Hot-rolled pickled plate with high surface requirement and production method thereof

By adjusting the heating, rolling and cooling processes and controlling the thickness of the scale, the problem of scale defects in hot-rolled pickled plates is solved, the surface quality and qualification rate are improved, and an efficient production process is achieved.

CN118756044APending Publication Date: 2024-10-11HEBEI IRON AND STEEL
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410837701.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-26
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

In the production process of hot-rolled pickled plates, oxide scale defects (primary, secondary, and tertiary) seriously affect the surface quality, resulting in a high scrap rate. It is difficult to effectively prevent and reduce secondary and tertiary scale defects with existing technology.

Method used

By adjusting the heating process, rolling process parameters and cooling process, using low-temperature heating technology, five passes of descaling, laminar cooling and anti-flaking water, the thickness of the iron oxide scale is controlled within 11 μm to ensure surface quality.

Benefits of technology

It effectively reduces the generation of iron oxide scale and improves the surface quality of hot-rolled pickled plates. The pass rate reaches 99.1%, meets FC grade standards and avoids surface defects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention discloses a hot-rolled pickled plate with high surface requirements and a production method thereof, and belongs to the technical field of hot-rolled strip steel rolling, the hot-rolled pickled plate comprises the following chemical components by weight: 0.025-0.055% of C, less than or equal to 0.030% of Si, 0.25-0.35% of Mn, less than or equal to 0.012% of P, less than or equal to 0.006% of S, 0.030-0.050% of Als, and the balance Fe and inevitable impurity elements. The production method comprises the working procedures of heating, rolling, cooling and coiling. By adjusting parameters of the heating process and the rolling process and optimizing the cooling process, generation of the oxide scale is effectively avoided, the thickness of the oxide scale of the low-carbon steel hot-rolled pickled plate can be controlled within 11 microns, and the percent of pass of the hot-rolled pickled plate is larger than or equal to 99.1%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of hot-rolled strip steel rolling, and in particular relates to a hot-rolled pickled plate with high surface requirements and a production method thereof. Background Art

[0002] Hot-rolled pickled sheet is an intermediate product between hot-rolled sheet and cold-rolled sheet, and is an ideal substitute for some hot-rolled sheet and cold-rolled sheet. Compared with hot-rolled sheet, pickled sheet has higher surface quality and higher dimensional accuracy. Since hot-rolled pickled sheet removes surface oxide scale, the surface quality of steel is improved, which is convenient for welding, oiling and painting. Compared with cold-rolled sheet, the advantage of pickled sheet is that it allows users to effectively reduce procurement costs while ensuring the use requirements of surface quality. Many companies have put forward higher and higher requirements for high performance and low cost of steel. With the continuous advancement of steel rolling process technology, the performance of hot-rolled thin sheet is approaching that of cold-rolled sheet, making "replacing cold with heat" technically possible. It can be said that pickled sheet is a product with a relatively high performance-price ratio between cold-rolled sheet and hot-rolled sheet, and has a good market development prospect.

[0003] Low carbon steel accounts for a large proportion in hot-rolled pickled plates, but in the production process of hot-rolled pickled plates, iron oxide scale is a common defect, mainly primary iron oxide scale, secondary iron oxide scale, and tertiary iron oxide scale. Severe iron oxide scale shedding will cause pitting defects, which will seriously affect the surface quality of the pickled plate and even result in waste.

[0004] Patent No. CN111663078B discloses a hot-rolled pickled plate and a method for eliminating pit defects in hot-rolled pickled plate, including: Si: ≤0.05-0.5%, P: ≤0.015-0.07%, the mass fraction ratio of Si to P is 3-6, a descaling water device is provided between F1 and F2, a dust suppression water header is provided between F2 and F3, and the inlet working roll cooling water volume of F1-F4 rack is 60-80m 3 / h, the cooling water volume of the working rolls at the outlet of the F1-F4 stands is 370-400m 3 / h. This patent requires the addition of a descaling water device and a dust suppression water header, and the high Si and P content will increase the cost of the alloy.

[0005] Patent No. CN14472557B discloses a heating method for preventing scale defects of hot-rolled pickled plates, including solving the problem of serious scale defects of pickled plates by controlling the heating temperature and time of each heating section from the perspective of optimizing the heating process. This patent can only reduce the defect rate of primary scale of pickled plates, and does not provide detailed instructions on how to prevent and reduce secondary and tertiary scale. Summary of the invention

[0006] The invention provides a hot-rolled pickled plate with high surface requirements and a production method thereof. The oxide scale thickness of the low-carbon steel hot-rolled pickled plate can be controlled within 11 μm by adjusting the heating process and rolling process parameters and optimizing the cooling process, and the surface quality of the hot-rolled pickled plate is significantly improved.

[0007] In order to solve the above technical problems, the technical solution adopted by the present invention is: a hot-rolled pickled plate with high surface requirements, the chemical composition weight percentage of the hot-rolled pickled plate is: C: 0.025-0.055%, Si≤0.030%, Mn: 0.25-0.35%, P≤0.012%, S≤0.006%, Als: 0.030-0.050%, and the rest is Fe and unavoidable impurity elements.

[0008] The hot-rolled pickled plate of the present invention has a yield strength of 200-320 MPa, a tensile strength of 320-400 MPa, and an elongation after fracture of ≥37%.

[0009] The hot-rolled pickled plate of the present invention has a thickness specification of 3.0-8.0 mm and a width of 900-1630 mm.

[0010] The hot-rolled pickled plate of the present invention has an iron oxide scale thickness of ≤11 μm and a surface quality of FC grade, that is, no surface defects are allowed after pickling.

[0011] Another object of the present invention is to provide a production method for the above-mentioned hot-rolled pickled plate with high surface requirements, the production method comprising heating, rolling, cooling and coiling processes; the heating process adopts low-temperature heating technology, and the air-fuel ratio is controlled by a weak reducing atmosphere of 0.65-0.7.

[0012] The rolling process of the present invention includes rough rolling and finish rolling. The temperature of the rough rolling intermediate billet is set to 1000±20°C, and five passes of descaling are adopted, with the final pass speed of 3.0-4.5 m / s.

[0013] In the rolling process of the present invention, the hot coil box adopts a coiling mode, the coiling speed is 3.0-4.5 m / s, and is set to be consistent with the final pass speed of rough rolling.

[0014] The rolling process of the present invention includes rough rolling and finishing rolling. The finishing rolling rolls are first 5 pieces, and the finishing rolling rolls are hot-rolled according to a 3-minute rolling rhythm. Anti-stripping water is used in finishing rolling F1-F3, and high-speed steel working rolls are selected for F2 and F3.

[0015] The cooling process of the present invention is laminar cooling, adopts a front-stage dispersed cooling process, and the upper and lower spray ratios are 25%-75% and 25%-75% respectively.

[0016] In the coiling process of the present invention, the coiling temperature is set to 570±20°C.

[0017] The beneficial effects of the above technical solution are as follows: the present invention effectively reduces the generation of primary iron oxide scale by adjusting the process parameters, adopting low-temperature heating technology for heating, and controlling the air-fuel ratio by a weak reducing atmosphere of 0.65-0.70; the temperature of the rough rolling intermediate billet is set to 1000±20℃, five passes of descaling are adopted, and the speed of the last rough rolling pass and the coiling speed of the hot coil box are adjusted to be consistent, which effectively avoids the generation of secondary iron oxide scale; the first 5 rolls are hot-rolled according to the 3-minute rolling rhythm for finishing rolling, anti-stripping water is used for finishing rolling F1-F3, and high-speed steel working rolls are used for F2F3 , effectively avoiding the formation of tertiary iron scale; the laminar cooling adopts the front-stage dispersed cooling process and the coiling temperature is adjusted to 570±20℃, which can make the iron scale on the surface of the strip steel thinnest during coiling, improve the surface quality of the hot-rolled pickled plate, and the surface quality FC grade meets the quality requirement that no surface defects are allowed for the hot-rolled pickled plate after pickling; the present invention effectively avoids the generation of iron scale by adjusting the heating process and rolling process parameters and optimizing the cooling process, and can control the iron scale thickness of the low-carbon steel hot-rolled pickled plate within 11μm, so that the qualified rate of the hot-rolled pickled plate is ≥99.1%. DETAILED DESCRIPTION

[0018] The present invention will be further described in detail below in conjunction with specific embodiments. Throughout the specification, unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by those skilled in the art to which the present invention belongs, and if there is a conflict, the present specification takes precedence.

[0019] Examples 1-10 The hot-rolled pickled plate has the following chemical composition weight percentages: C: 0.025-0.055%, Si≤0.030%, Mn: 0.25-0.35%, P≤0.012%, S≤0.006%, Als: 0.030-0.050%, and the rest are Fe and unavoidable impurity elements. The chemical composition of the hot-rolled pickled plate of Examples 1-10 is specifically shown in Table 1.

[0020] A production method for hot-rolled pickled plates with high surface requirements, including heating, rolling, cooling and coiling processes; the specific steps are as follows: 1) Heating process: 10 slabs of Z-DD12-SFL brand are heated by low temperature technology, and the air-fuel ratio is controlled by 0.65-0.7 weak reducing atmosphere. The higher the heating temperature and the greater the air-fuel ratio, the thicker the primary oxide scale is, which is not conducive to descaling.

[0021] 2) Rolling process: including rough rolling and finishing rolling. During rough rolling, the slab is descaled in five passes, and the temperature of the rough rolling intermediate slab is set to 1000±20℃. Five passes are used for descaling, and the speed of the last pass is 3.0-4.5m / s. If the rough rolling outlet temperature is too high, it is easy to form a thicker secondary oxide scale, which is not conducive to the control of oxide scale in finishing rolling. If the rough rolling outlet temperature is too low, the finishing rolling bite is not used, which is not conducive to finishing rolling; The first 5 rollers of the finishing mill are hot-rolled in a 3-minute rolling rhythm. Anti-scaling water is used for finishing mills F1-F3, and high-speed steel working rolls are used for F2 and F3. Too fast a hot-rolling rhythm will affect the formation of oxide film on the finishing mill working rolls; anti-scaling water is used for F1-F3, and high-speed steel working rolls are used for F2 and F3, which can effectively avoid the tertiary iron scale caused by the shedding of the oxide film on the finishing mill working rolls; The hot coil box adopts coiling mode with a coiling speed of 3.0-4.5m / s, and is set consistent with the speed of the last pass of rough rolling. The inconsistency between the speed of the last pass of rough rolling and the coiling speed of the hot coil box will lead to the appearance of secondary iron oxide scale such as scratches.

[0022] 3) Cooling process: laminar cooling, using front-end dispersed cooling process, with upper and lower spray ratios of 25%-75% and 25%-75% respectively.

[0023] 4) Coiling process: The coiling temperature is set to 570±20℃, which can make the iron oxide scale on the surface of the strip thinnest during coiling, which is more conducive to the subsequent pickling of the strip.

[0024] It should be noted that, in the production schedule, 5 DD11-MDs were rolled before the 10 slabs and hot rolled at a 3-minute rhythm. The specific control parameters of each step of the production method of Examples 1-10 are shown in Table 2, and the performance is shown in Table 3.

[0025] Table 1 Chemical composition and mass percentage of hot-rolled pickled plate slabs of Examples 1-10 (%)

[0026] Table 2 Specific control parameters of each process of the production method of Examples 1-10

[0027] Table 3 Specifications and performance parameters of hot-rolled pickled plates of Examples 1-10

[0028] As can be seen from Table 1, Table 2 and Table 3, Examples 1-10 adopt the chemical composition and process of the present invention. The low-carbon hot-rolled pickled plate produced has fewer production processes, low energy consumption and cost, smooth surface quality, FC grade, and no surface defects after pickling.

[0029] The above embodiments are only used to illustrate rather than limit the technical solutions of the present invention. Although the present invention is described in detail with reference to the above embodiments, those skilled in the art should understand that the present invention can still be modified or replaced by equivalents. Any modification or partial replacement that does not depart from the spirit and scope of the present invention should be included in the scope of the claims of the present invention.

Claims

1. A hot-rolled pickled plate with high surface requirements, characterized in that: The chemical composition weight percentage of the hot-rolled pickled plate is: C: 0.025-0.055%, Si≤0.030%, Mn: 0.25-0.35%, P≤0.012%, S≤0.006%, Als: 0.030-0.050%, and the rest is Fe and unavoidable impurity elements.

2. A hot-rolled pickled plate with high surface requirements according to claim 1, characterized in that: The hot-rolled pickled plate has a yield strength of 200-320 MPa, a tensile strength of 320-400 MPa, and an elongation after fracture of ≥37%.

3. The hot-rolled pickled plate with high surface requirements according to claim 1, characterized in that: The hot-rolled pickled plate has a thickness specification of 3.0-8.0 mm and a width of 900-1630 mm.

4. The hot-rolled pickled plate with high surface requirements according to claim 1, characterized in that: The hot-rolled pickled plate has an iron oxide scale thickness of ≤11 μm and a surface quality of FC grade, that is, no surface defects are allowed after pickling.

5. A method for producing a hot-rolled pickled plate with high surface requirements according to any one of claims 1 to 4, characterized in that: The production method includes heating, rolling, cooling and coiling processes; the heating process adopts low-temperature heating technology, and the air-fuel ratio is controlled by a weak reducing atmosphere of 0.65-0.

7.

6. The method for producing a hot-rolled pickled plate with high surface requirements according to claim 5, characterized in that: The rolling process includes rough rolling and finish rolling. The temperature of the rough rolling intermediate billet is set to 1000±20°C, and five passes of descaling are adopted, with the final pass speed of 3.0-4.5 m / s.

7. The method for producing a hot-rolled pickled plate with high surface requirements according to claim 5, characterized in that: In the rolling process, the hot coil box adopts a coiling mode, the coiling speed is 3.0-4.5 m / s, and is set consistent with the final rough rolling speed.

8. The method for producing a hot-rolled pickled plate with high surface requirements according to any one of claims 5 to 7, characterized in that: The rolling process includes rough rolling and finishing rolling. The finishing rolling rolls are first 5 pieces, and the finishing rolling rolls are hot-rolled according to a 3-minute rolling rhythm. Anti-stripping water is used in finishing rolling F1-F3, and high-speed steel working rolls are used for F2 and F3.

9. The method for producing a hot-rolled pickled plate with high surface requirements according to any one of claims 5 to 7, characterized in that: The cooling process is laminar cooling, which adopts a front-stage dispersed cooling process, with upper and lower spray ratios of 25%-75% and 25%-75% respectively.

10. A method for producing a hot-rolled pickled plate with high surface requirements according to any one of claims 5 to 7, characterized in that: In the coiling process, the coiling temperature is set to 570±20°C.