Polymer for mRNA delivery, lipid / polymer hybrid nanoparticle using same, and preparation method and application thereof

By adding hydrophobic groups and the auxiliary lipid DOTAP to the PBAE polymer, lipid/polymer hybrid nanoparticles are formed, which solves the problem of insufficient stability of mRNA molecules and cellular uptake, and improves the delivery efficiency and stability of mRNA. Efficient mRNA vaccine delivery was achieved.

CN118755084AActive Publication Date: 2024-10-11ZHEJIANG UNIV OF TECH
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202410758382.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-13
Publication Date
2024-10-11
Estimated Expiration
2044-06-13

AI Technical Summary

Technical Problem

The mRNA molecule itself is extremely unstable and difficult to be taken up by cells, resulting in low expression efficiency of mRNA vaccines. Existing delivery carriers based on cationic polymers are not ideal, limiting the development of mRNA treatments.

Method used

By adding hydrophobic group modification and auxiliary lipid DOTAP to the PBAE polymer, the formula composition of the nanoparticles is optimized to improve the physical encapsulation efficiency and cellular uptake ability of nucleic acids, form lipid/polymer hybrid nanoparticles, and promote the incorporation of mRNA. Delivery inside and outside.

Benefits of technology

It improves the in vitro transfection efficiency and in vivo stability of mRNA, enhances the delivery effect of mRNA, and has high application value and broad prospects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118755084A_ABST
    Figure CN118755084A_ABST
Patent Text Reader

Abstract

The invention discloses a polymer for mRNA delivery, lipid / polymer hybrid nanoparticles using the polymer and a preparation method and application of the lipid / polymer hybrid nanoparticles, and the preparation method of the cationic polymer comprises the following steps: synthesizing a precursor polymer with double bonds at the tail end by taking 1, 6-hexanediol diacrylate (DAHE) and hydrophilic amine as raw materials through Michael addition reaction; and carrying out an end-capping reaction by using hydrophobic amine. According to the invention, poly-beta-amino ester (PBAE) containing a hydrophilic main chain and a water delivery terminal is prepared, and auxiliary lipids such as (2, 3-dioleoyl-propyl)-trimethyl ammonium chloride (DOTAP) are added into the PBAE polymer, so that the surface charge of the nanoparticles is increased in a proper range, the uptake of the nanoparticles by cells is promoted, and the delivery efficiency of mRNA is improved. The mRNA nano preparation prepared by adopting the cationic polymer and the formula thereof provided by the invention can effectively improve the delivery efficiency of mRNA in cells and mice.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of pharmaceutical preparations, and in particular to a polymer for mRNA delivery, lipid / polymer hybrid nanoparticles using the polymer, and a preparation method and application thereof. Background Art

[0002] Messenger RNA (mRNA), as a new type of nucleic acid drug, has recently become a research hotspot. Synthetic mRNA encoding specific proteins can express corresponding functional proteins in cells just like natural mRNA, and therefore has broad application prospects in immunotherapy, regenerative medicine, infectious disease vaccines, and protein replacement / supplementation. Compared with plasmid DNA (pDNA) or small interfering RNA therapy, mRNA therapy has many potential advantages: 1) mRNA directly expresses functional proteins in the cytoplasm and does not need to enter the nucleus like pDNA. Therefore, mRNA therapy has fewer obstacles such as crossing the nuclear membrane and can also work efficiently in non-dividing cells or cells that divide very slowly, such as dendritic cells; 2) mRNA does not need to be integrated into the chromosomes of cells, which can avoid the risk of insertional gene mutations; 3) Compared with RNA interference, the process of mRNA translation of target proteins is simpler and more direct, without off-target problems similar to siRNA. In addition, compared with the corresponding recombinant protein, high-charge-density and flexible mRNA has higher loading efficiency in the carrier; mRNA preparation is relatively simple and has low biosafety risks.

[0003] However, mRNA vaccines also have major problems that limit their development. The mRNA molecule itself is extremely unstable and easily degraded by mRNA enzymes inside and outside the body; secondly, mRNA itself is negatively charged and difficult to be taken up by cells, resulting in low expression efficiency. Therefore, developing an efficient mRNA delivery system, improving the mRNA expression efficiency, and improving the level of vaccine-induced cellular and humoral immunity in the body are key technologies for the development of mRNA therapy. However, the mRNA expression efficiency of the cationic polymer-based delivery vector reported in the prior art is not ideal. Therefore, it is urgent to develop a new cationic polymer-based mRNA delivery system and construct a stable, high-molecular-weight mRNA nanovaccine. Summary of the invention

[0004] In order to overcome the above-mentioned shortcomings and deficiencies of the prior art, in order to improve the stability of drug carriers and drug encapsulation efficiency, improve drug delivery efficiency and therapeutic effects, the present invention provides a polymer for mRNA delivery, lipid / polymer hybrid nanoparticles using the polymer, and preparation methods and applications thereof. The present invention modifies PBAE by hydrophobic groups, increases the physical encapsulation effect of nucleic acids, and is conducive to promoting cell adsorption. At the same time, a cationic polymer / lipid hybrid strategy is used to combine lipids with good biocompatibility with structurally stable polymers, and auxiliary lipids such as (2,3-dioleoyl-propyl)-trimethylammonium chloride (DOTAP) are added to the PBAE polymer to increase the surface charge of the nanoparticles within an appropriate range, promote cell uptake of the nanoparticles, and enhance the in vivo and in vitro delivery effect of mRNA.

[0005] The technical solution adopted by the present invention is as follows:

[0006] A method for preparing a polymer for mRNA delivery comprises the following steps:

[0007] 1) Using 1,6-hexanediol diacrylate DAHE and a hydrophilic amine as raw materials, heating and dissolving at 80-95° C., and carrying out Michael addition reaction for 40-60 hours. After the reaction, washing and drying are performed to obtain a precursor polymer with acrylates at both ends; wherein the hydrophilic amine raw material is one of A7, A8, A9, A13, and A15:

[0008] 2) using a hydrophobic amine to end-cap the precursor polymer with acrylates at both ends obtained in step 1), wherein the precursor polymer and the hydrophobic amine are stirred and reacted in an organic solvent at a reaction temperature of 50-65° C. for a reaction time of 20-55 hours, and then dried to obtain an end-capped final product, which is recorded as polymer PBAE; wherein the hydrophobic amine raw material is one of 2C4, 2C6, 2C8, 2C10, C8', and C12':

[0009] The reaction formula for preparing the polymer of the present invention is as follows:

[0010]

[0011] The structure of the hydrophilic main chain is one of the following:

[0012]

[0013] The hydrophobic end-capping structure is one of the following:

[0014]

[0015] Furthermore, the structure of the polymer for mRNA delivery is selected from one of the following:

[0016]

[0017] Furthermore, in step 1), the molar ratio of DAHE to hydrophilic amine is 0.8-1.5:1, preferably 1-1.1:1; the reaction temperature of step 1) is 85-90° C., and the reaction time is 45-50 h.

[0018] Further, in step 2), the molar ratio of the precursor polymer to the hydrophobic amine is 1:3-5, preferably 1:4, the reaction temperature is 55-60°C, and the reaction time is 45-50h;

[0019] In step 2), the organic solvent is tetrahydrofuran, and the concentration of the hydrophobic amine in the organic solvent is 0.01-0.1 mol / L, preferably 0.03-0.0625 mol / L.

[0020] Furthermore, the polymer for mRNA delivery prepared by the method of the present invention has a molecular weight between 1.5 kDa and 37 kDa and a degree of polymerization between 10 and 52.

[0021] A method for preparing lipid / polymer hybrid nanoparticles comprises the following steps:

[0022] S1: dissolving luciferase mRNA in an acidic solution to obtain a first solution;

[0023] S2: dissolving the polymer prepared by the present invention and auxiliary lipids cholesterol, DOPE, PEG2000-DMG, and DOTAP in anhydrous ethanol to obtain a second solution;

[0024] S3: mixing the first solution and the second solution to obtain a mixed solution, and incubating the mixed solution on a shaking table;

[0025] S4: The mixed solution after incubation is diluted with sterile PBS to obtain a suspension containing the prepared lipid / polymer hybrid nanoparticles.

[0026] Furthermore, in step S1, the acidic solution is a sodium citrate solution, 10 mM, pH = 4.2.

[0027] Further, in step S2, the molar ratio of polymer to cholesterol is 1:0.8-1.2, preferably 1:0.9-1.0;

[0028] The molar ratio of polymer to DOPE is 1:0.2-0.3, preferably 1:0.25;

[0029] The molar ratio of polymer to DOTAP is 1:0.2-0.3, preferably 1:0.25;

[0030] The molar ratio of polymer to PEG2000-DMG is 1:0.02-0.05, preferably 1:0.035-0.04;

[0031] The total mass of the polymer and DOTAP in the second solution of step S2 is 15-25 times, preferably 20 times, the mass of the luciferase mRNA in the first solution of step S1;

[0032] Wherein, in step S2, the mass concentration of the polymer dissolved in anhydrous ethanol is 0.5-2 g / L, preferably 1 g / L.

[0033] Furthermore, in step S3, the shaking incubation time is 0.5 to 1.5 hours, and in step S4, the mixed solution after incubation is diluted with PBS by 4 to 6 times, and the content of organic phase ethanol in the diluted solution is not higher than 10%.

[0034] The present invention also provides the use of the lipid / polymer hybrid nanoparticles in the preparation of mRNA vaccine drugs.

[0035] The beneficial effects achieved by the present invention are:

[0036] The present invention innovatively adopts a new polymer molecule, optimizes the formula composition of the nanoparticles by incorporating auxiliary lipids such as DOTAP, and obtains a new hybrid nanoparticle composition. The terminal modification of PBAE is changed from a conventional hydrophilic group to a hydrophobic group modification, thereby improving the physical encapsulation efficiency and delivery efficiency of nucleic acids. On the other hand, auxiliary lipids such as DOTAP are added to increase the surface charge of the nanoparticles within an appropriate range, thereby solving the problem of insufficient cell uptake of nanoparticles. The preparation strategy of this lipid / polymer hybrid nanoparticle (LPH) is simple, fast and easy to control. The nanoparticles have high transfection efficiency in vitro and good stability in vivo, and have high application value and very broad application prospects. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] Figure 1 The precursor polymer A7 1 H-NMR spectrum.

[0038] Figure 2 Represents the precursor polymer A8 1 H-NMR spectrum.

[0039] Figure 3 The precursor polymer A9 1 H-NMR spectrum.

[0040] Figure 4 Represents the precursor polymer A13 1 H-NMR spectrum.

[0041] Figure 5Represents the precursor polymer A15 1 H-NMR spectrum.

[0042] Figure 6 It shows the molecular weight of the precursor polymers A7, A8, A9, A11, A13, and A15.

[0043] Figure 7 Indicates A7-2C4, A7-2C6, A7-2C10 1 H-NMR spectrum.

[0044] Figure 8 Indicates A8-C8', A8-2C8 1 H-NMR spectrum.

[0045] Fig. 9 Indicates A9-2C10 1 H-NMR spectrum.

[0046] Fig.10 Indicates A13-C8', A15-C12' 1 H-NMR spectrum.

[0047] Fig.11 It shows the test results of in vitro mRNA delivery efficiency of LPH prepared by different polymer carriers.

[0048] Fig.12 It shows the particle size and potential of LPH prepared with different polymer carriers;

[0049] Fig.13 It indicates the encapsulation efficiency (Binding) (%) of LPH prepared by different polymer carriers for Fluc mRNA;

[0050] Fig.14 It shows the expression of luciferase in mice 6 hours after tail vein injection of LPH prepared with different polymer carriers.

[0051] Fig.15 It shows the expression of luciferase in various organs of mice 8 hours after tail vein injection of LPH prepared by different polymer carriers.

[0052] Fig.16 The particle size potential of LPH prepared by polymer carrier A7-2C10 under various formulations is shown.

[0053] Fig.17 The graph shows the uptake of Cy5-mRNA-LPH prepared by polymer carrier A7-2C10 in various formulations by IGrov1 cells under fluorescence microscopy.

[0054] Fig.18It shows the uptake of Cy5-mRNA-LPH prepared by polymer carrier A7-2C10 in various formulations by IGrov1 cells after flow cytometry treatment. DETAILED DESCRIPTION

[0055] The present invention will be further described below in conjunction with specific embodiments, but the protection scope of the present invention is not limited thereto.

[0056] Example 1: Synthesis of A7-2C6

[0057] (1) In a 10 mL sample bottle equipped with a stirrer, add hydrophilic amine A7 (0.6683 g, 5.3387 mmol) and DAHE (1.3346 g, 5.8850 mmol) to a molar ratio of 1:1.1, control the total mass to about 2 g, stir and dissolve at 90°C, and react for 48 hours. After the reaction is completed and cooled, wash with n-hexane three times, wash and purify, and dry in a vacuum drying oven overnight to obtain the precursor polymer A7.

[0058] (2) Use hydrophobic amine to cap the precursor polymer with acrylate at both ends. Add the precursor polymer A7 (0.1046 g, 0.0232 mmol), hydrophobic amine 2C6 (0.0173 g, 0.0933 mmol), and tetrahydrofuran THF (2 mL) into a 4 mL sample bottle, respectively, and control the molar ratio of the precursor polymer to the hydrophobic amine to be 1:4. After stirring at 55° C. for 48 hours, dry in a fume hood for two days, and then dry in a vacuum drying oven for one day to obtain the final product A7-2C6.

[0059] In addition, the preparation method of polymers A7-2C4 and A7-2C10 repeats the above experimental steps, except that the hydrophobic amine 2C6 is replaced by the same molar amount of hydrophobic amine 2C4 or hydrophobic amine 2C10.

[0060] Example 2: Synthesis of A8-2C8

[0061] (1) In a 10 mL sample bottle equipped with a stirrer, add hydrophilic amine A8 (0.6321 g, 5.4393 mmol) and DAHE (1.3638 g, 6.0273 mmol) to a molar ratio of 1:1.1, control the total mass to about 2 g, stir and dissolve at 90°C, and react for 48 hours. After the reaction is completed and cooled, wash with n-hexane three times, and after washing and purification, put it into a vacuum drying oven and dry it overnight to obtain the precursor polymer A8.

[0062] (2) Use hydrophobic amine to cap the precursor polymer with acrylate at both ends. Add the precursor polymer A8 (0.1032 g, 0.0159 mmol), hydrophobic amine 2C8 (0.0153 g, 0.0635 mmol) to a 4 mL sample bottle, respectively, and control the molar ratio of the precursor polymer to the hydrophobic amine to be 1:4, and tetrahydrofuran THF (2 mL). After stirring at 55 ° C for 48 hours, dry in a fume hood for two days, and then dry in a vacuum drying oven for one day to obtain the final product A8-2C8.

[0063] In addition, the preparation method of polymer A8-C8' repeats the above experimental steps, except that the hydrophobic amine 2C8 is replaced by the same molar amount of hydrophobic amine C8'.

[0064] Example 3: Synthesis of A9-2C10

[0065] (1) In a 10 mL sample bottle equipped with a stirrer, add hydrophilic amine A9 (0.8123 g, 4.6872 mmol) and DAHE (1.1806 g, 5.2177 mmol) to a molar ratio of 1:1.1, control the total mass to about 2 g, stir and dissolve at 90°C, and react for 48 hours. After the reaction is completed and cooled, wash with n-hexane three times, wash and purify, and dry in a vacuum drying oven overnight to obtain the precursor polymer A9.

[0066] (2) Use hydrophobic amine to cap the precursor polymer with acrylate at both ends. Precursor polymer A9 (0.1078 g, 0.0117 mmol), hydrophobic amine 2C10 (0.0142 g, 0.0478 mmol), tetrahydrofuran THF (2 mL) were added to a 4 mL sample bottle, and the molar ratio of the precursor polymer to the hydrophobic amine was controlled to be 1:4. After stirring at 55° C. for 48 hours, it was dried in a fume hood for two days and then dried in a vacuum drying oven for one day to obtain the final product A9-2C10.

[0067] Example 4: Synthesis of A13-C8'

[0068] (1) In a 10 mL sample bottle equipped with a stirrer, add hydrophilic amine A13 (0.5342 g, 5.9928 mmol) and DAHE (1.4781 g, 6.5325 mmol) to a molar ratio of 1:1.1, control the total mass to about 2 g, stir and dissolve at 90°C, and react for 48 hours. After the reaction is completed and cooled, wash with n-hexane three times, wash and purify, and dry in a vacuum drying oven overnight to obtain the precursor polymer A13.

[0069] (2) Use hydrophobic amine to cap the precursor polymer with acrylate at both ends. Precursor polymer A13 (0.1097 g, 0.0233 mmol), hydrophobic amine C8' (0.0136 g, 0.0949 mmol), tetrahydrofuran THF (2 mL) were added to a 4 mL sample bottle, and the molar ratio of the precursor polymer to the hydrophobic amine was controlled to be 1:4. After stirring at 55° C. for 48 h, it was dried in a fume hood for two days and then dried in a vacuum drying oven for one day to obtain the final product A13-C8'.

[0070] Example 5: Synthesis of A15-C12'

[0071] (1) In a 10 mL sample bottle equipped with a stirrer, add hydrophilic amine A15 (0.5931 g, 5.7488 mmol) and DAHE (1.4208 g, 6.2792 mmol) to a molar ratio of 1:1.1, control the total mass to about 2 g, stir and dissolve at 90°C, and react for 48 hours. After the reaction is completed and cooled, wash with n-hexane three times, wash and purify, and dry in a vacuum drying oven overnight to obtain the precursor polymer A15.

[0072] (2) Use hydrophobic amine to cap the precursor polymer with acrylate at both ends. Precursor polymer A15 (0.1021 g, 0.0309 mmol), hydrophobic amine C12' (0.0248 g, 0.1246 mmol), tetrahydrofuran THF (2 mL) were added to a 4 mL sample bottle, and the molar ratio of the precursor polymer to the hydrophobic amine was controlled to be 1:4. After stirring at 55° C. for 48 hours, it was dried in a fume hood for two days and then dried in a vacuum drying oven for one day to obtain the final product A15-C12'.

[0073] Example 6: Determination of polymer structure and molecular weight

[0074] The precursor polymers A7, A8, A9, A13, and A15 prepared in Examples 1-5 were tested respectively by dissolving 10 mg of the dried precursor polymer sample in deuterated chloride, transferring the sample to a nuclear magnetic resonance tube, and performing nuclear magnetic resonance spectroscopy ( 1 H nuclear magnetic resonance, 1 H NMR) was used to characterize the structure and molecular weight of the cc-PBAE precursor polymer. 1 The precursor polymers A7, A8, A9, A13, and A15 were characterized by H NMR. 1 The H-NMR spectra are shown in Figure 1-5 As shown, 1In HNMR, 6.4ppm, 6.1ppm, and 5.8ppm are the proton peaks of the double bonds in the precursor polymer, indicating that the double bonds have not reacted completely; 4.1ppm, 1.6ppm, and 1.4ppm are the proton peaks of the main chain -O-CH2-CH2-CH2-. According to the spectrum analysis, the molecular weights of the precursor polymers A7, A8, A9, A13, and A15 are as follows: Figure 6 shown.

[0075] The final polymer products prepared in Examples 1-5 were tested respectively by dissolving 10 mg of the dried final polymer product sample in deuterated chloride, transferring it to a nuclear magnetic resonance tube, and measuring the final polymer product by nuclear magnetic resonance hydrogen spectrum ( 1 H nuclear magnetic resonance, 1 H NMR) was used to characterize the structure of the final cc-PBAE polymer. 1 H-NMR spectra are summarized in Figure 7 , polymers A8-C8' and A8-2C8 prepared in Example 2 1 H-NMR spectra are summarized in Figure 8 , polymer A9-2C10 1 H-NMR spectrum Fig. 9 As shown, polymers A13-C8', A15-C12' 1 H-NMR spectra are summarized in Fig.10 .

[0076] Example 7: In vitro delivery efficiency of LPH

[0077] The synthesized polymer carrier PBAE, DOTAP, DOPE, cholesterol, and PEG2000-DMG were dissolved in anhydrous ethanol, wherein the concentration of the polymer carrier PBAE in anhydrous ethanol was 1 g / L, and the above five components were prepared according to the molar ratio of PBAE:DOTAP:DOPE:Chol:PEG2000-DMG=40:10:10:38.5:1.5, and luciferase mRNA (Fluc mRNA) was dissolved in a sodium citrate solution (10 mM, pH=4.2). The above-prepared ethanol solution and sodium citrate solution (10 mM, pH=4.2) were mixed at a volume ratio of 1:1, and the mass ratio of (DOTAP+PBAE) to luciferase mRNA (Fluc mRNA) was about 20:1. After incubation, it was diluted 5 times with PBS to obtain a composite nanoparticle solution (each liter of composite nanoparticle solution contained 2.5 mg luciferase mRNA), and the composite nanoparticle was recorded as LPH.

[0078] After IGrov1 cells were cultured in DMEM medium until they were adherent, the composite nanosolution prepared above was added (the amount added was 12.5 / 25 / 50 ng per 10,000 cells). Under this condition, transfection was performed for 48 hours, the medium was removed, and luciferin, a substrate of luciferase, was added to test the in vitro mRNA delivery efficiency by the luminescence value.

[0079] Through the above operation process, the A7-2C4, A7-2C6, A7-2C8, A8-C8', A8-2C8, A9-2C10, A13-C8', and A15-C12' polymer molecules synthesized in Examples 1-6 of the present invention were used as delivery vectors, and the approved lipid molecule ALC-0315 was used as a positive control group of the delivery vector, mixed with auxiliary lipids and mRNA encoding luciferase to prepare nanoparticles, which were added to IGrov1 cells. After 48 hours of transfection, the in vitro delivery efficiency of mRNA was evaluated by the expression of luciferase in the cells. The in vitro mRNA delivery efficiency test results of different delivery vectors are shown in Fig.11 . Fig.11 It shows that the polymer carrier synthesized by the present invention has comparable mRNA delivery efficiency to that of ALC0315, the main delivery vector in the new crown vaccine preparation, and its luminescence value shows good dose responsiveness under different mRNA doses.

[0080] Example 8: Particle size, surface charge and mRNA loading efficiency of LPH

[0081] Hybrid nanoparticles were prepared according to the method described in Example 7. The particle size and surface potential of LPH were measured by dynamic light scattering (DLS). The particle size and surface charge test results of nanoparticle suspensions prepared from polymers with different structures are summarized in Fig.12 middle.

[0082] Hybrid nanoparticles were prepared according to the method described in Example 7, and the free mRNA concentration in the nanoparticle suspension was determined using the Quant-iT RiboGreenAssay kit to quantify the loading efficiency of LPH on Fluc mRNA. The specific implementation steps were as follows: 100 μL of nanoparticle solution diluted 10 times with TE buffer (mRNA concentration was 0.25 mg / L) was added to a 96-well black board, followed by 100 μL of RiboGreen reagent diluted 800 times with TE buffer, and the wells were measured using an ELISA reader (λ ex =485nm,λ em=535nm) to detect the fluorescence intensity. The free mRNA content in each well can be obtained by the standard curve of the fluorescence intensity of mRNA and RiboGreen. Combined with the total amount of mRNA in the added nanoparticle solution, the loading efficiency of LPH on mRNA can be calculated. The test results of the loading efficiency of LPH on mRNA prepared by each polymer carrier are summarized in Fig.13 .

[0083] Example 9: In vivo mRNA delivery effect test of LPH

[0084] The synthesized polymer carrier PBAE was dissolved in anhydrous ethanol with DOTAP, DOPE, cholesterol, and PEG2000-DMG. The concentration of each polymer carrier in anhydrous ethanol was 20 g / L, and the molar ratio of the five was PBAE:DOTAP:DOPE:Chol:PEG2000-DMG=40:10:10:38.5:1.5. Luciferase mRNA (Fluc mRNA) was dissolved in sodium citrate solution (10 mM, pH=4.2). The volume ratio of ethanol solution and sodium citrate solution (10 mM, pH=4.2) was controlled to be 1:1.

[0085] The mass ratio of (DOTAP+PBAE) to luciferase mRNA (Fluc mRNA) was about 20:1. After incubation, the solution was diluted 5 times with PBS to obtain a composite nanoparticle solution (each liter of composite nanoparticle solution contained 50 mg of luciferase mRNA).

[0086] Naked mRNA group: Luciferase mRNA (Fluc mRNA) was dissolved in sodium citrate solution (10 mM, pH = 4.0), and diluted with PBS after incubation to obtain mRNA nanoparticle solution (each liter of nanoparticle solution contained 50 mg of luciferase mRNA).

[0087] The nanoparticle solution prepared by the above polymer molecule experimental group or naked mRNA group was used to select 6-week-old female BALB / c mice weighing about 20g, and the mRNA injection dose was 0.5mg / kg. The injection volume of each mouse was 0.2mL of composite nanoparticle solution. Under this condition, the in vivo mRNA delivery effect was tested. The composite nanoparticle solution or mRNA nanoparticle solution formed by the corresponding lipid molecule and mRNA was injected into the mouse through the tail vein, and the expression efficiency of luciferase in the mouse was detected by a small animal imaging instrument 6 hours after administration.

[0088] According to the above process, when the polymer carriers are A7-2C4, A7-2C6, A7-2C8, A8-C8', A8-2C8, A9-2C10, A13-C8', and A15-C12', the expression results of luciferase in mice are shown in Figure 2. Fig.14As shown. Fig.14 It can be seen that 6 hours after the injection of 9 hybrid nanoparticle solutions, most of the mice had fluorescence expression of varying intensities, among which the LPH made from the polymer molecule A13C8' showed a strong delivery effect in mice.

[0089] According to the above process, when the injected drug is a naked mRNA nanoparticle solution, the expression results of luciferase in mice are shown in Fig.14 As shown. Fig.14 It can be seen that there was no expression of luciferase after naked mRNA was injected into the tail vein of mice.

[0090] Example 10: Distribution of LPH in organs in vivo

[0091] After 6 hours of the in vivo mRNA delivery effect test of LPH according to Example 9, the mice in the LPH experimental group and the naked mRNA group were dissected and their organs were imaged (the organs dissected were liver, spleen, lung, heart and kidney, respectively). The expression results of luciferase in each organ of the mice are shown in the figure. Fig.15 .according to Fig.15 As a result, A7-2C4, A7-2C6, A7-2C8, A8-C8', A8-2C8, A9-2C10, A13-C8', and A15-C12' synthesized in Examples 1-6 of the present invention can deliver mRNA to the lungs and spleen to express a large amount of luciferase.

[0092] The contents described in this specification are merely an enumeration of implementation forms of the inventive concept, and the protection scope of the present invention should not be regarded as being limited to the specific forms described in the embodiments.

[0093] Example 11: Verification of DOTAP-promoted cellular uptake in LPH

[0094] The synthesized polymer carrier A7-2C10 was dissolved in anhydrous ethanol with DOTAP, DOPE, cholesterol and PEG2000-DMG. The solubility concentration of the polymer carrier A7-2C10 in ethanol was 1 g / L. The molar ratio of the five was (DOTAP+polymer carrier A7-2C10):DOPE:Chol:PEG2000-DMG=50:10:38.5:1.5, wherein the molar ratios of DOTAP and polymer carrier A7-2C10 were set to 1:1, 4:1 and 8:1, respectively. The mass ratio of (DOTAP+polymer carrier A7-2C10) and luciferase mRNA (Fluc mRNA) was about 20:1. The prepared composite nanoparticles LPH were recorded as D / P1-1, D / P4-1 and D / P8-1, respectively.

[0095] The polymer nanoparticles prepared by the mass ratio of the single polymer A7-2C10 to mRNA of 20:1 were recorded as PBAE. LPH without DOTAP was recorded as DOT0, wherein the molar ratio of A7-2C10, DOPE, cholesterol, and PEG2000-DM was A7-2C10:DOPE:Chol:PEG2000-DMG=50:10:38.5:1.5. The other preparation conditions were according to the method described in Example 7.

[0096] The particle size and surface potential of the composite nanoparticles were measured by dynamic light scattering (DLS). The particle size potential of LPH under each formulation was measured as follows: Fig.16 ,The results showed that the incorporation of auxiliary lipids such as DOTAP effectively increased the surface charge of nanoparticles.

[0097] The cellular uptake of Cy5-mRNA-composite nanoparticles was analyzed by fluorescence microscopy and flow cytometry. The composite nanoparticle solution was prepared according to the above method, with the only difference being "using Cy5-mRNA (i.e., Cy5-labeled mRNA) instead of luc mRNA", and other conditions remained unchanged. The prepared LPH was recorded as Cy5-mRNA-composite nanoparticles.

[0098] IGROV 1 cells were seeded in a 6-well plate at a density of 100,000 cells / well. After culturing for 24 hours, 2 mL of fresh DMEM medium was replaced. The above five Cy5-mRNA-loaded composite nanoparticle solutions were added at a dose of 150 μL per well (dose of 250 ng mRNA / well). After incubation for 2 hours or 6 hours, the DMEM medium was removed, the plates were washed with PBS, and 1 mL of 4% paraformaldehyde was added for fixation for 30 minutes. After removing the fixative, the plates were washed with PBS, and DAPI (10 μg / mL) was added for staining for 15 minutes. The plates were washed with PBS, and observed and photographed under a fluorescence microscope. The results are shown in Fig.17 As shown, the Cy5 fluorescence signal was stronger after treatment with DOTAP-incorporated LPH.

[0099] IGROV 1 cells were seeded in 6-well plates at a density of 300,000 cells / well. After culturing for 24 hours, 2 mL of fresh DMEM medium was replaced. Cy5-mRNALPH (250 ng mRNA / well) was added at a dose of 150 μL per well. After 6 hours of incubation after administration, the cells were collected by digestion and centrifugation and resuspended in PBS. Fluorescence histograms were recorded using a flow cytometer and data were processed and analyzed using FlowJo software. The results are shown in Figure 2. Fig.18 As shown, the average Cy5 fluorescence signal of cells treated with DOTAP-incorporated LPH was higher, and the proportion of Cy5 signal-positive cells was higher.

Claims

1. A method for preparing a polymer for mRNA delivery, characterized in that The following steps are involved: 1) Using 1,6-hexanediol diacrylate DAHE and hydrophilic amine as raw materials, heating and dissolving at 80-95°C for 40-60h, washing and drying after the reaction to obtain a precursor polymer with acrylates at both ends; wherein the hydrophilic amine raw material is one of A7, A8, A9, A13, and A15: 2) using a hydrophobic amine to end-cap the precursor polymer with acrylates at both ends obtained in step 1), wherein the precursor polymer and the hydrophobic amine are stirred and reacted in an organic solvent at a reaction temperature of 50-65° C. for a reaction time of 20-55 hours, and then dried to obtain an end-capped final product, which is recorded as polymer PBAE; wherein the hydrophobic amine raw material is one of 2C4, 2C6, 2C8, 2C10, C8', and C12':

2. A method for preparing a polymer for mRNA delivery as claimed in claim 1, characterized in that In step 1), the molar ratio of DAHE to hydrophilic amine is 0.8-1.5:1, preferably 1-1.1:1; the reaction temperature of step 1) is 85-90° C., and the reaction time is 45-50 h.

3. The method for preparing a polymer for mRNA delivery according to claim 1, characterized in that In step 2), the molar ratio of the precursor polymer to the hydrophobic amine is 1:3-5, preferably 1:4, the reaction temperature is 55-60°C, and the reaction time is 45-50h; In step 2), the organic solvent is tetrahydrofuran, and the concentration of the hydrophobic amine in the organic solvent is 0.01-0.1 mol / L, preferably 0.03-0.0625 mol / L.

4. A polymer for mRNA delivery prepared by the method according to any one of claims 1 to 3, characterized in that: Its molecular weight is between 1.5kDa and 37kDa, and its degree of polymerization is between 10 and 52.

5. A method for preparing lipid / polymer hybrid nanoparticles, characterized in that The following steps are involved: S1: dissolving luciferase mRNA in an acidic solution to obtain a first solution; S2: dissolving the polymer described in claim 4 and auxiliary lipids cholesterol, DOPE, PEG2000-DMG, and DOTAP in anhydrous ethanol respectively, and obtaining a second solution by mixing the above five components; S3: mixing the first solution and the second solution to obtain a mixed solution, and incubating the mixed solution on a shaking table; S4: The mixed solution after incubation is diluted with sterile PBS to obtain a suspension containing the prepared lipid / polymer hybrid nanoparticles.

6. The method for preparing lipid / polymer hybrid nanoparticles according to claim 5, characterized in that In step S1, the acidic solution is a sodium citrate solution, 10 mM, pH = 4.

2.

7. The method for preparing lipid / polymer hybrid nanoparticles according to claim 5, characterized in that In step S2, The molar ratio of polymer to cholesterol is 1:0.8-1.2, preferably 1:0.9-1.0; The molar ratio of polymer to DOPE is 1:0.2-0.3, preferably 1:0.25; The molar ratio of polymer to DOTAP is 1:0.2-0.3, preferably 1:0.25; The molar ratio of polymer to PEG2000-DMG is 1:0.02-0.05, preferably 1:0.035-0.04; Wherein, the mass concentration of the polymer dissolved in anhydrous ethanol in step S2 is 0.5-2 g / L, preferably 1 g / L; The total mass of the polymer and DOTAP in the second solution of step S2 is 15-25 times, preferably 20 times, the mass of the luciferase mRNA in the first solution of step S1.

8. The method for preparing lipid / polymer hybrid nanoparticles according to claim 5, characterized in that In step S3, the shaking incubation time is 0.5 to 1.5 hours. In step S4, the mixed solution after incubation is diluted with PBS by 4 to 6 times. The content of organic phase ethanol in the diluted solution is not higher than 10%.

9. A lipid / polymer hybrid nanoparticle prepared according to any one of claims 5 to 8.

10. Use of a lipid / polymer hybrid nanoparticle as described in claim 9 in the preparation of an mRNA vaccine drug.

Citation Information

Patent Citations

  • Cationic lipid molecule for mRNA delivery and preparation method and application thereof

    CN115073345A

  • Cationic lipid compound as well as composition and application thereof

    CN116730857A

  • Tissue selective single-component mRNA delivery carrier and delivery system

    CN117479964A

  • Star-shaped poly (beta-amino ester) taking polyamine as core, composite nanoparticle based on star-shaped poly (beta-amino ester) and preparation method and application of star-shaped poly (beta-amino ester)

    CN117736435A

  • Biodegradable poly(beta-amino esters) and uses thereof

    US20040071654A1