Formula and preparation method of waterborne polyurethane formaldehyde-free reaction adhesive
The formula of water-based polyurethane aldehyde-free reactive adhesive without formaldehyde, combined with plant extracts and nano-silicates, solves the problem of performance degradation of traditional adhesives under high humidity and high temperature conditions, improves water resistance and heat resistance, and meets complex needs. Environmental applications, and achieved the goals of environmental protection and cost reduction.
Patent Information
- Application Number
- CN202410877136.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-02
- Publication Date
- 2024-10-11
AI Technical Summary
Traditional water-based polyurethane adhesives tend to absorb water and swell under conditions of high humidity and high temperature, resulting in reduced bonding performance and poor chemical resistance, which limits their application in humid and chemical environments. The preparation process is complex and increases production costs.
It adopts a water-based polyurethane aldehyde-free reactive adhesive formula without formaldehyde addition, combined with plant extracts and nano-silicates to enhance the water resistance and heat resistance of the adhesive, and uses environmentally friendly preservatives and pH regulators to ensure that it is ensured through a sophisticated preparation process. Adhesive stability and environmental performance.
It improves the bonding performance, water resistance, heat resistance and chemical resistance of the adhesive, meets the application requirements in complex environments, reduces production costs, reduces environmental pollution, and achieves the goals of green chemistry and sustainable development.
Smart Images

Figure CN118755433A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of waterborne polyurethane aldehyde-free reaction glue, in particular to a formula and a preparation method of waterborne polyurethane aldehyde-free reaction glue. Background Art
[0002] As global environmental awareness gradually increases, traditional formaldehyde-containing adhesives have become one of the main sources of environmental pollution due to the harmful formaldehyde substances released during production and use. Formaldehyde not only has a strong irritating odor, but also has great harm to human health. Long-term exposure may lead to respiratory diseases, skin allergies, and decreased immunity. Therefore, the development of environmentally friendly, formaldehyde-free adhesives has become an important development direction for the current adhesive industry.
[0003] However, traditional reaction glue is easy to absorb water and swell during long-term use, especially in high humidity environment conditions, and its water resistance and bonding properties are easily affected, resulting in a decrease in bonding strength or even failure. This instability limits the application of traditional reaction glue in humid environments, and many water-based polyurethane adhesives are prone to thermal decomposition or oxidative degradation under high temperature conditions, resulting in a decrease in bonding performance. This poor heat resistance makes it difficult to use in situations that require high temperature treatment. Secondly, some products are cumbersome to operate during the preparation process, which is not conducive to industrial production.
[0004] Some chemical solvents, acidic and alkaline substances or oxidants may corrode waterborne polyurethane adhesives, causing their surfaces to be eroded, internal structures to change or their adhesive ability to be lost, which limits the application of waterborne polyurethane adhesives in some chemical environments, such as the chemical and pharmaceutical industries. In order to improve the chemical resistance of waterborne polyurethane adhesives, it is usually necessary to add some special additives or perform surface modification treatments, but these methods may increase production costs and process complexity. Therefore, it is necessary to make technical improvements to the formula and preparation method of traditional reaction adhesives, and develop a product with good adhesion, environmental protection, water resistance, heat resistance and chemical resistance to meet the application requirements in various complex environments. At the same time, the preparation process of these products is simple and easy to operate, which is conducive to industrial production. Summary of the invention
[0005] The purpose of the present invention is to make up for the deficiencies of the prior art and to provide a formula and preparation method of a water-based polyurethane formaldehyde-free reaction adhesive. It can fundamentally eliminate the release of formaldehyde harmful substances by adopting a formula without formaldehyde addition and combining environmentally friendly raw materials such as plant extracts and nano-silicates, thereby greatly improving the environmental performance of the adhesive. In today's context of increasingly emphasizing green and low-carbon production and consumption, this innovative formula meets the market's urgent demand for environmentally friendly adhesives. In addition, the use of environmentally friendly preservatives and pH adjusters further reduces the potential impact of the product on the environment, which is in line with the concept of sustainable development.
[0006] In order to solve the above technical problems, the present invention provides the following technical solutions: On the one hand, a formula of a water-based polyurethane formaldehyde-free reaction glue, the formaldehyde-free reaction glue material is composed of:
[0007] Polyurethane prepolymer: As the basis of water-based polyurethane formaldehyde-free reaction adhesive, it provides the basic framework and performance of the adhesive. It is first added to the reactor, and the agitator is turned on and stirred at a low speed to make it evenly distributed in the reactor;
[0008] Reinforced and modified materials: Plant extract soybean oil is used to enhance the water resistance and heat resistance of adhesives, providing additional functionality for adhesives, while nano-silicate has excellent dispersibility and stability, which can improve the overall performance of adhesives;
[0009] Auxiliary raw materials: Natural rubber latex is used as an auxiliary raw material to increase the viscosity and flexibility of the adhesive;
[0010] Functional additives: cross-linking agents based on polycarbodiimide are used to form cross-linking structures between polyurethane prepolymers to improve the strength and stability of the adhesive. Sodium bicarbonate, a pH regulator, can quickly and accurately adjust the pH value of the adhesive to keep it within a stable working range. Environmentally friendly preservatives prevent the adhesive from being contaminated by microorganisms during storage and use.
[0011] Diluent: Deionized water is used as a diluent to reduce the viscosity of the adhesive, facilitate construction, and ensure the purity and stability of the adhesive.
[0012] Furthermore, the polyurethane prepolymer as the main raw material of the waterborne polyurethane formaldehyde-free reaction adhesive has a mass percentage of 60%-74%.
[0013] Furthermore, the mass percentage of the plant extract soybean oil in the reinforcing and modifying material is 8%-12%, and nano-silicate and natural rubber latex are used as modifying materials and auxiliary raw materials in combination with the plant extract, and their proportions are 3%-7% and 8%-12% respectively.
[0014] Furthermore, the environmentally friendly crosslinking agent in the functional additive promotes the crosslinking reaction between polyurethane prepolymers, and its mass percentage is 2%-4%, the pH value of the adhesive is adjusted to 0.5%-2%, and the mass percentage of the preservative based on natural plant extracts is 0.3%-1%.
[0015] Furthermore, after the preservative is added, the speed and amount of adding water are controlled by a flow meter, 10% by weight of deionized water is gradually added, and the stirring speed is increased to fully mix the deionized water and the adhesive to form a uniform solution.
[0016] On the other hand, a method for preparing a waterborne polyurethane non-aldehyde reactive adhesive is provided, wherein the specific steps of the preparation method are as follows:
[0017] S100, raw material preparation and pretreatment: according to the formula ratio, use accurate weighing equipment to weigh the required solid raw materials of polyurethane prepolymer, plant extract, nanosilicate, and natural rubber latex, and ensure that they are of qualified quality and pollution-free. At the same time, check the high purity of deionized water;
[0018] S200, Mixing and stirring: Stir the polyurethane prepolymer at a low speed in the reactor, gradually add other solid raw materials, and increase the stirring speed to ensure that all components are mixed evenly without lumps;
[0019] S300, cross-linking agent addition and reaction: after the solid components are evenly mixed, an environmentally friendly cross-linking agent is added, and the addition speed is controlled so that the cross-linking agent and the base adhesive react fully to form a stable cross-linking structure;
[0020] S400, pH adjustment: adjusting the pH value of the system by adding a pH adjusting agent, sodium bicarbonate, so that the reaction system tends to a stable state;
[0021] S500, preservative addition: after pH adjustment, add environmentally friendly preservatives and continue stirring to make it evenly dispersed in the system to play an anti-corrosion role;
[0022] S600, dilution and homogenization: gradually add deionized water, and control the speed and amount of water addition, while increasing the stirring speed to fully mix the deionized water and the adhesive to form a uniform solution;
[0023] S700, Finished product inspection and packaging: Perform performance inspection on the prepared products to ensure that all indicators meet quality requirements, and package them and mark them with necessary information;
[0024] S800, Cleaning and Maintenance: Clean and maintain the equipment regularly to ensure the normal operation of the equipment and the quality of the products.
[0025] Furthermore, the raw material ratio of the S100 is: 70% polyurethane prepolymer, 10% plant extract soybean oil, 5% nanosilicate, 10% natural rubber latex, 3% polycarbodiimide-based crosslinking agent, 1% pH adjuster sodium bicarbonate, 0.5% preservative, and the rest is deionized water.
[0026] Furthermore, the S200 stirs the polyurethane prepolymer in the reactor at a low speed of 50 rpm, and gradually increases the stirring speed to 150 rpm, so that the components are fully mixed and uniform without agglomeration.
[0027] Furthermore, the S300 is added with a crosslinking agent and stirred at 150 rpm, so that the crosslinking agent and the base adhesive are fully reacted at a temperature of 60° C. for 60 minutes to form a stable crosslinking structure.
[0028] Furthermore, the S400 adds sodium bicarbonate as a pH regulator to adjust the pH value of the system to 7, the S500 is stirred at 150 rpm for 15 minutes and a preservative is added, a flow meter is used to control the speed of adding water to 5 L / min, deionized water is gradually added, and the stirring speed is increased to 300 rpm to fully mix the deionized water and the adhesive to form a uniform solution.
[0029] Compared with the prior art, the formula and preparation method of the waterborne polyurethane formaldehyde-free reaction glue have the following beneficial effects:
[0030] 1. The water-based polyurethane formaldehyde-free reaction adhesive prepared by the present invention not only has excellent bonding performance, but also has outstanding water resistance, heat resistance and chemical resistance. The improvement of these properties is due to the unique formula design and sophisticated preparation process. Through reasonable raw material ratio and cross-linking agent selection, the adhesive can achieve the performance level of traditional formaldehyde-containing adhesives or even higher while maintaining environmental protection. In addition, the adhesive of the present invention also has good flexibility and cold resistance, and can adapt to a variety of complex application environments.
[0031] 2. The water-based polyurethane formaldehyde-free reaction adhesive of the present invention adopts environmentally friendly raw materials, completely abandons the aldehyde compounds in traditional adhesives, fundamentally solves the problem of formaldehyde release, and meets modern environmental protection requirements. At the same time, through carefully selected plant extracts, nano-silicates and natural rubber latex raw materials, the environmental performance of the adhesive is further improved. This formaldehyde-free formula not only protects the health of users, but also reduces the burden on the environment. It is a powerful practice of green chemistry and sustainable development.
[0032] 3. The preparation method of the present invention is simple and easy to understand, easy to operate, and easy to realize industrial production. The quality and stability of the adhesive are guaranteed by accurate raw material weighing and deionized water quality control. At the same time, by gradually adding solid raw materials and cross-linking agents and controlling their addition speed and stirring speed, sufficient mixing and reaction of the adhesive components are guaranteed. In addition, the present invention also adds a pH regulator to make the pH of the reaction system reach a predetermined value, thereby ensuring the stable performance of the adhesive. This preparation process not only improves production efficiency, but also reduces production costs, and has broad market application prospects.
[0033] Other advantages, objectives and features of the present invention will be set forth in part in the following description and, in part, will be apparent to those skilled in the art based on an examination of the following or may be taught from the practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the prior art descriptions are briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention, and for ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.
[0035] Figure 1 This is a material composition diagram of a water-based polyurethane formaldehyde-free reaction adhesive.
[0036] Figure 2 The present invention is a flow chart of a method for preparing a formula of a water-based polyurethane formaldehyde-free reaction adhesive. DETAILED DESCRIPTION
[0037] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0038] A formula of a water-based polyurethane formaldehyde-free reaction adhesive, characterized in that the formaldehyde-free reaction adhesive material consists of:
[0039] Polyurethane prepolymer: As the basis of water-based polyurethane formaldehyde-free reaction adhesive, it provides the basic framework and performance of the adhesive. It is first added to the reactor, and the agitator is turned on and stirred at a low speed to make it evenly distributed in the reactor;
[0040] Reinforced and modified materials: Plant extract soybean oil is used to enhance the water resistance and heat resistance of adhesives, providing additional functionality for adhesives, while nano-silicate has excellent dispersibility and stability, which can improve the overall performance of adhesives;
[0041] Auxiliary raw materials: Natural rubber latex is used as an auxiliary raw material to increase the viscosity and flexibility of the adhesive;
[0042] Functional additives: cross-linking agents based on polycarbodiimide are used to form cross-linking structures between polyurethane prepolymers to improve the strength and stability of the adhesive. Sodium bicarbonate, a pH regulator, can quickly and accurately adjust the pH value of the adhesive to keep it within a stable working range. Environmentally friendly preservatives prevent the adhesive from being contaminated by microorganisms during storage and use.
[0043] Diluent: Deionized water is used as a diluent to reduce the viscosity of the adhesive, facilitate construction, and ensure the purity and stability of the adhesive.
[0044] Embodiment 1
[0045] A method for preparing a water-based polyurethane formaldehyde-free reaction adhesive, the method comprising the following steps: raw material preparation and pretreatment, mixing and stirring, cross-linking agent addition and reaction, pH adjustment, preservative addition, dilution and homogenization, finished product inspection and packaging, cleaning and maintenance.
[0046] First, enter the raw material preparation and pretreatment (S100), according to the formula ratio, use precise weighing equipment to weigh the required solid raw materials of polyurethane prepolymer, plant extract, nanosilicate, and natural rubber latex, and ensure that their quality is qualified and pollution-free. Use a conductivity meter to check the quality of deionized water to ensure that it is high-purity deionized water to avoid affecting the performance of the adhesive.
[0047] Next, enter the mixing and stirring (S200), first add the polyurethane prepolymer into the reactor, turn on the agitator, and stir at a low speed to make it evenly distributed in the reactor, gradually add the plant extract, nanosilicate and natural rubber latex, and gradually increase the stirring speed according to the mixing situation to ensure that the components are fully mixed and evenly without agglomeration. During the stirring process, closely observe the state of the mixture and appropriately adjust the stirring speed and time to ensure uniform mixing.
[0048] Subsequently, the crosslinking agent addition and reaction stage (S300) is entered. After the solid components are evenly mixed, an environmentally friendly crosslinking agent is added to the reactor. When adding the crosslinking agent, a metering pump device is used to control the addition speed to avoid local concentration being too high or too low. Stirring is continued to allow the crosslinking agent to fully react with the base adhesive to form a stable crosslinked structure. This process takes a certain amount of time. During the reaction, the reaction progress is monitored by sampling and analysis methods to ensure that the crosslinking reaction is fully carried out.
[0049] Then, enter the pH adjustment stage (S400). After the cross-linking reaction proceeds to a certain extent, add the pH adjuster sodium bicarbonate to the reactor. According to the pH value of the reaction system, gradually add the adjuster until the pH value of the system reaches a predetermined value. In the process of adjusting the pH value, pay close attention to the changes in the pH value of the system, and use the agitator controller to adjust the stirring speed and the amount of addition in time to ensure the stability of the system.
[0050] Next, enter the preservative addition stage (S500). When the pH value of the system is adjusted to a predetermined value, add an environmentally friendly preservative into the reactor and stir to evenly disperse the preservative in the system to ensure that it effectively plays an anti-corrosion role. Continue stirring for a period of time to ensure that the preservative and the adhesive are fully mixed.
[0051] Secondly, enter the dilution and homogenization stage (S600). After the preservative is added, deionized water is gradually added to the reactor. During the water addition process, a flow meter is used to control the speed and amount of water addition to avoid foaming or stratification. The stirring speed is increased to fully mix the deionized water and the adhesive to form a uniform solution.
[0052] Finally, the finished product inspection and packaging stage (S700) is entered, and the prepared water-based polyurethane formaldehyde-free reaction glue is subjected to performance inspection, including viscosity, solid content, pH value, water resistance, and heat resistance indicators to ensure that the product meets quality requirements. The qualified products are packaged and marked with product name, production date, and shelf life information.
[0053] In addition, entering the cleaning and maintenance stage (S800), during the preparation process, the reactor and agitator equipment must be cleaned regularly to ensure the normal operation of the equipment and the quality of the product. The preparation equipment must be inspected and maintained regularly, and damaged parts and consumables must be replaced in time to ensure the normal operation of the equipment.
[0054] Through the implementation of the steps in the above embodiments, a formula preparation method for a water-based polyurethane formaldehyde-free reaction glue that meets the requirements is successfully processed. The preparation method is simple, efficient, and low-cost, has important practical significance and broad market prospects, and produces water-based polyurethane formaldehyde-free reaction glues with stable performance and low cost. These reaction glues greatly reduce the pollution to the environment during production and use, and also ensure the health and safety of users during use.
[0055] Embodiment 2
[0056] This embodiment aims to describe in detail the specific preparation process of a water-based polyurethane formaldehyde-free reaction glue product and provide specific numerical monitoring results. We can comprehensively evaluate the overall performance of the reaction glue and provide data support for product quality control and performance improvement.
[0057] In the specific implementation, the mass percentages of the raw materials are accurately measured, including: polyurethane prepolymer: 72%, plant extract soybean oil: 10%, nanosilicate: 4%, natural rubber latex: 10%, polycarbodiimide-based cross-linking agent: 2.5%, pH adjuster sodium bicarbonate: 0.8%, environmentally friendly preservative: 0.5%, deionized water: the rest. The quality of the deionized water is checked using a conductivity meter to ensure that it is high-purity deionized water to avoid affecting the performance of the adhesive.
[0058] The weighed polyurethane prepolymer is added into the reactor, and the agitator is turned on and stirred at a low speed of 50 rpm to evenly distribute the prepolymer in the reactor. Subsequently, the plant extract soybean oil, nanosilicate and natural rubber latex solid raw materials are gradually added. During the addition process, the stirring speed is gradually increased to 150 rpm to ensure that all components are fully mixed without caking. After uniform mixing, it can be observed that the adhesive presents a uniform and delicate texture. In order to ensure that the cross-linking agent and the base adhesive fully react, it is necessary to control the addition speed of the cross-linking agent and maintain the stirring speed at 150 rpm. At the same time, the temperature of the reactor is controlled at 60°C, so that the cross-linking agent and the base adhesive fully react at a suitable temperature for 60 minutes to form a stable cross-linked structure. During the reaction process, it can be observed that the viscosity of the adhesive gradually increases to form a stable gel-like substance. After the cross-linking reaction is completed, the pH value of the adhesive needs to be adjusted. By adding the pH adjuster sodium bicarbonate, the pH value of the system is adjusted to 7. When adding the pH adjuster, it is necessary to stir while adding. , ensure that the pH value is evenly distributed. After the pH value is adjusted, add an environmentally friendly preservative. The selection of preservatives needs to take into account its inhibitory effect on microorganisms and its impact on the performance of the adhesive. After adding the preservative, continue stirring at 150rpm for 15 minutes to evenly disperse the preservative in the system and play an anti-corrosion role. After the preservative is added, begin to gradually add deionized water for dilution. The speed and amount of water addition are controlled by the flow meter. At the same time, increase the stirring speed to 200rpm to fully mix the deionized water and the adhesive to form a uniform solution. Perform performance tests on the prepared products, including viscosity, pH value, and curing time. After ensuring that all indicators meet the quality requirements, package them and indicate the necessary information. The packaging materials need to be environmentally friendly and durable to ensure the safety of the product during transportation and use. After preparation, clean and maintain the equipment in a timely manner, thoroughly clean the reactor and agitator equipment, remove residual adhesive, and regularly inspect and maintain the equipment to ensure the normal operation of the equipment and the quality of the product.
[0059] In summary, a formula of water-based polyurethane formaldehyde-free reaction adhesive with excellent heat resistance can be prepared, and precise control of the performance of the reaction adhesive can be achieved. The improvement of these properties is due to the unique formula design and sophisticated preparation process. Through reasonable raw material ratio and cross-linking agent selection, the adhesive can achieve the performance level of traditional formaldehyde-containing adhesives or even higher while maintaining environmental protection, thereby improving the environmental performance of the adhesive. This formaldehyde-free formula not only protects the health of users, but also reduces the burden on the environment. It is a powerful practice of green chemistry and sustainable development.
[0060] Embodiment 3
[0061] The present embodiment aims to describe in detail the specific preparation process of a water-based polyurethane formaldehyde-free reaction glue product, and comprehensively evaluate the chemical resistance of the reaction glue by changing the raw material ratio and specific parameter data, so as to provide data support for the quality control and performance improvement of reaction glue products in different fields, so that it can meet the application requirements in various complex environments.
[0062] In the specific implementation, the raw material percentages of polyurethane prepolymer 72%, plant extract corn oil 10%, nano silicate 4%, natural rubber latex 10%, polycarbodiimide-based cross-linking agent 2.5%, pH adjuster sodium bicarbonate 0.8%, environmentally friendly preservative 0.5%, and the remaining part deionized water are selected, and the quality of the deionized water is checked using a conductivity meter to ensure that it is high-purity deionized water to avoid affecting the performance of the adhesive.
[0063] The weighed polyurethane prepolymer is added into the reactor, and the agitator is turned on and stirred at a low speed of 50 rpm to evenly distribute the prepolymer in the reactor. Subsequently, the plant extract soybean oil, nanosilicate and natural rubber latex solid raw materials are gradually added. During the addition process, the stirring speed is gradually increased to 200 rpm to ensure that all components are fully mixed without caking. After uniform mixing, it can be observed that the adhesive presents a uniform and delicate texture. In order to ensure that the cross-linking agent and the base adhesive fully react, it is necessary to control the addition speed of the cross-linking agent and maintain the stirring speed at 200 rpm. At the same time, the temperature of the reactor is controlled at 65°C, so that the cross-linking agent and the base adhesive fully react at a suitable temperature for 70 minutes to form a stable cross-linked structure. During the reaction process, it can be observed that the viscosity of the adhesive gradually increases to form a stable gel-like substance. After the cross-linking reaction is completed, the pH value of the system is adjusted to 7.2 by adding the pH regulator sodium bicarbonate. When adding the pH adjuster, stir while adding it to ensure that the pH value is evenly distributed. After the pH value is adjusted, add the environmentally friendly preservative and continue stirring at 200rpm for 20 minutes to evenly disperse the preservative in the system and play an anti-corrosion role. After the preservative is added, begin to gradually add deionized water for dilution. The speed and amount of water addition are controlled by the flow meter. At the same time, increase the stirring speed to 200rpm to fully mix the deionized water and the adhesive to form a uniform solution. Perform performance tests on the prepared products, including viscosity, pH value, and curing time. After ensuring that all indicators meet the quality requirements, package them and indicate necessary information. The packaging materials need to be environmentally friendly and durable to ensure the safety of the product during transportation and use. After preparation, clean and maintain the equipment in a timely manner, thoroughly clean the reactor and agitator equipment, remove residual adhesive, and regularly inspect and maintain the equipment to ensure the normal operation of the equipment and the quality of the product.
[0064] Through the above embodiments, the present invention provides a formulation preparation method for a water-based polyurethane formaldehyde-free reaction adhesive, the reaction adhesive has improved water resistance, heat resistance and chemical resistance, the addition of nano-silicate improves the mechanical strength and heat resistance of the adhesive, and the natural rubber latex enhances the elasticity and adhesion of the reaction adhesive, the comprehensive improvement of these properties enables the reaction adhesive of the present invention to meet a wider range of application needs, especially in some fields with higher performance requirements.
[0065] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered exemplary and non-limiting in all respects, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations falling within the meaning and scope of the equivalent elements of the claims be included in the invention. Any reference numeral in a claim should not be considered as limiting the claim to which it relates.
Claims
1. A formula of a water-based polyurethane formaldehyde-free reaction adhesive, characterized in that: The material of the aldehyde-free reactive adhesive composition: Polyurethane prepolymer: As the basis of water-based polyurethane formaldehyde-free reaction adhesive, it provides the basic framework and performance of the adhesive. It is first added to the reactor, and the agitator is turned on and stirred at a low speed to make it evenly distributed in the reactor; Reinforced and modified materials: Plant extract soybean oil is used to enhance the water resistance and heat resistance of adhesives, providing additional functionality for adhesives, while nano-silicate has excellent dispersibility and stability, which can improve the overall performance of adhesives; Auxiliary raw materials: Natural rubber latex is used as an auxiliary raw material to increase the viscosity and flexibility of the adhesive; Functional additives: cross-linking agents based on polycarbodiimide are used to form cross-linking structures between polyurethane prepolymers to improve the strength and stability of the adhesive. Sodium bicarbonate, a pH regulator, can quickly and accurately adjust the pH value of the adhesive to keep it within a stable working range. Environmentally friendly preservatives prevent the adhesive from being contaminated by microorganisms during storage and use. Diluent: Deionized water is used as a diluent to reduce the viscosity of the adhesive, facilitate construction, and ensure the purity and stability of the adhesive.
2. The formulation of a water-based polyurethane formaldehyde-free reaction adhesive according to claim 1, characterized in that: The polyurethane prepolymer is used as the main raw material of the waterborne polyurethane formaldehyde-free reaction glue and its mass percentage is 60%-74%.
3. The formula of the water-based polyurethane formaldehyde-free reaction adhesive according to claim 1, characterized in that: The mass percentage of soybean oil, a plant extract, in the reinforcing and modifying material is 8%-12%, and nano-silicate and natural rubber latex are used as modifying materials and auxiliary raw materials in combination with the plant extract, and their proportions are 3%-7% and 8%-12% respectively.
4. The formula of the water-based polyurethane formaldehyde-free reaction adhesive according to claim 1, characterized in that: The environmentally friendly crosslinking agent in the functional additive promotes the crosslinking reaction between polyurethane prepolymers, and its mass percentage is 2%-4%. The pH value of the adhesive is adjusted to 0.5%-2%, and the mass percentage of the preservative based on natural plant extracts is 0.3%-1%.
5. The formula of the water-based polyurethane formaldehyde-free reaction adhesive according to claim 1, characterized in that: After the preservative is added, the deionized water is gradually added at a rate and amount controlled by a flow meter to control the speed and amount of water addition, and the stirring speed is increased to fully mix the deionized water and the adhesive to form a uniform solution.
6. A method for preparing a waterborne polyurethane formaldehyde-free reaction adhesive, characterized in that: The specific steps of the preparation method are: S100, raw material preparation and pretreatment: according to the formula ratio, use accurate weighing equipment to weigh the required solid raw materials of polyurethane prepolymer, plant extract, nanosilicate, and natural rubber latex, and ensure that they are of qualified quality and pollution-free. At the same time, check the high purity of deionized water; S200, Mixing and stirring: Stir the polyurethane prepolymer at a low speed in the reactor, gradually add other solid raw materials, and increase the stirring speed to ensure that all components are mixed evenly without lumps; S300, cross-linking agent addition and reaction: after the solid components are evenly mixed, an environmentally friendly cross-linking agent is added, and the addition speed is controlled so that the cross-linking agent and the base adhesive react fully to form a stable cross-linking structure; S400, pH adjustment: adjusting the pH value of the system by adding a pH adjusting agent, sodium bicarbonate, so that the reaction system tends to a stable state; S500, preservative addition: after pH adjustment, add environmentally friendly preservatives and continue stirring to make it evenly dispersed in the system to play an anti-corrosion role; S600, dilution and homogenization: gradually add deionized water, and control the speed and amount of water addition, while increasing the stirring speed to fully mix the deionized water and the adhesive to form a uniform solution; S700, Finished Product Inspection and Packaging: Perform performance inspection on the prepared products to ensure that all indicators meet quality requirements, and then package and mark the necessary information; S800, Cleaning and Maintenance: Clean and maintain the equipment regularly to ensure the normal operation of the equipment and the quality of the products.
7. The method for preparing a water-based polyurethane formaldehyde-free reaction adhesive according to claim 6, characterized in that: The raw material ratio of the S100 is: 70% polyurethane prepolymer, 10% plant extract soybean oil, 5% nano-silicate, 10% natural rubber latex, 3% polycarbodiimide-based crosslinking agent, 1% pH regulator sodium bicarbonate, 0.5% preservative, and the rest is deionized water.
8. The method for preparing a water-based polyurethane formaldehyde-free reaction adhesive according to claim 6, characterized in that: The S200 is used to stir the polyurethane prepolymer in the reaction kettle at a low speed of 50 rpm, and the stirring speed is gradually increased to 150 rpm to ensure that the components are fully mixed and uniform without agglomeration.
9. The method for preparing a water-based polyurethane formaldehyde-free reaction adhesive according to claim 6, characterized in that: The S300 was added with a crosslinking agent and stirred at 150 rpm to allow the crosslinking agent and the base adhesive to fully react at a temperature of 60° C. for 60 minutes to form a stable crosslinking structure.
10. The method for preparing a water-based polyurethane formaldehyde-free reaction adhesive according to claim 6, characterized in that: The S400 was added with a pH regulator, sodium bicarbonate, to adjust the pH value of the system to 7. The S500 was stirred at 150 rpm for 15 minutes and a preservative was added. A flow meter was used to control the speed of adding water to 5 L / min. Deionized water was gradually added, and the stirring speed was increased to 300 rpm to fully mix the deionized water and the adhesive to form a uniform solution.
Citation Information
Cited By
Two-component polyurethane adhesive for OSB (oriented strand board) and application of two-component polyurethane adhesive