Regenerated aluminum alloy material for automobile and production method thereof

By adjusting the composition and production process of recycled aluminum alloy materials for automobiles, the high cost and production difficulty problems caused by rare earth elements have been solved, and recycled aluminum alloy materials with high mechanical properties have been achieved to meet the performance requirements of automobile anti-collision beam energy-absorbing boxes. and reduce production costs.

CN118756015APending Publication Date: 2024-10-11DONGLIANG ALUMINIUM CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410769699.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-14
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Existing recycled aluminum alloy materials for automobiles contain rare earth elements, which results in high costs and difficulty in production. It is also difficult to meet the high mechanical performance requirements of automobile anti-collision beam energy-absorbing boxes without using rare earth metals.

Method used

By recycling scrap automobile engine blocks, wheel hubs and frames, the composition of aluminum alloy materials is adjusted to ensure that the weight proportion of scrap aluminum recycled materials is 40-60%, and through pretreatment, melting, refinement, deterioration, refining and aging treatment, etc. Through the steps, a recycled aluminum alloy material containing no rare earth elements is prepared, which has high yield strength, tensile strength and absorbed energy.

Benefits of technology

It is possible to meet the high mechanical performance requirements of the automobile anti-collision beam energy-absorbing box without using rare earth elements, reduce production costs, and improve the corrosion resistance of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118756015A_ABST
    Figure CN118756015A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of regenerated aluminum alloy, and particularly relates to a regenerated aluminum alloy material for an automobile and a production method of the regenerated aluminum alloy material. The invention provides a regenerated aluminum alloy material for an automobile, which can be prepared by recovering a waste automobile engine cylinder body, a waste automobile hub and a waste automobile frame body, controlling the weight ratio of the waste aluminum recovered material to be 40-60%, and finally adjusting the components to be 0.40-0.45% of Si, 0.150-0.170% of Fe, 0.016-0.018% of Cu, 0.010-0.012% of Mn, 0.550-0.560% of Mg, 0.009-0.010% of Cr, 0.020-0.025% of Zn, 0.011-0.014% of Ti, less than or equal to 0.20% of impurity elements in total and the balance of Al. The regenerated aluminum alloy material can still achieve higher mechanical properties on the premise that rare earth metal is not used, and the use requirement of the automobile anti-collision beam energy absorption box is met. Specifically, the mechanical properties of the regenerated aluminum alloy material are as follows: the yield strength is 230-260 MPa, the tensile strength is greater than or equal to 260 MPa, the ductility is 8-9%, and the absorbing energy is greater than or equal to 21.0 kJ.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of recycled aluminum alloys, and in particular relates to a recycled aluminum alloy material for automobiles, and a production method thereof. Background Art

[0002] Recycled aluminum alloy material refers to a relatively special aluminum alloy material that includes an appropriate amount of aluminum alloy recycled materials, as opposed to primary aluminum alloy material.

[0003] Compared with primary aluminum alloy materials, the main advantages of recycled aluminum alloy materials are energy saving and environmental protection, while the main disadvantage is that it is difficult to obtain the same performance level. However, considering comprehensive resources, environment, technology and other aspects, recycled aluminum alloy materials have great development prospects.

[0004] On the other hand, recycled aluminum alloy materials are commonly used in automobiles, such as the energy absorption box of the anti-collision beam. The function of the energy absorption box of the anti-collision beam is to absorb the impact energy, thereby protecting the vehicle structure and the safety of the occupants. The general principle is that it undergoes plastic deformation to prevent a large amount of impact energy from being transmitted to the interior of the vehicle.

[0005] Therefore, an anti-collision beam energy absorption box with excellent performance has at least the following characteristics: greater yield strength, greater tensile strength, appropriate elongation, and greater absorption work.

[0006] For example, the Chinese invention patent application with application publication number CN117144205A and application publication date 2023.12.01 discloses a recycled aluminum alloy material for an automobile energy absorption box, which is composed of the following components in mass percentage: Si 0.7-0.8%, Mg 0.75-0.85%, Cu 0.1-0.2%, Fe 0.13-0.4%, Cr 0.05-0.15%, Mn 0.2-0.35%, V 0.03-0.1%, Zr 0.02-0.08%, Ti 0.005-0.02%, RE 0.01-0.05%, Sr 0.005-0.02%, and the total amount of other impurity elements ≤0.30%, and the balance is Al; the RE is at least one of La and Ce, and the RE and Sr are added in the form of Al-Sr-RE.

[0007] The recycled aluminum alloy material for automobile crash boxes in this invention patent application achieves the regulation of the structure and performance of automobile crash box profiles through alloy composition optimization design, solves the problem of imbalance between the tensile mechanical properties, plasticity and uniformity of the crash boxes, fully utilizes the energy-saving and consumption-reducing effect of waste aluminum materials, and prepares high-performance automobile crash box aluminum alloy profiles through composition optimization design, realizing high-value recovery and utilization of recycled aluminum.

[0008] However, the recycled aluminum alloy material still has at least the following disadvantages in the actual production and use process, which is also the technical problem to be solved by the present invention, namely: Its composition includes rare earth elements La or Ce, so the cost of the recycled aluminum alloy material is relatively high and the production difficulty is relatively large.

[0009] So in summary, there is an urgent need for a new type of recycled aluminum alloy material that does not include rare earth elements and whose final automobile energy absorption box performance can still meet the requirements of automobile safety design. Summary of the invention

[0010] The invention provides a recycled aluminum alloy material for automobiles. The recycled aluminum alloy material can be recycled from waste automobile engine cylinder blocks, waste automobile wheels and waste automobile frames, and the weight proportion of recycled aluminum waste materials is controlled to be 40-60%. The components are finally adjusted to be: Si 0.40-0.45%, Fe 0.150-0.170%, Cu 0.016-0.018%, Mn 0.010-0.012%, Mg0.550-0.560%, Cr 0.009-0.010%, Zn 0.020-0.025%, Ti 0.011-0.014%, the total amount of impurity elements is ≤0.20%, and the balance is Al. In this way, the recycled aluminum alloy material can still achieve higher mechanical properties without using rare earth metals, and meet the use requirements of an automobile anti-collision beam energy absorption box.

[0011] Specifically, the mechanical properties of the recycled aluminum alloy material are as follows: yield strength: 230-260 MPa, tensile strength: ≥260 MPa, elongation: 8-9%, and absorbed energy: ≥21.0 kJ.

[0012] In addition, the present invention also provides a production method of the above-mentioned recycled aluminum alloy material, which comprises the following steps in sequence: pretreatment, melting, refinement and modification, first refining, composition adjustment, second refining, ingot casting, and aging treatment, to ensure that the above-mentioned recycled aluminum alloy material finally obtained has the above-mentioned high mechanical properties and can be used to manufacture automobile anti-collision beam energy absorption boxes.

[0013] The technical solution adopted by the present invention to solve the above problem is: a recycled aluminum alloy material for automobiles, the raw material composition includes the following components by weight: Si 0.40-0.45%, Fe 0.150-0.170%, Cu 0.016-0.018%, Mn 0.010-0.012%, Mg 0.550-0.560%, Cr 0.009-0.010%, Zn 0.020-0.025%, Ti 0.011-0.014%, the total amount of impurity elements is ≤0.20%, and the balance is Al; The weight proportion of recycled aluminum scrap in the raw material composition is 40-60%, and the recycled aluminum scrap includes used automobile engine blocks, used automobile wheels, and used automobile frames.

[0014] In the present invention, the recycled aluminum alloy material belongs to the 6XXX series aluminum alloy, so that the final automobile anti-collision beam energy absorption box product has sufficient and appropriate mechanical properties and outstanding corrosion resistance.

[0015] The scrap automobile engine cylinder block, scrap automobile wheel hub, and scrap automobile frame mainly include 4XXX, 5XXX, and 6XXX series aluminum alloys. Such scrap aluminum alloys have relatively excellent comprehensive properties, including: greater tensile strength, high elongation, wear resistance, and light weight.

[0016] More importantly, the raw material composition of the above three series of aluminum alloys is similar, so the total amount of impurity elements can be controlled below 0.20% in the end. Otherwise, the value may be as high as 0.50%, which is not conducive to the yield and tensile properties of the final automobile anti-collision beam energy absorption box product.

[0017] A further preferred technical solution is that the raw material composition includes the following components by weight: Si 0.41%, Fe 0.17%, Cu 0.016%, Mn 0.01%, Mg 0.55%, Cr 0.009%, Zn 0.02%, Ti 0.011%, the total amount of impurity elements ≤ 0.20%, and the balance is Al.

[0018] A method for producing recycled aluminum alloy materials for automobiles comprises the following steps in sequence: S1, pretreatment: crushing the waste aluminum recovery material to obtain crushed material; S2, melting: heating and melting the crushed material in a smelting furnace to obtain a molten material; S3, refinement and modification: adding Mg-Si alloy to the molten material, continuing heating and melting, to obtain a refined material; S4, first refining: adding a refining agent to the refined material, performing degassing and deslagging operations to obtain a coarse material; S5. Composition adjustment: sampling the coarse material, testing the chemical composition, and adding alloy material, magnesium ingot and aluminum ingot so that the raw material composition meets the preset range to obtain a recycled aluminum alloy melt; S6, second refining: adding a refining agent to the recycled aluminum alloy melt for a second time, performing a degassing and deslagging operation to obtain a recycled material; S7, ingot casting: introducing the recycled material into a crystallizer, and adopting a semi-continuous casting method to prepare a recycled aluminum alloy ingot; S8. Aging treatment: performing solid solution treatment, water quenching and aging treatment on the recycled aluminum alloy ingot in sequence to obtain the final recycled aluminum alloy material for automobiles.

[0019] In S3, refinement modification of the present invention, the principle is that both Mg and Si elements can act as nucleating agents in the molten material system, and eventually form fine casting grains inside the molten material system, which has a prominent improvement effect on the mechanical properties of the final recycled aluminum alloy material.

[0020] On the other hand, compared with Al-Mg-Si alloy, the advantages of Mg-Si alloy are: lower density, faster dispersion, better dispersion uniformity, and better thermal conductivity, which is also beneficial to the purpose of rapid and uniform dispersion of Mg and Si elements as nucleating agents.

[0021] In addition, if Mg and Si elements are added separately, not only will their shapes be unstable, but special protective solvents need to be added during melting, which further increases the final total amount of impurity elements.

[0022] A further preferred technical solution is that in S2, the temperature of the heating and melting operation is 750-900°C.

[0023] A further preferred technical solution is that in the Mg-Si alloy of S3, the addition amounts of Si and Mg are both less than 15% of the total amounts of Si and Mg in the raw material composition.

[0024] In the present invention, the effects of Mg on the final recycled aluminum alloy material mainly include: improving strength and rigidity, enhancing ductility, and improving work hardening performance, while the main effects of Si include: improving strength, hardness and wear resistance.

[0025] However, if a relatively large amount of Si and Mg are used as the above nucleating agents, the main effect of the two on increasing the lattice compactness will be relatively reduced. In particular, if Si is added in large amounts in the relatively early S3, its relatively late-stage effect of reducing the shrinkage of the aluminum liquid during solidification will also be significantly reduced.

[0026] Therefore, the amount of Mg and Si added in S3 needs to be controlled at a relatively low ratio.

[0027] A further preferred technical solution is that in S4, the amount of the refining agent added is 45-50% of the total amount of the refining agent.

[0028] A further preferred technical solution is that in S5, the alloy material includes Mg-Si alloy, Mg-Fe-Cu alloy, Mg-Mn alloy, Mg-Cr alloy, and Mg-Zn-Ti alloy.

[0029] In the present invention, the above-mentioned elements that differ from the set ratio of the raw material composition of the recycled aluminum alloy material are added in the form of magnesium alloy. The reasons and advantages are as follows: First, in addition to Al, the most abundant element in the material is Mg, so the above-mentioned method of adding magnesium alloy is completely applicable; Second, compared with aluminum alloy, the advantages of magnesium alloy include at least good thermal conductivity and low density, so various factors can be dispersed more quickly and evenly, ultimately improving the castability, dimensional stability and machinability of the recycled aluminum alloy material.

[0030] A further preferred technical solution is that in S5, the amount of magnesium ingot added accounts for 22-35% of the total amount of Mg in the raw material composition.

[0031] In the present invention, all Mg elements required for the recycled aluminum alloy material are mainly added in the form of magnesium alloy, followed by Mg-Si nucleating agent and magnesium ingot. The reason is to ensure that the insufficient elements after chemical composition test can be combined with Mg element first to obtain a fast dispersion speed and dispersion degree in the molten system.

[0032] A further preferred technical solution is that in the semi-continuous casting method of S7, the temperature of the recycled material is 650-780°C.

[0033] A further preferred technical solution is that in S8, the temperature of the solutionizing operation is 460-480°C and the time is 1-3h, the end point of the water quenching operation is until the temperature of the regenerated aluminum alloy ingot is ≤150°C, and the time of the aging operation is 10-15h. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1 It is the average value result of the performance test of the energy absorption box products in 4 embodiments and 6 comparative examples of the present invention.

[0035] Figure 2 This is a schematic diagram of the casting structure of the recycled aluminum alloy material in Example 1 of the present invention. DETAILED DESCRIPTION

[0036] The following descriptions are merely preferred embodiments of the present invention and are not intended to limit the scope of the present invention.

[0037] Example 1 As attached Figure 1-2As shown, a recycled aluminum alloy material for automobiles, the raw material composition of which includes the following components by weight: Si 0.41%, Fe 0.17%, Cu 0.016%, Mn 0.01%, Mg 0.55%, Cr0.009%, Zn 0.02%, Ti0.011%, the total amount of impurity elements ≤0.20%, and the balance is Al.

[0038] The weight proportion of scrap aluminum recycling materials in the raw material composition is 45%, and among the scrap aluminum recycling materials, the weight proportion of scrap automobile engine blocks, scrap automobile wheels and scrap automobile frames is ≥95%.

[0039] The above-mentioned method for producing the recycled aluminum alloy material for automobiles comprises the following steps in sequence: S1, pretreatment: crushing the waste aluminum recovery material to obtain crushed material; S2, melting: heating and melting the crushed material in a smelting furnace to obtain a molten material; S3, refinement and modification: adding Mg-Si alloy to the molten material, continuing heating and melting, to obtain a refined material; S4, first refining: adding a refining agent to the refined material, performing degassing and deslagging operations to obtain a coarse material; S5. Composition adjustment: sampling the coarse material, testing the chemical composition, and adding alloy material, magnesium ingot and aluminum ingot so that the raw material composition meets the preset range to obtain a recycled aluminum alloy melt; S6, second refining: adding a refining agent to the recycled aluminum alloy melt for a second time, performing a degassing and deslagging operation to obtain a recycled material; S7, ingot casting: introducing the recycled material into a crystallizer, and adopting a semi-continuous casting method to prepare a recycled aluminum alloy ingot; S8. Aging treatment: performing solid solution treatment, water quenching and aging treatment on the recycled aluminum alloy ingot in sequence to obtain the final recycled aluminum alloy material for automobiles.

[0040] In S1, the waste aluminum recycling material is subjected to necessary cleaning and water removal operations before being crushed, and finally the maximum length of the crushed material is controlled within 5 cm.

[0041] In S2, the temperature of the heating and melting operation is 820°C.

[0042] In the Mg-Si alloy of S3, the addition amounts of Si and Mg are both less than 15% of the total amounts of Si and Mg in the raw material composition, respectively, and the heating and melting temperature is continued at 850° C. for 2 hours.

[0043] In S4 and S6, the refining agent is a commercially available sodium type refining agent. The amount of refining agent added in S4 is 45% of the total amount of refining agent, while the total amount of refining agent is 0.5% of the weight of the recycled aluminum alloy melt in S5.

[0044] In S5, the alloy material includes Mg-Si alloy, Mg-Fe-Cu alloy, Mg-Mn alloy, Mg-Cr alloy, and Mg-Zn-Ti alloy.

[0045] In addition, when Fe, Cu, Zn and Ti are missing individually, the following alloys, such as Mg-Fe alloy and Mg-Cu alloy, can be used to ultimately ensure that the contents of all components required by the recycled aluminum alloy material reach a preset ratio.

[0046] In S5, the amount of magnesium ingot added accounts for 25-30% of the total Mg in the raw material composition.

[0047] In the semi-continuous casting method of S7, the temperature of the recycled material is 700°C.

[0048] In S8, the temperature of the solutionizing operation is 480°C and the time is 3 hours. The end point of the water quenching operation is until the temperature of the regenerated aluminum alloy ingot reaches 140°C. The time of the aging operation is 10 hours.

[0049] Finally, the recycled aluminum alloy material was made into an automobile anti-collision beam energy absorption box through machining method, and 50 groups were sampled for mechanical property test and impact test, and the average value was taken. The final result was recorded in the attached Figure 1 in the table.

[0050] Example 2 As attached Figure 1 As shown, a recycled aluminum alloy material for automobiles, whose raw material composition includes the following components by weight: Si 0.42%, Fe 0.17%, Cu 0.018%, Mn 0.01%, Mg 0.55%, Cr0.009%, Zn 0.02%, Ti0.012%, the total amount of impurity elements ≤0.20%, and the balance is Al.

[0051] The weight proportion of scrap aluminum recycling materials in the raw material composition is 52%, and the weight proportion of scrap automobile engine blocks, scrap automobile wheels and scrap automobile frames in the scrap aluminum recycling materials is ≥95%.

[0052] The above-mentioned method for producing the recycled aluminum alloy material for automobiles comprises the following steps in sequence: S1, pretreatment: crushing the waste aluminum recovery material to obtain crushed material; S2, melting: heating and melting the crushed material in a smelting furnace to obtain a molten material; S3, refinement and modification: adding Mg-Si alloy to the molten material, continuing heating and melting, to obtain a refined material; S4, first refining: adding a refining agent to the refined material, performing degassing and deslagging operations to obtain a coarse material; S5. Composition adjustment: sampling the coarse material, testing the chemical composition, and adding alloy material, magnesium ingot and aluminum ingot so that the raw material composition meets the preset range to obtain a recycled aluminum alloy melt; S6, second refining: adding a refining agent to the recycled aluminum alloy melt for a second time, performing a degassing and deslagging operation to obtain a recycled material; S7, ingot casting: introducing the recycled material into a crystallizer, and adopting a semi-continuous casting method to prepare a recycled aluminum alloy ingot; S8. Aging treatment: performing solid solution treatment, water quenching and aging treatment on the recycled aluminum alloy ingot in sequence to obtain the final recycled aluminum alloy material for automobiles.

[0053] In S1, the waste aluminum recycling material is subjected to necessary cleaning and water removal operations before being crushed, and finally the maximum length of the crushed material is controlled within 5 cm.

[0054] In S2, the temperature of the heating and melting operation is 900°C.

[0055] In the Mg-Si alloy of S3, the addition amounts of Si and Mg are both less than 15% of the total amounts of Si and Mg in the raw material composition, respectively, and the heating and melting temperature is continued at 860° C. for 3 hours.

[0056] In S4 and S6, the refining agent is a commercially available sodium type refining agent. The amount of refining agent added in S4 is 50% of the total amount of refining agent, while the total amount of refining agent is 0.7% of the weight of the recycled aluminum alloy melt in S5.

[0057] In S5, the alloy material includes Mg-Si alloy, Mg-Fe-Cu alloy, Mg-Mn alloy, Mg-Cr alloy, and Mg-Zn-Ti alloy.

[0058] In addition, when Fe, Cu, Zn and Ti are missing individually, the following alloys, such as Mg-Fe alloy and Mg-Zn alloy, can be used to ultimately ensure that the contents of all components required by the recycled aluminum alloy material reach a preset ratio.

[0059] In S5, the amount of magnesium ingot added accounts for 25-26% of the total Mg in the raw material composition.

[0060] In the semi-continuous casting method of S7, the temperature of the recycled material is 750°C.

[0061] In S8, the temperature of the solutionizing operation is 480°C and the time is 2 hours. The end point of the water quenching operation is until the temperature of the regenerated aluminum alloy ingot reaches 120°C. The time of the aging operation is 15 hours.

[0062] Finally, the recycled aluminum alloy material was made into an automobile anti-collision beam energy absorption box through machining method, and 50 groups were sampled for mechanical property test and impact test, and the average value was taken. The final result was recorded in the attached Figure 1 in the table.

[0063] Example 3 As attached Figure 1 As shown, a recycled aluminum alloy material for automobiles, the raw material composition of which includes the following components by weight: Si 0.44%, Fe 0.17%, Cu 0.018%, Mn 0.011%, Mg 0.55%, Cr0.01%, Zn 0.025%, Ti0.012%, the total amount of impurity elements ≤0.20%, and the balance is Al.

[0064] The weight proportion of scrap aluminum recycling materials in the raw material composition is 60%, and among the scrap aluminum recycling materials, the weight proportion of scrap automobile engine blocks, scrap automobile wheels and scrap automobile frames is ≥95%.

[0065] The above-mentioned method for producing the recycled aluminum alloy material for automobiles comprises the following steps in sequence: S1, pretreatment: crushing the waste aluminum recovery material to obtain crushed material; S2, melting: heating and melting the crushed material in a smelting furnace to obtain a molten material; S3, refinement and modification: adding Mg-Si alloy to the molten material, continuing heating and melting, to obtain a refined material; S4, first refining: adding a refining agent to the refined material, performing degassing and deslagging operations to obtain a coarse material; S5. Composition adjustment: sampling the coarse material, testing the chemical composition, and adding alloy material, magnesium ingot and aluminum ingot so that the raw material composition meets the preset range to obtain a recycled aluminum alloy melt; S6, second refining: adding a refining agent to the recycled aluminum alloy melt for a second time, performing a degassing and deslagging operation to obtain a recycled material; S7, ingot casting: introducing the recycled material into a crystallizer, and adopting a semi-continuous casting method to prepare a recycled aluminum alloy ingot; S8. Aging treatment: performing solid solution treatment, water quenching and aging treatment on the recycled aluminum alloy ingot in sequence to obtain the final recycled aluminum alloy material for automobiles.

[0066] In S1, the waste aluminum recycling material is subjected to necessary cleaning and water removal operations before being crushed, and finally the maximum length of the crushed material is controlled within 5 cm.

[0067] In S2, the temperature of the heating and melting operation is 800°C.

[0068] In the Mg-Si alloy of S3, the addition amounts of Si and Mg are both less than 15% of the total amounts of Si and Mg in the raw material composition, respectively, and the heating and melting temperature is continued at 820° C. for 3 hours.

[0069] In S4 and S6, the refining agent is a commercially available sodium type refining agent. The amount of refining agent added in S4 is 50% of the total amount of refining agent, while the total amount of refining agent is 1.0% of the weight of the recycled aluminum alloy melt in S5.

[0070] In S5, the alloy material includes Mg-Si alloy, Mg-Fe-Cu alloy, Mg-Mn alloy, Mg-Cr alloy, and Mg-Zn-Ti alloy.

[0071] In addition, when Fe, Cu, Zn and Ti are missing individually, the following alloys, such as Mg-Fe alloy and Mg-Zn alloy, can be used to ultimately ensure that the contents of all components required by the recycled aluminum alloy material reach a preset ratio.

[0072] In S5, the amount of magnesium ingot added accounts for 22-25% of the total Mg in the raw material composition.

[0073] In the semi-continuous casting method of S7, the temperature of the recycled material is 780°C.

[0074] In S8, the temperature of the solutionizing operation is 460°C and the time is 2 hours, the end point of the water quenching operation is until the temperature of the regenerated aluminum alloy ingot reaches 150°C, and the time of the aging operation is 15 hours.

[0075] Finally, the recycled aluminum alloy material was made into an automobile anti-collision beam energy absorption box through machining method, and 50 groups were sampled for mechanical property test and impact test, and the average value was taken. The final result was recorded in the attached Figure 1 in the table.

[0076] Example 4 As attached Figure 1 As shown, a recycled aluminum alloy material for automobiles, whose raw material composition includes the following components by weight: Si 0.44%, Fe 0.17%, Cu 0.017%, Mn 0.011%, Mg 0.552%, Cr0.01%, Zn 0.025%, Ti0.012%, the total amount of impurity elements ≤0.20%, and the balance is Al.

[0077] The weight proportion of scrap aluminum recycling materials in the raw material composition is 58%, and among the scrap aluminum recycling materials, the weight proportion of scrap automobile engine blocks, scrap automobile wheels and scrap automobile frames is ≥95%.

[0078] The above-mentioned method for producing the recycled aluminum alloy material for automobiles comprises the following steps in sequence: S1, pretreatment: crushing the waste aluminum recovery material to obtain crushed material; S2, melting: heating and melting the crushed material in a smelting furnace to obtain a molten material; S3, refinement and modification: adding Mg-Si alloy to the molten material, continuing heating and melting, to obtain a refined material; S4, first refining: adding a refining agent to the refined material, performing degassing and deslagging operations to obtain a coarse material; S5. Composition adjustment: sampling the coarse material, testing the chemical composition, and adding alloy material, magnesium ingot and aluminum ingot so that the raw material composition meets the preset range to obtain a recycled aluminum alloy melt; S6, second refining: adding a refining agent to the recycled aluminum alloy melt for a second time, performing a degassing and deslagging operation to obtain a recycled material; S7, ingot casting: introducing the recycled material into a crystallizer, and adopting a semi-continuous casting method to prepare a recycled aluminum alloy ingot; S8. Aging treatment: performing solid solution treatment, water quenching and aging treatment on the recycled aluminum alloy ingot in sequence to obtain the final recycled aluminum alloy material for automobiles.

[0079] In S1, the waste aluminum recycling material is subjected to necessary cleaning and water removal operations before being crushed, and finally the maximum length of the crushed material is controlled within 5 cm.

[0080] In S2, the temperature of the heating and melting operation is 880°C.

[0081] In the Mg-Si alloy of S3, the addition amounts of Si and Mg are both less than 15% of the total amounts of Si and Mg in the raw material composition, respectively, and the heating and melting temperature is continued at 820° C. for 3 hours.

[0082] In S4 and S6, the refining agent is a commercially available sodium type refining agent. The amount of refining agent added in S4 is 50% of the total amount of refining agent, while the total amount of refining agent is 1.1% of the weight of the recycled aluminum alloy melt in S5.

[0083] In S5, the alloy material includes Mg-Si alloy, Mg-Fe-Cu alloy, Mg-Mn alloy, Mg-Cr alloy, and Mg-Zn-Ti alloy.

[0084] In addition, when Fe, Cu, Zn and Ti are missing individually, the following alloys, such as Mg-Fe alloy and Mg-Zn alloy, can be used to ultimately ensure that the contents of all components required by the recycled aluminum alloy material reach a preset ratio.

[0085] In S5, the amount of magnesium ingot added accounts for 25-30% of the total Mg in the raw material composition.

[0086] In the semi-continuous casting method of S7, the temperature of the recycled material is 690°C.

[0087] In S8, the temperature of the solutionizing operation is 460°C and the time is 1 hour, the end point of the water quenching operation is until the temperature of the regenerated aluminum alloy ingot reaches 150°C, and the time of the aging operation is 15 hours.

[0088] Finally, the recycled aluminum alloy material was made into an automobile anti-collision beam energy absorption box through machining method, and 50 groups were sampled for mechanical property test and impact test, and the average value was taken. The final result was recorded in the attached Figure 1 in the table.

[0089] Comparative Example 1 The recycled aluminum alloy material in this comparative example has only the following differences in formulation and process compared with the recycled aluminum alloy material in Example 1: The weight proportion of recycled waste aluminum in the raw material composition is 10%.

[0090] Finally, the recycled aluminum alloy material was made into an automobile anti-collision beam energy absorption box by machining, and 50 groups were sampled for mechanical property test and impact test, and the average value was taken. The final result was recorded in the attached Figure 1 in the table.

[0091] Comparative Example 2 The recycled aluminum alloy material in this comparative example has only the following differences in formulation and process compared with the recycled aluminum alloy material in Example 1: The weight proportion of recycled waste aluminum in the raw material composition is 65%.

[0092] Finally, the recycled aluminum alloy material was made into an automobile anti-collision beam energy absorption box by machining, and 50 groups were sampled for mechanical property test and impact test, and the average value was taken. The final result was recorded in the attached Figure 1 in the table.

[0093] Comparative Example 3 The recycled aluminum alloy material in this comparative example has only the following differences in formulation and process compared with the recycled aluminum alloy material in Example 1: The weight proportion of recycled waste aluminum in the raw material composition is 85%.

[0094] Finally, the recycled aluminum alloy material was made into an automobile anti-collision beam energy absorption box by machining, and 50 groups were sampled for mechanical property test and impact test, and the average value was taken. The final result was recorded in the attached Figure 1 in the table.

[0095] Comparative Example 4 The recycled aluminum alloy material in this comparative example has only the following differences in formulation and process compared with the recycled aluminum alloy material in Example 1: In S3, during the refinement and modification operation, the Mg-Si alloy is replaced with an AL-Mg alloy and an AL-Si alloy having the same Mg weight and Si weight.

[0096] Finally, the recycled aluminum alloy material was made into an automobile anti-collision beam energy absorption box by machining, and 50 groups were sampled for mechanical property test and impact test, and the average value was taken. The final result was recorded in the attached Figure 1 in the table.

[0097] Comparative Example 5 The recycled aluminum alloy material in this comparative example has only the following differences in formulation and process compared with the recycled aluminum alloy material in Example 1: In S5, during the composition adjustment operation, all magnesium alloys are replaced with aluminum alloys, including: AL-Mg-Si alloy, AL-Fe-Cu alloy, AL-Mn alloy, AL-Cr alloy, and AL-Zn-Ti alloy, or as needed, such as: AL-Cu alloy, AL-Zn alloy, etc.

[0098] Finally, the recycled aluminum alloy material was made into an automobile anti-collision beam energy absorption box by machining, and 50 groups were sampled for mechanical property test and impact test, and the average value was taken. The final result was recorded in the attached Figure 1 in the table.

[0099] Comparative Example 6 The recycled aluminum alloy material in this comparative example has only the following differences in formulation and process compared with the recycled aluminum alloy material in Example 1: In S5, the amount of magnesium ingot added accounts for 55% of the total Mg in the raw material composition.

[0100] Finally, the recycled aluminum alloy material was made into an automobile anti-collision beam energy absorption box by machining, and 50 groups were sampled for mechanical property test and impact test, and the average value was taken. The final result was recorded in the attached Figure 1 in the table.

[0101] Results Analysis First, as attached Figure 2 As shown, the casting structure of the recycled aluminum alloy material in Example 1 is dense and orderly, corresponding to its higher mechanical tensile properties, so that it can meet the performance requirements of the energy absorption box of the automobile anti-collision beam.

[0102] Second, as attached Figure 1 As shown in the test results of the four embodiments, these four batches of automobile anti-collision beam energy absorption box products all have excellent mechanical tensile properties and impact absorption capabilities. The specific numerical ranges are as follows: yield strength: 230-260MPa, tensile strength: ≥260MPa, elongation: 8-9%, absorbed energy: ≥21.0kJ, ensuring that the automobile anti-collision beam energy absorption box product has sufficient safety performance.

[0103] Third, as shown in the test results of Comparative Example 1, the weight of recycled waste aluminum accounts for only 10% of its raw material composition, so it has greater yield strength, tensile strength, and outstanding impact energy absorption capacity, which is relatively reasonable. The aluminum alloy material at this time is similar to the original aluminum alloy, so the performance is relatively outstanding.

[0104] However, its elongation is relatively small. The reason may be that after the aluminum added in the form of aluminum ingots accounts for the vast majority, the timing of adding aluminum materials into the molten system is too late, which is not conducive to the improvement of its ductility. This will affect the machining performance of aluminum alloy materials and is not conducive to the forming and preparation of energy absorption boxes. In addition, it does not have the advantages of energy saving and environmental protection.

[0105] Fourth, as shown in the test results of Comparative Examples 2 and 3, the weight proportion of recycled waste aluminum in the raw material composition is too high. Even after sufficient refinement, refining, and aging treatment, the overall mechanical properties of the aluminum alloy cannot be significantly improved, and it can be determined that it does not meet the use requirements of the automotive anti-collision beam energy absorption box.

[0106] Fifth, as shown in the test results of Comparative Example 4, during the refinement and metamorphism operation, all magnesium alloys were replaced with aluminum alloys. It is precisely because the latter has a relatively large density and relatively poor thermal conductivity that the refinement effect is reduced, which is ultimately reflected in the performance of the energy absorption box, that is, the tensile strength is insufficient and the elongation is not appropriate, and it is also impossible to produce qualified automobile anti-collision beam energy absorption boxes.

[0107] Sixth, as shown in the test results of Comparative Examples 5 and 6, the performance parameters of the energy absorption boxes of both are lower than those of the embodiment, because the aluminum alloy cannot quickly disperse the missing elements compared to the magnesium alloy. In Comparative Example 6, the content of the Mg element is mainly added in the form of magnesium ingots, which reduces the amount of the above-mentioned magnesium alloy, and also makes it impossible to obtain a sufficiently fast and uniform dispersion effect for the missing elements such as Cu and Mn, which is ultimately reflected in the performance of the energy absorption box, that is, the mechanical tensile properties and impact energy absorption properties are insufficient.

[0108] The embodiments of the present invention are described in detail above in conjunction with the accompanying drawings, but the present invention is not limited to the above embodiments. Various modifications can be made within the knowledge of ordinary technicians in the technical field without departing from the purpose of the present invention. These are all non-creative modifications and are protected by patent law as long as they are within the scope of the claims of the present invention.

Claims

1. A recycled aluminum alloy material for automobiles, characterized in that The raw material composition includes the following components by weight: Si 0.40-0.45%, Fe 0.150-0.170%, Cu 0.016-0.018%, Mn 0.010-0.012%, Mg 0.550-0.560%, Cr 0.009-0.010%, Zn 0.020-0.025%, Ti 0.011-0.014%, the total amount of impurity elements ≤ 0.20%, and the balance is Al; The weight proportion of recycled aluminum scrap in the raw material composition is 40-60%, and the recycled aluminum scrap includes used automobile engine blocks, used automobile wheels, and used automobile frames.

2. The recycled aluminum alloy material for automobile according to claim 1, characterized in that The raw material composition includes the following components by weight: Si 0.41%, Fe 0.17%, Cu 0.016%, Mn 0.01%, Mg 0.55%, Cr 0.009%, Zn 0.02%, Ti 0.011%, the total amount of impurity elements ≤ 0.20%, and the balance is Al.

3. A method for producing recycled aluminum alloy material for automobiles as claimed in claim 1, characterized in that The following steps are included in sequence: S1, pretreatment: crushing the waste aluminum recovery material to obtain crushed material; S2, melting: heating and melting the crushed material in a smelting furnace to obtain a molten material; S3, refinement and modification: adding Mg-Si alloy to the molten material, continuing heating and melting, to obtain a refined material; S4, first refining: adding a refining agent to the refined material, performing degassing and deslagging operations to obtain a coarse material; S5. Composition adjustment: sampling the coarse material, testing the chemical composition, and adding alloy material, magnesium ingot and aluminum ingot so that the raw material composition meets the preset range to obtain a recycled aluminum alloy melt; S6, second refining: adding a refining agent to the recycled aluminum alloy melt for a second time, performing a degassing and deslagging operation to obtain a recycled material; S7, ingot casting: introducing the recycled material into a crystallizer, and adopting a semi-continuous casting method to prepare a recycled aluminum alloy ingot; S8. Aging treatment: performing solid solution treatment, water quenching and aging treatment on the recycled aluminum alloy ingot in sequence to obtain the final recycled aluminum alloy material for automobiles.

4. The method for producing a recycled aluminum alloy material for automobiles according to claim 3, characterized in that: In S2, the temperature of the heating and melting operation is 750-900°C.

5. The method for producing a recycled aluminum alloy material for automobiles according to claim 3, characterized in that: In the Mg-Si alloy of S3, the added amounts of Si and Mg are each less than 15% of the total amounts of Si and Mg in the raw material composition.

6. The method for producing a recycled aluminum alloy material for automobiles according to claim 3, characterized in that: In S4, the amount of the refining agent added is 45-50% of the total amount of the refining agent.

7. The method for producing a recycled aluminum alloy material for automobiles according to claim 3, characterized in that: In S5, the alloy material includes Mg-Si alloy, Mg-Fe-Cu alloy, Mg-Mn alloy, Mg-Cr alloy, and Mg-Zn-Ti alloy.

8. The method for producing a recycled aluminum alloy material for automobiles according to claim 3, characterized in that: In S5, the amount of magnesium ingot added accounts for 22-35% of the total Mg in the raw material composition.

9. The method for producing a recycled aluminum alloy material for automobiles according to claim 3, characterized in that: In the semi-continuous casting method of S7, the temperature of the recycled material is 650-780°C.

10. The method for producing a recycled aluminum alloy material for automobiles according to claim 3, characterized in that: In S8, the temperature of the solutionizing operation is 460-480°C and the time is 1-3h, the end point of the water quenching operation is until the temperature of the regenerated aluminum alloy ingot is ≤150°C, and the time of the aging operation is 10-15h.

Citation Information

Cited By

  • Method for regenerating 6XXX series aluminum alloy microelement composite regulation and control thermal deformation synergistic grain refinement

    CN121204480A