Modified polypropylene composite material and preparation method thereof

Through the preparation of modified polypropylene composite materials, the problems of poor light and thermal stability of PVC Teslin mesh and resource waste have been solved, and a polypropylene yarn covering material with excellent performance and environmental protection has been realized, which is suitable for a variety of application scenarios. Meets environmental protection requirements and reduces resource waste.

CN118755191AInactive Publication Date: 2024-10-11DONGGUAN PRIDE NEW MATERIALS CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410926504.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-11
Publication Date
2024-10-11
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing PVC Teslin mesh has poor stability to light and heat, is easily decomposed to produce harmful substances, has reduced physical and mechanical properties, has a short service life, and produces carcinogens when recycled and incinerated, resulting in serious waste of resources and failing to meet environmental protection requirements.

Method used

It is made of modified polypropylene composite material, which is made of polypropylene, nano-calcium carbonate, stearate, ethylene-butylene polymer and other raw materials. It is prepared by activating nano-calcium carbonate and mixed material twin-screw extrusion process to achieve high performance. Excellent polypropylene yarn covering material with good photothermal stability and degradability.

Benefits of technology

A high-performance alternative to PVC products made of polypropylene composite materials has been achieved. It has good toughness and appearance, is suitable for outdoor and indoor applications, supports recycling, meets environmental protection standards, reduces resource waste, and expands market applicability.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a modified polypropylene composite material, which is prepared from the following raw materials in parts by weight: 40 to 65 parts of polypropylene, 10 to 20 parts of nano calcium carbonate, 0.5 to 2 parts of stearate, 10 to 35 parts of ethylene-butylene high polymer, 10 to 35 parts of separation and diffusion oil agent, 0.1 to 3 parts of titanium dioxide, 0.1 to 1.2 parts of antioxidant, 0.5 to 3 parts of light stabilizer, 0.3 to 5 parts of ultraviolet absorbent, 2 to 5 parts of scratch-resistant agent and 2 to 5 parts of coupling agent. And 10-12 parts of a metallocene catalyst. A PVC (polyvinyl chloride) material used in the prior art is replaced, a polypropylene raw material is adopted, a PVC mesh product which is excellent in performance and capable of completely replacing the mainstream PVC mesh product in the current market is produced after a modification process, polypropylene yarns can be coated, the consistency of the material is achieved, a huge market space is provided for later recycling, and resource waste is avoided.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polymer materials, and in particular to a modified polypropylene composite material and a preparation method thereof. Background Art

[0002] The existing market products are also called Teslin mesh, which is made of PVC (polyvinyl chloride) resin coated with a high-strength PET yarn, stretched and rolled, and later woven into meshes of different colors and patterns on a loom for use in indoor and outdoor furniture and various home decoration and outdoor products. However, PVC (polyvinyl chloride) has poor stability to light and heat, is easy to decompose to produce hydrogen chloride, and further autocatalytic decomposition, causing color change, and the physical and mechanical properties also drop rapidly. It is necessary to add stabilizers and other materials to improve the stability to light and heat, and a large amount of plasticizers are also needed to improve the softness and elasticity. The colorability is not good and it is easy to scale. As a result, the product has a short service life, and surface precipitation and discoloration often occur in the later stage. The production process is also difficult to control. Especially when it is recycled and incinerated in the later stage, a large amount of dioxin carcinogens are produced. Therefore, on October 27, 2017, the World Health Organization's International Agency for Research on Cancer has already listed polyvinyl chloride as a Class 3 carcinogen. Moreover, the softening point of PVC (polyvinyl chloride) resin is low, and it is not suitable for high temperature environment for long-term use. Its cold resistance is also poor, and it is prone to yellowing and brittleness.

[0003] In the existing technology, the yarn density of PVC (polyvinyl chloride) and PET reaches 1.4g / cm 3 The above mentioned, excessive weight, has greatly increased the difficulty of subsequent production, processing, transportation and construction. The finished PVC (polyvinyl chloride) coated PET yarn products have no advantages in terms of recyclability due to the high degree of compounding of the two materials and cannot be separated, and cannot be naturally degraded or granulated for reuse. They can only be landfilled or incinerated, and the waste of resources also causes great pollution to the society. They seriously fail to meet the standards of the relevant domestic and foreign plastic bans, and cannot meet the modern international requirements.

[0004] Therefore, the existing PVC (polyvinyl chloride) Textilene mesh products have great shortcomings in the manufacture of placemats, wall coverings, curtains, etc. They cannot come into contact with the skin, let alone food. It takes a lot of time and effort to improve the physical properties, but with little success. Many products with environmental protection requirements cannot be involved, and the market has great limitations. Summary of the invention

[0005] In order to solve the above technical problems, the present invention provides a modified polypropylene composite material and a preparation method thereof.

[0006] The purpose of the present invention can be achieved through the following technical solutions:

[0007] A modified polypropylene composite material is prepared from the following raw materials in parts by weight: 40-65 parts of polypropylene, 10-20 parts of nano calcium carbonate, 0.5-2 parts of stearate, 10-35 parts of ethylene-butene polymer, 10-35 parts of separation and diffusion oil, 0.1-3 parts of titanium dioxide, 0.1-1.2 parts of antioxidant, 0.5-3 parts of light stabilizer, 0.3-5 parts of ultraviolet absorber, 2-5 parts of anti-scratch agent, 2-5 parts of coupling agent and 10-12 parts of metallocene catalyst.

[0008] Furthermore, the stearate is a mixture of one or more of sodium stearate, magnesium stearate and calcium stearate in any proportion.

[0009] Furthermore, the separation and diffusion oil agent is toluene.

[0010] Furthermore, the antioxidant is antioxidant 1010 or antioxidant 168.

[0011] Furthermore, the light stabilizer is light stabilizer 119 or light stabilizer 292.

[0012] Furthermore, the ultraviolet absorber is a mixture of one or more of salicylate phenyl ester, ultraviolet absorber UV-P and ultraviolet absorber UV-O in any proportion.

[0013] Furthermore, the anti-scratch agent is SR-100 (BASF).

[0014] Furthermore, the coupling agent is a mixture of one or more of KH550, KH560 and KH570 in any proportion.

[0015] A method for preparing a modified polypropylene composite material comprises the following steps:

[0016] Step 1: Activate nano calcium carbonate: Add nano calcium carbonate and stearate into a high-speed mixer, heat to 120-125°C, stir at high speed for 2 hours, then cool to 85°C, continue stirring for 2 hours to obtain activated nano calcium carbonate;

[0017] Step 2: Add polypropylene and ethylene-butene polymer into a mixing barrel, stir evenly, add separation and diffusion oil, stir evenly, add metallocene catalyst, titanium dioxide, coupling agent, anti-scratch agent in sequence, stir evenly, and obtain a mixture;

[0018] The third step is to mix the prepared mixed material with activated nano-calcium carbonate, add the remaining raw materials, stir evenly, and then feed it into a twin-screw extruder, extrude and granulate at 200-220°C to obtain a modified polypropylene composite material.

[0019] Beneficial effects of the present invention:

[0020] The present invention prepares a modified polypropylene composite material, which replaces the PVC material used in the prior art. The polypropylene raw material is used and a product with excellent performance is produced after a modification process. The product can completely replace the mainstream PVC mesh product in the current market, and can be coated with polypropylene yarn to achieve material consistency, thereby providing a huge market space for later recycling and eliminating resource waste.

[0021] The present invention adopts degradable polypropylene raw material modification, has stable performance, is non-toxic, and greatly improves toughness and appearance. Flame retardant, antistatic, waterproof and other additives can also be added as needed to blend production to meet different process requirements.

[0022] The present invention adds an anti-aging additive to fully meet outdoor weather resistance requirements, and the weather resistance time period can be adjusted according to process requirements, greatly improving the market applicability of the product.

[0023] The present invention has a wide range of applicable temperatures, and can be used at temperatures between -40 and 140°C. It has no precipitation at high temperatures, no brittleness at low temperatures, no color change, and can ensure various normal physical and chemical indicators.

[0024] The density of the present invention is only 0.86-0.92g / cm 3 The great lightness makes the product have great advantages in production, weaving, transportation and finished products, greatly reduces the intensity of manual operation and maximizes the utilization of materials.

[0025] The products produced by the present invention can be recycled and reused, and can also be combined with polypropylene yarn to produce mesh products, which can be recycled and reused, and can also be in skin contact or naturally degraded in nature. They meet domestic and international environmental protection requirements and meet various standards of the plastic ban, greatly eliminating the waste of resources and bringing relatively objective economic benefits to society.

[0026] Moreover, the polypropylene composite material prepared by the present invention can be mixed with the required masterbatch, and the polypropylene composite material or polyester high-strength yarn is coated by screw extrusion, and different specifications of outer diameters are produced according to process requirements. After later weaving, weather-resistant outdoor textilene mesh fabrics are produced, which are widely used in outdoor furniture, carpets, wall coverings, placemats and other fields.

[0027] The prepared composite material can also be mixed with the required masterbatch, directly extruded by screw, drawn, shaped and rolled into shape, stretched into different shapes and outer diameters according to process requirements, and then woven into weather-resistant mesh products, or used in the field of indoor and outdoor decorative building materials, with a wider range of applications.

[0028] The manufactured composite materials can be processed by injection molding to produce products with high impact resistance, high toughness and high weather resistance, which are widely used in the automotive industry, such as wire coil floor mats, bumpers, interior fillings, etc. DETAILED DESCRIPTION

[0029] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0030] Example 1

[0031] A modified polypropylene composite material is prepared from the following raw materials in parts by weight: 40 parts of polypropylene, 10 parts of nano calcium carbonate, 0.5 parts of stearate, 10 parts of ethylene-butene polymer, 10 parts of separation and diffusion oil, 0.1 parts of titanium dioxide, 0.1 parts of antioxidant, 0.5 parts of light stabilizer, 0.3 parts of ultraviolet absorber, 2 parts of anti-scratch agent, 2 parts of coupling agent and 10 parts of metallocene catalyst.

[0032] The stearate is sodium stearate.

[0033] The separation and diffusion oil agent is toluene.

[0034] The antioxidant is antioxidant 1010.

[0035] The light stabilizer is light stabilizer 119.

[0036] The ultraviolet absorber is phenyl salicylate.

[0037] The anti-scratch agent is SR-100 (BASF).

[0038] The coupling agent is KH550.

[0039] A method for preparing a modified polypropylene composite material comprises the following steps:

[0040] Step 1: Activate nano calcium carbonate: Add nano calcium carbonate and stearate into a high-speed mixer, heat to 120°C, stir at high speed for 2 hours, then cool to 85°C, continue stirring for 2 hours to obtain activated nano calcium carbonate;

[0041] Step 2: Add polypropylene and ethylene-butene polymer into a mixing barrel, stir evenly, add separation and diffusion oil, stir evenly, add metallocene catalyst, titanium dioxide, coupling agent, anti-scratch agent in sequence, stir evenly, and obtain a mixture;

[0042] The third step is to mix the prepared mixture with activated nano-calcium carbonate, add the remaining raw materials, stir evenly, and then feed it into a twin-screw extruder, extrude and granulate at 200° C. to obtain a modified polypropylene composite material.

[0043] Example 2

[0044] A modified polypropylene composite material is prepared from the following raw materials in parts by weight: 50 parts of polypropylene, 15 parts of nano calcium carbonate, 1 part of stearate, 20 parts of ethylene-butene polymer, 25 parts of separation and diffusion oil, 2 parts of titanium dioxide, 1 part of antioxidant, 2 parts of light stabilizer, 3 parts of ultraviolet absorber, 3 parts of anti-scratch agent, 3 parts of coupling agent and 10 parts of metallocene catalyst.

[0045] The stearate is magnesium stearate.

[0046] The separation and diffusion oil agent is toluene.

[0047] The antioxidant is antioxidant 168.

[0048] The light stabilizer is light stabilizer 292.

[0049] The ultraviolet absorber is an ultraviolet absorber UV-P.

[0050] The anti-scratch agent is SR-100 (BASF).

[0051] The coupling agent is KH560.

[0052] A method for preparing a modified polypropylene composite material comprises the following steps:

[0053] Step 1: Activate nano calcium carbonate: Add nano calcium carbonate and stearate into a high-speed mixer, heat to 125°C, stir at high speed for 2 hours, then cool to 85°C, continue stirring for 2 hours to obtain activated nano calcium carbonate;

[0054] Step 2: Add polypropylene and ethylene-butene polymer into a mixing barrel, stir evenly, add separation and diffusion oil, stir evenly, add metallocene catalyst, titanium dioxide, coupling agent, anti-scratch agent in sequence, stir evenly, and obtain a mixture;

[0055] The third step is to mix the prepared mixture with activated nano-calcium carbonate, add the remaining raw materials, stir evenly, and then feed it into a twin-screw extruder, extrude and granulate at 220° C. to obtain a modified polypropylene composite material.

[0056] Example 3

[0057] A modified polypropylene composite material is prepared from the following raw materials in parts by weight: 65 parts of polypropylene, 20 parts of nano calcium carbonate, 2 parts of stearate, 35 parts of ethylene-butene polymer, 35 parts of separation and diffusion oil, 3 parts of titanium dioxide, 1.2 parts of antioxidant, 3 parts of light stabilizer, 5 parts of ultraviolet absorber, 5 parts of anti-scratch agent, 5 parts of coupling agent and 12 parts of metallocene catalyst.

[0058] The stearate is calcium stearate.

[0059] The separation and diffusion oil agent is toluene.

[0060] The antioxidant is antioxidant 1010.

[0061] The light stabilizer is light stabilizer 119.

[0062] The ultraviolet absorber is an ultraviolet absorber UV-O.

[0063] The anti-scratch agent is SR-100 (BASF).

[0064] The coupling agent is KH570.

[0065] A method for preparing a modified polypropylene composite material comprises the following steps:

[0066] Step 1: Activate nano calcium carbonate: Add nano calcium carbonate and stearate into a high-speed mixer, heat to 125°C, stir at high speed for 2 hours, then cool to 85°C, continue stirring for 2 hours to obtain activated nano calcium carbonate;

[0067] Step 2: Add polypropylene and ethylene-butene polymer into a mixing barrel, stir evenly, add separation and diffusion oil, stir evenly, add metallocene catalyst, titanium dioxide, coupling agent, anti-scratch agent in sequence, stir evenly, and obtain a mixture;

[0068] The third step is to mix the prepared mixture with activated nano-calcium carbonate, add the remaining raw materials, stir evenly, and then feed it into a twin-screw extruder, extrude and granulate at 220° C. to obtain a modified polypropylene composite material.

[0069] The above contents are merely examples and explanations of the concept of the present invention. The technicians in this technical field may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the concept of the invention or exceed the scope defined by the claims, they should all fall within the protection scope of the present invention.

Claims

1. A modified polypropylene composite material, characterized in that: The invention is prepared from the following raw materials in parts by weight: 40-65 parts of polypropylene, 10-20 parts of nano calcium carbonate, 0.5-2 parts of stearate, 10-35 parts of ethylene-butene polymer, 10-35 parts of separation and diffusion oil agent, 0.1-3 parts of titanium dioxide, 0.1-1.2 parts of antioxidant, 0.5-3 parts of light stabilizer, 0.3-5 parts of ultraviolet absorber, 2-5 parts of anti-scratch agent, 2-5 parts of coupling agent and 10-12 parts of metallocene catalyst.

2. A modified polypropylene composite material according to claim 1, characterized in that: The stearate is a mixture of one or more of sodium stearate, magnesium stearate and calcium stearate in any proportion.

3. A modified polypropylene composite material according to claim 1, characterized in that: The separation and diffusion oil agent is toluene.

4. The modified polypropylene composite material according to claim 1, characterized in that: The antioxidant is antioxidant 1010 or antioxidant 168.

5. The modified polypropylene composite material according to claim 1, characterized in that: The light stabilizer is light stabilizer 119 or light stabilizer 292.

6. The modified polypropylene composite material according to claim 1, characterized in that: The ultraviolet absorber is a mixture of one or more of salicylate phenyl ester, ultraviolet absorber UV-P and ultraviolet absorber UV-O in any proportion.

7. The modified polypropylene composite material according to claim 1, characterized in that: The anti-scratch agent is SR-100.

8. The modified polypropylene composite material according to claim 1, characterized in that: The coupling agent is a mixture of one or more of KH550, KH560 and KH570 in any proportion.

9. The method for preparing a modified polypropylene composite material according to claim 1, characterized in that: The steps include: Step 1: Activate nano calcium carbonate: Add nano calcium carbonate and stearate into a high-speed mixer, heat to 120-125°C, stir at high speed for 2 hours, then cool to 85°C, continue stirring for 2 hours to obtain activated nano calcium carbonate; Step 2: Add polypropylene and ethylene-butene polymer into a mixing barrel, stir evenly, add separation and diffusion oil, stir evenly, add metallocene catalyst, titanium dioxide, coupling agent, anti-scratch agent in sequence, stir evenly, and obtain a mixture; The third step is to mix the prepared mixed material with activated nano-calcium carbonate, add the remaining raw materials, stir evenly, and then feed it into a twin-screw extruder, extrude and granulate at 200-220°C to obtain a modified polypropylene composite material.

Citation Information

Patent Citations

  • Composite material for vehicle bumper and preparation method thereof

    CN102219959A

  • Easy-to-clean scratch-resistant composite PP material with three-dimensional flickering effect, and preparation method thereof

    CN111087699A

  • Low-warpage, scratch-resistant and soft-touch modified polypropylene composite material and preparation method thereof

    CN114316434A