Synthesis process of smoke suppression biomass-based phosphorus-containing flame retardant

Through the combination of water-soluble rosin-based phosphorus-based cross-linked flame retardants and smoke-suppressing multi-metal complex phosphorus-based cross-linked flame retardants, a smoke-suppressing biomass-based phosphorus-containing flame retardant is formed, which solves the problem of phosphorus-based flame retardants. Solve the problems of agent smoke and environmental impact, achieving efficient flame retardant performance and environmental protection performance.

CN118755487APending Publication Date: 2024-10-11DEHUA TB NEW DECORATION MATERIAL CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410741915.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-11
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Existing phosphorus-based flame retardants are prone to produce smoke and toxic substances when burned, and have potential impacts on the environment. The pollutants produced by burning bromine-based flame retardants are harmful to human health, limiting their development.

Method used

Water-soluble rosin-based phosphorus-based cross-linked flame retardants and smoke-suppressing multi-metal complex phosphorus-based cross-linked flame retardants are used to synthesize smoke-suppressing biomass-based phosphorus-containing flame retardants, using phosphorus, nitrogen, and silicon elements. The synergistic effect forms non-flammable gas and dense carbon layer, reducing the generation of smoke and toxic substances.

Benefits of technology

It achieves efficient flame retardant performance, reduces the release of smoke and toxic substances, and improves fire safety performance. The flame retardant is derived from renewable resources, has excellent environmental performance, and meets the requirements of green chemistry.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118755487A_ABST
    Figure CN118755487A_ABST
Patent Text Reader

Abstract

The invention relates to a synthesis process of a smoke suppression biomass-based phosphorus-containing flame retardant. The preparation method comprises the following steps: preparing phosphorus-containing and nitrogen-containing structural flame-retardant polyol, synthesizing a water-soluble rosin-based flame-retardant modifier, preparing a water-soluble rosin-based phosphorus cross-linked flame retardant, preparing a phosphorus / nitrogen / silicon multi-flame-retardant element compound, preparing a novel multi-metal complex flame-retardant modifier, and preparing a smoke-suppression multi-metal complex phosphorus cross-linked flame retardant. According to the preparation method, an intermediate synthesis method, a liquid phase method and a calcination method are creatively combined, and the prepared material has the advantages of being excellent in flame retardance, good in environmental protection performance, good in heat resistance and chemical resistance, excellent in adhesive performance and the like and has wide application prospects in the fields of home decoration, machine manufacturing and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a synthesis process of a smoke-suppressing biomass-based phosphorus-containing flame retardant, and belongs to the field of flame retardant materials. Background Art

[0002] The technical research of phosphorus-based flame retardants is developing rapidly. Organic flame retardants are gradually developing from small molecules to polymer-type macromolecules and organic-inorganic composites. New varieties of efficient, environmentally friendly and non-toxic composite flame retardants are the future development trend of flame retardants.

[0003] In addition to inorganic flame retardants, brominated flame retardants are still the main ones in the world. However, when brominated flame retardants burn, they easily form polybrominated benzoxazolines (PBDD) and polybrominated dibenzofurans (PBDF), which can damage human organs and produce a large amount of smoke that can suffocate people. Therefore, the development of halogenated flame retardants is subject to certain restrictions.

[0004] Transition metals have excellent flame retardant properties in polymer matrices. Introducing transition metal elements into polymers as part of flame retardants has attracted great attention from researchers. The catalytic carbonization of transition metals during polymer combustion is the key part of the flame retardant effect of metal compounds. Among them, phosphorus-containing flame retardants have high flame retardant efficiency, good thermal stability, and extremely low volatility. In particular, reactive organic phosphorus flame retardants (containing alcohol hydroxyl or amino groups) can be firmly combined with polymer chains, and the flame retardant effect is more durable. Phosphite flame retardants are an important branch of phosphorus flame retardants. They not only have the flame retardant plasticizing effect unique to phosphate flame retardants, but also have antioxidant effects. However, there are still some areas for improvement in phosphorus flame retardants. Organic phosphorus products are mostly oily and not easy to add directly. They are more selective in processing technology, so they are mostly used in polyurethane foam, soft PVC, transformer oil, cellulose resin, natural and synthetic rubber. However, phosphorus compounds have a certain impact on the water quality, plants, animals and microorganisms in the soil in the surrounding environment. Summary of the invention

[0005] In order to overcome the above technical problems existing in the prior art, the object of the present invention is to provide a synthesis process of a smoke-suppressing biomass-based phosphorus-containing flame retardant.

[0006] The first technical purpose of the present invention is to prepare a water-soluble rosin-based phosphorus-based cross-linked flame retardant.

[0007] The first technical purpose of the present invention is to prepare a smoke-suppressing multi-metal complex phosphorus-based cross-linked flame retardant.

[0008] The third technical purpose of the present invention is to prepare a smoke-suppressing biomass-based phosphorus-containing flame retardant.

[0009] The present invention provides a preparation method of a synthetic process for a smoke-suppressing biomass-based phosphorus-containing flame retardant, which specifically comprises the following steps: preparation of phosphorus- and nitrogen-containing flame-retardant polyols, synthesis of a water-soluble rosin-based flame-retardant modifier, a water-soluble rosin-based phosphorus-based cross-linked flame retardant, a phosphorus / nitrogen / silicon multi-flame-retardant element compound, a novel multi-metal complex flame-retardant modifier, a smoke-suppressing multi-metal complex phosphorus-based cross-linked flame retardant, and preparation of a smoke-suppressing biomass-based phosphorus-containing flame retardant.

[0010] Preferably, step (1) preparation of phosphorus- and nitrogen-containing flame retardant polyols

[0011] The paraformaldehyde, ethanolamine and tris(hydroxymethyl)aminomethane (THAM) are mixed for reaction, the paraformaldehyde, ethanolamine and tris(hydroxymethyl)aminomethane (THAM) are added into a container equipped with a constant pressure dropping funnel and a reflux condenser, stirred for reaction, and heated for reaction under nitrogen protection, wherein the ethanol solution of the aromatic phenol compound can be the ethanol solution of the aromatic phenol compound, and the obtained phosphorus-containing and nitrogen-containing flame retardant polyol is prepared;

[0012] Step (2) Synthesis of water-soluble rosin-based flame retardant modifier

[0013] Abietic acid, formic acid, concentrated H 2 SO 4 (sulfuric acid) is added to a three-necked flask equipped with a thermometer and a condenser, the temperature is raised, and hydrogen peroxide is added dropwise under stirring. After the addition is completed, the reaction is continued for a period of time, and the reaction is continued under reflux for a period of time. The product is allowed to stand for stratification, and the lower layer of waste liquid is separated. The oil layer is poured into a three-necked flask, and a catalyst and the phosphorus- and nitrogen-containing flame retardant polyol obtained in step (1) are added. The reaction is carried out under reduced pressure at high temperature for several hours to obtain a water-soluble rosin-based flame retardant modifier;

[0014] Step (3) Water-soluble rosin-based phosphorus cross-linked flame retardant

[0015] Tetrakis(hydroxymethyl)phosphonium chloride, formaldehyde aqueous solution, distilled water, and the phosphorus- and nitrogen-containing flame retardant polyol prepared in step (1) are sequentially added into a round-bottom flask, and refluxed for a period of time to obtain an intermediate product of tetraethylenepentamineheptamethylenephosphonic acid (TEPAHP), and then the water-soluble rosin-based flame retardant modifier prepared in step (2) is added, and aminated with urea in a beaker to obtain tetraethylenepentamineheptamethylenephosphonic acid ammonium salt (ATEPAHP), and purified with ethanol to obtain a water-soluble rosin-based phosphorus-based cross-linked flame retardant;

[0016] Step (4) Phosphorus / nitrogen / silicon multi-flame retardant element compound

[0017] The ethanol and hydrochloric acid aqueous solution provide the water required for the hydrolysis reaction and are added to a single-mouth bottle, and mixed evenly at a certain temperature; MEL-KH dissolved in ethylene glycol is taken, and DOPO-VTMS (full name 9,10-dihydro-9-oxa-10-phosphophananthrene-10-oxa (DOPO)-vinyltrimethoxysilane adduct) and MTMS (methyltrimethoxysilane) are uniformly mixed into anhydrous ethanol, and then slowly added dropwise to the hydrolysis system. After the addition is completed, the hydrolysis reaction is continued, and finally triethylamine is added to neutralize the hydrochloric acid to obtain a phosphorus / nitrogen / silicon multi-flame retardant element compound dissolved in a mixed solvent of ethanol and ethylene glycol;

[0018] Step (5) Novel multi-metal complex flame retardant modifier

[0019] Weigh glutathione and dissolve it completely in distilled water. Add copper sulfate solution dropwise to the glutathione aqueous solution. Adjust the pH with NaOH (sodium hydroxide) solution. Stir the reaction at a certain temperature. Dissolve the MgCl 2 (MgCl2) is slowly added to the ligand system and reacted for a period of time, then cooled and placed to obtain a metal complex. 3 ) 3 ·5H 2 O (bismuth nitrate pentahydrate) and KCl (potassium chloride) are dissolved in a mannitol solution, and ferrous sulfate, stannous sulfate, and the phosphorus / nitrogen / silicon multi-flame retardant element compound prepared in step (4) are added to the above solution respectively, and after ultrasonic treatment, a uniform solution is formed by stirring, and then stirred under magnetic stirring at room temperature, and the obtained solution is transferred to a polytetrafluoroethylene-lined autoclave, and reacted, cooled to room temperature, and a precipitate is obtained, and filtered several times with hydrogen peroxide and ethanol. As the amount of hydrogen peroxide increases, the decomposed free radicals HOO· and hydroxyl free radicals increase as bleaching active components, and after drying, a novel multi-metal complex flame retardant modifier is obtained;

[0020] Step (6) Smoke-suppressing multimetallic complex phosphorus-based cross-linked flame retardant

[0021] 3-aminopropylsilane, phosphorous acid, formaldehyde aqueous solution, and tetrakis(hydroxymethyl)phosphonium chloride are sequentially added into a round-bottom flask, and the mixed solution is refluxed under magnetic stirring. After the solution is cooled, it is poured into a beaker, and then urea and the novel multi-metal complex flame retardant modifier prepared in step (5) are added into the beaker to obtain a smoke-suppressing multi-metal complex phosphorus-based cross-linked flame retardant.

[0022] Step (7) Preparation of smoke-suppressing biomass-based phosphorus-containing flame retardant

[0023] The water-soluble rosin-based phosphorus-based cross-linked flame retardant prepared in step (3) and the smoke-suppressing multimetallic complex phosphorus-based cross-linked flame retardant prepared in step (6) are prepared by ultrasonic dispersion compatibility to obtain a smoke-suppressing biomass-based phosphorus-containing flame retardant, which is then calcined in a muffle furnace in an air atmosphere at a certain temperature through thermal weight loss under nitrogen conditions to obtain a smoke-suppressing biomass-based phosphorus-containing flame retardant.

[0024] The first technical purpose of the present invention is achieved through the following technical solutions:

[0025] Preferably, step (1) preparation of phosphorus- and nitrogen-containing flame retardant polyols

[0026] The paraformaldehyde, ethanolamine and tris(hydroxymethyl)aminomethane (THAM) are mixed for reaction, and the paraformaldehyde, ethanolamine and tris(hydroxymethyl)aminomethane (THAM) are added into a container equipped with a constant pressure dropping funnel and a reflux condenser, and the reaction is stirred at 15-20°C for 0.5-1.0h; the temperature of the temperature-raising reaction under nitrogen protection can be 60-80°C, and the temperature-raising reaction time can be 2-4h. The ethanol solution of the aromatic phenol compound can use an ethanol solution of the aromatic phenol compound with a mass fraction of 30%-50%; the reflux reaction time can be 2-4h; and the phosphorus-containing and nitrogen-containing flame-retardant polyol is prepared.

[0027] The invention has the advantages of excellent flame retardant performance. The phosphorus- and nitrogen-containing flame retardant polyol can produce non-combustible gases such as nitrogen and water vapor through its unique molecular design, effectively dilute the oxygen concentration in the air, take away part of the heat, and reduce the combustion temperature, thereby achieving an excellent flame retardant effect.

[0028] This flame retardant polyol does not contain harmful substances such as halogens. The introduction of phosphorus and nitrogen improves the thermal stability of the flame retardant polyol. There is a synergistic and synergistic effect between the flame retardant elements of phosphorus and nitrogen, making the flame retardant performance more durable and stable. The flame retardant polyol can reduce the generation of smoke, reduce the release of toxic substances, and improve fire safety performance.

[0029] Preferably, step (2) the synthesis of a water-soluble rosin-based flame retardant modifier

[0030] Abietic acid, formic acid, concentrated H 2 SO 4 Add to a three-necked flask equipped with a thermometer and a condenser, raise the temperature to 30-35°C, add hydrogen peroxide dropwise under stirring, react at 45-75°C for 25-30 minutes, heat under reflux for 55-60 minutes, let the product stand for stratification, separate the lower layer of waste liquid, pour the oil layer into a three-necked flask, add a catalyst and the phosphorus- and nitrogen-containing flame retardant polyol obtained in step (1), react at high temperature under reduced pressure for several hours to obtain a water-soluble rosin-based flame retardant modifier.

[0031] The invention has the advantage that the water-soluble rosin-based flame retardant modifier improves the phenomenon of mutual attraction and aggregation caused by the neat molecular structure due to molecular chain saturation, thereby improving the storage stability and low-temperature performance of the polyol.

[0032] The introduction of water-soluble rosin-based flame retardant modifiers can improve stability, giving it better construction performance and long-term stability.

[0033] Preferably, in step (3), a water-soluble rosin-based phosphorus-based cross-linked flame retardant

[0034] 15-19 g of tetrakis(hydroxymethyl)phosphonium chloride, 0.50-0.90 mol of 30-37% formaldehyde aqueous solution, 15-20 L of distilled water, and 55-60 g of the phosphorus- and nitrogen-containing flame retardant polyol prepared in step (1) are sequentially added into a 245-250 mL round-bottom flask, and refluxed for 1-3 h to obtain an intermediate product of tetraethylenepentamineheptamethylenephosphonic acid (TEPAHP). Then, 80-85 g of the water-soluble rosin-based flame retardant modifier prepared in step (2) is added, and 0.5-0.9 mol of urea is stirred and aminated in a beaker for 1-5 h to obtain tetraethylenepentamineheptamethylenephosphonic acid ammonium salt (ATEPAHP). After purification with ethanol, a water-soluble rosin-based phosphorus-based cross-linked flame retardant is obtained.

[0035] The invention has the advantage that the phosphorus-based flame retardant can form a dense foam carbon layer when heated, which plays the role of heat insulation, oxygen isolation and smoke suppression. The cross-linked phosphorus-containing flame retardant usually has the characteristics of low toxicity and has little harm to the environment and human health. The compound use of the water-soluble rosin-based phosphorus-based cross-linked flame retardant and other flame retardants can achieve a higher flame retardant grade without sacrificing other properties of the material.

[0036] The second technical purpose of the present invention is achieved through the following technical solutions:

[0037] Preferably, in step (4), phosphorus / nitrogen / silicon multi-flame retardant element compound

[0038] 1-5g of ethanol and a hydrochloric acid aqueous solution with a pH value of 1-5 provide water required for the hydrolysis reaction, and the molar ratio of water to alkoxy is 0.5-1.0:1-5, which are added into a single-mouth bottle and mixed evenly at 35-40°C; MEL-KH dissolved in ethylene glycol is taken, and DOPO-VTMS and MTMS are evenly mixed into 1-5g of anhydrous ethanol, and then slowly added to the hydrolysis system at a speed of 1-2 drops per second, and after the addition is completed, the hydrolysis reaction is continued at 35-40°C for 25-30 minutes, and finally triethylamine is added to neutralize the hydrochloric acid to obtain a phosphorus / nitrogen / silicon multi-flame retardant element compound dissolved in a mixed solvent of ethanol and ethylene glycol.

[0039] The advantage of adopting the present invention is that the phosphorus / nitrogen / silicon multi-flame retardant element compound can also improve the mechanical properties, processing properties, and heat resistance, forming a more comprehensive and three-dimensional flame retardant system. The addition of silicon element can improve the thermal stability of the carbon layer on the surface of the material, inhibit the oxidation of the phosphorus-containing carbon layer under high temperature conditions, and form a more stable carbon layer with better barrier effect.

[0040] The phosphorus / nitrogen / silicon multi-flame retardant element compound has good compatibility, ensuring the uniform distribution and effective action of the flame retardant, has good thermal stability and mechanical properties, significantly improves the limiting oxygen index, and shows a significant dual-phase flame retardant effect.

[0041] Preferably, in step (5), a novel multi-metal complex flame retardant modifier is used.

[0042] Weigh 0.1-0.5mmol glutathione and dissolve it completely in 1-5ml distilled water. Add 0.1-0.5mol / L copper sulfate solution to the glutathione aqueous solution, adjust the pH to 3-5 with NaOH solution, stir the reaction at 30-35℃, and dissolve the MgCl 2 Slowly add the ligand system to react for 15-20 minutes, cool and place for 12-24 hours to obtain a metal complex. 3 ) 3 ·5H 2 O and 0.5-1.0g KCl are dissolved in 100-110mL mannitol solution, and ferrous sulfate, stannous sulfate, and the phosphorus / nitrogen / silicon multi-flame retardant element compound prepared in step (4) are added to the above solution respectively. After ultrasonic treatment for 5-10min, the solution is stirred for 25-30min to form a uniform solution. The solution is then stirred under magnetic stirring at room temperature for 1-3h. The obtained solution is transferred to a polytetrafluoroethylene-lined autoclave and reacted at 150-180°C for 5-10h. After the reaction is completed, the solution is cooled to room temperature to obtain a precipitate, which is filtered 1-3 times with hydrogen peroxide and ethanol. As the amount of hydrogen peroxide increases, the decomposed free radicals HOO· and hydroxyl radicals increase as bleaching active components. After drying at 50-80°C, a novel multi-metal complex flame retardant modifier is obtained.

[0043] The invention has the advantage that the novel multi-metal complex flame retardant modifier can more effectively capture active free radicals in the gas phase through its unique complex structure and the synergistic effect of multi-metal elements, thereby significantly improving the flame retardant performance.

[0044] The third technical objective of the present invention is achieved through the following technical solutions:

[0045] Preferably, step (6) includes a smoke-suppressing multimetallic complex phosphorus-based cross-linked flame retardant

[0046] 20-25 g of 3-aminopropylsilane, 15-20 g of phosphorous acid, 0.1-0.5 mol of formaldehyde aqueous solution and 10-15 g of tetrakis(hydroxymethyl)phosphonium chloride are sequentially added into a 200-250 mL round-bottom flask. The mixed solution is refluxed for 1-6 h under magnetic stirring. After the solution is cooled, it is poured into a 450-500 mL beaker. Subsequently, 0.1-0.5 mol of urea and the novel multi-metal complex flame retardant modifier prepared in step (5) are added into the beaker to obtain a smoke-suppressing multi-metal complex phosphorus-based cross-linked flame retardant.

[0047] The advantage of adopting the present invention is that the flame retardant combines the stability of the multi-metal complex and the high efficiency of the phosphorus-based flame retardant, can effectively capture active free radicals during the combustion process, interrupt the combustion chain reaction, and through the design of the cross-linked structure, can further enhance the weather resistance and durability of the material, which is conducive to significantly improving the flame retardant properties of the material.

[0048] Preferably, step (7) is to prepare a smoke suppressant biomass-based phosphorus-containing flame retardant.

[0049] The water-soluble rosin-based phosphorus-based cross-linked flame retardant prepared in step (3) and the smoke-suppressing multimetallic complex phosphorus-based cross-linked flame retardant prepared in step (6) are ultrasonically dispersed and compatible in a ratio of 1-2:1-5 and 2-5:3-5 to obtain a smoke-suppressing biomass-based phosphorus-containing flame retardant, and the smoke-suppressing biomass-based phosphorus-containing flame retardant is obtained by thermal weight loss under nitrogen conditions and calcination in a muffle furnace in an air atmosphere at 95-100°C and 110-115°C.

[0050] The advantages of adopting the present invention are that the biomass-based flame retardant is derived from renewable resources, has good sustainability and renewability, generates less environmental pollution during the preparation process, and complies with the concept of environmental protection; the smoke suppression property improves its environmental protection, helps to reduce dependence on limited resources, and also helps to reduce production costs, thereby promoting the widespread application of flame retardants.

[0051] In summary, the present invention has the following beneficial effects:

[0052] 1. The advantage of the present invention is that it has excellent flame retardant properties. The phosphorus- and nitrogen-containing flame retardant polyol can produce non-combustible gases such as nitrogen and water vapor through its unique molecular structure design, effectively dilute the oxygen concentration in the air, take away part of the heat, and reduce the combustion temperature, thereby achieving an excellent flame retardant effect.

[0053] 2. The advantage of adopting the present invention is that the flame retardant polyol does not contain harmful substances such as halogens, the introduction of phosphorus and nitrogen improves the thermal stability of the flame retardant polyol, and there is a synergistic and synergistic effect between the flame retardant elements of phosphorus and nitrogen, making the flame retardant performance more durable and stable. The flame retardant polyol can reduce the generation of smoke, reduce the release of toxic substances, and improve fire safety performance.

[0054] 3. The present invention has the advantage that the water-soluble rosin-based flame retardant modifier improves the phenomenon of mutual attraction and aggregation caused by the neat molecular structure caused by molecular chain saturation, thereby improving the storage stability and low-temperature performance of the polyol.

[0055] 4. The present invention has the advantage that the introduction of the water-soluble rosin-based flame retardant modifier can improve the adhesion and stability of the flame retardant, so that it has better construction performance and long-term stability;

[0056] 5. The present invention has the advantage that the phosphorus-based flame retardant can form a dense foam carbon layer when heated, which plays the role of heat insulation, oxygen isolation and smoke suppression. The cross-linked phosphorus-containing flame retardant is usually low in toxicity and has little harm to the environment and human health. The compound use of water-soluble rosin-based phosphorus-based cross-linked flame retardant and other flame retardants can achieve a higher flame retardant grade without sacrificing other properties of the material.

[0057] 6. The present invention has the advantage that the water-soluble rosin-based phosphorus cross-linked flame retardant is water-soluble and can be more easily mixed with water-soluble polymers such as amino resins, which is beneficial to the uniform distribution and effective action of the flame retardant.

[0058] 7. The advantage of adopting the present invention is that the phosphorus / nitrogen / silicon multi-flame retardant element compound can also improve the mechanical properties, processing properties, and heat resistance, forming a more comprehensive and three-dimensional flame retardant system. The addition of silicon element can improve the thermal stability of the carbon layer on the surface of the material, inhibit the oxidation of the phosphorus-containing carbon layer under high temperature conditions, and form a more stable carbon layer with better barrier effect.

[0059] 8. The advantage of adopting the present invention is that the phosphorus / nitrogen / silicon multi-flame retardant element compound has good compatibility, ensuring the uniform distribution and effective effect of the flame retardant. When the phosphorus-nitrogen flame retardant system is added to the epoxy resin to obtain a flame retardant composite material, it has good thermal stability and mechanical properties, and the limiting oxygen index is significantly improved, showing a significant dual-phase flame retardant effect.

[0060] 9. The advantage of the present invention is that the novel multi-metal complex flame retardant modifier can more effectively capture active free radicals in the gas phase through its unique complex structure and the synergistic effect of multi-metal elements, thereby significantly improving the flame retardant performance.

[0061] 10. The advantage of adopting the present invention is that the flame retardant combines the stability of the multi-metal complex and the high efficiency of the phosphorus-based flame retardant, can effectively capture active free radicals during the combustion process, interrupt the combustion chain reaction, and through the design of the cross-linked structure, can further enhance the weather resistance and durability of the material, which is conducive to significantly improving the flame retardant properties of the material.

[0062] 11. The advantages of adopting the present invention are that the biomass-based flame retardant is derived from renewable resources, has good sustainability and renewability, generates less environmental pollution during the preparation process, and complies with the concept of environmental protection; the smoke suppression property improves its environmental protection, helps to reduce dependence on limited resources, and also helps to reduce production costs, promoting the widespread application of flame retardants. BRIEF DESCRIPTION OF THE DRAWINGS

[0063] Figure 1 The present invention is a flow chart of the synthesis process of a smoke-suppressing biomass-based phosphorus-containing flame retardant. DETAILED DESCRIPTION

[0064] Example 1

[0065] Step (1) Preparation of phosphorus- and nitrogen-containing flame-retardant polyols

[0066] The paraformaldehyde, ethanolamine and tris(hydroxymethyl)aminomethane (THAM) are mixed for reaction, and the paraformaldehyde, ethanolamine and tris(hydroxymethyl)aminomethane (THAM) are added into a container equipped with a constant pressure dropping funnel and a reflux condenser, and stirred at 15°C for reaction for 0.6h; the temperature of the temperature-raising reaction under nitrogen protection can be 70°C, and the temperature-raising reaction time can be 3h, and the ethanol solution of the aromatic phenol compound can be an ethanol solution of the aromatic phenol compound with a mass fraction of 40%; the reflux reaction time can be 3h; and the phosphorus-containing and nitrogen-containing flame-retardant polyol is prepared;

[0067] Step (2) Synthesis of water-soluble rosin-based flame retardant modifier

[0068] Abietic acid, formic acid, concentrated H 2 SO 4 Add to a three-necked flask equipped with a thermometer and a condenser, raise the temperature to 35°C, add hydrogen peroxide dropwise while stirring, react at 50°C for 25 minutes, heat under reflux for 55 minutes, let the product stand for stratification, separate the lower layer of waste liquid, pour the oil layer into a three-necked flask, add the catalyst and the phosphorus- and nitrogen-containing flame retardant polyol obtained in step (1), react at high temperature and under reduced pressure for several hours to obtain a water-soluble rosin-based flame retardant modifier;

[0069] Step (3) Water-soluble rosin-based phosphorus cross-linked flame retardant

[0070] 18.93 g of tetrakis(hydroxymethyl)phosphonium chloride, 0.70 mol of 37% formaldehyde aqueous solution, 20 L of distilled water, and 57.40 g of the phosphorus- and nitrogen-containing flame retardant polyol prepared in step (1) are sequentially added into a 250 mL round-bottom flask, and refluxed for 3 h to obtain an intermediate product of tetraethylenepentamineheptamethylenephosphonic acid (TEPAHP). Then, 84.00 g of the water-soluble rosin-based flame retardant modifier prepared in step (2) is added, and aminated with 0.70 mol of urea in a beaker for 1 h to obtain tetraethylenepentamineheptamethylenephosphonic acid ammonium salt (ATEPAHP). After purification with ethanol, a water-soluble rosin-based phosphorus-based cross-linked flame retardant is obtained.

[0071] Step (4) Phosphorus / nitrogen / silicon multi-flame retardant element compound

[0072] 5g of ethanol and a hydrochloric acid aqueous solution with a pH of 3 provide the water required for the hydrolysis reaction. The molar ratio of water to alkoxy is 0.8:1. They are added into a single-mouth bottle and mixed evenly at 40°C. MEL-KH dissolved in ethylene glycol is taken, and DOPO-VTMS and MTMS are evenly mixed into 5g of anhydrous ethanol, and then slowly added to the hydrolysis system at a rate of 1 drop per second. After the addition is completed, the hydrolysis reaction is continued at 40°C for 30 minutes. Finally, triethylamine is added to neutralize the hydrochloric acid to obtain a phosphorus / nitrogen / silicon multi-flame retardant element compound dissolved in a mixed solvent of ethanol and ethylene glycol.

[0073] Step (5) Novel multi-metal complex flame retardant modifier

[0074] Weigh 0.5mmol glutathione and dissolve it completely in 5ml distilled water. Add 0.1mol / L copper sulfate solution to the glutathione aqueous solution, adjust the pH to 3 with NaOH solution, stir the reaction at 30℃, and dissolve the MgCl 2 After slowly adding the ligand system to react for 15 min, cooling and standing for 24 h, a metal complex was obtained. 4.8507 g Bi(NO 3 ) 3 ·5H 2 O and 0.7455g KCl are dissolved in 110mL mannitol solution, and ferrous sulfate, stannous sulfate, and the phosphorus / nitrogen / silicon multi-flame retardant element compound prepared in step (4) are added to the above solution respectively. After ultrasonication for 10 minutes, stirring is carried out for 30 minutes to form a uniform solution. Subsequently, stirring is carried out at room temperature under magnetic stirring for 3 hours. The obtained solution is transferred to a polytetrafluoroethylene-lined autoclave and reacted at 180°C for 10 hours. After the reaction is completed, the solution is cooled to room temperature to obtain a precipitate, which is filtered once with hydrogen peroxide and ethanol. As the amount of hydrogen peroxide increases, the decomposed free radicals HOO· and hydroxyl radicals increase as bleaching active components. After drying at 80°C, a novel multi-metal complex flame retardant modifier is obtained;

[0075] Step (6) Smoke-suppressing multimetallic complex phosphorus-based cross-linked flame retardant

[0076] 22.14 g of 3-aminopropylsilane, 16.4 g of phosphorous acid, 0.2 mol of formaldehyde aqueous solution, and 12 g of tetrakis(hydroxymethyl)phosphonium chloride were added to a 250 mL round-bottom flask in sequence. The mixed solution was refluxed for 6 h under magnetic stirring. After the solution was cooled, it was poured into a 500 mL beaker. Subsequently, 0.2 mol of urea and the novel multimetallic complex flame retardant modifier prepared in step (5) were added to the beaker to obtain a smoke-suppressing multimetallic complex phosphorus-based cross-linked flame retardant.

[0077] Step (7) Preparation of smoke-suppressing biomass-based phosphorus-containing flame retardant

[0078] The water-soluble rosin-based phosphorus-based cross-linked flame retardant prepared in step (3) and the smoke-suppressing multimetallic complex phosphorus-based cross-linked flame retardant prepared in step (6) are ultrasonically dispersed and compatible at a ratio of 2:1 and 2:3 to obtain a smoke-suppressing biomass-based phosphorus-containing flame retardant, and the smoke-suppressing biomass-based phosphorus-containing flame retardant is obtained by thermal weight loss under nitrogen conditions and calcination in a muffle furnace in an air atmosphere at 100°C and 115°C.

[0079] Example 2

[0080] Step (1) Preparation of phosphorus- and nitrogen-containing flame-retardant polyols

[0081] The paraformaldehyde, ethanolamine and tris(hydroxymethyl)aminomethane (THAM) are mixed for reaction, and the paraformaldehyde, ethanolamine and tris(hydroxymethyl)aminomethane (THAM) are added into a container equipped with a constant pressure dropping funnel and a reflux condenser, and stirred at 15°C for reaction for 0.5h; the temperature of the temperature-raising reaction under nitrogen protection can be 80°C, and the temperature-raising reaction time can be 4h, and the ethanol solution of the aromatic phenol compound can be an ethanol solution of the aromatic phenol compound with a mass fraction of 50%; the reflux reaction time can be 2h; and the phosphorus-containing and nitrogen-containing flame-retardant polyol is prepared;

[0082] Step (2) Synthesis of water-soluble rosin-based flame retardant modifier

[0083] Abietic acid, formic acid, concentrated H 2 SO 4 Add to a three-necked flask equipped with a thermometer and a condenser, raise the temperature to 30°C, add hydrogen peroxide dropwise under stirring, react at 45°C for 26 minutes, heat under reflux for 56 minutes, let the product stand for stratification, separate the lower layer of waste liquid, pour the oil layer into a three-necked flask, add the catalyst and the phosphorus- and nitrogen-containing flame retardant polyol obtained in step (1), react at high temperature and under reduced pressure for several hours to obtain a water-soluble rosin-based flame retardant modifier;

[0084] Step (3) Water-soluble rosin-based phosphorus cross-linked flame retardant

[0085] 15 g of tetrakis(hydroxymethyl)phosphonium chloride, 0.50 mol of 30% formaldehyde aqueous solution, 20 L of distilled water, and 60 g of the phosphorus- and nitrogen-containing flame-retardant polyol prepared in step (1) are sequentially added into a 250 mL round-bottom flask, and refluxed for 3 h to obtain an intermediate product of tetraethylenepentamineheptamethylenephosphonic acid (TEPAHP). Then, 85 g of the water-soluble rosin-based flame-retardant modifier prepared in step (2) is added, and aminated with 0.9 mol of urea in a beaker for 5 h to obtain tetraethylenepentamineheptamethylenephosphonic acid ammonium salt (ATEPAHP). After purification with ethanol, a water-soluble rosin-based phosphorus-based cross-linked flame retardant is obtained.

[0086] Step (4) Phosphorus / nitrogen / silicon multi-flame retardant element compound

[0087] 1g of ethanol and a hydrochloric acid aqueous solution with a pH of 1 provide the water required for the hydrolysis reaction. The molar ratio of water to alkoxy is 0.5:1. The mixture is added into a single-mouth bottle and mixed evenly at 35°C. MEL-KH dissolved in ethylene glycol is taken, and DOPO-VTMS and MTMS are evenly mixed into 1g of anhydrous ethanol. The mixture is then slowly dripped into the hydrolysis system at a rate of 1 drop per second. After the dripping is completed, the hydrolysis reaction is continued at 35°C for 25 minutes. Finally, triethylamine is added to neutralize the hydrochloric acid, and a phosphorus / nitrogen / silicon multi-flame retardant element compound dissolved in a mixed solvent of ethanol and ethylene glycol is obtained.

[0088] Step (5) Novel multi-metal complex flame retardant modifier

[0089] Weigh 0.1mmol glutathione and dissolve it completely in 1ml distilled water. Add 0.1mol / L copper sulfate solution to the glutathione aqueous solution, adjust the pH to 3 with NaOH solution, stir the reaction at 31℃, and dissolve the MgCl 2 After slowly adding the ligand system to react for 16 min, cooling and standing for 12 h, a metal complex was obtained. 3 g Bi(NO 3 ) 3 ·5H 2 O and 0.5g KCl are dissolved in 100mL mannitol solution, and ferrous sulfate, stannous sulfate, and the phosphorus / nitrogen / silicon multi-flame retardant element compound prepared in step (4) are added to the above solution respectively. After ultrasonic treatment for 5 minutes, stirring is carried out for 25 minutes to form a uniform solution. Subsequently, stirring is carried out at room temperature under magnetic stirring for 1 hour. The obtained solution is transferred to a polytetrafluoroethylene-lined autoclave and reacted at 150°C for 5 hours. After the reaction is completed, the solution is cooled to room temperature to obtain a precipitate, which is filtered twice with hydrogen peroxide and ethanol. As the amount of hydrogen peroxide increases, the decomposed free radicals HOO· and hydroxyl radicals increase as bleaching active components. After drying at 50°C, a novel multi-metal complex flame retardant modifier is obtained;

[0090] Step (6) Smoke-suppressing multimetallic complex phosphorus-based cross-linked flame retardant

[0091] 20 g of 3-aminopropylsilane, 15 g of phosphorous acid, 0.1 mol of formaldehyde aqueous solution, and 10 g of tetrakis(hydroxymethyl)phosphonium chloride are sequentially added into a 200 mL round-bottom flask, and the mixed solution is refluxed for 1 h under magnetic stirring. After the solution is cooled, it is poured into a 450 mL beaker, and then 0.1 mol of urea and the novel multi-metal complex flame retardant modifier prepared in step (5) are added into the beaker to obtain a smoke-suppressing multi-metal complex phosphorus-based cross-linked flame retardant.

[0092] Step (7) Preparation of smoke-suppressing biomass-based phosphorus-containing flame retardant

[0093] The water-soluble rosin-based phosphorus-based cross-linked flame retardant prepared in step (3) and the smoke-suppressing multimetallic complex phosphorus-based cross-linked flame retardant prepared in step (6) are ultrasonically dispersed and compatible at a ratio of 1:1 and 2:3 to obtain a smoke-suppressing biomass-based phosphorus-containing flame retardant, which is then calcined in a muffle furnace in an air atmosphere at 95°C and 110°C by thermal weight loss under nitrogen conditions to obtain the smoke-suppressing biomass-based phosphorus-containing flame retardant.

[0094] Example 3

[0095] Step (1) Preparation of phosphorus- and nitrogen-containing flame-retardant polyols

[0096] The paraformaldehyde, ethanolamine and tris(hydroxymethyl)aminomethane (THAM) are mixed for reaction, and the paraformaldehyde, ethanolamine and tris(hydroxymethyl)aminomethane (THAM) are added into a container equipped with a constant pressure dropping funnel and a reflux condenser, and stirred at 16°C for reaction for 0.6h; the temperature of the temperature-raising reaction under nitrogen protection can be 70°C, and the temperature-raising reaction time can be 3h, and the ethanol solution of the aromatic phenol compound can be an ethanol solution of the aromatic phenol compound with a mass fraction of 40%; the reflux reaction time can be 3h; and the phosphorus-containing and nitrogen-containing flame-retardant polyol is prepared;

[0097] Step (2) Synthesis of water-soluble rosin-based flame retardant modifier

[0098] Abietic acid, formic acid, concentrated H 2 SO 4 Add to a three-necked flask equipped with a thermometer and a condenser, raise the temperature to 32°C, add hydrogen peroxide dropwise under stirring, react at 50°C for 27 minutes, heat under reflux for 57 minutes, let the product stand for stratification, separate the lower layer of waste liquid, pour the oil layer into a three-necked flask, add the catalyst and the phosphorus- and nitrogen-containing flame retardant polyol obtained in step (1), react at high temperature and under reduced pressure for several hours to obtain a water-soluble rosin-based flame retardant modifier;

[0099] Step (3) Water-soluble rosin-based phosphorus cross-linked flame retardant

[0100] 16 g of tetrakis(hydroxymethyl)phosphonium chloride, 0.60 mol of 35% formaldehyde aqueous solution, 16 L of distilled water, and 56 g of the phosphorus- and nitrogen-containing flame retardant polyol prepared in step (1) are sequentially added into a 246 mL round-bottom flask, and refluxed for 2 h to obtain an intermediate product of tetraethylenepentamineheptamethylenephosphonic acid (TEPAHP). Then, 82 g of the water-soluble rosin-based flame retardant modifier prepared in step (2) is added, and aminated with 0.6 mol of urea in a beaker for 3 h to obtain tetraethylenepentamineheptamethylenephosphonic acid ammonium salt (ATEPAHP). After purification with ethanol, a water-soluble rosin-based phosphorus-based cross-linked flame retardant is obtained.

[0101] Step (4) Phosphorus / nitrogen / silicon multi-flame retardant element compound

[0102] 6g of ethanol and a hydrochloric acid aqueous solution with a pH of 3 provide the water required for the hydrolysis reaction. The molar ratio of water to alkoxy is 0.5:1. They are added into a single-mouth bottle and mixed evenly at 36°C. MEL-KH dissolved in ethylene glycol is taken, and DOPO-VTMS and MTMS are evenly mixed into 3g of anhydrous ethanol, and then slowly added to the hydrolysis system at a rate of 1 drop per second. After the addition is completed, the hydrolysis reaction is continued at 36°C for 28 minutes. Finally, triethylamine is added to neutralize the hydrochloric acid to obtain a phosphorus / nitrogen / silicon multi-flame retardant element compound dissolved in a mixed solvent of ethanol and ethylene glycol.

[0103] Step (5) Novel multi-metal complex flame retardant modifier

[0104] Weigh 0.3mmol glutathione and dissolve it completely in 4ml distilled water. Add 0.3mol / L copper sulfate solution to the glutathione aqueous solution, adjust the pH to 3 with NaOH solution, stir the reaction at 34℃, and dissolve the MgCl 2 After slowly adding the ligand system to react for 16 min, cooling and standing for 16 h, a metal complex was obtained. 4 g Bi(NO 3 ) 3 ·5H 2 O and 0.6g KCl are dissolved in 100mL mannitol solution, and ferrous sulfate, stannous sulfate, and the phosphorus / nitrogen / silicon multi-flame retardant element compound prepared in step (4) are added to the above solution respectively. After ultrasonic treatment for 8 minutes, stirring is carried out for 26 minutes to form a uniform solution. Subsequently, stirring is carried out at room temperature under magnetic stirring for 2 hours. The obtained solution is transferred to a polytetrafluoroethylene-lined autoclave and reacted at 160°C for 6 hours. After the reaction is completed, the solution is cooled to room temperature to obtain a precipitate, which is filtered twice with hydrogen peroxide and ethanol. As the amount of hydrogen peroxide increases, the decomposed free radicals HOO· and hydroxyl radicals increase as bleaching active components. After drying at 60°C, a novel multi-metal complex flame retardant modifier is obtained;

[0105] Step (6) Smoke-suppressing multimetallic complex phosphorus-based cross-linked flame retardant

[0106] 23 g of 3-aminopropylsilane, 18 g of phosphorous acid, 0.4 mol of formaldehyde aqueous solution, and 12 g of tetrakis(hydroxymethyl)phosphonium chloride are sequentially added to a 210 mL round-bottom flask, and the mixed solution is refluxed for 3 h under magnetic stirring. After the solution is cooled, it is poured into a 460 mL beaker, and then 0.2 mol of urea and the novel multi-metal complex flame retardant modifier prepared in step (5) are added to the beaker to obtain a smoke-suppressing multi-metal complex phosphorus-based cross-linked flame retardant.

[0107] Step (7) Preparation of smoke-suppressing biomass-based phosphorus-containing flame retardant

[0108] The water-soluble rosin-based phosphorus-based cross-linked flame retardant prepared in step (3) and the smoke-suppressing multimetallic complex phosphorus-based cross-linked flame retardant prepared in step (6) are ultrasonically dispersed and compatible at a ratio of 2:1-2:3 to obtain a smoke-suppressing biomass-based phosphorus-containing flame retardant. The smoke-suppressing biomass-based phosphorus-containing flame retardant is obtained by thermal weight loss under nitrogen conditions and calcination in a muffle furnace at 96°C and 112°C in an air atmosphere.

[0109] Example 4

[0110] Step (1) Preparation of phosphorus- and nitrogen-containing flame-retardant polyols

[0111] The paraformaldehyde, ethanolamine and tris(hydroxymethyl)aminomethane (THAM) are mixed for reaction, and the paraformaldehyde, ethanolamine and tris(hydroxymethyl)aminomethane (THAM) are added into a container equipped with a constant pressure dropping funnel and a reflux condenser, and stirred at 20°C for reaction for 1.0h; the temperature of the temperature-raising reaction under nitrogen protection can be 80°C, and the temperature-raising reaction time can be 4h, and the ethanol solution of the aromatic phenol compound can be an ethanol solution of the aromatic phenol compound with a mass fraction of 50%; the reflux reaction time can be 4h; and the phosphorus-containing and nitrogen-containing flame-retardant polyol is prepared;

[0112] Step (2) Synthesis of water-soluble rosin-based flame retardant modifier

[0113] Abietic acid, formic acid, concentrated H 2 SO 4 Add to a three-necked flask equipped with a thermometer and a condenser, raise the temperature to 35°C, add hydrogen peroxide dropwise while stirring, react at 75°C for 30 minutes, heat under reflux for 60 minutes, let the product stand for stratification, separate the lower layer of waste liquid, pour the oil layer into a three-necked flask, add the catalyst and the phosphorus- and nitrogen-containing flame retardant polyol obtained in step (1), react at high temperature and under reduced pressure for several hours to obtain a water-soluble rosin-based flame retardant modifier;

[0114] Step (3) Water-soluble rosin-based phosphorus cross-linked flame retardant

[0115] 19 g of tetrakis(hydroxymethyl)phosphonium chloride, 0.90 mol of 37% formaldehyde aqueous solution, 20 L of distilled water, and 60 g of the phosphorus- and nitrogen-containing flame-retardant polyol prepared in step (1) are sequentially added into a 250 mL round-bottom flask, and refluxed for 3 h to obtain an intermediate product of tetraethylenepentamineheptamethylenephosphonic acid (TEPAHP). Then, 85 g of the water-soluble rosin-based flame-retardant modifier prepared in step (2) is added, and aminated with 0.9 mol of urea in a beaker for 5 h to obtain tetraethylenepentamineheptamethylenephosphonic acid ammonium salt (ATEPAHP). After purification with ethanol, a water-soluble rosin-based phosphorus-based cross-linked flame retardant is obtained.

[0116] Step (4) Phosphorus / nitrogen / silicon multi-flame retardant element compound

[0117] 5g of ethanol and a hydrochloric acid aqueous solution with a pH of 5 provide the water required for the hydrolysis reaction. The molar ratio of water to alkoxy is 0.5:5. The mixture is added into a single-mouth bottle and mixed evenly at 40°C. MEL-KH dissolved in ethylene glycol is taken, and DOPO-VTMS and MTMS are evenly mixed into 5g of anhydrous ethanol. Then, the mixture is slowly dripped into the hydrolysis system at a rate of 2 drops per second. After the dripping is completed, the hydrolysis reaction is continued at 40°C for 30 minutes. Finally, triethylamine is added to neutralize the hydrochloric acid to obtain a phosphorus / nitrogen / silicon multi-flame retardant element compound dissolved in a mixed solvent of ethanol and ethylene glycol.

[0118] Step (5) Novel multi-metal complex flame retardant modifier

[0119] Weigh 0.5mmol glutathione and dissolve it completely in 5ml distilled water. Add 0.5mol / L copper sulfate solution to the glutathione aqueous solution, adjust the pH to 4 with NaOH solution, stir the reaction at 34℃, and dissolve the MgCl 2 After slowly adding the ligand system to react for 20 min, cooling and placing for 24 h, a metal complex was obtained. 5 g Bi(NO 3 ) 3 ·5H 2 O and 1.0g KCl are dissolved in 110mL mannitol solution, and ferrous sulfate, stannous sulfate, and the phosphorus / nitrogen / silicon multi-flame retardant element compound prepared in step (4) are added to the above solution respectively. After ultrasonication for 10 minutes, stirring is carried out for 30 minutes to form a uniform solution. Subsequently, stirring is carried out at room temperature under magnetic stirring for 3 hours. The obtained solution is transferred to a polytetrafluoroethylene-lined autoclave and reacted at 180°C for 10 hours. After the reaction is completed, the solution is cooled to room temperature to obtain a precipitate, which is filtered three times with hydrogen peroxide and ethanol. As the amount of hydrogen peroxide increases, the decomposed free radicals HOO· and hydroxyl radicals increase as bleaching active components. After drying at 80°C, a novel multi-metal complex flame retardant modifier is obtained;

[0120] Step (6) Smoke-suppressing multimetallic complex phosphorus-based cross-linked flame retardant

[0121] 25 g of 3-aminopropylsilane, 20 g of phosphorous acid, 0.5 mol of formaldehyde aqueous solution and 15 g of tetrakis(hydroxymethyl)phosphonium chloride were added to a 250 mL round-bottom flask in sequence. The mixed solution was refluxed for 6 h under magnetic stirring. After the solution was cooled, it was poured into a 500 mL beaker. Subsequently, 0.5 mol of urea and the novel multimetallic complex flame retardant modifier prepared in step (5) were added to the beaker to obtain a smoke-suppressing multimetallic complex phosphorus-based cross-linked flame retardant.

[0122] Step (7) Preparation of smoke-suppressing biomass-based phosphorus-containing flame retardant

[0123] The water-soluble rosin-based phosphorus-based cross-linked flame retardant prepared in step (3) and the smoke-suppressing multimetallic complex phosphorus-based cross-linked flame retardant prepared in step (6) are ultrasonically dispersed and compatible at a ratio of 2:1 and 5:5 to obtain a smoke-suppressing biomass-based phosphorus-containing flame retardant. The smoke-suppressing biomass-based phosphorus-containing flame retardant is obtained by thermal weight loss under nitrogen conditions and calcination in a muffle furnace in an air atmosphere at 100°C and 115°C.

[0124] Comparative Example 1

[0125] Step (1) Preparation of phosphorus-containing and nitrogen-containing flame-retardant polyols

[0126] The paraformaldehyde, ethanolamine and tris(hydroxymethyl)aminomethane (THAM) are mixed for reaction, and the paraformaldehyde, ethanolamine and tris(hydroxymethyl)aminomethane (THAM) are added into a container equipped with a constant pressure dropping funnel and a reflux condenser, and stirred at 30°C for reaction for 2 hours; the temperature of the temperature-raising reaction under nitrogen protection can be 100°C, and the temperature-raising reaction time can be 5 hours, and the ethanol solution of the aromatic phenol compound can use an ethanol solution of the aromatic phenol compound with a mass fraction of 60%; the reflux reaction time can be 5 hours; and the phosphorus-containing and nitrogen-containing flame-retardant polyol is prepared;

[0127] Step (2) Synthesis of water-soluble rosin-based flame retardant modifier

[0128] Abietic acid, formic acid, concentrated H 2 SO 4 Add to a three-necked flask equipped with a thermometer and a condenser, raise the temperature to 50°C, add hydrogen peroxide dropwise while stirring, and after the addition is complete, heat at 80°C for 30 minutes, heat under reflux for 60 minutes, let the product stand for stratification, separate the lower layer of waste liquid, pour the oil layer into a three-necked flask, add the catalyst and the phosphorus- and nitrogen-containing flame retardant polyol obtained in step (1), and react at high temperature and reduced pressure for several hours to obtain a water-soluble rosin-based flame retardant modifier;

[0129] Step (3) Water-soluble rosin-based phosphorus cross-linked flame retardant

[0130] 20 g of tetrakis(hydroxymethyl)phosphonium chloride, 1.0 mol of 40% formaldehyde aqueous solution, 25 L of distilled water, and 65 g of the phosphorus- and nitrogen-containing flame-retardant polyol prepared in step (1) are sequentially added into a 300 mL round-bottom flask, and refluxed for 2 h to obtain an intermediate product of tetraethylenepentamineheptamethylenephosphonic acid (TEPAHP). Then, 90 g of the water-soluble rosin-based flame-retardant modifier prepared in step (2) is added, and aminated with 1.2 mol of urea in a beaker for 5 h to obtain tetraethylenepentamineheptamethylenephosphonic acid ammonium salt (ATEPAHP). After purification with ethanol, a water-soluble rosin-based phosphorus-based cross-linked flame retardant is obtained.

[0131] Step (4) Novel multi-metal complex flame retardant modifier

[0132] Weigh 0.7mmol glutathione and dissolve it completely in 6ml distilled water. Add 0.7mol / L copper sulfate solution to the glutathione aqueous solution, adjust the pH to 3 with NaOH solution, stir the reaction at a certain temperature, and dissolve the MgCl 2 After slowly adding the ligand system to react for 20 min, cooling and standing for 24 h, a metal complex was obtained. 6 g Bi(NO 3 ) 3 ·5H 2 O and 2.0g KCl were dissolved in 120mL mannitol solution, ferrous sulfate, stannous sulfate, were added to the above solution respectively, after ultrasonication for 15min, stirring was carried out for 35min to form a uniform solution, and then stirring was carried out under magnetic stirring at room temperature for 5h, the obtained solution was transferred to a polytetrafluoroethylene-lined autoclave, and reacted at 200°C for 15h, the reaction was completed, cooled to room temperature, a precipitate was obtained, and filtered once with hydrogen peroxide and ethanol. With the increase of the amount of hydrogen peroxide, the decomposed free radicals HOO· and hydroxyl radicals as bleaching active components increased, and the novel multi-metal complex flame retardant modifier was obtained after drying at 90°C;

[0133] Step (5) Smoke-suppressing multimetallic complex phosphorus-based cross-linked flame retardant

[0134] 30 g of 3-aminopropylsilane, 25 g of phosphorous acid, 0.8 mol of formaldehyde aqueous solution and 16 g of tetrakis(hydroxymethyl)phosphonium chloride are sequentially added into a 260 mL round-bottom flask, and the mixed solution is refluxed for 7 h under magnetic stirring. After the solution is cooled, it is poured into a 550 mL beaker, and then 0.3 mol of urea and the novel multi-metal complex flame retardant modifier prepared in step (4) are added into the beaker to obtain a smoke-suppressing multi-metal complex phosphorus-based cross-linked flame retardant.

[0135] Step (6) Preparation of smoke-suppressing biomass-based phosphorus-containing flame retardant

[0136] The water-soluble rosin-based phosphorus-based cross-linked flame retardant prepared in step (3) and the smoke-suppressing multimetallic complex phosphorus-based cross-linked flame retardant prepared in step (5) are ultrasonically dispersed and compatible at a ratio of 1:1 and 5:6 to obtain a smoke-suppressing biomass-based phosphorus-containing flame retardant, and the smoke-suppressing biomass-based phosphorus-containing flame retardant is obtained by thermal weight loss under nitrogen conditions and calcination in a muffle furnace in an air atmosphere at 100°C and 120°C.

[0137] Comparative Example 2

[0138] Step (1) Preparation of phosphorus- and nitrogen-containing flame-retardant polyols

[0139] The paraformaldehyde, ethanolamine and tris(hydroxymethyl)aminomethane (THAM) are mixed for reaction, and the paraformaldehyde, ethanolamine and tris(hydroxymethyl)aminomethane (THAM) are added into a container equipped with a constant pressure dropping funnel and a reflux condenser, and stirred at 5°C for reaction for 0.1h; the temperature of the temperature-raising reaction under nitrogen protection can be 50°C, and the temperature-raising reaction time can be 1h, and the ethanol solution of the aromatic phenol compound can be an ethanol solution of the aromatic phenol compound with a mass fraction of 20%; the reflux reaction time can be 1h; and the phosphorus-containing and nitrogen-containing flame-retardant polyol is prepared;

[0140] Step (2) Synthesis of water-soluble rosin-based flame retardant modifier

[0141] Abietic acid, formic acid, concentrated H 2 SO 4 Add to a three-necked flask equipped with a thermometer and a condenser, raise the temperature to 15°C, add hydrogen peroxide dropwise while stirring, and after the addition is complete, heat at 30°C for 30 minutes, heat under reflux for 60 minutes, let the product stand for stratification, separate the lower layer of waste liquid, pour the oil layer into a three-necked flask, add the catalyst and the phosphorus- and nitrogen-containing flame retardant polyol obtained in step (1), and react at high temperature and reduced pressure for several hours to obtain a water-soluble rosin-based flame retardant modifier;

[0142] Step (3) Water-soluble rosin-based phosphorus cross-linked flame retardant

[0143] 10 g of tetrakis(hydroxymethyl)phosphonium chloride, 0.20 mol of 40% formaldehyde aqueous solution, 10 L of distilled water, and 50 g of the phosphorus- and nitrogen-containing flame retardant polyol prepared in step (1) are sequentially added into a 200 mL round-bottom flask, and refluxed for 2 h to obtain an intermediate product of tetraethylenepentamineheptamethylenephosphonic acid (TEPAHP). Then, 50 g of the water-soluble rosin-based flame retardant modifier prepared in step (2) is added, and aminated with 0.2 mol of urea in a beaker for 2 h to obtain tetraethylenepentamineheptamethylenephosphonic acid ammonium salt (ATEPAHP). After purification with ethanol, a water-soluble rosin-based phosphorus-based cross-linked flame retardant is obtained.

[0144] Step (4) Phosphorus / nitrogen / silicon multi-flame retardant element compound

[0145] 2g of ethanol and a hydrochloric acid aqueous solution with a pH of 10 provide the water required for the hydrolysis reaction. The molar ratio of water to alkoxy is 1.0:5. Add them into a single-mouth bottle and mix them evenly at 40°C. Take MEL-KH dissolved in ethylene glycol, and evenly mix DOPO-VTMS and MTMS into 4g of anhydrous ethanol. Then slowly add them to the hydrolysis system at a rate of 5 drops per second. After the addition is completed, continue the hydrolysis reaction at 60°C for 10 minutes. Finally, add triethylamine to neutralize the hydrochloric acid to obtain a phosphorus / nitrogen / silicon multi-flame retardant element compound dissolved in a mixed solvent of ethanol and ethylene glycol.

[0146] Step (5) Smoke-suppressing multimetallic complex phosphorus-based cross-linked flame retardant

[0147] 10g of 3-aminopropylsilane, 10g of phosphorous acid, 0.3mol of formaldehyde aqueous solution, and 12g of tetrakis(hydroxymethyl)phosphonium chloride were added to a 150mL round-bottom flask in sequence, and the mixed solution was refluxed for 2h under magnetic stirring. After the solution was cooled, it was poured into a 160mL beaker, and then 0.6mol of urea was added to the beaker to obtain a smoke-suppressing multimetal complex phosphorus-based cross-linked flame retardant;

[0148] Step (6) Preparation of smoke-suppressing biomass-based phosphorus-containing flame retardant

[0149] The water-soluble rosin-based phosphorus-based cross-linked flame retardant prepared in step (3) and the smoke-suppressing multimetallic complex phosphorus-based cross-linked flame retardant prepared in step (5) are ultrasonically dispersed and compatible at a ratio of 1:1 and 5:3 to obtain a smoke-suppressing biomass-based phosphorus-containing flame retardant, and the smoke-suppressing biomass-based phosphorus-containing flame retardant is obtained by thermal weight loss under nitrogen conditions and calcination in a muffle furnace in an air atmosphere at 100°C and 115°C.

[0150] Comparison of detection experiments:

[0151] The smoke-suppressing biomass-based phosphorus-containing flame retardants obtained in Examples 1 to 4 and Comparative Example Products 1 and 2 were tested. The specific testing methods are as follows:

[0152] Limiting oxygen index test

[0153] The limiting oxygen index refers to the volume fraction concentration of oxygen in a polymer in a mixture of oxygen and nitrogen that can just support its combustion. It characterizes the index of the material's combustion behavior and is a key parameter for evaluating the flame retardant properties of the material. The corresponding weight gain of flame-retardant cotton fabrics finished with different concentrations and the limiting oxygen index values ​​before and after washing are summarized by concentration.

[0154] Determination of free formaldehyde content

[0155] Spectrophotometry: This is a method to calculate the formaldehyde content by measuring the absorbance of the adhesive at a specific wavelength. Commonly used spectrophotometry methods include phenol reagent spectrophotometry, acetylacetone spectrophotometry, etc. This method has the advantages of simple operation and low cost, and is currently the most widely used formaldehyde content detection method.

[0156] Flame retardant performance test

[0157] Samples of 100mm×100mm×15mm were sawn from 15mm thick flame retardant plywood, and their combustion performance was evaluated in the laboratory with reference to the cone calorimeter method, vertical combustion test and horizontal combustion test, etc. These test methods evaluate the flame retardant properties of materials by placing the sample on a specific combustion device, igniting one end or the lower end, observing the spread of the flame and the combustion characteristics of the sample, and measuring parameters such as burning time, burning length, and burning rate.

[0158] Flame Retardant Volatile Organic Compounds Testing

[0159] GB / T 18446-2009, GB 18581-2009, GB18582-2008 and other standard methods are used to detect the content of volatile organic compounds, benzene, soluble heavy metals, diisocyanates and other substances, and the synthesis process is optimized to make the volatile organic compounds (VOC) of the flame retardant <5g / L and the soluble heavy metals <1mg / kg.

[0160] Table 1 Limiting oxygen index test

[0161] Example Limiting oxygen value% 1 30 2 27 3 25 4 23 Comparative Example 1 19 Comparative Example 2 15

[0162] As can be seen from Table 1, Example 1 is the best and Comparative Example 2 is relatively poor. In Example 1, the limiting oxygen index is high, the material of Example 1 is difficult to burn, and has good flame retardant properties, while the limiting oxygen index of Comparative Example 2 is the lowest, and the material with a low limiting oxygen index is easy to burn. The flame retardant prepared in Example 1 significantly improves the flame retardant properties, can be evenly dispersed, and ensures the uniformity of the flame retardant effect; it combines the stability of the multi-metal complex and the high efficiency of the phosphorus-based flame retardant, can effectively capture active free radicals during the combustion process, improve stability, and is not easy to decompose or inactivate, thereby ensuring the long-term flame retardant properties of the material.

[0163] Table 2 Formaldehyde content

[0164] Example Formaldehyde content% 1 0.13 2 0.15 3 0.30 4 0.35 Comparative Example 1 0.50 Comparative Example 2 0.70

[0165] As can be seen from Table 2, Example 1 is the best, while Comparative Example 2 is relatively poor. Example 1 has a low formaldehyde content, and the phosphorus / nitrogen / silicon multi-flame retardant element compound produces less smoke and toxic substances during combustion. The novel multi-metal complex flame retardant modifier can more effectively capture active free radicals in the gas phase through its unique complex structure and the synergistic effect of multi-metal elements during the combustion process, thereby significantly improving the flame retardant performance; the flame retardant prepared in Example 1 is more in line with the requirements of green chemistry and sustainable development. By reducing the formaldehyde content, the flame retardant can maintain its excellent bonding performance and durability, ensuring the quality and reliability of the product.

[0166] Table 3 Flame retardant time test

[0167] Example Flame retardant time 1 30 2 28.3 3 27.4 4 25.8 Comparative Example 1 15.4 Comparative Example 2 20.2

[0168] As can be seen from Table 3, Example 1 is the best, while Comparative Example 1 is relatively poor. The flame retardant time of Example 1 is long. The phosphorus element in Example 1 can capture active free radicals in the gas phase to terminate the combustion chain reaction when burning, and at the same time, a stable carbon layer containing phosphorus is formed. The nitrogen element will generate non-combustible gas at high temperature, diluting the concentration of oxygen and combustible gas in the gas phase to isolate oxygen and combustibles; the silicon element has a low surface energy and is easy to migrate to the surface of the material to form a silicon-containing protective layer during the combustion process; it is conducive to forming a more stable carbon layer with better barrier effect, while Comparative Example 1 has a poorer flame retardant effect than Example 1, a shorter time, and relatively poor thermal stability.

[0169] Table 4 Volatile organic compounds of flame retardants

[0170] Example Flame retardant volatile organic compounds g / L Soluble heavy metals mg / kg 1 4.01 0.51 2 5.02 1.02 3 5.30 1.23 4 6.12 1.40 Comparative Example 1 10.23 3.69 Comparative Example 2 11.18 3.23

[0171] As can be seen from Table 3, Example 1 is the best and Comparative Example 1 is relatively poor. The VOC content of the flame retardant in Example 1 is lower than 5 g / L, which means that the flame retardant has good environmental performance and can reduce potential impacts on the environment and human body. The reduction in VOC content will not affect the ability to suppress smoke and reduce toxicity during combustion, making the flame retardant performance more stable. The soluble heavy metal content in Comparative Example 1 is high, and there is a reaction between the heavy metal and the organophosphorus flame retardant, which will lead to a decrease in flame retardant performance, while the low metal content helps to reduce the impact of the flame retardant on the environment during production, use and disposal.

Claims

1. A process for synthesizing a smoke-suppressing biomass-based phosphorus-containing flame retardant, characterized in that include: Preparation of phosphorus- and nitrogen-containing flame-retardant polyols, synthesis of water-soluble rosin-based flame-retardant modifiers, water-soluble rosin-based phosphorus-based cross-linked flame retardants, phosphorus / nitrogen / silicon multi-flame-retardant element compounds, new multi-metal complex flame-retardant modifiers, smoke-suppressing multi-metal complex phosphorus-based cross-linked flame retardants, and preparation of smoke-suppressing biomass-based phosphorus-containing flame retardants.

2. A process for synthesizing a smoke-suppressing biomass-based phosphorus-containing flame retardant according to claim 1, characterized in that: Step (1) Preparation of phosphorus- and nitrogen-containing flame-retardant polyols The paraformaldehyde, ethanolamine and tris(hydroxymethyl)aminomethane (THAM) are mixed for reaction, the paraformaldehyde, ethanolamine and tris(hydroxymethyl)aminomethane (THAM) are added into a container equipped with a constant pressure dropping funnel and a reflux condenser, stirred for reaction, and heated for reaction under nitrogen protection, wherein the ethanol solution of the aromatic phenol compound can be the ethanol solution of the aromatic phenol compound, and the obtained phosphorus-containing and nitrogen-containing flame retardant polyol is prepared; Step (2) Synthesis of water-soluble rosin-based flame retardant modifier Add rosin acid, formic acid and concentrated H2SO4 in a certain proportion to a three-necked flask equipped with a thermometer and a condenser, raise the temperature, and drop hydrogen peroxide under stirring. After the dropwise addition is completed, react for a period of time, heat under reflux and react for a period of time, let the product stand for stratification, separate the lower layer of waste liquid, pour the oil layer into the three-necked flask, add the catalyst and the phosphorus- and nitrogen-containing flame retardant polyol obtained in step (1), and react under reduced pressure at high temperature for several hours to obtain a water-soluble rosin-based flame retardant modifier; Step (3) Water-soluble rosin-based phosphorus cross-linked flame retardant Tetrakis(hydroxymethyl)phosphonium chloride, tetraethylenepentamine, formaldehyde aqueous solution, distilled water, and the phosphorus- and nitrogen-containing flame retardant polyol prepared in step (1) are sequentially added into a round-bottom flask, and refluxed for a period of time to obtain an intermediate product of tetraethylenepentamine hepta(methylenephosphonic acid) (TEPAHP), and then the water-soluble rosin-based flame retardant modifier prepared in step (2) is added, and aminated with urea in a beaker to obtain tetraethylenepentamine hepta(methylenephosphonic acid) ammonium salt (ATEPAHP), and purified with ethanol to obtain a water-soluble rosin-based phosphorus-based cross-linked flame retardant; Step (4) Phosphorus / nitrogen / silicon multi-flame retardant element compound The ethanol and hydrochloric acid aqueous solution provide the water required for the hydrolysis reaction and are added into a single-mouth bottle, and mixed evenly at a certain temperature; MEL-KH dissolved in ethylene glycol is taken, and DOPO-VTMS and MTMS are evenly mixed into anhydrous ethanol, and then slowly added dropwise to the hydrolysis system, and the hydrolysis reaction is continued after the addition is completed, and finally triethylamine is added to neutralize the hydrochloric acid, thereby obtaining a phosphorus / nitrogen / silicon multi-flame retardant element compound dissolved in a mixed solvent of ethanol and ethylene glycol; Step (5) Novel multi-metal complex flame retardant modifier Weigh glutathione and dissolve it completely in distilled water. Add copper sulfate solution to the glutathione aqueous solution in a certain proportion. Adjust the pH value with NaOH solution. Stir and react at a certain temperature. Slowly add MgCl2 fully dissolved in the aqueous solution to the ligand system and react for a period of time. Cool and place to obtain a metal complex. Dissolve Bi(NO3)3·5H2O and KCl in mannitol solution. Add ferrous sulfate, stannous sulfate and the phosphorus / nitrogen / silicon multi-flame retardant element compound prepared in step (4) to the above solution respectively. After ultrasonic treatment, stir to form a uniform solution. Then stir at room temperature under magnetic stirring. Transfer the obtained solution to a polytetrafluoroethylene-lined autoclave and react. Cool to room temperature to obtain a precipitate. Filter it several times with hydrogen peroxide and ethanol. As the amount of hydrogen peroxide increases, the decomposed free radicals HOO· and hydroxyl free radicals increase as bleaching active components. After drying, a novel multi-metal complex flame retardant modifier is obtained. Step (6) Smoke-suppressing multimetallic complex phosphorus-based cross-linked flame retardant 3-aminopropylsilane, phosphorous acid, formaldehyde aqueous solution, and tetrakis(hydroxymethyl)phosphonium chloride are sequentially added into a round-bottom flask, and the mixed solution is refluxed under magnetic stirring. After the solution is cooled, it is poured into a beaker, and then urea and the novel multi-metal complex flame retardant modifier prepared in step (5) are added into the beaker to obtain a smoke-suppressing multi-metal complex phosphorus-based cross-linked flame retardant. Step (7) Preparation of smoke-suppressing biomass-based phosphorus-containing flame retardant The water-soluble rosin-based phosphorus-based cross-linked flame retardant prepared in step (3) and the smoke-suppressing multimetallic complex phosphorus-based cross-linked flame retardant prepared in step (6) are prepared by ultrasonic dispersion compatibility to obtain a smoke-suppressing biomass-based phosphorus-containing flame retardant, which is then calcined in a muffle furnace in an air atmosphere at a certain temperature through thermal weight loss under nitrogen conditions to obtain a smoke-suppressing biomass-based phosphorus-containing flame retardant.

3. A process for synthesizing a smoke-suppressing biomass-based phosphorus-containing flame retardant according to claim 2, characterized in that: Step (1) Preparation of phosphorus- and nitrogen-containing flame-retardant polyols The paraformaldehyde, ethanolamine and tris(hydroxymethyl)aminomethane (THAM) are mixed for reaction, and the paraformaldehyde, ethanolamine and tris(hydroxymethyl)aminomethane (THAM) are added into a container equipped with a constant pressure dropping funnel and a reflux condenser, and the reaction is stirred at 15-20°C for 0.5-1.0h; the temperature of the temperature-raising reaction under nitrogen protection can be 60-80°C, and the temperature-raising reaction time can be 2-4h. The ethanol solution of the aromatic phenol compound can use an ethanol solution of the aromatic phenol compound with a mass fraction of 30%-50%; the reflux reaction time can be 2-4h; and the phosphorus-containing and nitrogen-containing flame-retardant polyol is prepared.

4. A process for synthesizing a smoke-suppressing biomass-based phosphorus-containing flame retardant according to claim 2, characterized in that: Step (2) Synthesis of water-soluble rosin-based flame retardant modifier Add rosin acid, formic acid and concentrated H2SO4 into a three-necked flask equipped with a thermometer and a condenser, raise the temperature to 30-35°C, add hydrogen peroxide dropwise under stirring, react at 45-75°C for 25-30 minutes, heat under reflux for 55-60 minutes, let the product stand for stratification, separate the lower layer of waste liquid, pour the oil layer into a three-necked flask, add a catalyst and the phosphorus- and nitrogen-containing flame retardant polyol obtained in step (1), and react at high temperature under reduced pressure for several hours to obtain a water-soluble rosin-based flame retardant modifier.

5. A process for synthesizing a smoke-suppressing biomass-based phosphorus-containing flame retardant according to claim 4, characterized in that: Step (3) Water-soluble rosin-based phosphorus cross-linked flame retardant Tetrakis(hydroxymethyl)phosphonium chloride, 15-19g of tetraethylenepentamine, 0.50-0.90mol of 30-37% formaldehyde aqueous solution, 15-20L of distilled water, and 55-60g of the phosphorus- and nitrogen-containing flame retardant polyol prepared in step (1) are sequentially added into a 245-250mL round-bottom flask, and refluxed for 1-3h to obtain an intermediate product of tetraethylenepentamine hepta(methylenephosphonic acid) (TEPAHP). Then, 80-85g of the water-soluble rosin-based flame retardant modifier prepared in step (2) is added, and 0.5-0.9mol of urea is stirred and aminated in a beaker for 1-5h to obtain tetraethylenepentamine hepta(methylenephosphonic acid) ammonium salt (ATEPAHP). After purification with ethanol, a water-soluble rosin-based phosphorus-based cross-linked flame retardant is obtained.

6. A process for synthesizing a smoke-suppressing biomass-based phosphorus-containing flame retardant according to claim 2, characterized in that: Step (4) Phosphorus / nitrogen / silicon multi-flame retardant element compound 1-5g of ethanol and a hydrochloric acid aqueous solution with a pH value of 1-5 provide water required for the hydrolysis reaction, and the molar ratio of water to alkoxy is 0.5-1.0:1-5, which are added into a single-mouth bottle and mixed evenly at 35-40°C; MEL-KH dissolved in ethylene glycol is taken, and DOPO-VTMS and MTMS are evenly mixed into 1-5g of anhydrous ethanol, and then slowly added to the hydrolysis system at a speed of 1-2 drops per second, and after the addition is completed, the hydrolysis reaction is continued at 35-40°C for 25-30 minutes, and finally triethylamine is added to neutralize the hydrochloric acid to obtain a phosphorus / nitrogen / silicon multi-flame retardant element compound dissolved in a mixed solvent of ethanol and ethylene glycol.

7. A process for synthesizing a smoke-suppressing biomass-based phosphorus-containing flame retardant according to claim 6, characterized in that: Step (5) Novel multi-metal complex flame retardant modifier Weigh 0.1-0.5mmol glutathione and dissolve it completely in 1-5ml distilled water. Add 0.1-0.5mol / L copper sulfate solution dropwise to the glutathione aqueous solution. Adjust the pH with NaOH solution. Stir the reaction at 30-35℃. Slowly add MgCl2 fully dissolved in the aqueous solution to the ligand system and react for 15-20min. Cool and place for 12-24h to obtain a metal complex. Add 3-5g Bi(NO3)3·5H2O and 0.5-1.0gKCl are dissolved in 100-110mL mannitol solution, and ferrous sulfate, stannous sulfate, and the phosphorus / nitrogen / silicon multi-flame retardant element compound prepared in step (4) are added to the above solution respectively. After ultrasonic treatment for 5-10min, the solution is stirred for 25-30min to form a uniform solution. The solution is then stirred for 1-3h under magnetic stirring at room temperature. The obtained solution is transferred to a polytetrafluoroethylene-lined autoclave and reacted at 150-180°C for 5-10h. After the reaction is completed, the solution is cooled to room temperature to obtain a precipitate, which is filtered 1-3 times with hydrogen peroxide and ethanol. As the amount of hydrogen peroxide increases, the decomposed free radicals HOO· and hydroxyl radicals increase as bleaching active components. After drying at 50-80°C, a novel multi-metal complex flame retardant modifier is obtained.

8. The process for synthesizing a smoke-suppressing biomass-based phosphorus-containing flame retardant according to claim 7, characterized in that: Step (6) Smoke-suppressing multimetallic complex phosphorus-based cross-linked flame retardant 20-25 g of 3-aminopropylsilane, 15-20 g of phosphorous acid, 0.1-0.5 mol of formaldehyde aqueous solution and 10-15 g of tetrakis(hydroxymethyl)phosphonium chloride are sequentially added into a 200-250 mL round-bottom flask. The mixed solution is refluxed for 1-6 h under magnetic stirring. After the solution is cooled, it is poured into a 450-500 mL beaker. Subsequently, 0.1-0.5 mol of urea and the novel multi-metal complex flame retardant modifier prepared in step (5) are added into the beaker to obtain a smoke-suppressing multi-metal complex phosphorus-based cross-linked flame retardant.

9. A process for synthesizing a smoke-suppressing biomass-based phosphorus-containing flame retardant according to claim 8, characterized in that: Step (7) Preparation of smoke-suppressing biomass-based phosphorus-containing flame retardant The water-soluble rosin-based phosphorus-based cross-linked flame retardant prepared in step (3) and the smoke-suppressing multimetallic complex phosphorus-based cross-linked flame retardant prepared in step (6) are ultrasonically dispersed and compatible in a ratio of 1-2:1-5 and 2-5:3-5 to obtain a smoke-suppressing biomass-based phosphorus-containing flame retardant, and the smoke-suppressing biomass-based phosphorus-containing flame retardant is obtained by thermal weight loss under nitrogen conditions and calcination in a muffle furnace in an air atmosphere at 95-100°C and 110-115°C.

Citation Information