Aluminum-based silicon carbide aerospace structural member size stability process

By slowing down the temperature change rate and increasing the extreme temperature of cold and heat treatment, the problem of internal stress and dimensional accuracy of the aluminum-based silicon carbide material is solved, higher dimensional stability and shape accuracy are achieved, and the application needs in special fields are met.

CN118756071APending Publication Date: 2024-10-11ZHEJIANG CHIYU AEROSPACE TECH CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410767131.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-14
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

The temperature of existing aluminum-based silicon carbide materials changes rapidly during the cold and heat treatment process, resulting in residual stress in the internal structure, affecting the dimensional accuracy and shape accuracy of the product. The thermal expansion coefficient is high, which limits its application in special fields.

Method used

By slowing down the temperature change rate, increasing the temperature extremes of hot and cold treatment, and extending the holding time, the specific steps include multiple heating and cooling processes, gradually controlling temperature changes, and ensuring the time and temperature uniformity of each heating and cooling.

Benefits of technology

It effectively reduces the thermal expansion coefficient of aluminum-based silicon carbide materials, eliminates internal stress, improves the dimensional accuracy and shape accuracy of the product, and meets the application needs of special fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118756071A_ABST
    Figure CN118756071A_ABST
Patent Text Reader

Abstract

The invention belongs to an aluminum-based silicon carbide material preparation technology, and discloses an aluminum-based silicon carbide aerospace structural member size stability process which comprises the following steps: (1) heating an aluminum-based silicon carbide material crude product from room temperature to 160 DEG C for 2 hours, keeping the temperature for 1 hour, heating to 280 DEG C for 2 hours, keeping the temperature for 1 hour, continuously heating to 320 DEG C for 2 hours, keeping the temperature for 8 hours, and cooling to room temperature; (2) soaking the aluminum-based silicon carbide material crude product cooled to the room temperature in liquid nitrogen, cooling to-100 DEG C for 2 hours, preserving heat for 1 hour, cooling to-160 DEG C for 2 hours, preserving heat for 1 hour, continuously cooling to-200 DEG C for 2 hours, preserving heat for 8 hours, and heating to the room temperature; and (3) heating the aluminum-based silicon carbide material crude product heated to the room temperature for 2 hours to 160 DEG C, preserving heat for 1 hour, continuously heating for 2 hours to 280 DEG C, preserving heat for 1 hour, continuously heating for 2 hours to 320 DEG C, preserving heat for 8 hours, and cooling to the room temperature. According to the method, the thermal expansion coefficient of the aluminum-based silicon carbide material is reduced, and the problems that the interior of the material obtained through an existing process is not uniform, large internal stress exists, and the size precision and form and position precision of a product are affected are solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of aluminum-based silicon carbide material preparation, and in particular to a dimensional stability process for aluminum-based silicon carbide aerospace structural parts. Background Art

[0002] Aluminum-based silicon carbide is a composite material made of two materials, silicon carbide and aluminum. In the high temperature, high pressure and high corrosion environment of aviation and automobile fields, aluminum-based silicon carbide shows good performance, such as excellent mechanical properties, thermal stability and corrosion resistance. However, problems such as difficult processing and easy cracking have limited the development of aluminum-based silicon carbide in industrial applications.

[0003] The existing aluminum-based silicon carbide material crude product commonly uses a cold and hot treatment process. For example, Chinese patent CN115896525A discloses a low-stress aluminum-based silicon carbide material and a preparation method thereof. In this method, the aluminum-based silicon carbide material crude product is heated to 280°C ± 10°C, the heating time is 2h ± 0.5h, and the temperature is kept for 4h ± 0.5h, and then naturally cooled to room temperature. The aluminum-based silicon carbide material crude product that has been cooled to room temperature is then soaked in liquid nitrogen to reduce it to -180°C ± 10°C, the cooling time is 2h ± 0.5h, and the temperature is kept for 4h ± 0.5h, and then naturally heated to room temperature. However, due to the rapid temperature change rate and short constant temperature time, the internal structure of the aluminum-based silicon carbide material still has residual stress, and the dimensional accuracy and shape and position accuracy of the obtained material are not high enough, and there are major defects in its application in special fields. Summary of the invention

[0004] The purpose of the present invention is to overcome the shortcomings of the above-mentioned background technology, provide a process method for dimensional stability of aluminum-based silicon carbide aerospace structural parts, further reduce the thermal expansion coefficient of aluminum-based silicon carbide materials, and solve the problems of internal unevenness and large internal stress of the materials obtained by the existing process, which affect the dimensional accuracy and shape and position accuracy of the products.

[0005] To achieve the purpose of the present invention, the dimensional stability process of aluminum-based silicon carbide aerospace structural parts of the present invention comprises the following steps:

[0006] Step (1): heating the crude aluminum-based silicon carbide material product from room temperature to 160° C. for 2 h, keeping the temperature for 1 h, further heating the temperature to 280° C. for 2 h, keeping the temperature for 1 h, further heating the temperature to 320° C. for 2 h, keeping the temperature for 8 h, and then naturally cooling the material to room temperature;

[0007] Step (2): soaking the crude aluminum-based silicon carbide material product cooled to room temperature in liquid nitrogen, cooling to -100°C for 2 hours, keeping warm for 1 hour, cooling to -160°C for 2 hours, keeping warm for 1 hour, cooling to -200°C for 2 hours, keeping warm for 8 hours, and then naturally heating to return to room temperature;

[0008] Step (3): heating the crude aluminum-based silicon carbide material product heated to room temperature from room temperature to 160° C. for 2 hours, keeping the temperature for 1 hour, further heating the temperature to 280° C. for 2 hours, keeping the temperature for 1 hour, further heating the temperature to 320° C. for 2 hours, keeping the temperature for 8 hours, and then naturally cooling the product to room temperature;

[0009] Wherein, the temperature in steps (1) to (3) may be + 10℃ fluctuation, the time can be + 10min fluctuation.

[0010] Further, in some embodiments of the present invention, the temperature in steps (1) to (3) may be + 5℃ fluctuation, the time can be + 5min fluctuation.

[0011] Compared with the prior art, the advantages of the present invention are as follows:

[0012] The present invention further reduces the thermal expansion coefficient of the aluminum-based silicon carbide material and eliminates the stress of the internal structure of the aluminum-based silicon carbide material by delaying the temperature change rate, increasing the extreme values ​​of the cold and hot treatment temperatures, and extending the insulation time, thereby stabilizing the dimensional accuracy and shape and position accuracy of the product and meeting the application requirements in special fields. BRIEF DESCRIPTION OF THE DRAWINGS

[0013] Figure 1 is the temperature-time curve of steps (1) and (3) in Example 1 of the present invention;

[0014] Figure 2 This is the temperature-time curve of step (2) in Example 1 of the present invention. DETAILED DESCRIPTION

[0015] In order to make the purpose, technical scheme and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. Additional aspects and advantages of the present invention will be partially given in the following description, partially become apparent from the following description, or be understood through the practice of the present invention. It should be understood that the following description is only used to explain the present invention and is not intended to limit the present invention.

[0016] As used herein, the terms "comprises," "including," "having," "containing," or any other variation thereof, are intended to cover a non-exclusive inclusion. For example, a composition, process, method, article, or apparatus that comprises the listed elements is not necessarily limited to only those elements but may include other elements not expressly listed or inherent to such composition, process, method, article, or apparatus.

[0017] When amount, concentration or other value or parameter is expressed as range, preferred range or a series of upper preferred value and lower preferred value limit range, this should be understood as specifically disclosing all ranges formed by any pairing of any range upper limit or preferred value and any range lower limit or preferred value, regardless of whether the range is disclosed separately. For example, when disclosing range "1 to 5", described range should be interpreted as including range "1 to 4", "1 to 3", "1 to 2", "1 to 2 and 4 to 5", "1 to 3 and 5" etc. When numerical range is described in this article, unless otherwise stated, the range is intended to include its end value and all integers and fractions within the range.

[0018] The indefinite articles "a" and "an" before the elements or components of the present invention have no limitation on the quantity requirements (i.e. the number of occurrences) of the elements or components. Therefore, "a" or "an" should be interpreted as including one or at least one, and the elements or components in the singular form also include the plural form, unless the quantity obviously refers to the singular form only.

[0019] In addition, the descriptions of the terms "one embodiment", "some embodiments", "examples", "specific examples", or "some examples" described below mean that the specific features, structures, materials, or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic expressions of the above terms do not necessarily refer to the same embodiment or example. Moreover, the technical features involved in the various embodiments of the present invention can be combined with each other as long as they do not conflict with each other.

[0020] Example 1

[0021] A dimensional stability process for aluminum-based silicon carbide aerospace structural parts, the process comprising the following steps:

[0022] Step 1: The crude aluminum-based silicon carbide material product is heated from room temperature to 160°C for 2 hours, kept warm for 1 hour, then heated to 280°C for 2 hours, kept warm for 1 hour, then heated to 320°C for 2 hours, kept warm for 8 hours, and then naturally cooled to room temperature;

[0023] Step 2: Soak the crude aluminum-based silicon carbide material product that has been cooled to room temperature in liquid nitrogen, cool it to -100°C for 2 hours, keep it warm for 1 hour, continue to cool it to -160°C for 2 hours, keep it warm for 1 hour, continue to cool it to -200°C for 2 hours, keep it warm for 8 hours, and then naturally heat it up to room temperature;

[0024] Step 3: Heat the crude aluminum-based silicon carbide material product from room temperature to 160°C for 2 hours, keep it warm for 1 hour, continue to heat it to 280°C for 2 hours, keep it warm for 1 hour, continue to heat it to 320°C for 2 hours, keep it warm for 8 hours, and then naturally cool it to room temperature to obtain a dimensionally stable structural part.

[0025] Example 2

[0026] A dimensional stability process for aluminum-based silicon carbide aerospace structural parts, the process comprising the following steps:

[0027] Step 1: The crude aluminum-based silicon carbide material product is heated from room temperature to 160°C for 2 hours, kept warm for 1 hour, then heated to 280°C for 2 hours, kept warm for 1 hour, then heated to 315°C for 2 hours, kept warm for 8 hours, and then naturally cooled to room temperature;

[0028] Step 2: Soak the crude aluminum-based silicon carbide material product that has been cooled to room temperature in liquid nitrogen, cool it down to -100°C for 2 hours, keep it warm for 1 hour, continue to cool it down to -160°C for 2 hours, keep it warm for 1 hour, continue to cool it down to -195°C for 2 hours, keep it warm for 8 hours, and then naturally heat it up to room temperature;

[0029] Step 3: Heat the crude aluminum-based silicon carbide material product from room temperature to 160°C for 2 hours, keep it warm for 1 hour, continue to heat it to 280°C for 2 hours, keep it warm for 1 hour, continue to heat it to 315°C for 2 hours, keep it warm for 8 hours, and then naturally cool it to room temperature to obtain a dimensionally stable structural part.

[0030] Example 3

[0031] A dimensional stability process for aluminum-based silicon carbide aerospace structural parts, the process comprising the following steps:

[0032] Step 1: The crude aluminum-based silicon carbide material product is heated from room temperature to 160°C for 2 hours, kept warm for 1 hour, then heated to 280°C for 2 hours, kept warm for 1 hour, then heated to 310°C for 2 hours, kept warm for 8 hours, and then naturally cooled to room temperature;

[0033] Step 2: Soak the crude aluminum-based silicon carbide material product that has been cooled to room temperature in liquid nitrogen, cool it down to -100°C for 2 hours, keep it warm for 1 hour, continue to cool it down to -160°C for 2 hours, keep it warm for 1 hour, continue to cool it down to -190°C for 2 hours, keep it warm for 8 hours, and then naturally heat it up to room temperature;

[0034] Step 3: Heat the crude aluminum-based silicon carbide material product from room temperature to 160°C for 2 hours, keep it warm for 1 hour, continue to heat it to 280°C for 2 hours, keep it warm for 1 hour, continue to heat it to 310°C for 2 hours, keep it warm for 8 hours, and then naturally cool it to room temperature to obtain a dimensionally stable structural part.

[0035] Comparative Example 1

[0036] A dimensional stability process for aluminum-based silicon carbide aerospace structural parts, the process comprising the following steps:

[0037] Step 1: The crude aluminum-based silicon carbide material product is heated from room temperature to 160°C for 2 hours, kept warm for 1 hour, then continued to be heated to 280°C for 2 hours, kept warm for 8 hours, and then naturally cooled to room temperature;

[0038] Step 2: Soak the crude aluminum-based silicon carbide material product that has been cooled to room temperature in liquid nitrogen, cool it to -100°C for 2 hours, keep it warm for 1 hour, continue to cool it to -180°C for 2 hours, keep it warm for 8 hours, and then naturally heat it up to room temperature;

[0039] Step 3: The crude aluminum-based silicon carbide material product heated to room temperature is heated from room temperature to 160°C for 2 hours, kept warm for 1 hour, and then continued to be heated to 280°C for 2 hours, kept warm for 8 hours, and then naturally cooled to room temperature to obtain a structural part.

[0040] Comparative Example 2

[0041] A dimensional stability process for aluminum-based silicon carbide aerospace structural parts, the process comprising the following steps:

[0042] Step 1: The crude aluminum-based silicon carbide material product is heated from room temperature to 160°C for 2 hours, kept warm for 1 hour, then heated to 280°C for 2 hours, kept warm for 1 hour, then heated to 320°C for 2 hours, kept warm for 6 hours, and then naturally cooled to room temperature;

[0043] Step 2: Soak the crude aluminum-based silicon carbide material product that has been cooled to room temperature in liquid nitrogen, cool it down to -100°C for 2 hours, keep it warm for 1 hour, continue to cool it down to -160°C for 2 hours, keep it warm for 1 hour, continue to cool it down to -200°C for 2 hours, keep it warm for 6 hours, and then naturally heat it up to room temperature;

[0044] Step 3: Heat the crude aluminum-based silicon carbide material product from room temperature to 160°C for 2 hours, keep it warm for 1 hour, continue to heat it to 280°C for 2 hours, keep it warm for 1 hour, continue to heat it to 320°C for 2 hours, keep it warm for 6 hours, and then naturally cool it to room temperature to obtain a structural part.

[0045] The shape of the structural parts obtained in the above embodiments remains intact and stress-free, and the difference in the average thermal expansion coefficient (20°C-100°C) is within 1%, and the difference in the average thermal expansion coefficient (20°C-150°C) is within 1%.

[0046] The average thermal expansion coefficient (20°C-100°C) of the structural parts obtained in Example 1 is 5.9% lower than that of Comparative Example 1, and the average thermal expansion coefficient (20°C-150°C) is 8.0% lower than that of Comparative Example 1; the average thermal expansion coefficient (20°C-100°C) of the structural parts obtained in Example 1 is 5.1% lower than that of Comparative Example 2, and the average thermal expansion coefficient (20°C-150°C) is 5.8% lower than that of Comparative Example 2.

[0047] It will be easily understood by those skilled in the art that the above descriptions are only some examples of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A dimensional stability process for aluminum-based silicon carbide aerospace structural parts, It is characterized in that The process comprises the following steps: Step (1): heating the crude aluminum-based silicon carbide material product from room temperature to 160° C. for 2 h, keeping the temperature for 1 h, further heating the temperature to 280° C. for 2 h, keeping the temperature for 1 h, further heating the temperature to 320° C. for 2 h, keeping the temperature for 8 h, and then naturally cooling the material to room temperature; Step (2): soaking the crude aluminum-based silicon carbide material product cooled to room temperature in liquid nitrogen, cooling to -100°C for 2 hours, keeping warm for 1 hour, cooling to -160°C for 2 hours, keeping warm for 1 hour, cooling to -200°C for 2 hours, keeping warm for 8 hours, and then naturally heating to return to room temperature; Step (3): heating the crude aluminum-based silicon carbide material product heated to room temperature from room temperature to 160° C. for 2 hours, keeping the temperature for 1 hour, further heating the temperature to 280° C. for 2 hours, keeping the temperature for 1 hour, further heating the temperature to 320° C. for 2 hours, keeping the temperature for 8 hours, and then naturally cooling the product to room temperature; In particular, the temperature in steps (1) to (3) may fluctuate by ±10°C, and the time may fluctuate by ±10 minutes.

2. The dimensional stability process of aluminum-based silicon carbide aerospace structural parts according to claim 1, It is characterized in that The temperature in steps (1) to (3) may fluctuate within ±5°C.

3. The dimensional stability process of aluminum-based silicon carbide aerospace structural parts according to claim 1, It is characterized in that The time in steps (1) to (3) may fluctuate within ±5 min.

Citation Information

Cited By

  • Method for improving mechanical property of additive manufacturing Sc-containing high-strength aluminum alloy

    CN119351909A