.
[0024] Preferably, the average particle size of the silicon nitride powder in step (2) is 0.6-1.2 μm, for example, 0.6 μm, 0.8 μm, 1 μm or 1.2 μm, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0025] Preferably, the third mixing in step (3) is carried out in anhydrous ethanol.
[0026] Preferably, the binder solution in step (3) is an ethanol solution of the binder.
[0027] Preferably, the amount of the binder in step (3) is 2wt%-6wt% of the silicon nitride powder, for example, it can be 2wt%, 3wt%, 4wt%, 5wt% or 6wt%, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0028] Preferably, the binder comprises polyvinyl butyral.
[0029] Preferably, the average particle size of the spherical powder obtained in step (4) is 60-120 μm, for example, 60 μm, 80 μm, 90 μm, 100 μm or 120 μm, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0030] Preferably, the pressure of the cold isostatic pressing in step (5) is 200-250 MPa, for example, 200 MPa, 210 MPa, 220 MPa, 230 MPa, 240 MPa or 250 MPa, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0031] Preferably, the cold isostatic pressing time in step (5) is 5-10 min, for example, 5 min, 6 min, 8 min, 9 min or 10 min, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0032] Preferably, the degreasing temperature in step (6) is 500-600°C, for example, 500°C, 520°C, 550°C, 580°C or 600°C, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0033] The present invention avoids the adverse effects of degreasing on the density and component uniformity of silicon nitride green body by performing degreasing at a specific temperature, and ensures the density and component uniformity of large-sized silicon nitride ceramics obtained after hot isostatic pressing.
[0034] Preferably, the degreasing time in step (6) is 1-5 h, for example, 1 h, 2 h, 3 h, 4 h or 5 h, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0035] Preferably, step (6) comprises a first heat treatment, a second heat treatment, a third heat treatment and a fourth heat treatment performed sequentially.
[0036] Preferably, the temperature of the first heat treatment is 900-1200° C., and the time is 1-3 hours.
[0037] The temperature of the first heat treatment is 900-1200°C, for example, 900°C, 1000°C, 1100°C, 1200°C or 1300°C, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0038] The time of the first heat treatment is 1-3 hours, for example, 1 hour, 1.5 hours, 2 hours, 2.5 hours or 3 hours, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0039] Preferably, the temperature of the second heat treatment is 1300-1500° C., and the time is 1-3 hours.
[0040] The temperature of the second heat treatment is 1300-1500°C, for example, 1300°C, 1350°C, 1400°C, 1450°C or 1500°C, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0041] The time of the second heat treatment is 1-3 hours, for example, 1 hour, 1.5 hours, 2 hours, 2.5 hours or 3 hours, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0042] Preferably, the temperature of the third heat treatment is 1600-1700° C., and the time is 2-4 hours.
[0043] The temperature of the third heat treatment is 1600-1700°C, for example, 1600°C, 1630°C, 1650°C, 1680°C or 1700°C, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0044] The time of the third heat treatment is 2-4 hours, for example, 2 hours, 2.5 hours, 3 hours, 3.5 hours or 4 hours, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0045] Preferably, the temperature of the fourth heat treatment is 1750-1850° C., and the time is 2-6 hours.
[0046] The temperature of the fourth heat treatment is 1750-1850°C, for example, it can be 1750°C, 1780°C, 1800°C, 1820°C or 1850°C, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0047] The time of the fourth heat treatment is 2-6 hours, for example, 2 hours, 3 hours, 4 hours, 5 hours or 6 hours, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0048] Preferably, the pressure of the hot isostatic pressing in step (6) is 180-250 MPa, for example, 180 MPa, 200 MPa, 210 MPa, 240 MPa or 250 MPa, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0049] As a preferred technical solution of the preparation method of the present invention, the preparation method comprises the following steps:
[0050] (1) first mixing a sintering aid and a dispersant in a powder mixing barrel to obtain a first mixed powder;
[0051] The first mixing is carried out in anhydrous ethanol;
[0052] The sintering aid includes any one of Y2O3, CaF2 or MgO or a combination of at least two thereof, and the amount used is 1-5wt% of the silicon nitride powder;
[0053] The dispersant comprises any one of herring oil, castor oil or triolein or a combination of at least two thereof, and the amount used is 0.5-3wt% of the silicon nitride powder;
[0054] (2) adding silicon nitride powder having an average particle size of 0.6-1.2 μm to the first mixed powder, and performing a second mixing to obtain a second mixed powder;
[0055] (3) adding a binder solution to the second mixed powder and performing a third mixing to obtain a silicon nitride slurry;
[0056] The binder solution is an ethanol solution of the binder, and the amount of the binder is 2wt%-6wt% of the silicon nitride powder;
[0057] The binder includes polyvinyl butyral;
[0058] (4) using silicon nitride slurry for spray granulation to obtain spherical powder with an average particle size of 60-120 μm;
[0059] (5) After the spherical powder is filled into a mold, it is cold isostatically pressed to obtain a silicon nitride green body;
[0060] The cold isostatic pressing process is performed at a pressure of 200-250 MPa and a time of 5-10 min.
[0061] (6) Degreasing and hot isostatic pressing the silicon nitride green body to obtain the large-sized silicon nitride ceramic;
[0062] The degreasing temperature is 500-600°C and the time is 1-5h;
[0063] The hot isostatic pressing includes a first heat treatment, a second heat treatment, a third heat treatment and a fourth heat treatment performed in sequence; the temperature of the first heat treatment is 900-1200°C and the time is 1-3h; the temperature of the second heat treatment is 1300-1500°C and the time is 1-3h; the temperature of the third heat treatment is 1600-1700°C and the time is 2-4h; the temperature of the fourth heat treatment is 1750-1850°C and the time is 2-6h;
[0064] The hot isostatic pressing pressure is 180-250 MPa.
[0065] Compared with the prior art, the present invention has the following beneficial effects:
[0066] The preparation method provided by the present invention can realize the preparation of large-sized silicon nitride ceramics, and the process is simple and easy to mass produce, and the obtained large-sized silicon nitride ceramics have high density, good uniformity and excellent performance; the preparation method provided by the present invention realizes uniform mixing of silicon nitride powder, sintering aid, dispersant and binder through the first mixing, second mixing and third mixing performed in sequence, so that the composition of silicon nitride slurry is uniform, so that the size and composition of the obtained spherical powder are uniform; and then by strictly controlling the conditions of cold isostatic pressing, degreasing and hot isostatic pressing, large-sized silicon nitride ceramics with high density, good uniformity and excellent performance are obtained. DETAILED DESCRIPTION
[0067] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.
[0068] The length of the large-sized silicon nitride ceramic obtained in the specific implementation manner of the present invention is 2 m, which is only for the purpose of clearly illustrating the technical solution of the present invention and is not regarded as a further limitation of the present invention.
[0069] Example 1
[0070] This embodiment provides a method for preparing a large-size silicon nitride ceramic, the preparation method comprising the following steps:
[0071] (1) first mixing a sintering aid and a dispersant in a powder mixing barrel to obtain a first mixed powder;
[0072] The first mixing is carried out in anhydrous ethanol;
[0073] The sintering aid is Y2O3, and the amount used is 3wt% of the silicon nitride powder;
[0074] The dispersant is triolein, and the amount used is 2wt% of the silicon nitride powder;
[0075] (2) adding silicon nitride powder having an average particle size of 1 μm to the first mixed powder, and performing a second mixing to obtain a second mixed powder;
[0076] (3) adding a binder solution to the second mixed powder and performing a third mixing to obtain a silicon nitride slurry;
[0077] The binder solution is an ethanol solution of the binder, and the amount of the binder is 4wt% of the silicon nitride powder;
[0078] The binder includes polyvinyl butyral;
[0079] (4) using silicon nitride slurry for spray granulation to obtain spherical powder with an average particle size of 90 μm;
[0080] (5) After the spherical powder is filled into a mold, it is cold isostatically pressed to obtain a silicon nitride green body;
[0081] The cold isostatic pressing pressure is 220 MPa and the time is 8 min;
[0082] (6) Degreasing and hot isostatic pressing the silicon nitride green body to obtain the large-sized silicon nitride ceramic;
[0083] The degreasing temperature is 550°C and the degreasing time is 3h;
[0084] The hot isostatic pressing includes a first heat treatment, a second heat treatment, a third heat treatment and a fourth heat treatment performed in sequence; the temperature of the first heat treatment is 1100°C and the time is 2 hours; the temperature of the second heat treatment is 1400°C and the time is 2 hours; the temperature of the third heat treatment is 1650°C and the time is 3 hours; the temperature of the fourth heat treatment is 1800°C and the time is 4 hours;
[0085] The hot isostatic pressing pressure is 210 MPa.
[0086] Example 2
[0087] This embodiment provides a method for preparing a large-size silicon nitride ceramic, the preparation method comprising the following steps:
[0088] (1) first mixing a sintering aid and a dispersant in a powder mixing barrel to obtain a first mixed powder;
[0089] The first mixing is carried out in anhydrous ethanol;
[0090] The sintering aid is Y2O3, and the amount used is 1wt% of the silicon nitride powder;
[0091] The dispersant is triolein, and the amount used is 0.5wt% of the silicon nitride powder;
[0092] (2) adding silicon nitride powder having an average particle size of 1.2 μm to the first mixed powder, and performing a second mixing to obtain a second mixed powder;
[0093] (3) adding a binder solution to the second mixed powder and performing a third mixing to obtain a silicon nitride slurry;
[0094] The binder solution is an ethanol solution of the binder, and the amount of the binder is 6wt% of the silicon nitride powder;
[0095] The binder includes polyvinyl butyral;
[0096] (4) using silicon nitride slurry for spray granulation to obtain spherical powder with an average particle size of 120 μm;
[0097] (5) After the spherical powder is filled into a mold, it is cold isostatically pressed to obtain a silicon nitride green body;
[0098] The cold isostatic pressing process is performed at a pressure of 200 MPa and a time of 10 min.
[0099] (6) Degreasing and hot isostatic pressing the silicon nitride green body to obtain the large-sized silicon nitride ceramic;
[0100] The degreasing temperature is 500°C and the time is 5h;
[0101] The hot isostatic pressing includes a first heat treatment, a second heat treatment, a third heat treatment and a fourth heat treatment performed in sequence; the temperature of the first heat treatment is 1200°C and the time is 1 hour; the temperature of the second heat treatment is 1500°C and the time is 1 hour; the temperature of the third heat treatment is 1700°C and the time is 2 hours; the temperature of the fourth heat treatment is 1850°C and the time is 2 hours;
[0102] The hot isostatic pressing pressure is 250 MPa.
[0103] Example 3
[0104] This embodiment provides a method for preparing a large-size silicon nitride ceramic, the preparation method comprising the following steps:
[0105] (1) first mixing a sintering aid and a dispersant in a powder mixing barrel to obtain a first mixed powder;
[0106] The first mixing is carried out in anhydrous ethanol;
[0107] The sintering aid is Y2O3, and the amount used is 5wt% of the silicon nitride powder;
[0108] The dispersant is triolein, and the amount used is 3wt% of the silicon nitride powder;
[0109] (2) adding silicon nitride powder having an average particle size of 0.6 μm to the first mixed powder, and performing a second mixing to obtain a second mixed powder;
[0110] (3) adding a binder solution to the second mixed powder and performing a third mixing to obtain a silicon nitride slurry;
[0111] The binder solution is an ethanol solution of the binder, and the amount of the binder is 2wt% of the silicon nitride powder;
[0112] The binder includes polyvinyl butyral;
[0113] (4) using silicon nitride slurry for spray granulation to obtain spherical powder with an average particle size of 60 μm;
[0114] (5) After the spherical powder is filled into a mold, it is cold isostatically pressed to obtain a silicon nitride green body;
[0115] The cold isostatic pressing process is performed at a pressure of 250 MPa and a time of 5 min.
[0116] (6) Degreasing and hot isostatic pressing the silicon nitride green body to obtain the large-sized silicon nitride ceramic;
[0117] The degreasing temperature is 600°C and the time is 1h;
[0118] The hot isostatic pressing includes a first heat treatment, a second heat treatment, a third heat treatment and a fourth heat treatment performed in sequence; the temperature of the first heat treatment is 900°C and the time is 3 hours; the temperature of the second heat treatment is 1300°C and the time is 3 hours; the temperature of the third heat treatment is 1600°C and the time is 4 hours; the temperature of the fourth heat treatment is 1750°C and the time is 6 hours;
[0119] The hot isostatic pressing pressure is 180 MPa.
[0120] Example 4
[0121] This embodiment provides a method for preparing large-sized silicon nitride ceramics, which is the same as that of Embodiment 1 except that the sintering aid is Y2O3 and CaF2 in a mass ratio of 2:1.
[0122] Example 5
[0123] This embodiment provides a method for preparing large-sized silicon nitride ceramics, which is the same as that of Embodiment 1 except that the sintering aid is Y2O3 and CaF2 in a mass ratio of 4:1.
[0124] Example 6
[0125] This embodiment provides a method for preparing large-sized silicon nitride ceramics, which is the same as that of Embodiment 1 except that the degreasing temperature is 480°C.
[0126] Example 7
[0127] This embodiment provides a method for preparing large-sized silicon nitride ceramics, which is the same as that of Embodiment 1 except that the degreasing temperature is 620°C.
[0128] Example 8
[0129] This embodiment provides a method for preparing large-sized silicon nitride ceramics, which is the same as that of Embodiment 1 except that the pressure of cold isostatic pressing is 180 MPa.
[0130] Example 9
[0131] This embodiment provides a method for preparing large-sized silicon nitride ceramics, which is the same as that of Embodiment 1 except that the pressure of cold isostatic pressing is 280 MPa.
[0132] Comparative Example 1
[0133] This embodiment provides a method for preparing a large-size silicon nitride ceramic, the preparation method comprising the following steps:
[0134] (1) first mixing a sintering aid and a dispersant in a powder mixing barrel to obtain a first mixed powder;
[0135] The first mixing is carried out in anhydrous ethanol;
[0136] The sintering aid is Y2O3, and the amount used is 3wt% of the silicon nitride powder;
[0137] The dispersant is triolein, and the amount used is 2wt% of the silicon nitride powder;
[0138] (2) adding silicon nitride powder to the first mixed powder and performing a second mixing to obtain a second mixed powder;
[0139] (3) adding a binder solution to the second mixed powder and performing a third mixing to obtain a silicon nitride slurry;
[0140] The binder solution is an ethanol solution of the binder, and the amount of the binder is ...wt% of the silicon nitride powder;
[0141] The binder includes polyvinyl butyral;
[0142] (4) using silicon nitride slurry for spray granulation to obtain spherical powder;
[0143] (5) After the spherical powder is filled into a mold, it is subjected to cold isostatic pressing to obtain a silicon nitride green body;
[0144] The cold isostatic pressing pressure is 220 MPa and the time is 8 min;
[0145] (6) hot isostatic pressing the silicon nitride green body to obtain the large-size silicon nitride ceramic;
[0146] The hot isostatic pressing temperature is 1800° C. and the time is 3 hours.
[0147] Performance Characterization
[0148] The thermal conductivity and bending strength of the large-sized silicon nitride ceramics obtained in the above examples and comparative examples were measured, and the results are shown in Table 1.
[0149] Table 1
[0150] Thermal conductivity (W / (m·K)) Bending strength(MPa) Example 1 66 873 Example 2 48 956 Example 3 69 830 Example 4 73 980 Example 5 70 927 Example 6 53 632 Example 7 65 815 Example 8 62 756 Example 9 67 850 Comparative Example 1 32 410
[0151] In summary, the preparation method provided by the present invention can realize the preparation of large-sized silicon nitride ceramics, and the process is simple, easy to mass produce, and the obtained large-sized silicon nitride ceramics have high density, good uniformity and excellent performance; the preparation method provided by the present invention realizes the uniform mixing of silicon nitride powder, sintering aid, dispersant and binder through the first mixing, the second mixing and the third mixing performed in sequence, so that the composition of the silicon nitride slurry is uniform, so that the size and composition of the obtained spherical powder are uniform; and then by strictly controlling the conditions of cold isostatic pressing, degreasing and hot isostatic pressing, a large-sized silicon nitride ceramic with high density, good uniformity and excellent performance is obtained.
[0152] The above description is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention are within the protection scope and disclosure scope of the present invention.
Claims
1. A method for preparing large-size silicon nitride ceramics, It is characterized in that The preparation method comprises the following steps: (1) first mixing a sintering aid and a dispersant to obtain a first mixed powder; (2) mixing a second silicon nitride powder with the first mixed powder to obtain a second mixed powder; (3) mixing the third binder solution with the second mixed powder to obtain silicon nitride slurry; (4) using silicon nitride slurry for spray granulation to obtain spherical powder; (5) After the spherical powder is filled into a mold, it is cold isostatically pressed to obtain a silicon nitride green body; (6) The silicon nitride green body is degreased and hot isostatically pressed to obtain the large-sized silicon nitride ceramic.
2. The preparation method according to claim 1, It is characterized in that Step (1) the first mixing is carried out in anhydrous ethanol; Preferably, the sintering aid in step (1) includes Y 2 O 3 , CaF 2 or MgO, any one or a combination of at least two; Preferably, the amount of the sintering aid in step (1) is 1-5 wt % of the silicon nitride powder.
3. The preparation method according to claim 1 or 2, It is characterized in that The dispersant in step (1) comprises any one of herring oil, castor oil or triolein, or a combination of at least two thereof; Preferably, the amount of the dispersant in step (1) is 0.5-3 wt % of the silicon nitride powder.
4. The preparation method according to any one of claims 1 to 3, It is characterized in that Step (2) the second mixing is carried out in anhydrous ethanol; Preferably, the average particle size of the silicon nitride powder in step (2) is 0.6-1.2 μm.
5. The preparation method according to any one of claims 1 to 4, It is characterized in that The third mixing in step (3) is carried out in anhydrous ethanol; Preferably, the binder solution in step (3) is an ethanol solution of the binder; Preferably, the amount of the binder in step (3) is 2wt%-6wt% of the silicon nitride powder; Preferably, the binder comprises polyvinyl butyral.
6. The preparation method according to any one of claims 1 to 5, It is characterized in that The average particle size of the spherical powder obtained in step (4) is 60-120 μm.
7. The preparation method according to any one of claims 1 to 6, It is characterized in that The pressure of the cold isostatic pressing in step (5) is 200-250 MPa; Preferably, the cold isostatic pressing time in step (5) is 5-10 minutes.
8. The preparation method according to any one of claims 1 to 7, It is characterized in that The degreasing temperature in step (6) is 500-600°C; Preferably, the degreasing time in step (6) is 1-5 hours.
9. The preparation method according to any one of claims 1 to 8, It is characterized in that The hot isostatic pressing in step (6) includes a first heat treatment, a second heat treatment, a third heat treatment and a fourth heat treatment performed in sequence; Preferably, the temperature of the first heat treatment is 900-1200°C and the time is 1-3h; Preferably, the temperature of the second heat treatment is 1300-1500°C and the time is 1-3h; Preferably, the temperature of the third heat treatment is 1600-1700°C and the time is 2-4h; Preferably, the temperature of the fourth heat treatment is 1750-1850°C and the time is 2-6h; Preferably, the pressure of the hot isostatic pressing in step (6) is 180-250 MPa.
10. The preparation method according to claim 1, It is characterized in that The preparation method comprises the following steps: (1) first mixing a sintering aid and a dispersant in a powder mixing barrel to obtain a first mixed powder; The first mixing is carried out in anhydrous ethanol; The sintering aid includes Y 2 O 3 , CaF 2 or MgO, any one or a combination of at least two thereof, the amount of which is 1-5wt% of the silicon nitride powder; The dispersant comprises any one of herring oil, castor oil or triolein or a combination of at least two thereof, and the amount used is 0.5-3wt% of the silicon nitride powder; (2) adding silicon nitride powder having an average particle size of 0.6-1.2 μm to the first mixed powder, and performing a second mixing to obtain a second mixed powder; (3) adding a binder solution to the second mixed powder and performing a third mixing to obtain a silicon nitride slurry; The binder solution is an ethanol solution of the binder, and the amount of the binder is 2wt%-6wt% of the silicon nitride powder; The binder includes polyvinyl butyral; (4) using silicon nitride slurry for spray granulation to obtain spherical powder with an average particle size of 60-120 μm; (5) After the spherical powder is filled into a mold, it is cold isostatically pressed to obtain a silicon nitride green body; The cold isostatic pressing process is performed at a pressure of 200-250 MPa and a time of 5-10 min. (6) Degreasing and hot isostatic pressing the silicon nitride green body to obtain the large-sized silicon nitride ceramic; The degreasing temperature is 500-600°C and the time is 1-5h; The hot isostatic pressing includes a first heat treatment, a second heat treatment, a third heat treatment and a fourth heat treatment performed in sequence; the temperature of the first heat treatment is 900-1200°C and the time is 1-3h; the temperature of the second heat treatment is 1300-1500°C and the time is 1-3h; the temperature of the third heat treatment is 1600-1700°C and the time is 2-4h; the temperature of the fourth heat treatment is 1750-1850°C and the time is 2-6h; The hot isostatic pressing pressure is 180-250 MPa.
Citation Information
Patent Citations
Method for preparing large scale ceramic ball
CN101125755A
Preparation method of high performance large size silicon nitride ceramic material
CN106518089A
Preparation method of high-thermal-conductivity silicon nitride ceramic substrate
CN115028460A
Cited By
Large-size silicon nitride ceramic ball valve element and preparation method and application thereof
CN119176719A
A large-size silicon nitride ceramic ball valve core and its preparation method and application
CN119176719B
Preparation method of large-size silicon nitride bearing ball
CN121494576A