Solid Li-N2 / H2 battery, preparation method thereof and method for electrochemically synthesizing ammonia through battery
By using a network structure catalyst and a solid electrolyte in a lithium-nitrogen battery, the problems of gas transmission and solvent dependence are solved, and an efficient process of synthesizing ammonia from nitrogen and hydrogen at normal temperature and pressure is achieved, improving the safety and stability of the battery. sex.
Patent Information
- Application Number
- CN202410736006.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-07
- Publication Date
- 2024-10-11
AI Technical Summary
Existing lithium-nitrogen batteries have problems such as inconvenient gas transmission, strong dependence on organic solvents, and large voltage loss at normal temperatures and pressures, which limits their efficiency and safety in the application of ammonia synthesis.
A catalyst with a network structure is used as the positive electrode, combined with a solid electrolyte, and metal platinum or gold is loaded on the foam material through electrochemical deposition to construct a solid-state Li-N2/H2 battery to realize the electrochemical synthesis of ammonia from nitrogen and hydrogen.
It increases the output and gas phase content of ammonia, enhances the transport efficiency of nitrogen, prevents ammonia dissolution and electrolyte volatilization, improves the safety and stability of the battery, and realizes the efficient synthesis of ammonia from nitrogen and hydrogen at normal temperature and pressure.
Smart Images

Figure CN118756153A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of electrochemical synthesis of ammonia and relates to a solid Li-N 2 / H 2 A battery and its preparation and a method for electrochemically synthesizing ammonia by using the battery. Background Art
[0002] Ammonia (NH 3 ) is an important raw material for fertilizer production. With the continuous growth of the world's population, the demand for ammonia in agriculture is increasing day by day. 3 It is an efficient energy storage and hydrogen storage medium with high energy density, easy storage and transportation, high safety, environmental protection (no carbon emissions at the terminal), etc., which makes NH 3 It has broad application prospects in the future. The traditional method of synthesizing ammonia is to prepare it under high temperature and high pressure conditions (400-500℃, 150-200bar) by the Haber-Bosch (HB) process. The global energy consumption for synthesizing ammonia accounts for about 1-2% of the global total energy consumption. Based on this, electrocatalytic N 2 Reductive synthesis of ammonia is of great appeal. To this end, scientists have tried many methods to explore sustainable synthesis of ammonia under milder conditions, and lithium-nitrogen batteries (Li-N 2 ) because it gathers N at room temperature and pressure 2 The advantages of Li-N in combining fixation, energy storage and conversion have attracted wide attention. 2 The development of this technology still suffers from problems such as limited gas transmission, high dependence on organic solvents and significant voltage loss. Summary of the invention
[0003] In order to improve the above problems, the present invention provides a battery comprising a positive electrode, a lithium metal negative electrode and a solid electrolyte. 2 and H 2 .
[0004] According to an embodiment of the present invention, the positive electrode is selected from a catalyst, preferably a catalyst having a network structure.
[0005] According to an embodiment of the present invention, the catalyst is a bifunctional porous cathode material. For example, it is one or more combinations of platinum, gold, ruthenium, rhodium, nickel, cobalt, molybdenum, copper and stainless steel. For example, the catalyst is selected from foam copper (Cu) loaded with metal platinum (Pt), platinum mesh, foam nickel (Ni) loaded with metal platinum (Pt), foam copper (Cu) loaded with gold (Au) or foam nickel (Ni) loaded with gold (Au).
[0006] In one embodiment of the present invention, the copper foam loaded with metallic platinum is prepared by placing a platinum source (such as H2 PtCl 6 The solution was prepared by electrochemical deposition on copper foam.
[0007] For example, the working electrode of the electrochemical deposition method is foamed copper, the counter electrode is a platinum electrode, and the reference electrode is Ag / AgCl.
[0008] For example, the potential of the electrochemical deposition method is -0.5 V vs Ag / AgCl; and the time of the electrochemical deposition method is 1 h.
[0009] For example, the copper foam may be washed and dried before use. For example, the washing solvent may be water and ethanol.
[0010] For example, the H 2 PtCl 6 The concentration of the solution is 0.01-0.05M, exemplified by 0.02M.
[0011] In one embodiment of the present invention, the nickel foam loaded with metallic platinum is prepared by placing a platinum source (such as H 2 PtCl 6 The solution was prepared by electrochemical deposition on nickel foam.
[0012] For example, the working electrode of the electrochemical deposition method is nickel foam, the counter electrode is a platinum electrode, and the reference electrode is Ag / AgCl.
[0013] For example, the potential of the electrochemical deposition method is -0.5 V vs Ag / AgCl; and the time of the electrochemical deposition method is 1 h.
[0014] For example, the H 2 PtCl 6 The concentration of the solution is 0.01-0.05M, exemplified by 0.02M.
[0015] For example, the nickel foam may be washed and dried before use. For example, the washing solvent may be water and ethanol.
[0016] In one embodiment of the present invention, the foam copper is loaded with gold (Au) by placing a gold source (such as HAuCl 4 The solution was prepared by electrochemical deposition on copper foam.
[0017] For example, the working electrode of the electrochemical deposition method is foamed copper, the counter electrode is a platinum electrode, and the reference electrode is Ag / AgCl.
[0018] For example, the potential of the electrochemical deposition method is -0.5 V vs Ag / AgCl; and the time of the electrochemical deposition method is 1 h.
[0019] For example, the HAuCl 4 The concentration of the solution is 0.01-0.05M, exemplified by 0.02M.
[0020] For example, the copper foam may be washed and dried before use. For example, the washing solvent may be water and ethanol.
[0021] In one embodiment of the present invention, the nickel foam loaded with gold (Au) is prepared by placing a gold source (such as HAuCl 4 The solution was prepared by electrochemical deposition on nickel foam.
[0022] For example, the working electrode of the electrochemical deposition method is nickel foam, the counter electrode is a platinum electrode, and the reference electrode is Ag / AgCl.
[0023] For example, the potential of the electrochemical deposition method is -0.5 V vs Ag / AgCl; and the time of the electrochemical deposition method is 1 h.
[0024] For example, the HAuCl 4 The concentration of the solution is 0.01-0.05M, exemplified by 0.02M.
[0025] For example, the copper foam may be washed and dried before use. For example, the washing solvent may be water and ethanol.
[0026] According to an embodiment of the present invention, the solid electrolyte is selected from oxide solid electrolytes (LAGP, LATP, LLZO or LLTO, etc.), sulfide solid electrolytes (Li 2 S or LGPS, etc.), chloride-based solid electrolytes (LiCl or LiAlCl 4 The various combinations of the solid electrolytes may be sandwich and / or hybrid.
[0027] In one embodiment of the present invention, the solid electrolyte is selected from a combination of PEO and LAGP; specifically, the solid electrolyte includes a mixed layer prepared by mixing or stacking LAGP and PEO according to a mass ratio.
[0028] In one embodiment of the present invention, the solid electrolyte is assembled by stacking two, three or more layers of PEO layer and LAGP layer. Exemplarily, the solid electrolyte is selected from at least one of PEO layer-LAGP layer-PEO layer, LAGP layer-PEO layer-LAGP layer, LAGP layer-PEO layer and PEO layer-LAGP layer.
[0029] In one embodiment of the present invention, the solid electrolyte is prepared by sintering a mixture of LAGP and PEO at high temperature.
[0030] Preferably, the mixing mass ratio of LAGP and PEO is 1:(0.7-1.3), exemplified by 1:0.7, 1:1, 1:1.3.
[0031] Preferably, the LAGP comprises Li 2 CO 3 、Al 2 O 3 NH 4 H 2 PO 4 and GeO 2 The raw materials are prepared by grinding.
[0032] Preferably, the high temperature sintering may be performed multiple times, preferably 3 times. Preferably, the temperatures of the multiple sinterings may be the same or different, and may be 500-1000°C independently of each other, exemplarily 500°C, 600°C, 700°C, 800°C, 900°C, 1000°C; the calcining times of the multiple calcinings may be the same or different, and may be 1-10h independently of each other, preferably 4-6h, exemplarily 1h, 4h, 6h, 10h.
[0033] Preferably, the sintered product needs to be ground after the primary sintering and the secondary sintering. For example, the grinding speed is 100-500 rpm, exemplarily 400 rpm; the grinding time is 1-5 hours, exemplarily 4 hours.
[0034] Preferably, before the third sintering, the powder obtained after grinding is pressed into a shape, for example, into a disc with a diameter of 18 mm and a thickness of 0.7 mm.
[0035] In one embodiment of the present invention, the LAGP material comprises Li 2 CO 3 、Al 2 O 3 NH 4 H 2 PO 4 and GeO 2 The raw materials are ground and then sintered at high temperature to prepare it.
[0036] Preferably, Li 2 CO 3 、Al 2 O 3 NH 4 H 2 PO 4 and GeO2 The mixing molar ratio is (2-4):1:(2-4):(5-8), and exemplarily is 3:1:3:6.
[0037] Preferably, the grinding method is wet grinding. For example, the solvent used in the wet grinding is isopropanol. For another example, the rotation speed of the wet grinding is 100 to 500 rpm, exemplarily 400 rpm; the time of the wet grinding is 1 to 5 hours, exemplarily 4 hours.
[0038] Preferably, the preparation of the LAGP material further comprises drying the mixture obtained by grinding.
[0039] Preferably, the high temperature sintering may be performed multiple times, preferably 3 times. Preferably, the temperatures of the multiple sinterings may be the same or different, and may be 500-1000°C independently of each other, exemplarily 500°C, 600°C, 700°C, 800°C, 900°C, 1000°C; the calcining times of the multiple calcinings may be the same or different, and may be 1-10h independently of each other, preferably 4-6h, exemplarily 1h, 4h, 6h, 10h.
[0040] Preferably, the sintered product needs to be ground after the primary sintering and the secondary sintering. For example, the grinding speed is 100-500 rpm, exemplarily 400 rpm; the grinding time is 1-5 hours, exemplarily 4 hours.
[0041] Preferably, before the third sintering, the powder obtained after grinding is pressed into a shape, for example, into a disc with a diameter of 18 mm and a thickness of 0.7 mm.
[0042] In one embodiment of the present invention, the PEO material comprises dissolving PEO and lithium bis(trifluoromethanesulfonate) imide in tetrahydrofuran (THF) to obtain a mixed solution, and heating the mixed solution to obtain a gel-like PEO material.
[0043] Preferably, the mass ratio of PEO to lithium imide bistrifluoromethanesulfonate is 1:(0.5-2), exemplarily 1:2.
[0044] Preferably, in the mixed solution, the concentration of PEO is 0.01-0.1 g / mL, exemplarily 0.06 g / mL.
[0045] Preferably, in the mixed solution, the concentration of lithium imide bistrifluoromethanesulfonate is 0.01-0.1 g / mL, exemplarily 0.06 g / mL.
[0046] Preferably, the heating temperature is 30-60°C, exemplarily 45°C.
[0047] The present invention also provides a method for preparing the above-mentioned battery, the method comprising: assembling a positive electrode, a lithium metal negative electrode and a solid electrolyte, introducing N into the positive electrode side 2 , H 2 , constituting the battery.
[0048] Specifically, the method comprises: using a catalyst as a positive electrode, assembling it with a solid electrolyte and lithium metal as a negative electrode in sequence, and introducing N 2 , H 2 , forming Li-N 2 / H 2 Battery.
[0049] The present invention also provides application of the battery in electrochemical synthesis of ammonia.
[0050] The present invention also provides a method for electrochemically synthesizing ammonia, the method comprising: decoupling nitrogen reduction and hydrogen oxidation into positive electrode discharge and charge processes through the above-mentioned battery to synthesize NH 3 .
[0051] According to an embodiment of the present invention, the method for synthesizing ammonia comprises the following steps:
[0052] In the first step, under discharge conditions, lithium metal acts as the negative electrode to convert N 2 Reduction and Li + Combined to form Li 3 N;
[0053] In the second step, under charging conditions, H 2 Under the action of the catalyst, an oxidation reaction occurs to obtain hydrogen protons, which react with the Li 3 N combines to form NH 3 .
[0054] The battery for electrochemically synthesizing ammonia of the present invention utilizes a fully solid electrolyte to effectively prevent the generation of NH 3 dissolves into the solution, greatly increasing the NH 3 At the same time, it also inhibits the volatilization and leakage of electrolyte, improving battery safety and stability.
[0055] According to an embodiment of the present invention, the first step is preferably performed in an anhydrous and oxygen-free environment.
[0056] According to an embodiment of the present invention, in the first step, Li 3 The reaction of N is shown in the following formula 1:
[0057] 6Li+N 2 →2Li 3 N Formula 1.
[0058] According to an embodiment of the present invention, in the first step, the N 2 The flow rate is 1 to 20 sccm, exemplified by 10 sccm.
[0059] According to an embodiment of the present invention, in the first step, lithium metal and N 2 Li-N 2 Battery.
[0060] According to an embodiment of the present invention, the reaction in the second step is shown in the following formula 2 and formula 3:
[0061]
[0062] Li 3 N+3H + →NH 3 +3Li + Formula 3.
[0063] According to an embodiment of the present invention, in the second step, the NH 3 The preparation method specifically includes: after the first step is completed, in an environment without water and oxygen, the catalyst is used as the positive electrode and the lithium metal is used as the negative electrode, and H is introduced into the positive electrode side. 2 , charged to the cut-off potential, generating NH 3 .
[0064] According to an embodiment of the present invention, the H 2 The flow rate is 1 to 20 sccm, exemplified by 10 sccm.
[0065] According to an embodiment of the present invention, in the second step, lithium metal and H 2 Composition Li-H 2 Battery.
[0066] According to an embodiment of the present invention, the solid-state Li-N 2 / H 2 The battery uses lithium metal as the negative electrode, a catalyst as the positive electrode, and a solid electrolyte to carry out nitrogen reduction process (NRR) and hydrogen oxidation process (HOR), and synthesizes ammonia through electrochemical method to directly and efficiently obtain NH 3 Preferably, the voltage range of the electrochemical method is 0V-4V.
[0067] According to an embodiment of the present invention, a solid-state Li-N 2 / H 2 The experimental operation of the battery and the battery performance test were all carried out in a glove box.
[0068] According to an embodiment of the present invention, solid-state Li-N 2 / H 2The ammonia production performance and cycle performance of the battery were tested in an atmosphere of a mixture of nitrogen and hydrogen using an electrochemical workstation (CHI660E) and a blue-electric test system.
[0069] Beneficial effects of the present invention:
[0070] 1. The present invention proposes a battery for electrochemical synthesis of ammonia (specifically a solid-state Li-N 2 / H 2 Battery), the application of solid electrolyte can increase the ammonia content in the gas phase and effectively improve the nitrogen transport efficiency. At the same time, solid electrolyte can also effectively prevent the generation of NH 3 Dissolves into the solution, so NH can be directly and efficiently obtained 3 , thus directly and simply promoting NH 3 thus showing potential application value.
[0071] 2. The battery of the present invention (specifically a solid-state Li-N 2 / H 2 Batteries) have the characteristics of high energy density, operation at higher temperatures, large capacity, and long cycle life.
[0072] 3. The present invention provides a battery system (specifically a solid-state Li-N 2 / H 2 The battery system decouples nitrogen reduction and hydrogen oxidation into positive electrode discharge and charging processes, realizing the electrocatalytic synthesis of nitrogen and hydrogen to obtain ammonia at room temperature and pressure.
[0073] 4. The battery of the present invention (specifically a solid-state Li-N 2 / H 2 Battery) The nitrogen fixation process is simple and can effectively fix nitrogen in the atmosphere to reduce the consumption of fossil energy.
[0074] 5. The battery of the present invention (specifically a solid-state Li-N 2 / H 2 The solid electrolyte in the battery inhibits the volatilization of the electrolyte and avoids the leakage problem. BRIEF DESCRIPTION OF THE DRAWINGS
[0075] Figure 1 is a scanning electron microscope image (SEM) of the solid electrolyte in Example 1 of the present invention.
[0076] Figure 2 The solid Li-N in Example 1 of the present invention 2 / H 2 Graph of battery cycling performance.
[0077] Figure 3 Example 1 of the present invention prepares NH3 H NMR spectrum.
[0078] Figure 4 The solid-state Li-N 2 / H 2 Schematic diagram of the battery setup. DETAILED DESCRIPTION
[0079] The technical scheme of the present invention will be further described in detail below in conjunction with specific embodiments. It should be understood that the following embodiments are only exemplary descriptions and explanations of the present invention and should not be construed as limiting the scope of protection of the present invention. All technologies implemented based on the above content of the present invention are included in the scope that the present invention is intended to protect.
[0080] In the description of the present invention, if there is a description of first, second, etc., it is only for the purpose of distinguishing technical features, and cannot be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features or implicitly indicating the order of the indicated technical features.
[0081] In the description of the present invention, the terms "include" and "have" and any variations thereof are intended to cover non-exclusive inclusions. For example, a process, method, system, product or apparatus comprising a series of steps or units is not necessarily limited to those steps or units explicitly listed, but may include other steps or units not explicitly listed or inherent to these processes, methods, products or apparatuses.
[0082] Unless otherwise specified, the raw materials and reagents used in the following examples are commercially available or can be prepared by known methods.
[0083] Experimental drugs and equipment: high-purity nitrogen, high-purity hydrogen, high-purity argon, foam copper, lithium foil, lithium-rich electrolyte, chloroplatinic acid, lithium carbonate, alumina, diammonium phosphate, germanium dioxide, polyethylene oxide, tubular furnace (GSL-1200X), electrochemical workstation CHI 660E (Shanghai Chenhua), blue battery test system (CT 2001A).
[0084] In the following electrochemical ammonia synthesis process of the present invention, a nitrogen and hydrogen mixed gas with a volume ratio of 1:1 is introduced into a closed reaction container. After the gas is introduced, the battery is operated in this nitrogen and hydrogen atmosphere at normal pressure. Therefore, during the charge and discharge experiment, it is not necessary to continuously introduce nitrogen and hydrogen.
[0085] Example 1
[0086] A solid-state Li-N for electrochemical synthesis of ammonia 2 / H 2The battery uses metallic lithium as the negative electrode, copper foam loaded with metallic Pt as the positive electrode, and is assembled using a PEO-LAGP-PEO layer as a solid electrolyte.
[0087] Preparation of the positive electrode material copper foam loaded with metal Pt: The copper foam was cleaned with water and ethanol respectively, ultrasonically treated in ethanol solution for 20 min, and vacuum dried using a three-electrode system (the cleaned copper foam was used as the working electrode, the platinum electrode was used as the counter electrode, and the Ag / AgCl was used as the reference electrode). At a voltage of -0.5 V vs Ag / AgCl, 0.02 MH 2 PtCl 6 The electroplating was carried out in the solution at constant potential for 1 h. After the electroplating, the copper foam loaded with metal platinum was rinsed with deionized water and ethanol and dried in an argon-filled atmosphere.
[0088] The preparation of the PEO-LAGP-PEO layer solid electrolyte includes the following steps:
[0089] (1) Preparation of LAGP materials: Li 2 CO 3 、Al 2 O 3 NH 4 H 2 PO 4 and GeO 2 Add it to the ball mill in a molar ratio of 1.5:0.5:1.5:3, and grind it at 400 rpm for 4 hours using a planetary ball mill in an environment with the addition of isopropanol. Subsequently, the mixture was dried into powder, sintered at 600°C for 1 hour in a tube furnace, and ground at 400 rpm for 4 hours. Next, sintered at 900°C for 6 hours and ground at 400 rpm for 4 hours. Finally, the resulting powder was pressed into a disc with a diameter of 18 mm and a thickness of 0.7 mm, and sintered at 900°C for 6 hours to obtain a LAGP disc.
[0090] (2) Preparation of PEO material: 0.18 g of PEO and 0.18 g of lithium bis(trifluoromethanesulfonate) imide were dissolved in 3 mL of tetrahydrofuran (THF) and fully dissolved at 45° C. to obtain a gel-like PEO material.
[0091] (3) The gel-like material obtained in step (2) is coated on both sides of the LAGP disc obtained in step (1) to form a PEO layer with a thickness of 0.2 mm. After sufficient drying, a PEO-LAGP-PEO layer solid electrolyte is obtained.
[0092] The assembled solid-state Li-N 2 / H 2The battery was injected with an atmosphere of a nitrogen and hydrogen mixture with a volume ratio of 1:1, and an electrochemical workstation and a blue electric test system were used to study the catalytic process of discharge / charge and the cycle performance of the battery in the range of 0V-4V.
[0093] Figure 1 This is a scanning electron microscope (SEM) image of the solid electrolyte in Example 1 of the present invention. It can be seen from the image that the LAGP layer and the PEO layers on both sides are tightly attached to each other.
[0094] Figure 2 The solid Li-N in Example 1 2 / H 2 The battery cycle performance diagram. It can be seen from the figure that at a current density of 0.1 mA cm -2 When the battery can be cycled stably for 300h, the Faraday efficiency (FE NH3 ) was 10.01%, and the ammonia yield was 3.72 μmol·h -1 cm -2 .
[0095] NH 3 The Faraday efficiency of the output is calculated as:
[0096] FE = 3F*m / (17*Q), where: 3 is the electron transfer number of a N atom, F is the Faraday constant, m is the mass of ammonia obtained by colorimetry, and Q is the total charge.
[0097] Figure 3 NH prepared in Example 1 of the present invention 3 The H NMR spectrum of NH 3 The peak positions of solid Li-N 2 / H 2 The battery successfully synthesized NH by electrochemical method. 3 .
[0098] Example 2
[0099] A solid-state Li-N for electrochemical synthesis of ammonia 2 / H 2 The battery uses metallic lithium as the negative electrode, copper foam loaded with metallic Pt as the positive electrode, and is assembled using a PEO layer as a solid electrolyte.
[0100] The preparation method of the copper foam loaded with metal Pt is the same as the preparation method in Example 1.
[0101] The solid electrolyte layer is PEO, and its preparation method is as follows: 0.18g PEO and 0.18g lithium imide trifluoromethanesulfonate are dissolved in 3mL tetrahydrofuran (THF), fully dissolved at a temperature of 45°C to obtain a gel-like PEO material, and placed in a glove phase and dried at room temperature for 24 hours to obtain a PEO layer solid electrolyte.
[0102] The assembled solid-state Li-N 2 / H 2 The battery was injected with an atmosphere of a mixture of nitrogen and hydrogen in a volume ratio of 1:1, and an electrochemical workstation and a blue electric test system were used to study the catalytic process of discharge / charge and the cycle performance of the battery in the range of 0V-4V.
[0103] At a current density of 0.1 mA cm -2 The battery can be cycled stably for 170 hours, FE NH3 The ammonia yield was 6.82% and 2.13 μmol·h -1 cm -2 .
[0104] Example 3
[0105] A solid-state Li-N for electrochemical synthesis of ammonia 2 / H 2 The battery uses metallic lithium as the negative electrode, copper foam loaded with metallic Pt as the positive electrode, and is assembled using a LAGP layer as a solid electrolyte.
[0106] The preparation method of the copper foam loaded with metal Pt is the same as the preparation method in Example 1.
[0107] The solid electrolyte layer is a LAGP layer, and its preparation method is as follows: Li 2 CO 3 、Al 2 O 3 NH 4 H 2 PO 4 and GeO 2 Add it to the ball mill in a molar ratio of 1.5:0.5:1.5:3, and grind it at 400 rpm for 4 hours using a planetary ball mill in an environment with the addition of isopropanol. Subsequently, the mixture was dried into powder, sintered at 600°C for 1 hour in a tube furnace, and ground at 400 rpm for 4 hours. Next, sintered at 900°C for 6 hours and ground at 400 rpm for 4 hours. Finally, the resulting powder was pressed into a disc with a diameter of 18 mm and a thickness of 0.7 mm, and sintered at 900°C for 6 hours to obtain a LAGP disc.
[0108] The assembled solid-state Li-N2 / H 2 The battery was injected with an atmosphere of a nitrogen and hydrogen mixture with a volume ratio of 1:1, and an electrochemical workstation and a blue electric test system were used to study the catalytic process of discharge / charge and the cycle performance of the battery in the range of 0V-4V.
[0109] At a current density of 0.1 mA cm -2 When the battery can be stably cycled for 190h, FE NH3 The ammonia yield was 2.19 μmol·h -1 cm -2 .
[0110] Example 4
[0111] A solid-state Li-N for electrochemical synthesis of ammonia 2 / H 2 The battery uses metallic lithium as the negative electrode, copper foam loaded with metallic Pt as the positive electrode, and is assembled using a LAGP-PEO-LAGP layer as a solid electrolyte.
[0112] The preparation method of the copper foam loaded with metal Pt is the same as the preparation method in Example 1.
[0113] The solid electrolyte layer is LAGP-PEO-LAGP, and its preparation method is as follows:
[0114] (1) Preparation of LAGP materials: Li 2 CO 3 、Al 2 O 3 NH 4 H 2 PO 4 and GeO 2 Add it to the ball mill in a molar ratio of 1.5:0.5:1.5:3, and grind it at 400 rpm for 4 hours using a planetary ball mill in an environment with the addition of isopropanol. Subsequently, the mixture was dried into powder, sintered at 600°C for 1 hour in a tube furnace, and ground at 400 rpm for 4 hours. Next, sintered at 900°C for 6 hours and ground at 400 rpm for 4 hours. Finally, the resulting powder was pressed into a disc with a diameter of 18 mm and a thickness of 0.7 mm, and sintered at 900°C for 6 hours to obtain a LAGP disc.
[0115] (2) Preparation of PEO material: 0.18 g of PEO and 0.18 g of lithium bis(trifluoromethanesulfonate) imide were dissolved in 3 mL of tetrahydrofuran (THF) and fully dissolved at 45° C. to obtain a gel-like PEO material.
[0116] (3) The gel-like material obtained in step (2) is coated between the two LAGP discs obtained in step (1). After being fully dried, the two LAGP discs are bonded together to form a PEO layer with a thickness of 0.2 mm, thereby obtaining a LAGP-PEO-LAGP layer solid electrolyte.
[0117] The assembled solid-state Li-N 2 / H 2 The battery was injected with an atmosphere of a mixture of nitrogen and hydrogen in a volume ratio of 1:1, and an electrochemical workstation and a blue electric test system were used to study the catalytic process of discharge / charge and the cycle performance of the battery in the range of 0V-4V.
[0118] At a current density of 0.1 mA cm -2 When the battery can be stably cycled for 225h, FE NH3 The ammonia yield was 7.92% and 2.93 μmol·h -1 cm -2 .
[0119] Example 5
[0120] A solid-state Li-N for electrochemical synthesis of ammonia 2 / H 2 The battery uses metallic lithium as the negative electrode, copper foam loaded with metallic Pt as the positive electrode, uses a LAGP-PEO layer as a solid electrolyte, and is assembled according to the negative electrode-LAGP-PEO layer-positive electrode.
[0121] The preparation method of the copper foam loaded with metal Pt is the same as the preparation method in Example 1.
[0122] The solid electrolyte layer is LAGP-PEO, and its preparation method is as follows:
[0123] (1) Preparation of LAGP materials: Li 2 CO 3 、Al 2 O 3 NH 4 H 2 PO 4 and GeO 2Add it to the ball mill in a molar ratio of 1.5:0.5:1.5:3, and grind it at 400 rpm for 4 hours using a planetary ball mill in an environment with the addition of isopropanol. Subsequently, the mixture was dried into powder, sintered at 600°C for 1 hour in a tube furnace, and ground at 400 rpm for 4 hours. Next, sintered at 900°C for 6 hours and ground at 400 rpm for 4 hours. Finally, the resulting powder was pressed into a disc with a diameter of 18 mm and a thickness of 0.7 mm, and sintered at 900°C for 6 hours to obtain a LAGP disc.
[0124] (2) Preparation of PEO material: 0.18 g of PEO and 0.18 g of lithium bis(trifluoromethanesulfonate) imide were dissolved in 3 mL of tetrahydrofuran (THF) and fully dissolved at 45° C. to obtain a gel-like PEO material.
[0125] (3) The gel-like material obtained in step (2) is coated on one side of the LAGP disc obtained in step (1) to form a PEO layer with a thickness of 0.2 mm. After sufficient drying, a LAGP-PEO layer solid electrolyte is obtained.
[0126] The assembled solid-state Li-N 2 / H 2 The battery was injected with an atmosphere of a mixture of nitrogen and hydrogen in a volume ratio of 1:1, and an electrochemical workstation and a blue electric test system were used to study the catalytic process of discharge / charge and the cycle performance of the battery in the range of 0V-4V.
[0127] At a current density of 0.1 mA cm -2 When the battery can be stably cycled for 220h, FE NH3 The ammonia yield was 7.43% and 2.62 μmol·h -1 cm -2 .
[0128] Example 6
[0129] A solid-state Li-N for electrochemical synthesis of ammonia 2 / H 2 The battery uses metallic lithium as the negative electrode, copper foam loaded with metallic Pt as the positive electrode, uses a PEO-LAGP layer as a solid electrolyte, and is assembled according to the negative electrode-PEO-LAGP-positive electrode.
[0130] The preparation method of copper foam loaded with metal Pt is the same as the preparation method in Example 1.
[0131] The solid electrolyte layer is PEO-LAGP, and the preparation method of the solid electrolyte layer LAGP-PEO is the same as that in Example 5, except that: when the battery is assembled, the PEO layer is in contact with the negative electrode, and the LAGP layer is in contact with the positive electrode.
[0132] The assembled solid-state Li-N 2 / H 2 The battery was injected with an atmosphere of a mixture of nitrogen and hydrogen in a volume ratio of 1:1, and an electrochemical workstation and a blue electric test system were used to study the catalytic process of discharge / charge and the cycle performance of the battery in the range of 0V-4V.
[0133] At a current density of 0.1 mA cm -2 When the battery can be stably cycled for 215h, FE NH3 The ammonia yield was 7.31% and 2.56 μmol·h -1 cm -2 .
[0134] Example 7
[0135] A solid-state Li-N for electrochemical synthesis of ammonia 2 / H 2 The battery uses metallic lithium as a negative electrode, copper foam loaded with metallic Pt as a positive electrode, and a solid electrolyte assembled by mixing LAGP and PEO in a mass ratio of 1:0.7.
[0136] The preparation method of the positive electrode material is the same as that in Example 1.
[0137] Preparation of solid electrolyte materials. 2 CO 3 、Al 2 O 3 NH 4 H 2 PO 4 and GeO 2 Add it to the ball mill in a molar ratio of 1.5:0.5:1.5:3, and use a planetary ball mill to grind it at 400 rpm for 4 hours in an environment with the addition of isopropanol. Subsequently, the mixture is dried into LAGP powder. Then LAGP and PEO are mixed evenly at a mass ratio of 1:0.7. Use a tubular furnace to sinter at 600°C for 1 hour and grind at 400rpm for 4 hours. Next, sinter at 900°C for 6 hours and grind at 400rpm for 4 hours. Finally, the resulting powder is pressed into a disc with a diameter of 18 mm and a thickness of 0.7 mm, and sintered at 900°C for 6 hours to obtain a solid electrolyte disc.
[0138] The assembled solid-state Li-N 2 / H2 The battery was injected with an atmosphere of a mixture of nitrogen and hydrogen in a volume ratio of 1:1, and an electrochemical workstation and a blue electric test system were used to study the catalytic process of discharge / charge and the cycle performance of the battery in the range of 0V-4V.
[0139] At a current density of 0.1 mA cm -2 When the battery can be stably cycled for 200h, FE NH3 The ammonia yield was 7.12% and 2.34 μmol·h -1 cm -2 .
[0140] Example 8
[0141] A solid-state Li-N for electrochemical synthesis of ammonia 2 / H 2 The battery uses metallic lithium as a negative electrode, copper foam loaded with metallic Pt as a positive electrode, and a solid electrolyte assembled by mixing LAGP and PEO in a mass ratio of 1:1.
[0142] The preparation method of the copper foam loaded with metal Pt is the same as the preparation method in Example 1.
[0143] The preparation method of the solid electrolyte is the same as that of Example 7, except that the mixing mass ratio of LAGP and PEO is 1:1.
[0144] The assembled solid-state Li-N 2 / H 2 The battery was injected with an atmosphere of a mixture of nitrogen and hydrogen in a volume ratio of 1:1, and an electrochemical workstation and a blue electric test system were used to study the catalytic process of discharge / charge and the cycle performance of the battery in the range of 0V-4V.
[0145] At a current density of 0.1 mA cm -2 The battery can cycle stably for 230 hours, FE NH3 The ammonia yield was 7.53% and 2.72 μmol·h -1 cm -2 .
[0146] Example 9
[0147] A solid-state Li-N for electrochemical synthesis of ammonia 2 / H 2 The battery uses metallic lithium as a negative electrode, copper foam loaded with metallic Pt as a positive electrode, and a solid electrolyte assembled by mixing LAGP and PEO in a mass ratio of 1:1.3.
[0148] The preparation method of the copper foam loaded with metal Pt is the same as the preparation method in Example 1.
[0149] The preparation method of the solid electrolyte is the same as that of Example 7, except that the mixing mass ratio of LAGP and PEO is 1:1.3.
[0150] The assembled solid-state Li-N 2 / H 2 The battery was injected with an atmosphere of a mixture of nitrogen and hydrogen in a volume ratio of 1:1, and an electrochemical workstation and a blue electric test system were used to study the catalytic process of discharge / charge and the cycle performance of the battery in the range of 0V-4V.
[0151] At a current density of 0.1 mA cm -2 When the battery can be stably cycled for 220h, FE NH3 The ammonia yield was 2.30 μmol·h -1 cm -2 .
[0152] Example 10
[0153] A solid-state Li-N for electrochemical synthesis of ammonia 2 / H 2 The battery uses metallic lithium as the negative electrode, a Pt mesh as the positive electrode, and a PEO-LAGP-PEO layer as the solid electrolyte for assembly.
[0154] The preparation method of the solid electrolyte PEO-LAGP-PEO layer is the same as that in Example 1. The positive electrode material is a purchased Pt mesh (purchased from Shanghai Yueci Electronic Technology Co., Ltd.).
[0155] The assembled solid-state Li-N 2 / H 2 The battery was injected with an atmosphere of a mixture of nitrogen and hydrogen in a volume ratio of 1:1, and an electrochemical workstation and a blue electric test system were used to study the catalytic process of discharge / charge and the cycle performance of the battery in the range of 0V-4V.
[0156] At a current density of 0.1 mA cm -2 The battery can cycle stably for 290 hours, FE NH3 The ammonia yield was 9.82% and 3.51 μmol·h -1 cm -2 .
[0157] Embodiment 11
[0158] A solid-state Li-N for electrochemical synthesis of ammonia 2 / H 2The battery uses metallic lithium as the negative electrode, foamed Ni loaded with metallic Pt as the positive electrode, and is assembled using a PEO-LAGP-PEO layer as a solid electrolyte.
[0159] The preparation method of the solid electrolyte PEO-LAGP-PEO layer is the same as that in Example 1.
[0160] Preparation of positive electrode material Ni foam loaded with metal Pt: The Ni foam was washed with water and ethanol respectively, ultrasonically treated in ethanol solution for 20 min, and vacuum dried using a three-electrode system (the washed Ni foam was used as the working electrode, the platinum electrode was used as the counter electrode, and the Ag / AgCl was used as the reference electrode). At a voltage of -0.5 V vs Ag / AgCl, 0.02 MH 2 PtCl 6 The electroplating was carried out in the solution at constant potential for 1 h. After that, the Ni foam loaded with metal Pt was rinsed with deionized water and ethanol and dried in an argon-filled atmosphere.
[0161] The assembled solid-state Li-N 2 / H 2 The battery was injected with a mixed gas atmosphere of nitrogen and hydrogen in a mixing ratio of 1:1, and an electrochemical workstation and a blue electric test system were used to study the catalytic process of discharge / charge and the cycle performance of the battery in the range of 0V-4V.
[0162] At a current density of 0.1 mA cm -2 The battery can cycle stably for 270 hours, FE NH3 The ammonia yield was 8.02% and 3.03 μmol·h -1 cm -2 .
[0163] Example 12
[0164] A solid-state Li-N for electrochemical synthesis of ammonia 2 / H 2 The battery uses metallic lithium as the negative electrode, copper foam loaded with metallic Au as the positive electrode, and is assembled using a PEO-LAGP-PEO layer as a solid electrolyte.
[0165] The preparation method of the solid electrolyte PEO-LAGP-PEO layer is the same as that in Example 1.
[0166] Preparation of Au-loaded copper foam as the positive electrode material: The copper foam was cleaned with water and ethanol respectively, ultrasonically treated in ethanol solution for 20 min, and vacuum dried using a three-electrode system (the cleaned copper foam was used as the working electrode, the platinum electrode was used as the counter electrode, and the Ag / AgCl was used as the reference electrode). At a voltage of -0.5 V vs Ag / AgCl, 0.02 M HAuCl4 The electroplating was carried out in the solution at constant potential for 1 h. After the deposition, the copper foam loaded with metal Au was rinsed with deionized water and ethanol and dried in an argon-filled atmosphere.
[0167] The assembled solid-state Li-N 2 / H 2 The battery was injected with an atmosphere of a mixture of nitrogen and hydrogen in a volume ratio of 1:1, and an electrochemical workstation and a blue electric test system were used to study the catalytic process of discharge / charge and the cycle performance of the battery in the range of 0V-4V.
[0168] At a current density of 0.1 mA cm -2 When the battery can be stably cycled for 260h, FE NH3 The ammonia yield was 8.42% and 3.16 μmol·h -1 cm -2 .
[0169] Embodiment 13
[0170] A solid-state Li-N for electrochemical synthesis of ammonia 2 / H 2 The battery uses metallic lithium as the negative electrode, foamed Ni loaded with metallic Au as the positive electrode, and is assembled using a PEO-LAGP-PEO layer as a solid electrolyte.
[0171] The preparation method of the solid electrolyte PEO-LAGP-PEO layer is the same as that in Example 1.
[0172] Preparation of positive electrode material Ni foam loaded with metal Au: Ni foam was washed with water and ethanol respectively, ultrasonically treated in ethanol solution for 20 min, and vacuum dried using a three-electrode system (cleaned Ni foam as working electrode, platinum electrode as counter electrode, Ag / AgCl as reference electrode) at a voltage of -0.5 V vs Ag / AgCl, 0.02 M HAuCl 4 The constant potential electrodeposition was carried out in the solution for 1 h. After the electrodeposition, the foamed Ni loaded with metal Au was rinsed with deionized water and ethanol and dried in an argon-filled atmosphere.
[0173] The assembled solid-state Li-N 2 / H 2 The battery was injected with an atmosphere of a mixture of nitrogen and hydrogen in a volume ratio of 1:1, and an electrochemical workstation and a blue electric test system were used to study the catalytic process of discharge / charge and the cycle performance of the battery in the range of 0V-4V.
[0174] At a current density of 0.1 mA cm -2 The battery can cycle stably for 240 hours, FE NH3The ammonia yield was 7.42% and 2.81 μmol·h -1 cm -2 .
[0175] The above is a description of the exemplary embodiments of the present invention. However, the protection scope of the present application is not limited to the above embodiments. Any modification, equivalent substitution, improvement, etc. made by those skilled in the art within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A battery, It is characterized in that The battery comprises a positive electrode, a lithium metal negative electrode and a solid electrolyte. 2 and H 2 .
2. The battery according to claim 1, It is characterized in that The positive electrode is selected from a catalyst, preferably a catalyst having a network structure. Preferably, the catalyst is a bifunctional porous cathode material, for example, one or more combinations of platinum, gold, ruthenium, rhodium, nickel, cobalt, molybdenum, copper and stainless steel. Preferably, the catalyst is selected from copper (Cu) foam loaded with platinum (Pt), platinum mesh, nickel (Ni) foam loaded with platinum (Pt), copper (Cu) foam loaded with gold (Au) or nickel (Ni) foam loaded with gold (Au).
3. The battery according to claim 1 or 2, It is characterized in that The solid electrolyte is selected from oxide solid electrolytes (LAGP, LATP, LLZO or LLTO, etc.), sulfide solid electrolytes (Li 2 S or LGPS, etc.), chloride-based solid electrolytes (LiCl or LiAlCl 4 One or more combinations of solid electrolytes (such as PEO or PPC, etc.) and polymer solid electrolytes (such as PEO or PPC, etc.); wherein the various combinations of the above solid electrolytes are sandwich and / or hybrid.
4. The battery according to claim 3, It is characterized in that The solid electrolyte is selected from a combination of PEO and LAGP; Preferably, the solid electrolyte comprises a mixed layer prepared by mixing or stacking LAGP and PEO according to a mass ratio.
5. The battery according to claim 4, It is characterized in that The solid electrolyte is obtained by stacking and assembling two, three or more layers of the PEO layer and the LAGP layer. Preferably, the solid electrolyte is prepared by sintering a mixture of LAGP and PEO at high temperature.
6. A method for preparing a battery according to any one of claims 1 to 5, It is characterized in that The method comprises: assembling a positive electrode, a lithium metal negative electrode and a solid electrolyte, introducing N 2 , H 2 , constituting the battery.
7. The preparation method according to claim 6, It is characterized in that The catalyst was used as the positive electrode, and was assembled with the solid electrolyte and lithium metal as the negative electrode in sequence. 2 , H 2 , forming Li-N 2 / H 2 Battery.
8. Use of the battery according to any one of claims 1 to 5 in electrochemical synthesis of ammonia.
9. A method for synthesizing ammonia, It is characterized in that The method comprises the following steps: the method comprises decoupling nitrogen reduction and hydrogen oxidation into positive electrode discharge and charge processes through the battery according to any one of claims 1 to 5, synthesizing NH 3 .
10. The method according to claim 9, It is characterized in that The steps include: In the first step, under discharge conditions, lithium metal acts as the negative electrode to convert N 2 Reduction and Li + Combined to form Li 3 N; In the second step, under charging conditions, H 2 Under the action of the catalyst, an oxidation reaction occurs to obtain hydrogen protons, which react with the Li 3 N combines to form NH 3 .