Coating of anticorrosive primer and hydrophilic finish paint based on modified graphene as well as preparation method and application of coating
By coating aluminum foil with histidine-modified graphene anti-corrosion primer and hydrophilic surface paint, the problems of moisture corrosion and low thermal conductivity of aluminum foil in air conditioners are solved, improving anti-corrosion and hydrophilic properties, extending service life and The effect of improving heat exchange efficiency.
Patent Information
- Application Number
- CN202410796210.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-19
- Publication Date
- 2024-10-11
AI Technical Summary
Aluminum foil is easily corroded by moisture in air-conditioning heat exchangers, causing water droplets to form, increasing wind resistance and reducing heat exchange efficiency. Existing anti-corrosion coatings cannot effectively solve the problem of low thermal conductivity efficiency.
Histidine-modified graphene is used as an anti-corrosion primer and a hydrophilic topcoat. By combining the modified graphene with epoxy resin and other ingredients, an anti-corrosion primer and a hydrophilic topcoat are formed, which are coated on the aluminum foil. Improve anti-corrosion and hydrophilic properties.
Effectively prevents the formation of water droplets, improves heat exchange efficiency, extends the service life of aluminum foil, and significantly improves anti-corrosion performance.
Smart Images

Figure CN118755345A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of functional materials, and in particular relates to a coating of an anticorrosive primer and a hydrophilic topcoat based on modified graphene, and a preparation method and application thereof. Background Art
[0002] Aluminum foil is widely used in daily life, but during the production process, circulation process, and application process, the product is easily affected by moisture or water, causing corrosion. Applying an organic coating on the surface of aluminum foil can avoid and slow down metal corrosion, and has the advantages of low cost, convenient construction, and good protective effect. However, when aluminum foil is used in air-conditioning heat exchangers, simply applying an anti-corrosion coating on the surface of the aluminum foil cannot improve the disadvantage of low thermal conductivity caused by the formation of water droplets.
[0003] Normally, the aluminum foil used for heat exchange in air conditioners converts heat absorption and heat dissipation during operation. However, moisture in the air can easily condense on the fins with lower surface temperature, forming water droplets, which then build "water bridges" between the fins. The formation of such "water bridges" will hinder air circulation, increase wind resistance and noise, and reduce heat exchange efficiency. The formation of "water bridges" will also reduce the service life of the heat exchanger, because the aluminum foil is more susceptible to corrosion when it is in a humid environment for a long time. Summary of the invention
[0004] The purpose of the present invention is to solve some problems existing in the prior art and to achieve the purpose of improving the corrosion resistance and hydrophilicity of an aluminum foil substrate. The present invention provides a coating of an anti-corrosion primer and a hydrophilic topcoat based on modified graphene, and a preparation method and application thereof. The modified graphene is histidine-modified graphene, and the primer and the topcoat are respectively coated on the aluminum foil to prepare an anti-corrosion hydrophilic aluminum foil.
[0005] In order to achieve the above technical purpose, the technical solution adopted by the present invention is as follows:
[0006] The present invention first provides a coating of an anticorrosive primer and a hydrophilic topcoat based on modified graphene, wherein the modified graphene is histidine-modified graphene. The anticorrosive primer coating and the hydrophilic topcoat coating prepared by the present invention are successively coated on an aluminum foil, so that the aluminum foil has both anticorrosive and hydrophilic functions.
[0007] The present invention also provides a method for preparing the coating of the anticorrosive primer and hydrophilic topcoat based on modified graphene, the method comprising the following steps:
[0008] Preparation of modified graphene: citric acid and histidine are added to a graphene dispersion, and histidine-modified graphene is obtained by high-temperature modification.
[0009] Wherein, the molar ratio of citric acid to histidine is 1:0.1 to 1:0.3;
[0010] The high temperature modification is modification at 180-220° C. for 3-5 hours.
[0011] Preparation of anti-corrosion primer coating: under ultrasonic conditions, epoxy resin and alkylphenol polyoxyethylene ether phosphate are added to modified graphene acetone dispersion, the temperature is raised to a certain temperature after ultrasonic dispersion, and the acetone is evaporated by stirring to obtain component I; at the same time, a curing agent is weighed, a solvent and an auxiliary agent are added, and ultrasonic dispersion is uniformly performed to obtain component II; component I and component II are stirred and mixed uniformly to obtain an anti-corrosion primer coating.
[0012] The modified graphene acetone dispersion is obtained by adding histidine-modified graphene into an acetone solution, and the mass fraction of the histidine-modified graphene in the dispersion is 0.5% to 1%.
[0013] The mass fraction of alkylphenol polyoxyethylene ether phosphate in the modified graphene acetone dispersion is 0.3% to 0.7%, and the mass fraction of the epoxy resin is 68% to 78%.
[0014] The epoxy resin and alkylphenol polyoxyethylene ether phosphate are added into the modified graphene acetone dispersion, and the temperature is raised to 60° C. after ultrasonic dispersion for 2 to 3 hours.
[0015] Wherein, the curing agent is isocyanate, the solvent is propylene glycol methyl ether, and the auxiliary agent is acrylic acid and polysiloxane.
[0016] Furthermore, in the component II, the mass fraction of the isocyanate is 18% to 22%, the mass fraction of the propylene glycol methyl ether is 2% to 6%, the mass fraction of the acrylic acid is 0.5% to 1.5%, and the mass fraction of the polysiloxane is 0.2% to 0.8%.
[0017] Preparation of hydrophilic topcoat coating: acrylic resin, silica, amino resin, butyl acrylate, polyoxyacrylate, propylene glycol methyl ether, butyl glycol butyl ether, ethylene glycol, sodium alkyl glyceryl ether sulfonate, polybutyl acrylate and tert-butyl perbenzoate are mixed to obtain a water-based coating, and the obtained water-based coating is diluted with water to 25% to 35% for subsequent use.
[0018] Among them, in the water-based paint, the mass fraction of acrylic resin is 50% to 60%, the mass fraction of silicon dioxide is 10% to 15%, the mass fraction of amino resin is 5% to 15%, the mass fraction of butyl acrylate is 10% to 15%, the mass fraction of polyoxyacrylate is 4% to 6%, the mass fraction of propylene glycol methyl ether is 6% to 8%, the mass fraction of butylene glycol methyl ether is 2% to 5%, the mass fraction of ethylene glycol is 2% to 5%, the mass fraction of sodium alkyl glyceryl ether sulfonate is 1% to 2%, the mass fraction of polybutyl acrylate is 0.5% to 1%, and the mass fraction of tert-butyl perbenzoate is 2% to 5%.
[0019] The present invention also provides an application of the coating of the anticorrosion primer and the hydrophilic topcoat based on modified graphene, and the application includes preparing an anticorrosion hydrophilic aluminum foil.
[0020] The invention also provides an anti-corrosion hydrophilic aluminum foil. The aluminum foil is coated with an anti-corrosion primer layer, and the anti-corrosion coating is coated with a hydrophilic topcoat layer.
[0021] The present invention also provides a method for preparing the anticorrosive hydrophilic aluminum foil, which comprises the following steps:
[0022] The aluminum sheet was ultrasonically cleaned with acetone solution and deionized water respectively and then dried to obtain a clean aluminum foil substrate;
[0023] The anti-corrosion primer is coated on the aluminum foil, dried and kept warm for a period of time, and cooled to room temperature to obtain the anti-corrosion aluminum foil; the hydrophilic topcoat is coated on the anti-corrosion aluminum foil, kept warm in a drying oven for a period of time, and cooled to room temperature to obtain the anti-corrosion hydrophilic aluminum foil.
[0024] The drying and heat preservation conditions are as follows: drying and heat preservation at 60-80° C. in a drying oven for 5-10 hours.
[0025] Beneficial effects of the present invention:
[0026] Compared with the prior art, the raw material of the present invention uses graphene modified by histidine as a filler to fill the gaps of epoxy resin during the curing process. In the present invention, histidine reacts with the functional groups on the surface of graphene and connects different layers, making the graphene smoother, thereby improving the dispersibility of graphene in epoxy resin. The imidazole ring contained in histidine will undergo a ring-opening reaction with the epoxy resin, which can enhance the interfacial effect between them. The present invention uses histidine-modified graphene, which is different from the prior art, as a filler, which is used to improve the dispersibility of graphene in epoxy resin, so that the filler can better fill the tiny gaps of epoxy resin during the curing process, more effectively prevent the corrosive medium from contacting the aluminum foil substrate, and achieve the effect of improving the anti-corrosion life of the aluminum foil.
[0027] The hydrophilic topcoat is rolled on the surface of the aluminum foil coated with the anti-corrosion primer to prevent the formation of water droplets, thereby preventing the water droplets from forming a "water bridge" on the surface of the aluminum foil and affecting the ventilation effect of the heat exchanger. The addition of the hydrophilic topcoat can not only prevent the formation of "water bridges" and improve the heat exchange efficiency, but also reduce the contact between the corrosive medium and the primer due to the absence of water droplets, greatly improving the anti-corrosion performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 This is the SEM image of the histidine-modified graphene prepared in Example 1.
[0029] Figure 2 This is a picture of the aluminum foil prepared in Example 1.
[0030] Figure 3 This is a picture of the aluminum foil prepared in Example 2.
[0031] Figure 4 This is a picture of the aluminum foil prepared in Example 3.
[0032] Figure 5 This is a picture of the aluminum foil prepared in Example 4.
[0033] Figure 6 The contact angle test results of commercial aluminum foil and the aluminum foil prepared in Example 2 are shown.
[0034] Figure 7 These are the anti-corrosion test results of commercial aluminum foil and the aluminum foil prepared in Example 2. DETAILED DESCRIPTION
[0035] To help those skilled in the art better understand the technical solution of the present invention, preferred embodiments are described in detail below, but the following embodiments are not limited to the protection scope of the present invention.
[0036] The contents not described in detail in the examples are usually completed according to conventional experimental methods, and the processes involved can also be understood and simply implemented by technicians in the field according to product specifications or basic knowledge. Obviously, the examples only represent some applications of the present invention, not all.
[0037] Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making any creative work shall fall within the scope of protection of the present invention.
[0038] Embodiment 1:
[0039] In this embodiment, a coating of an anticorrosive primer and a hydrophilic topcoat based on modified graphene is first prepared, comprising the following steps:
[0040] Preparation of modified graphene: citric acid and histidine were added to the graphene dispersion at a molar ratio of 1:0.1, and histidine-modified graphene was obtained by high-temperature modification at 200°C for 3h.
[0041] Figure 1 This is a SEM image of the histidine-modified graphene prepared in Example 1. It can be seen from the figure that the graphene prepared in this example is a lamellar structure with a thin thickness and can be better dispersed in the epoxy resin.
[0042] Preparation of anti-corrosion primer coating: under ultrasonic conditions, epoxy resin and alkylphenol polyoxyethylene ether phosphate are added to the modified graphene acetone dispersion, the temperature is raised to 60°C after ultrasonic dispersion for 5 hours, and the acetone is evaporated with stirring to obtain component I, wherein the modified graphene acetone dispersion is obtained by adding histidine-modified graphene to acetone solution, the mass fraction of histidine-modified graphene in the dispersion is 0.5%, the mass fraction of alkylphenol polyoxyethylene ether phosphate is 0.4%, and the mass fraction of epoxy resin is 70%.
[0043] At the same time, weigh the curing agent isocyanate, add the solvent propylene glycol methyl ether, the auxiliary agent acrylic acid and polysiloxane, and disperse them uniformly by ultrasonication to obtain component II; stir and mix component I and component II to obtain an anticorrosive primer coating. Among them, the mass fraction of isocyanate in component II is 20%, the mass fraction of propylene glycol methyl ether is 3%, the mass fraction of acrylic acid is 0.7%, and the mass fraction of polysiloxane is 0.5%.
[0044] This step obtains an anti-corrosion coating with a mass fraction of histidine-modified graphene of 0.5%.
[0045] Preparation of hydrophilic topcoat layer: acrylic resin, silicon dioxide, amino resin, butyl acrylate, polyoxyacrylate, propylene glycol methyl ether, butyl glycol butyl ether, ethylene glycol, sodium alkyl glyceryl ether sulfonate, polybutyl acrylate and tert-butyl perbenzoate are mixed to obtain a water-based coating, and the obtained water-based coating is diluted with water to 25% to 35% for subsequent use. Among them, the mass fraction of acrylic resin in the water-based coating is 55%, the mass fraction of silicon dioxide is 10%, the mass fraction of amino resin is 10%, the mass fraction of butyl acrylate is 12%, the mass fraction of polyoxyacrylate is 5%, the mass fraction of propylene glycol methyl ether is 6%, the mass fraction of butyl glycol methyl ether is 3%, the mass fraction of ethylene glycol is 3%, the mass fraction of sodium alkyl glyceryl ether sulfonate is 1%, the mass fraction of polybutyl acrylate is 0.5%, and the mass fraction of tert-butyl perbenzoate is 3%.
[0046] The prepared anticorrosive primer and hydrophilic topcoat coating are used to prepare anticorrosive hydrophilic aluminum foil, and the specific method includes:
[0047] The aluminum sheet was ultrasonically cleaned with acetone solution and deionized water respectively and then dried to obtain a clean aluminum foil substrate;
[0048] A layer of anti-corrosion primer coating with a mass fraction of histidine-modified graphene of 0.5% is coated on the aluminum foil, dried and kept warm at 60° C. for 10 hours in a forced air drying oven, and cooled to room temperature to obtain an anti-corrosion aluminum foil; a layer of hydrophilic topcoat is coated on the anti-corrosion aluminum foil, dried and kept warm at 60° C. for 5 hours in a forced air drying oven, and cooled to room temperature to obtain an anti-corrosion hydrophilic aluminum foil. The obtained aluminum foil is as follows Figure 2 As shown, when the anticorrosive primer and the hydrophilic topcoat prepared in this embodiment are coated one layer at a time on the aluminum foil, the coating can be evenly coated on the aluminum foil.
[0049] Embodiment 2:
[0050] The preparation of the coating of the anticorrosive primer and hydrophilic topcoat based on modified graphene in this embodiment is the same as that in Example 1.
[0051] The prepared anticorrosive primer layer and hydrophilic topcoat layer are used to prepare an anticorrosive hydrophilic aluminum foil, and the specific method includes:
[0052] The aluminum sheet was ultrasonically cleaned with acetone solution and deionized water respectively and then dried to obtain a clean aluminum foil substrate;
[0053] Two layers of anti-corrosion primer with a graphene mass fraction of 0.5% are coated on the aluminum foil, dried and kept warm at 60° C. for 10 hours in a forced air drying oven, and cooled to room temperature to obtain an anti-corrosion aluminum foil; a hydrophilic topcoat layer is coated on the anti-corrosion aluminum foil, dried and kept warm at 60° C. for 5 hours in a forced air drying oven, and cooled to room temperature to obtain an anti-corrosion hydrophilic aluminum foil. The obtained aluminum foil is as follows Figure 3 As shown in the figure, it can be seen that when an anti-corrosion coating with a mass fraction of histidine-modified graphene of 0.5% and a layer of hydrophilic topcoat are coated on the aluminum foil, the surface color of the aluminum foil becomes darker.
[0054] Embodiment 3:
[0055] In this example, based on Example 1, only the mass fraction of histidine-modified graphene in the modified graphene acetone dispersion was changed to 1%, and an anticorrosive primer coating with a mass fraction of histidine-modified graphene of 1% was prepared. The preparation of the hydrophilic topcoat layer was the same as in Example 1.
[0056] The prepared anticorrosive primer and hydrophilic topcoat coating are used to prepare anticorrosive hydrophilic aluminum foil, and the specific method includes:
[0057] The aluminum sheet was ultrasonically cleaned with acetone solution and deionized water respectively and then dried to obtain a clean aluminum foil substrate;
[0058] A layer of anti-corrosion primer with a mass fraction of 1% histidine-modified graphene is coated on the aluminum foil, dried and kept warm at 60°C in a forced air drying oven for 10 hours, and cooled to room temperature to obtain an anti-corrosion aluminum foil; a layer of hydrophilic topcoat is coated on the anti-corrosion aluminum foil, dried and kept warm at 60°C in a forced air drying oven for 5 hours, and cooled to room temperature to obtain an anti-corrosion hydrophilic aluminum foil. The obtained aluminum foil is as follows: Figure 4 As shown, Figure 4 The aluminum foil is obtained by coating a layer of anti-corrosion primer coating with a mass fraction of 1% of histidine-modified graphene and a layer of hydrophilic topcoat on the aluminum foil. When the concentration of histidine-modified graphene increases to 1%, the effect of coating a layer of anti-corrosion primer and a layer of hydrophilic topcoat on the aluminum foil is not as good as the effect of coating a layer of anti-corrosion coating with a mass fraction of 0.5% of histidine-modified graphene and a layer of hydrophilic coating. Increasing the concentration of histidine-modified graphene will lead to the deterioration of the dispersibility of graphene in epoxy resin and the occurrence of graphene agglomeration.
[0059] Embodiment 4:
[0060] The preparation of the coating of the anti-corrosion primer and hydrophilic topcoat based on modified graphene in this embodiment is the same as that in Example 3.
[0061] The prepared anticorrosive primer layer and hydrophilic topcoat layer are used to prepare an anticorrosive hydrophilic aluminum foil, and the specific method includes:
[0062] The aluminum sheet was ultrasonically cleaned with acetone solution and deionized water respectively and then dried to obtain a clean aluminum foil substrate;
[0063] Two layers of anti-corrosion primer with a mass fraction of 1% histidine-modified graphene are coated on aluminum foil, dried and kept warm at 60°C in a forced air drying oven for 10 hours, and cooled to room temperature to obtain an anti-corrosion aluminum foil; a hydrophilic topcoat layer is coated on the anti-corrosion aluminum foil, dried and kept warm at 60°C in a forced air drying oven for 5 hours, and cooled to room temperature to obtain an anti-corrosion hydrophilic aluminum foil. The obtained aluminum foil is as follows: Figure 5 As shown, Figure 5 For aluminum foil coated with 2 layers of anti-corrosion primer coating with a mass fraction of 1% histidine-modified graphene and 1 layer of hydrophilic topcoat coating, it can be seen in the figure that the dispersion of graphene in epoxy resin (compared to Figure 4 ) is lower, the color of the coating surface is darker and the graphene is more aggregated.
[0064] Comparative Example 1:
[0065] The contact angle, thermal conductivity and anti-corrosion performance of commercial aluminum foil (commonly available in the market) and the anti-corrosion hydrophilic aluminum foil prepared in Example 2 were compared. The experimental results are as follows:
[0066] (1) Contact angle test results:
[0067] Test results such as Figure 6 As shown, Figure 6The left picture in the middle shows the contact angle test result of commercial aluminum foil currently sold on the market, and the right picture shows the contact angle test result of the aluminum foil prepared in Example 2. Figure 6 It can be seen from the figure that the contact angle of the aluminum foil prepared in Example 2 is 14°, proving that the topcoat layer prepared in the present invention is a hydrophilic topcoat layer.
[0068] After the anticorrosive primer layer and the hydrophilic topcoat layer prepared by the present invention are coated on the aluminum foil, the hydrophilic property thereof is obviously better than the aluminum foil currently available on the market, and the formation of water droplets can be effectively reduced, and the thermal conductivity can be improved.
[0069] (2) Thermal conductivity test:
[0070] The thermal conductivity of commercial aluminum foil and the aluminum foil prepared in Example 2 of the present invention were tested. The results showed that the thermal conductivity of the commercial aluminum foil was 0.25-0.3 W / m·K, while the thermal conductivity of the aluminum foil prepared in the present invention reached 0.28-0.35 W / m·K. It is obvious that the anti-corrosion hydrophilic aluminum foil prepared in the present invention has higher thermal conductivity efficiency.
[0071] (3) Anticorrosion test:
[0072] Commercial aluminum foil and the aluminum foil prepared in Example 2 were subjected to an anti-corrosion test experiment. The specific experimental steps are as follows:
[0073] Dissolve 10mL of hydrochloric acid and 20g of copper sulfate in 70mL of deionized water to prepare a corrosive solution; drop an appropriate amount of the corrosive solution onto the surfaces of the two aluminum foils and observe the corrosion at intervals. Figure 7 As shown in the results, the anti-corrosion hydrophilic aluminum foil prepared by coating the anti-corrosion primer layer and the hydrophilic topcoat layer prepared in Example 2 of the present invention on the aluminum foil can effectively prevent the corrosive medium from contacting the aluminum foil and has excellent anti-corrosion performance.
[0074] The above results show that the anti-corrosion hydrophilic aluminum foil prepared by coating the anti-corrosion primer layer and the hydrophilic topcoat layer prepared by the present invention on aluminum foil has good anti-corrosion and hydrophilic properties.
[0075] The above embodiments are only used to illustrate the present invention and are not intended to limit the technical solutions described in the present invention; therefore, although the present invention has been described in detail in this specification with reference to the above embodiments, it should be understood by those skilled in the art that the present invention may still be modified or replaced by equivalents; and all technical solutions and improvements thereof that do not depart from the spirit and scope of the present invention should be included in the scope of the claims of the present invention.
Claims
1. A method for preparing a coating of an anticorrosive primer and a hydrophilic topcoat based on modified graphene, characterized in that: The method comprises the following steps: Preparation of modified graphene: adding citric acid and histidine to a graphene dispersion, and obtaining histidine-modified graphene by high-temperature modification; Preparation of anticorrosive primer coating: under ultrasonic conditions, epoxy resin and alkylphenol polyoxyethylene ether phosphate are added to modified graphene acetone dispersion, the temperature is raised to a certain temperature after ultrasonic dispersion, and acetone is evaporated by stirring to obtain component I; at the same time, a curing agent is weighed, a solvent and an auxiliary agent are added, and ultrasonic dispersion is uniformly performed to obtain component II; component I and component II are stirred and mixed uniformly to obtain an anticorrosive primer coating; Preparation of hydrophilic topcoat coating: acrylic resin, silica, amino resin, butyl acrylate, polyoxyacrylate, propylene glycol methyl ether, butyl glycol butyl ether, ethylene glycol, sodium alkyl glyceryl ether sulfonate, polybutyl acrylate and tert-butyl perbenzoate are mixed to obtain a water-based coating, and the obtained water-based coating is diluted with water for subsequent use.
2. The method according to claim 1, characterized in that In the process of preparing modified graphene, the molar ratio of citric acid to histidine is 1:0.1 to 1:0.3; the high-temperature modification is carried out at 180 to 220° C. for 3 to 5 hours.
3. The method according to claim 1, characterized in that: In the process of preparing the anticorrosive primer layer, the modified graphene acetone dispersion is obtained by adding histidine-modified graphene to an acetone solution, and the mass fraction of the histidine-modified graphene in the dispersion is 0.5% to 1%; the mass fraction of the alkylphenol polyoxyethylene ether phosphate in the modified graphene acetone dispersion is 0.3% to 0.7%, and the mass fraction of the epoxy resin is 68% to 78%; The epoxy resin and alkylphenol polyoxyethylene ether phosphate are added into the modified graphene acetone dispersion, and the temperature is raised to 60° C. after ultrasonic dispersion for 2 to 3 hours.
4. The method according to claim 1, characterized in that: In the process of preparing the anticorrosive primer coating, the curing agent is isocyanate, the solvent is propylene glycol methyl ether, and the auxiliary agents are acrylic acid and polysiloxane; in the component II, the mass fraction of the isocyanate is 18% to 22%, the mass fraction of the propylene glycol methyl ether is 2% to 6%, the mass fraction of the acrylic acid is 0.5% to 1.5%, and the mass fraction of the polysiloxane is 0.2% to 0.8%.
5. The method according to claim 1, characterized in that In the process of preparing the hydrophilic topcoat coating, in the water-based coating, the mass fraction of acrylic resin is 50% to 60%, the mass fraction of silicon dioxide is 10% to 15%, the mass fraction of amino resin is 5% to 15%, the mass fraction of butyl acrylate is 10% to 15%, the mass fraction of polyoxyacrylate is 4% to 6%, the mass fraction of propylene glycol methyl ether is 6% to 8%, the mass fraction of butylene glycol methyl ether is 2% to 5%, the mass fraction of ethylene glycol is 2% to 5%, the mass fraction of sodium alkyl glyceryl ether sulfonate is 1% to 2%, the mass fraction of polybutyl acrylate is 0.5% to 1%, and the mass fraction of tert-butyl perbenzoate is 2% to 5%.
6. A coating of an anticorrosive primer and a hydrophilic topcoat based on modified graphene prepared by the method according to any one of claims 1 to 5, wherein the modified graphene is histidine-modified graphene.
7. The application of the coating of the anticorrosive primer and hydrophilic topcoat based on modified graphene prepared by the method described in any one of claims 1 to 5 or the coating of the anticorrosive primer and hydrophilic topcoat based on modified graphene according to claim 6, wherein the application comprises preparing an anticorrosive hydrophilic aluminum foil.
8. A method for preparing an anticorrosive hydrophilic aluminum foil, characterized in that: The method comprises the following steps: The aluminum sheet was ultrasonically cleaned with acetone solution and deionized water respectively and then dried to obtain a clean aluminum foil substrate; The anti-corrosion primer coating prepared by the method described in any one of claims 1 to 5 is coated on the aluminum foil, dried and kept warm for a period of time, and cooled to room temperature to obtain the anti-corrosion aluminum foil; the hydrophilic topcoat coating prepared by the method described in any one of claims 1 to 5 is coated on the anti-corrosion aluminum foil, kept warm in a drying oven for a period of time, and cooled to room temperature to obtain the anti-corrosion hydrophilic aluminum foil.
9. The preparation method according to claim 8, characterized in that: The drying and heat preservation conditions are drying and heat preservation at 60-80° C. in a drying oven for 5-10 hours.
10. The anticorrosive hydrophilic aluminum foil prepared according to the method according to any one of claims 8 to 9.
Citation Information
Patent Citations
High-corrosion-resistance high-thermal-conductivity composite aluminum foil and production method thereof
CN109926294A
Modified graphene heavy anti-corrosion coating as well as preparation method and application thereof