High-barrier PBAT material and preparation method and application thereof

By adding polydioxanone and isocyanate with a specific viscosity average molecular weight into the PBAT material, a cross-linked network structure is formed, which solves the problem of insufficient barrier properties of traditional PBAT materials and obtains high barrier, excellent mechanical and degradable properties. PBAT material is suitable for a variety of packaging and agricultural mulch films.

CN118755237APending Publication Date: 2024-10-11HENAN TECHUANG BIOTECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410936168.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-12
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Traditional PBAT materials have deficiencies in barrier properties, making it difficult to improve barrier properties while maintaining mechanical properties and degradability.

Method used

By adding a mixture of polydioxanone with a viscosity average molecular weight of 200,000-300,000 and polydioxanone with a viscosity average molecular weight of 600,000-700,000 into PBAT, and controlling the addition amount within a certain proportion, the combination Isocyanate forms a cross-linked network structure to prepare high-barrier PBAT materials.

Benefits of technology

A PBAT material with excellent air/water barrier properties, mechanical properties and degradability has been obtained. It is suitable for food packaging, pharmaceutical packaging, cosmetic packaging and agricultural mulch films. The water vapor transmission rate is <300g/m2·24h, and the oxygen transmission rate is <10cc/m2·24h·0.1MPa, tensile strength>45MPa, elongation at break>580%.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004941394050000051
    Figure BDA0004941394050000051
  • Figure BDA0004941394050000071
    Figure BDA0004941394050000071
Patent Text Reader

Abstract

The invention relates to the technical field of functional polymer materials, and particularly discloses a high-barrier PBAT material and a preparation method and application thereof. The high-barrier PBAT material provided by the invention is prepared from the following components in parts by weight: 40 to 48 parts of PBAT, 10 to 15 parts of poly (p-dioxanone), 5 to 10 parts of a barrier material and 1 to 2 parts of a compatilizer, the poly (p-dioxanone) is a mixture of poly (p-dioxanone) with the viscosity average molecular weight of 200,000-300,000 and poly (p-dioxanone) with the viscosity average molecular weight of 600,000-700,000; the invention also provides a preparation method of the high-barrier PBAT material, and the preparation method comprises the following steps: weighing the high-barrier PBAT material according to the weight parts, uniformly mixing, and then carrying out melt extrusion at 165 + / -5 DEG C to prepare the high-barrier PBAT material. The high-barrier PBAT material provided by the invention is good in gas / water barrier property, excellent in mechanical property and excellent in degradability, and has a very good application prospect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of functional polymer materials, and in particular to a high-barrier PBAT material and a preparation method and application thereof. Background Art

[0002] With the improvement of environmental awareness, biodegradable materials are increasingly used in packaging, agriculture and other fields. PBAT (polybutylene adipate terephthalate) is a biodegradable material with good ductility, elongation at break, heat resistance and impact resistance. However, traditional PBAT materials have certain deficiencies in barrier properties, which limits their application in certain occasions with high barrier requirements.

[0003] At present, there are many methods to improve the barrier properties of PBAT materials. For example, related studies have reported a method of adding inorganic or organic barrier fillers to PBAT, but the above method often leads to a decrease in the mechanical properties or processing properties of the material; there are also documents that point out that the barrier properties of PBAT materials can be improved by blending PBAT with other polymer barrier materials, but the resulting PBAT materials have poor degradability. Therefore, the existing methods for improving the barrier properties of PBAT materials are difficult to maintain other properties while improving the barrier properties of PBAT materials. Summary of the invention

[0004] In order to improve the barrier properties of PBAT materials while maintaining their mechanical properties and degradability, the present application provides a high-barrier PBAT material.

[0005] In the first aspect, the present application provides a high barrier PBAT material, which adopts the following technical solution:

[0006] A high barrier PBAT material comprises the following components in parts by weight: 40-48 parts of PBAT, 10-15 parts of polydioxanone, 5-10 parts of barrier material and 1-2 parts of compatibilizer;

[0007] The polydioxanone is a mixture of polydioxanone with a viscosity average molecular weight of 200,000-300,000 and polydioxanone with a viscosity average molecular weight of 600,000-700,000.

[0008] The present application uses PBAT, polydioxanone and barrier materials to prepare a high-barrier PBAT material. By controlling the addition amount of each component and the viscosity-average molecular weight of polydioxanone within the above range, the obtained PBAT material has excellent air / water barrier properties, mechanical properties and degradability, and can meet the performance and environmental protection requirements of food packaging, pharmaceutical packaging, cosmetic packaging and agricultural mulch.

[0009] In the present application, polydioxanone is an aliphatic polyether ester, the ester bond in its structure gives it good biocompatibility and biodegradability, and the ether bond in its structure gives it good flexibility, so polydioxanone is usually used for biological suture materials. The inventors of the present application have found through experimental research that adding polydioxanone to PBAT and controlling the addition amount and viscosity-average molecular weight of polydioxanone within the above range can improve the barrier properties of PBAT materials to air and water on the one hand, and significantly improve the toughness and plasticity of PBAT materials on the other hand, thereby obtaining a PBAT material with excellent comprehensive performance in barrier properties, mechanical properties and biodegradability.

[0010] Optionally, the weight ratio of the polydioxanone having a viscosity average molecular weight of 200,000-300,000 to the polydioxanone having a viscosity average molecular weight of 600,000-700,000 is 10:(2-4.5).

[0011] In the present application, the molecular weight and ratio of polydioxanone will affect the gas / water barrier properties and mechanical properties of the PBAT material. The inventors of the present application have found through experimental research that by further controlling the viscosity-average molecular weight and ratio of polydioxanone within the above range, the comprehensive performance of the gas / water barrier properties, mechanical properties and biodegradability of the obtained PBAT material is better.

[0012] In some embodiments, the weight ratio of the polydioxanone having a viscosity average molecular weight of 200,000-300,000 to the polydioxanone having a viscosity average molecular weight of 600,000-700,000 can be 10:(2-3), 10:(2-4.5), 10:(2-5), 10:(3-4.5), 10:(3-5) or 10:(4.5-5).

[0013] In a specific embodiment, the weight ratio of the polydioxanone with a viscosity average molecular weight of 200,000-300,000 to the polydioxanone with a viscosity average molecular weight of 600,000-700,000 can also be 1:1, 1:2, 10:2, 10:3, 10:4.5 or 10:5.

[0014] Optionally, the high barrier PBAT material further includes 2-6 parts of isocyanate.

[0015] In the present application, by adding isocyanate to the high barrier PBAT material, the isocyanate can react with PBAT, compatibilizer, etc. to form a cross-linked network structure. The cross-linked network structure can, on the one hand, enhance the isolation effect against air and water, and on the other hand, improve the mechanical properties of the PBAT material, thereby further improving the water vapor barrier and mechanical properties of the PBAT material.

[0016] In a specific embodiment, the weight portion of isocyanate in the high barrier PBAT material is 3 parts.

[0017] Optionally, the isocyanate is selected from L-lysine diisocyanate, L-lysine triisocyanate, isophorone diisocyanate, hexamethylene diisocyanate and 3,3'-dichlorobiphenyl-4,4'-diisocyanate.

[0018] Optionally, the isocyanate is a mixture of L-lysine triisocyanate and 3,3'-dichlorobiphenyl-4,4'-diisocyanate, and the weight ratio of the L-lysine triisocyanate to the 3,3'-dichlorobiphenyl-4,4'-diisocyanate is 1:(0.18-0.43).

[0019] In some embodiments, the isocyanate is a mixture of L-lysine triisocyanate and 3,3'-dichlorobiphenyl-4,4'-diisocyanate, a mixture of isophorone diisocyanate and 3,3'-dichlorobiphenyl-4,4'-diisocyanate, or a mixture of L-lysine triisocyanate and isophorone diisocyanate.

[0020] In some embodiments, the weight ratio of L-lysine triisocyanate to 3,3'-dichlorobiphenyl-4,4'-diisocyanate may be 1:(0.18-0.25), 1:(0.18-0.3), 1:(0.18-0.43), 1:(0.25-0.3), 1:(0.25-0.43) or 1:(0.3-0.43).

[0021] In a specific embodiment, the weight ratio of the L-lysine triisocyanate to 3,3'-dichlorobiphenyl-4,4'-diisocyanate may also be 1:0.18, 1:0.25, 1:0.3 or 1:0.43.

[0022] Optionally, the barrier material is selected from polyvinylidene chloride, ethylene-vinyl alcohol copolymer, mica, aluminum oxide and titanium oxide;

[0023] Optionally, the compatibilizer is selected from epoxy type, carboxyl type, imide type and oxazoline type.

[0024] In a specific embodiment, the barrier material is ethylene-vinyl alcohol copolymer and mica in a weight ratio of 1:2.

[0025] Optionally, the high barrier PBAT material also includes one or more of a plasticizer, a dispersant and a stabilizer.

[0026] In a second aspect, the present application provides a method for preparing a high barrier PBAT material.

[0027] A method for preparing a high-barrier PBAT material comprises the following steps: weighing each component of the high-barrier PBAT material in parts by weight, mixing them uniformly, and then melt-extruding them at 165±5° C. to obtain the high-barrier PBAT material.

[0028] On the third aspect, the high barrier PBAT material of the present application is used in food packaging, pharmaceutical packaging, cosmetic packaging and agricultural mulch film.

[0029] The high-barrier PBAT material provided in the present application has good air / water barrier properties, good mechanical properties, and excellent degradability, and therefore can be used for food packaging, pharmaceutical packaging, cosmetic packaging, and agricultural mulch, and has good application prospects.

[0030] In summary, this application has the following beneficial effects:

[0031] 1. The present application prepares a PBAT material with excellent comprehensive performance in barrier properties, mechanical properties and biodegradability by adding polydioxanone of a certain viscosity molecular weight to the PBAT material. The high barrier PBAT material can be used to prepare food packaging, pharmaceutical packaging, cosmetic packaging and agricultural mulch, and has good application prospects.

[0032] 2. In this application, the weight ratio of polydioxanone with a viscosity average molecular weight of 200,000-300,000 to polydioxanone with a viscosity average molecular weight of 600,000-700,000 is controlled within the range of 10: (2-4.5), and the gas-water barrier and mechanical properties of the prepared PBAT material are better, and its water vapor permeability is <300g / m 2 24h, oxygen transmission rate <10cc / m 2 ·24h·0.1MPa, tensile strength is>45MPa, elongation at break is>580%.

[0033] 3. In this application, by adding isocyanate to the PBAT material, the gas and water barrier and mechanical properties of the high barrier PBAT material are further improved, and its water vapor permeability is less than 270g / m 2 24h, oxygen transmission rate <9cc / m 2 ·24h·0.1MPa, tensile strength is>49MPa, elongation at break is>600%. DETAILED DESCRIPTION

[0034] The present application provides a high barrier PBAT material, comprising the following components in parts by weight: 40-48 parts of PBAT, 10-15 parts of polydioxanone, 5-10 parts of barrier material, 1-2 parts of compatibilizer and 1-2 parts of dispersant.

[0035] In the present application, polydioxanone is a mixture of polydioxanone with a viscosity average molecular weight of 200,000-300,000 and polydioxanone with a viscosity average molecular weight of 600,000-700,000; further, the weight ratio of polydioxanone with a viscosity average molecular weight of 200,000-300,000 and polydioxanone with a viscosity average molecular weight of 600,000-700,000 is 10:(2-4.5).

[0036] In the present application, the high barrier PBAT material may also include 2-6 parts of isocyanate. Further, the isocyanate is selected from L-lysine diisocyanate, L-lysine triisocyanate, isophorone diisocyanate, hexamethylene diisocyanate and 3,3'-dichlorobiphenyl-4,4'-diisocyanate. Further, the isocyanate is a mixture of L-lysine triisocyanate and 3,3'-dichlorobiphenyl-4,4'-diisocyanate, and the weight ratio of L-lysine triisocyanate to 3,3'-dichlorobiphenyl-4,4'-diisocyanate is 1:(0.18-0.43).

[0037] The present application also provides a method for preparing the above-mentioned high-barrier PBAT material, comprising the following steps: weighing the components of the high-barrier PBAT material according to parts by weight, mixing them evenly, and then melt-extruding them at 165±5°C to obtain the high-barrier PBAT material.

[0038] In the embodiments of the present application, the barrier material is ethylene-vinyl alcohol copolymer and mica in a weight ratio of 1:2; the compatibilizer is ethylene methyl acrylate, purchased from Exxon EMA; the dispersant is trimethylolpropane oleate TMPTO; polydioxanone is purchased from Wuhan Shuer Biotechnology Co., Ltd.; L-lysine triisocyanate is purchased from Hubei Jiahui Xingcheng Biotechnology Co., Ltd.; 3,3'-dichlorobiphenyl-4,4'-diisocyanate is purchased from Shanghai Jizhi Biochemical Technology Co., Ltd.; isophorone diisocyanate is purchased from McLean; the remaining raw materials, reagents, etc. in the present application can be obtained commercially.

[0039] The present application is further described in detail below in conjunction with embodiments and performance testing experiments.

[0040] Examples 1-5

[0041] Examples 1-5 each provide a high barrier PBAT material.

[0042] The difference between the above embodiments is that the addition amounts of PBAT and polydioxanone in the high barrier PBAT material are specifically shown in Table 1 below.

[0043] The preparation method of the high barrier PBAT material provided in Examples 1-5 comprises the following steps: according to the addition amounts in Table 1, PBAT, polydioxanone (the weight ratio of 250,000 viscosity average molecular weight Mv and 650,000 viscosity average molecular weight Mv is 1:1), barrier material, compatibilizer and dispersant are respectively weighed, mixed evenly, and then melt-extruded at 165° C. to obtain a high barrier PBAT material.

[0044] Comparative Examples 1-3

[0045] Comparative Examples 1-3 each provide a high barrier PBAT material.

[0046] The difference between the comparative example and Example 2 is that the addition amounts of PBAT and polydioxanone in the high barrier PBAT material are specifically shown in Table 1 below.

[0047] Table 1 Addition amount of each component of high barrier PBAT material provided by Examples 1-5 and Comparative Examples 1-3

[0048]

[0049] Embodiment 6-10

[0050] Examples 6-10 each provide a high barrier PBAT material.

[0051] The difference between the above embodiment and embodiment 2 is that the molecular weight and ratio of polydioxanone are shown in Table 2 below.

[0052] Comparative Examples 4-7

[0053] Comparative Examples 4-7 each provide a high barrier PBAT material.

[0054] The difference between the comparative example and Example 2 is that the molecular weight and ratio of polydioxanone are shown in Table 2 below.

[0055] Table 2 Molecular weight and ratio of polydioxanone in Examples 6-10 and Comparative Examples 4-7

[0056] / Molecular weight and ratio of polydioxanone Example 2 The weight ratio of 250,000Mv and 650,000Mv is 1:1 Example 6 The weight ratio of 250,000Mv and 650,000Mv is 10:2 Example 7 The weight ratio of 250,000Mv and 650,000Mv is 10:3 Example 8 The weight ratio of 250,000Mv and 650,000Mv is 10:4.5 Example 9 The weight ratio of 250,000Mv and 650,000Mv is 10:5 Example 10 The weight ratio of 250,000Mv and 650,000Mv is 5:10 Comparative Example 4 250,000 Mv Comparative Example 5 450,000 Mv Comparative Example 6 The weight ratio of 250,000Mv to 800,000Mv is 10:3 Comparative Example 7 The weight ratio of 400,000Mv and 800,000Mv is 10:3

[0057] Examples 11-17

[0058] Examples 11-17 each provide a high barrier PBAT material.

[0059] The difference between the above embodiment and embodiment 7 is that the high barrier PBAT material also includes 3 kg of isocyanate, and the type and proportion of the isocyanate are shown in Table 3 below.

[0060] Table 3 Types and ratios of isocyanates in high barrier PBAT materials of Examples 11-17

[0061] / Isocyanate types and ratios Embodiment 11 L-Lysine triisocyanate Example 12 L-lysine triisocyanate and 3,3'-dichlorobiphenyl-4,4'-diisocyanate in a weight ratio of 1:0.18 Embodiment 13 L-lysine triisocyanate and 3,3'-dichlorobiphenyl-4,4'-diisocyanate in a weight ratio of 1:0.25 Embodiment 14 L-lysine triisocyanate and 3,3'-dichlorobiphenyl-4,4'-diisocyanate in a weight ratio of 1:0.3 Embodiment 15 L-lysine triisocyanate and 3,3'-dichlorobiphenyl-4,4'-diisocyanate in a weight ratio of 1:0.43 Example 16 Isophorone diisocyanate and 3,3'-dichlorobiphenyl-4,4'-diisocyanate in a weight ratio of 1:0.3 Embodiment 17 L-lysine triisocyanate and isophorone diisocyanate in a weight ratio of 1:0.3

[0062] Performance testing

[0063] The high barrier PBAT materials obtained in Examples 1-17 and Comparative Examples 1-7 were blow molded into films of 10±0.1 μm, and then the water vapor permeability, mechanical properties and degradation properties were tested. The results are shown in Table 4 below.

[0064] The water vapor permeability test method is carried out in accordance with GB / T1037-2021 Determination of water vapor permeability of plastic films and sheets; the oxygen permeability test method is carried out in accordance with GB / T1038-2000 Plastic Film and Sheet Gas Permeability Test Method Pressure Difference Method; the tensile strength and elongation at break test method are carried out in accordance with GB / T1040.3-2006 Determination of Tensile Properties of Plastics; the 90-day biodegradation rate test method is carried out in accordance with Method C in GB / T19275-2003.

[0065] Table 4 Performance test results of high barrier PBAT materials prepared in Examples 1-17 and Comparative Examples 1-7

[0066]

[0067] The test results of Examples 1-5 and Comparative Examples 1-3 show that the water vapor transmission rate of the high barrier PBAT material prepared in Examples 1-5 of the present application is ≤340g / m 2 24h, oxygen transmission rate ≤12cc / m 2 ·24h·0.1MPa, tensile strength ≥40MPa, elongation at break ≥530%, 90-day biodegradation rate ≥80%; while the tensile strength of the high-barrier PBAT material prepared in Comparative Example 1 is only 38.8MPa, and the elongation at break is only 494.4%; the tensile strength of the high-barrier PBAT material prepared in Comparative Example 2 is only 38.2MPa, and the elongation at break is only 466.9%; the water vapor permeability of the high-barrier PBAT material prepared in Comparative Example 3 is as high as 374g / m 2 24h, oxygen transmission rate up to 12.5cc / m 2 ·24h·0.1MPa, the tensile strength is only 32.5MPa, and the elongation at break is only 432.7%. Therefore, it is explained that the present application uses PBAT, polydioxanone, etc. to prepare high-barrier PBAT materials, and by controlling the weight of PBAT to 40-48 parts and the weight of polydioxanone to 10-15 parts, a high-barrier PBAT material with good comprehensive performance of air / water barrier, mechanical properties and degradability can be obtained.

[0068] The test results of Example 2, Examples 6-10, and Comparative Examples 4-7 show that the water vapor permeability of the high barrier PBAT materials prepared in Example 2 and Examples 6-10 is 274-332 g / m 2 24h, oxygen permeability is 9.1-10.9cc / m 2 ·24h·0.1MPa, the tensile strength is 40.7-48.9MPa, and the elongation at break is 549.1-593.7%; while the water vapor permeability of the high barrier PBAT materials prepared in Comparative Examples 4-7 is 354-372g / m 2 24h, oxygen permeability is 12.7-15.1cc / m 2 ·24h·0.1MPa, tensile strength is 35.6-37.4MPa, elongation at break is 462.8-486.2%. Therefore, it is explained that the present application uses a mixture of polydioxanone with a viscosity average molecular weight of 200,000-300,000 and polydioxanone with a viscosity average molecular weight of 600,000-700,000 to prepare a high barrier PBAT material, which can obtain a high barrier PBAT material with good comprehensive performance of gas / water barrier, mechanical properties and degradability. Further comparison found that the water vapor permeability of the high barrier PBAT material prepared in Examples 6-8 is 274-296g / m 2 24h(<300g / m 2 24h), oxygen permeability is 9.1-9.9cc / m 2 ·24h·0.1MPa(<10cc / m 2 ·24h·0.1MPa), the tensile strength is 46.7-48.9MPa (>45MPa), and the elongation at break is 586.1-593.7% (>580%), which means that the weight ratio of polydioxanone with a viscosity-average molecular weight of 200,000-300,000 to polydioxanone with a viscosity-average molecular weight of 600,000-700,000 is further controlled within the range of 10:(2-4.5), and the gas-water barrier and mechanical properties of the high-barrier PBAT material are better.

[0069] The test results of Examples 7 and 11-17 show that the air-water barrier and mechanical properties of the high barrier PBAT materials with isocyanate added in Examples 11-17 are further improved, and the water vapor permeability is 247-266 g / m 2 24h(<270g / m 2 24h), oxygen permeability is 6.8-8.5cc / m 2 ·24h·0.1MPa(<9cc / m 2·24h·0.1MPa), the tensile strength is 49.6-55.5MPa (>49MPa), and the elongation at break is 614.8-656.4% (>600%). Therefore, it is shown that adding isocyanate to the high-barrier PBAT material can further improve the gas-water barrier and mechanical properties of the high-barrier PBAT material, making the high-barrier PBAT material have excellent comprehensive performance in gas / water barrier, mechanical properties and degradability.

[0070] Although the present invention has been described in detail above with general descriptions and specific embodiments, it is obvious to those skilled in the art that some modifications or improvements may be made thereto based on the present invention. Therefore, these modifications or improvements made without departing from the spirit of the present invention all fall within the scope of protection claimed by the present invention.

Claims

1. A high barrier PBAT material, characterized in that: The invention comprises the following components in parts by weight: 40-48 parts of PBAT, 10-15 parts of polydioxanone, 5-10 parts of barrier material and 1-2 parts of compatibilizer; The polydioxanone is a mixture of polydioxanone with a viscosity average molecular weight of 200,000-300,000 and polydioxanone with a viscosity average molecular weight of 600,000-700,000.

2. The high barrier PBAT material according to claim 1, characterized in that: The weight ratio of the polydioxanone with a viscosity average molecular weight of 200,000-300,000 to the polydioxanone with a viscosity average molecular weight of 600,000-700,000 is 10:(2-4.5).

3. The high barrier PBAT material according to claim 1, characterized in that: The high barrier PBAT material also includes 2-6 parts of isocyanate.

4. The high barrier PBAT material according to claim 3, characterized in that: The isocyanate is selected from L-lysine diisocyanate, L-lysine triisocyanate, isophorone diisocyanate, hexamethylene diisocyanate and 3,3'-dichlorobiphenyl-4,4'-diisocyanate.

5. The high barrier PBAT material according to claim 4, characterized in that: The isocyanate is a mixture of L-lysine triisocyanate and 3,3'-dichlorobiphenyl-4,4'-diisocyanate, and the weight ratio of the L-lysine triisocyanate to the 3,3'-dichlorobiphenyl-4,4'-diisocyanate is 1:(0.18-0.43).

6. The high barrier PBAT material according to claim 1, characterized in that: The barrier material is selected from polyvinylidene chloride, ethylene-vinyl alcohol copolymer, mica, aluminum oxide and titanium oxide.

7. The high barrier PBAT material according to claim 1, characterized in that: The compatibilizer is selected from epoxy type, carboxyl type, imide type and oxazoline type.

8. The high barrier PBAT material according to any one of claims 1 to 7, characterized in that: The high barrier PBAT material also includes one or more of a plasticizer, a dispersant and a stabilizer.

9. The method for preparing a high barrier PBAT material according to any one of claims 1 to 8, characterized in that: The following steps are involved: The components of the high barrier PBAT material were weighed in parts by weight, mixed evenly, and then melt-extruded at 165±5° C. to obtain the high barrier PBAT material.

10. The high barrier PBAT material according to any one of claims 1 to 8 is used in food packaging, pharmaceutical packaging, cosmetic packaging and agricultural mulch film.