Method for synergistically producing calcium-carbon-based biochar ceramsite from sewage sludge and carbide slag
Through the low-temperature aerobic pyrolysis reaction of sewage sludge and carbide slag in an O2-CO2 atmosphere, maintenance-free and high mechanical strength calcium carbon-based biochar ceramsite is generated, which solves the high cost and long-term wet curing problems in the existing technology. problem, achieving cost reduction and optimization of the preparation process.
Patent Information
- Application Number
- CN202410906045.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-08
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2044-07-08
AI Technical Summary
The existing biochar ceramsite preparation method requires the addition of a high proportion of quicklime as an activator, which is costly and requires a long period of wet curing to form high mechanical strength, which limits the optimization of the preparation process and cost reduction.
Using sewage sludge and calcium carbide slag to collaboratively produce calcium carbon-based biochar ceramsite, a low-temperature aerobic pyrolysis reaction is carried out in an O2-CO2 atmosphere. Calcium carbonate is generated by reacting carbide slag with CO2 in the ambient atmosphere, providing granular machinery. Strength, achieving maintenance-free and high mechanical strength products.
It greatly reduces the cost of raw materials, shortens the preparation time, and forms calcium-carbon-based biochar ceramsite with high mechanical strength and excellent adsorption performance, which is suitable for industrial production and realizes the harmless coordinated treatment and resources of sewage sludge and calcium carbide slag. utilization.
Smart Images

Figure FT_1
Abstract
Description
Technical Field
[0001] The invention belongs to the field of resource utilization of solid waste in environmental engineering, and in particular relates to a method for collaboratively producing calcium carbon-based biochar ceramsite by using sewage sludge and carbide slag. Background Art
[0002] As the main solid waste of urban sewage treatment plants, the output of wastewater sludge is increasing year by year. There is still a lot of room for development in the low-carbon and resource-based treatment and disposal of sewage sludge. The preparation of biochar by pyrolysis of sludge is a commonly used method for sludge resource utilization. The prepared biochar has the advantages of large specific surface area, stable pore structure, and rich surface functional groups. It has great application potential in removing various specific pollutants in gas and water phases.
[0003] Chinese patent CN115477527A discloses a method for producing biochar ceramsite particle filler, which produces biochar ceramsite by heating and stirring sewage sludge and industrial waste such as fly ash, quicklime, phosphogypsum, etc., mechanically dehydrating, pressure forming granulation, particle preheating, aerobic pyrolysis, combustion, wet curing, etc. The method uses low-temperature aerobic pyrolysis technology to achieve low-temperature harmlessness of sewage sludge and form biochar ceramsite with a spatial porous structure, which can be used for the adsorption of gas-liquid multi-media pollutants.
[0004] However, the mechanical strength of the biochar expanded clay product comes from the "volcanic ash effect" of fly ash, that is, it needs to be wet-cured to form cementitious substances such as hydrated calcium silicate and hydrated calcium aluminate to form the final mechanical strength.
[0005] The actual biochar ceramsite preparation experiment shows that in order to ensure the high mechanical strength of the biochar ceramsite product, the addition ratio of quicklime ("volcanic ash effect" activator) in the raw material should be greater than 5%, and the curing time should be 7-14 days. The quicklime raw material cost of this preparation method is high and the wet curing time is long. Therefore, the raw material ratio and curing time further limit the cost reduction and optimization of the preparation process of biochar ceramsite.
[0006] In summary, how to further optimize the raw material ratio in the preparation process of biochar ceramsite and reduce the raw material cost while retaining the original adsorption properties of biochar ceramsite products, so as to form biochar ceramsite products with excellent mechanical strength with a shorter wet curing time or even without curing is an urgent problem to be solved. Summary of the invention
[0007] The problems that need to be solved in the prior art are as follows: (1) Biochar ceramsite products need to add a certain proportion of quicklime (>5%) as a fly ash "volcanic ash effect" activator, and the raw material cost is relatively high; (2) Biochar ceramsite requires a long period of wet curing (7-14d) to form a certain mechanical strength.
[0008] In order to solve the above problems, the present invention provides a method for synergistically producing calcium carbon-based biochar ceramsite by using sewage sludge and carbide slag, wherein sewage sludge, carbide slag and fly ash are mixed and 2 -CO 2 The sludge organic carbon is converted into biochar through low-temperature aerobic pyrolysis reaction under the atmosphere to achieve harmlessness of sewage sludge. The mechanical strength of the particles is directly provided by the reaction of calcium carbide slag with carbon dioxide in the ambient atmosphere and pyrolysis, finally forming a calcium carbon-based biochar ceramsite product that does not require maintenance and has high mechanical strength.
[0009] The technical solution adopted by the present invention is as follows:
[0010] A method for synergistically producing calcium carbon-based biochar ceramsite by using sewage sludge and carbide slag, the method comprising:
[0011] (1) Mixing sewage sludge, carbide slag and fly ash;
[0012] (2) The mixed material is conveyed to a twin-screw extruder and pressure-formed to obtain wet-based columnar particles with a moisture content of 40 to 50%;
[0013] (3) sending the wet-based columnar particles to a low-temperature aerobic pyrolysis rotary reactor; preheating the wet-based columnar particles at the front end of the reactor using the waste heat of the tail gas to reduce the moisture content of the particles to 20-30%; aerobically pyrolyzing the biomass contained in the sewage sludge to form biochar in the low-temperature aerobic pyrolysis zone in the middle of the reactor, and at the same time, the carbide slag and CO in the ambient atmosphere are reacted to form biochar. 2 or CO produced by pyrolysis 2 The reaction directly provides mechanical strength to the particles; at the end of the reactor, the surface liquid phase products are instantly burned and removed; and finally the calcium carbon-based biochar ceramsite which is maintenance-free and has high mechanical strength is formed.
[0014] Furthermore, in step (1), the mass ratio of sewage sludge: fly ash: carbide slag is (3-4): (1-1.5): (1-2); and the stirring time is 2-10 min.
[0015] Furthermore, the sewage sludge is first dehydrated, and the water content of the sewage sludge after dehydration is less than 80%.
[0016] Furthermore, the wet-based columnar particles have a diameter of 3-20 mm and a length of 5-20 mm.
[0017] Furthermore, the low-temperature aerobic pyrolysis zone: by means of reaction heating and self-oxidation heat release, the biomass contained in the sewage sludge is aerobic pyrolyzed and converted into biochar, and the carbide slag and CO in the ambient atmosphere are 2 and pyrolysis to produce CO 2The reaction produces calcium carbonate which provides mechanical strength to the biochar.
[0018] Furthermore, in step (3), the preheating temperature is 150-200°C, the residence time is 5-10 minutes, and the capillary water and attached water in the particles are removed; the temperature of low-temperature aerobic pyrolysis is 300-350°C, and the residence time is 20-30 minutes; the temperature of instantaneous combustion is 800-1000°C, and the reaction time is 10-15 seconds.
[0019] Furthermore, the step (3) is as follows: determining the proportion of air and industrial flue gas added according to the carbide slag content and the oxygen demand for low-temperature aerobic pyrolysis.
[0020] Compared with the prior art, the present invention has the following beneficial effects:
[0021] (1) The present invention uses carbide slag to replace the raw materials such as quicklime and cement in the production of biochar ceramsite. The prepared product does not require a wet curing process and is directly curing-free. The test cycle is greatly shortened, saving time and effort.
[0022] (2) The present invention uses carbide slag to replace the raw materials such as quicklime and cement in the production of biochar ceramsite, which greatly reduces the cost of raw materials, reduces cost expenditure, and is suitable for industrial production.
[0023] (3) The present invention retains the excellent adsorption and phosphorus removal efficiency of the original biochar ceramsite and the biochar adsorption performance of carbon-containing organic matter, and uses carbide slag to replace the raw materials such as quicklime and cement in the production of the original biochar ceramsite. 2 The generated calcium carbonate directly provides mechanical strength to the particles, forming a calcium carbon-based biochar ceramsite product with high mechanical strength; the product has high mechanical strength and is not easy to break when used as a biofilter filler later.
[0024] (4) The calcium carbon-based biochar ceramsite product prepared by the present invention has a large porosity and specific surface area, and realizes spatial connectivity between internal pores and external pores, and has a good environmental decontamination ability.
[0025] (5) The present invention is based on CO from industrial flue gas 2 and O from air 2 The production process is carried out by low-temperature aerobic pyrolysis in an atmosphere of 200 °C. The production process realizes the harmless coordinated treatment and resource utilization of solid wastes such as sewage sludge and carbide slag. At the same time, the industrial flue gas and CO generated by pyrolysis are treated by carbide slag. 2 Fixation reduces carbon emissions during the preparation of biochar pellets and has high economic and environmental benefits.
[0026] (6) The present invention utilizes high-water content biomass waste (such as sewage sludge) and industrial waste (carbide slag and fly ash) to produce a new type of calcium carbon-based biochar pellets. The raw materials are easily available, the cost is low, the process is simple and practical, the impact on the environment is small, and it has good economic and environmental benefits. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 The present invention is a process flow chart of the method for synergistically producing calcium carbon-based biochar ceramsite from sewage sludge and carbide slag. DETAILED DESCRIPTION
[0028] In order to make the technical means, creative features, objectives and effects achieved by the present invention easy to understand, the technical solutions in the embodiments of the present invention are clearly and completely described below in conjunction with the accompanying drawings.
[0029] This embodiment provides a method for synergistically producing calcium carbon-based biochar ceramsite by using sewage sludge and carbide slag, comprising the following steps:
[0030] Step 1): Dehydrated sewage sludge (water content <80%) is used as the main material of the formula (sludge ratio is greater than 50%), and fly ash and calcium carbide slag are used as auxiliary materials of the formula. The materials are fully mixed in a drum mixer or other mechanical mixing equipment according to a certain mass ratio.
[0031] Preferably, the mass ratio of sludge: fly ash: carbide slag is 3:1:1 or 3:1:2; and the stirring time is 2 to 10 minutes.
[0032] Step 2): The uniformly mixed materials are added into a twin-screw extruder and pressure-formed to obtain wet-based columnar particles with a certain strength.
[0033] Preferably, the extrusion molding obtains wet-basis columnar particles with a diameter of 3-20 mm and a length of 5-20 mm.
[0034] Step 3): The wet columnar particles are transported to the entrance of the low-temperature aerobic pyrolysis rotary reactor. The waste heat of the tail gas is used to preheat the particles at the front end of the reactor to further reduce the moisture content of the particles. The particles then enter the low-temperature aerobic pyrolysis section to achieve aerobic pyrolysis of biomass into biochar with the help of system heating and self-oxidation heat release. The carbide slag reacts with the ambient atmosphere and pyrolysis to produce carbon dioxide to generate calcium carbonate to provide mechanical strength for the particles. Then enter the instantaneous combustion section to remove the liquid products produced by the pyrolysis process. Finally, a calcium-carbon-based biochar ceramsite product that is maintenance-free and has high mechanical strength is formed.
[0035] Preferably, the low-temperature aerobic pyrolysis rotary reactor is a horizontal rotary aerobic pyrolysis furnace described in Chinese patent CN 115477527A.
[0036] Preferably, the temperature of the preheating section of the low-temperature aerobic pyrolysis equipment is controlled at 150-200°C, with a residence time of 5-10 minutes, to remove capillary water, attached water, etc. in the particles; the temperature of the low-temperature aerobic pyrolysis section is controlled at 300-350°C, with a residence time of 20-30 minutes; the temperature of the instantaneous combustion stage is 800-1000°C, with a residence time of 10-15 seconds.
[0037] Preferably, the proportion of air and industrial flue gas added is determined according to the carbide slag content and the oxygen demand for low-temperature aerobic pyrolysis.
[0038] Embodiment 1:
[0039] (1) Dehydrated sewage sludge (water content 70%) is used as the main material of the formula (sludge ratio is greater than 50%), and fly ash and calcium carbide slag are used as auxiliary materials of the formula in a mass ratio of 3:1:1 in a drum mixer or other mechanical mixing equipment. The materials are fully mixed for 10 minutes.
[0040] (2) The uniformly mixed material is added into a twin-screw extruder by using a shaftless screw, and pressure molding is performed to obtain wet-based columnar particles with a certain strength, a diameter of 10 mm, and a length of 10 mm.
[0041] (3) The wet columnar particles are transported to the inlet of the low-temperature aerobic pyrolysis rotary reactor. The waste heat of the tail gas is used at the front end of the reactor to preheat the particles (the temperature is set to 150°C and the residence time is 5 minutes) to remove capillary water and attached water in the particles and further reduce the moisture content of the particles. The particles then enter the low-temperature aerobic pyrolysis section (the temperature is set to 300°C and the residence time is 20 minutes). With the help of system heating and self-oxidation heat release, the biomass is aerobic pyrolysis and converted into biochar. The calcium carbide slag reacts with the ambient atmosphere (intake air: industrial flue gas = 3:1) and the carbon dioxide produced by pyrolysis to produce calcium carbonate to provide mechanical strength for the particles. Finally, it enters the instantaneous combustion section (the temperature is set to 900°C and the residence time is 10 seconds) to remove the liquid products produced by the pyrolysis process. Finally, a maintenance-free calcium carbon-based biochar ceramsite product with high mechanical strength is formed, with a compressive strength of 67.2N and a specific surface area of 14.0779m 2 / g; average pore size: 14.0779m 2 / g; total pore volume: 0.056835cm 3 / g.
[0042] Embodiment 2:
[0043] (1) Dehydrated sewage sludge (water content 70%) is used as the main material of the formula (sludge ratio is greater than 50%), and fly ash and calcium carbide slag are used as auxiliary materials of the formula in a mass ratio of 3:1:1 in a drum mixer or other mechanical mixing equipment. The materials are fully mixed for 10 minutes.
[0044] (2) The uniformly mixed material is added into a twin-screw extruder by using a shaftless screw, and pressure molding is performed to obtain wet-based columnar particles with a certain strength, a diameter of 15 mm, and a length of 10 mm.
[0045] (3) The wet columnar particles are transported to the inlet of the low-temperature aerobic pyrolysis rotary reactor. The waste heat of the tail gas is used at the front end of the reactor to preheat the particles (the temperature is set to 200℃, the residence time is 5min), and the capillary water and attached water in the particles are removed to further reduce the moisture content of the particles. Then the particles enter the low-temperature aerobic pyrolysis section (the temperature is set to 300℃, the residence time is 30min), and the biomass is aerobic pyrolysis and converted into biochar with the help of system heating and self-oxidation heat release. The calcium carbide slag reacts with the ambient atmosphere (intake air: industrial flue gas = 3:1) and the carbon dioxide produced by pyrolysis to produce calcium carbonate to provide mechanical strength for the particles. Finally, it enters the instantaneous combustion section (the temperature is set to 900℃, the residence time is 10s) to remove the liquid products produced by the pyrolysis process. Finally, a maintenance-free calcium carbon-based biochar ceramsite product with high mechanical strength is formed, with a compressive strength of 70.4N and a specific surface area of 15.5371m 2 / g; average pore size: 19.0634m 2 / g; overall pore volume: 0.058621cm 3 / g.
[0046] Embodiment 3:
[0047] (1) Dehydrated sewage sludge (water content 70%) is used as the main material of the formula (sludge ratio is greater than 50%), and fly ash and calcium carbide slag are used as auxiliary materials of the formula in a mass ratio of 3:1:2. The materials are fully mixed in a drum mixer or other mechanical mixing equipment for 10 minutes.
[0048] (2) The uniformly mixed material is added into a twin-screw extruder by using a shaftless screw, and pressure molding is performed to obtain wet-based columnar particles with a certain strength, a diameter of 20 mm, and a length of 10 mm.
[0049] (3) The wet columnar particles are transported to the inlet of the low-temperature aerobic pyrolysis rotary reactor. The waste heat of the tail gas is used at the front end of the reactor to preheat the particles (the temperature is set to 200℃, the residence time is 10min), and the capillary water and attached water in the particles are removed to further reduce the moisture content of the particles. Then the particles enter the low-temperature aerobic pyrolysis section (the temperature is set to 350℃, the residence time is 30min), and the biomass is aerobic pyrolysis is converted into biochar with the help of system heating and self-oxidation heat release. The calcium carbide slag reacts with the ambient atmosphere (intake air: industrial flue gas = 4:1) and the carbon dioxide produced by pyrolysis to produce calcium carbonate to provide mechanical strength for the particles. Finally, it enters the instantaneous combustion section (the temperature is set to 900℃, the residence time is 15s) to remove the liquid products produced by the pyrolysis process. Finally, a maintenance-free calcium carbon-based biochar ceramsite product with high mechanical strength is formed, with a compressive strength of 72.1N and a specific surface area of 16.2173m 2 / g; average pore size: 18.9255m 2 / g; overall pore volume: 0.060407cm 3 / g.
[0050] Comparative Example 1:
[0051] The method of steps (1) to (5) of Example 2 of Chinese patent CN 115477527 B is used:
[0052] (1) adding a small amount of lime to the dehydrated cake of biomass waste with a moisture content of 80%, and heating and stirring the cake at 60° C. for pretreatment;
[0053] (2) The pretreated material is placed in a plate and frame filter press to further reduce the moisture content of the material to 50% as the main material, accounting for 50%. Fly ash, phosphogypsum and lime are prepared in a mass ratio of about 8:1:1. The waste plastic residue is crushed to less than 2 mm and added to an intermittently operated horizontal mixing tank by screw conveyor at a ratio of 6% of the mass of the main and auxiliary mixed materials to be fully mixed.
[0054] (3) The mixed materials are evenly fed into the inlet of a twin-screw extruder. The die head of the extruder adopts a 5 mm orifice plate and is equipped with an automatic scraper. The mixed materials are processed by pressure molding into wet-based columnar particles with a diameter of 5 mm and a length of 5-10 mm (water content 30-40%).
[0055] (4) The wet-based columnar particles are sent to the entrance of the horizontal rotary aerobic pyrolysis furnace through a belt conveyor. The wet-based columnar particles are heated to 150° C. in the waste heat tail gas preheating and drying section, and the moisture content is reduced to 25%; then they enter the low-temperature aerobic pyrolysis section, the temperature is gradually raised to 250° C., and the particles slowly rotate for 35 minutes; finally, the particles enter the instantaneous combustion section, at 250-350° C., using natural gas or other combustible gases as fuel, and the annular porous burner technology, the particles are subjected to short-term combustion treatment to burn out the liquid phase product; finally, the dry-based particle product is discharged from the pyrolysis furnace outlet, and after natural cooling in the air cooling section, it enters the wet curing tank;
[0056] (5) The dry particles were humidified by water mist and electrically heated at 50°C in a wet curing tank for 5 days to obtain an environmentally friendly biochar pellet product with a compressive strength of 14.63N, a BET specific surface area of 10.9021m2 / g, an average pore size of 7.3225nm (mainly mesopores), and a total pore volume of 0.027538cm3 / g.
[0057] The above description is only a preferred embodiment of the present invention and does not constitute a limitation on the protection scope of the present invention. Any modification, equivalent substitution and improvement made within the spirit and principle of the present invention shall be included in the protection scope of the claims of the present invention.
Claims
1. A method for producing calcium carbon-based biochar ceramsite by synergistically using sewage sludge and carbide slag, characterized in that: The method comprises: (1) Mixing sewage sludge, carbide slag and fly ash; (2) The mixed material is conveyed to a twin-screw extruder and pressure-formed to obtain wet-based columnar particles with a moisture content of 40 to 50%; (3) The wet-based columnar particles are sent to a low-temperature aerobic pyrolysis rotary reactor; the waste heat of the exhaust gas is used to preheat the wet-based columnar particles at the front end of the reactor to reduce the moisture content of the particles to 20-35%; in the low-temperature aerobic pyrolysis zone in the middle of the reactor, the biomass contained in the sewage sludge is aerobically pyrolyzed to form biochar, and at the same time, the carbide slag reacts with CO2 in the ambient atmosphere or CO2 produced by pyrolysis to directly provide mechanical strength for the particles; at the end of the reactor, the surface liquid phase products are removed by instantaneous combustion; and finally the maintenance-free and high mechanical strength calcium carbon-based biochar pellets are formed.
2. The method for producing calcium carbon-based biochar ceramsite by synergistically using sewage sludge and carbide slag as claimed in claim 1, characterized in that: In the step (1), the mass ratio of sewage sludge: fly ash: carbide slag is (3-4): (1-1.5): (1-2); and the stirring time is 2-10 minutes.
3. The method for producing calcium carbon-based biochar ceramsite by synergistically using sewage sludge and carbide slag as claimed in claim 2, characterized in that: The sewage sludge needs to be dehydrated first, and the water content of the sewage sludge after dehydration is less than 80%.
4. A method for synergistically producing calcium carbon-based biochar ceramsite from sewage sludge and carbide slag as described in any one of claims 1 to 3, characterized in that: The wet-based columnar particles have a diameter of 3-20 mm and a length of 5-20 mm.
5. A method for synergistically producing calcium carbon-based biochar ceramsite from sewage sludge and carbide slag as described in any one of claims 1 to 3, characterized in that: The low-temperature aerobic pyrolysis zone: the biomass contained in the sewage sludge is aerobically pyrolyzed and converted into biochar by means of reaction heating and self-oxidation heat release, and the carbide slag reacts with CO2 in the ambient atmosphere and CO2 produced by pyrolysis to form calcium carbonate, thereby providing mechanical strength for the biochar.
6. A method for producing calcium carbon-based biochar ceramsite by synergistically using sewage sludge and carbide slag as described in any one of claims 1 to 3, characterized in that: The step (3) comprises: preheating at a temperature of 150 to 200° C. for a residence time of 5 to 10 minutes to remove capillary water and attached water in the particles; low-temperature aerobic pyrolysis at a temperature of 300 to 350° C. for a residence time of 20 to 30 minutes; and instantaneous combustion at a temperature of 800 to 1000° C. for a reaction time of 10 to 15 seconds.
7. A method for producing calcium carbon-based biochar ceramsite by synergistically using sewage sludge and carbide slag as described in any one of claims 1 to 3, characterized in that: The step (3) is to determine the proportion of air and industrial flue gas added according to the carbide slag content and the oxygen demand for low-temperature aerobic pyrolysis.
Citation Information
Patent Citations
Production method of biochar ceramsite particle filler
CN115477527A
A method for producing biochar ceramsite granular filler
CN115477527B
Riverway bottom mud ecological brick for riverway restoration work and preparing method thereof
CN110117185A
CO2-driven consolidated lightweight concrete and preparation method thereof
CN113968701A
Carbonized porous steel slag aggregate and preparation method thereof
CN115448628A