Compound rubidium niobium germanate second-order nonlinear optical crystal as well as preparation method and application thereof

Rubidium germanate (RbNbGe3O9) is synthesized through high-temperature solid-state reaction method and high-temperature solution method, which solves the problem of limited transmission range of existing nonlinear optical crystals in the mid-infrared range and prepares a product with wide transmission range and high second harmonic. High-strength rubidium germanate crystal, suitable for mid-infrared nonlinear optics.

CN118756338APending Publication Date: 2024-10-11TIANJIN UNIVERSITY OF TECHNOLOGY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410756730.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-13
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Existing nonlinear optical crystals have a limited transmission range in the mid-infrared range and are difficult to cover the 3-5 μm atmospheric transmission window. They also have deficiencies in frequency conversion performance and cannot meet the needs of scientific and technological development.

Method used

The compound rubidium germanate (RbNbGe3O9) was synthesized using traditional high-temperature solid-state reaction methods and high-temperature solution methods. Through multiple grinding and flux-assisted growth, a second-order non-linear rubidium germanate with wide transmission range and high second harmonic intensity was prepared. Linear optical crystals.

Benefits of technology

Within the same particle size range, the second harmonic intensity of rubidium germanate crystal is similar to that of KDP crystal, with a larger band gap and an infrared cutoff edge wider than 5 μm. It has excellent thermal stability and high laser damage threshold, and is suitable for mid-infrared applications. The field of nonlinear optics.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118756338A_ABST
    Figure CN118756338A_ABST
Patent Text Reader

Abstract

The invention provides a rubidium niobium germanate second-order nonlinear optical crystal as well as a preparation method and application thereof, and belongs to the technical field of optical crystal materials. The compound is prepared by adopting a high-temperature solid-phase method and a fluxing agent method, and the preparation method comprises the step of growing the rubidium niobium germanate nonlinear optical crystal by adopting the fluxing agent method. The obtained product has a moderate frequency-doubled effect, a large optical band gap and a wide transmission range, has stable physical and chemical properties, can stably exist in air, and can be used for preparing near-intermediate infrared nonlinear optical frequency conversion devices.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for preparing a niobium-rubidium-germanate second-order nonlinear optical crystal and a nonlinear optical device made by using the crystal. The chemical formula of the crystal is RbNbGe3O9. Background Art

[0002] Lasers have excellent directivity, monochromaticity, coherence and high brightness, so they have been widely used in many fields such as military and medical. The development of lasers is inseparable from the progress of nonlinear optical crystals. Optical frequency conversion is mainly achieved by utilizing the frequency doubling, sum frequency, difference frequency and optical parametric amplification of nonlinear optical crystals, thereby obtaining lasers with different frequencies from the incident light waves. At present, widely used nonlinear optical materials include KBe2BO3F2 (KBBF) crystals, β-BaB2O4 (BBO) crystals, LiB3O5 (LBO) crystals, KH2PO4 (KDP) crystals and KTiOPO4 (KTP). However, these materials still have some shortcomings, such as limited optical transmittance range, and it is difficult to cover the 3-5μm atmospheric transmission window. With the development of science and technology, it is urgent to explore more nonlinear optical crystals with excellent performance, especially those with a wide transmittance range.

[0003] Germanate crystals are favored for their low phonon energy, high laser damage value, stable physical and chemical properties, and excellent heat resistance. Therefore, germanate is considered a candidate system for exploring mid-infrared nonlinear optical crystal materials. 0 Electronic configuration of Nb 5+ cations and alkali metal cations Rb without dd or ff electron transitions + The introduction of the germanate system aims to maintain the wide transmission range of germanate while enhancing the frequency response. Based on the above design ideas, the inventors prepared an alkali metal germanium niobate nonlinear optical crystal with good comprehensive performance, which has potential application value in the field of mid-infrared nonlinear optics. Summary of the invention

[0004] The first object of the present invention is to provide a niobium germanate rubidium second-order nonlinear optical crystal, the chemical formula of which is RbNbGe3O9;

[0005] The second object of the present invention is to provide a method for synthesizing niobium germanate compound rubidium niobate by a traditional high temperature solid phase reaction method and growing niobium germanate rubidium nonlinear optical crystal by a high temperature solution method;

[0006] The third object of the present invention is to provide the use of niobium rubidium germanate nonlinear optical devices.

[0007] The technical solution to achieve the above purpose is as follows:

[0008] The compound niobium germanate rubidium provided by the present invention has a chemical formula of RbNbGe3O9. The preparation method of the compound niobium germanate rubidium second-order nonlinear optical material is as follows: uniformly mix and fully grind raw materials containing rubidium compound, niobium compound and germanium compound according to a certain stoichiometric ratio, place them in a muffle furnace, pre-sinter at low temperature to remove moisture and gas in the raw materials, then heat and calcine for no less than three days, take them out and grind them several times during the period, and finally obtain the compound niobium germanate rubidium polycrystalline pure phase;

[0009] The rubidium-containing compound includes at least one of rubidium oxide, rubidium hydroxide or a rubidium salt; the rubidium salt includes at least one of rubidium chloride, rubidium bromide, rubidium fluoride, rubidium nitrate, rubidium carbonate and rubidium sulfate;

[0010] The niobium-containing compound is at least one of niobium oxide or niobium salt; the niobium salt includes at least one of niobium chloride and niobium fluoride;

[0011] The germanium-containing compound is at least one of germanium oxide or germanium salt; the germanium salt includes at least one of germanium chloride and germanium bromide.

[0012] The high temperature solid phase reaction method can be used to prepare niobium germanate rubidium compounds according to the following chemical reaction formula:

[0013] 1)Rb2CO3+Nb2O5+6GeO2→2RbNbGe3O9+CO2↑

[0014] 2)2RbNO3+Nb2O5+6GeO2→2RbNbGe3O9+2NO2↑+0.5O2↑

[0015] 3)2RbOH+Nb2O5+6GeO2→2RbNbGe3O9+H2O↑

[0016] 4)Rb2SO4+Nb2O5+6GeO2→2RbNbGe3O9+SO2↑+0.5O2↑

[0017] 5)Rb2O+Nb2O5+6GeCl4+6O2→2RbNbGe3O9+12Cl2↑

[0018] 6)2RbF+Nb2O5+6GeO2+0.5O2→2RbNbGe3O9+F2↑

[0019] 7)2RbCl+Nb2O5+6GeO2+0.5O2→2RbNbGe3O9+Cl2↑

[0020] 8)2RbBr+Nb2O5+6GeO2+0.5O2→2RbNbGe3O9+Br2↑

[0021] 9)Rb2O+Nb2O5+6GeO2→2RbNbGe3O9

[0022] 10)Rb2CO3+2NbCl5+2.5O2+6GeO2→2RbNbGe3O9+CO2↑+5Cl2↑

[0023] 11)Rb2CO3+2NbF5+6GeO2+1.5O2→2RbNbGe3O9+5F2↑

[0024] The present invention provides a method for preparing a niobium rubidium germanate mid-infrared second-order nonlinear optical crystal and a nonlinear optical device made using the crystal. The compound is synthesized by a high-temperature solid phase method, and its chemical formula is RbNbGe3O9. Under the same particle size range, the crystal has a second harmonic intensity similar to that of a KDP crystal, and has a larger band gap (3.91eV) and a wide mid-infrared transmission range, and the infrared cutoff edge is wider than 5μm.

[0025] The present invention provides a method for preparing a niobium rubidium germanate second-order nonlinear optical crystal. The niobium rubidium germanate second-order nonlinear optical crystal is grown by a flux method. The specific growth scheme is as follows:

[0026] a. Evenly mix the compound niobium germanate rubidium single-phase polycrystalline powder and flux, heat the mixture to 600-1200°C at a heating rate of 5-100°C / h, keep the mixture at this temperature for not less than 24h, and cool the mixture to 550-1000°C, wherein the molar ratio of the compound niobium germanate rubidium single-phase polycrystalline powder to the flux is 1:0-20;

[0027] or directly heating a mixture of a rubidium-containing compound, a niobium-containing compound and a germanium-containing compound or a mixture of a rubidium-containing compound, a niobium-containing compound and a germanium-containing compound and a flux to 600-1200° C. at a heating rate of 5-100° C. / h, keeping the temperature constant for not less than 24 hours, and cooling the mixed solution to 550-1000° C., wherein the molar ratio of the rubidium-containing compound, the niobium-containing compound and the germanium-containing compound to the flux is 1:1:3:0-20;

[0028] The flux mainly includes Rb2O, RbOH, GeO2, rubidium salt, germanium salt, PbO, KF, and composite flux, such as one or more of Rb2O-GeO2, RbF-GeO2, RbF-PbO, Rb2O-PbO, RbF-KF, GeO2-KF or KF-PbO-RbF.

[0029] The compound niobium germanate rubidium single-phase polycrystalline powder is prepared by a high-temperature solid phase method, comprising the following steps: mixing a rubidium-containing compound, a niobium-containing compound and a germanium-containing compound, and preparing niobium germanate rubidium by a high-temperature solid phase reaction method, wherein the molar ratio of the element rubidium in the rubidium-containing compound, the element niobium in the niobium-containing compound and the element germanium in the germanium-containing compound is 1:1:3; fully grinding the raw materials of the rubidium-containing compound, the niobium-containing compound and the germanium-containing compound, mixing them evenly, putting them into a Pt crucible or an Al2O3 crucible and placing them in a muffle furnace, first pre-burning to discharge moisture and gas in the raw materials, then heating to 930°C for continuous sintering, the calcination time is not less than 72 hours, taking them out for grinding several times during the calcination, and finally cooling to room temperature to obtain the compound niobium germanate rubidium single-phase polycrystalline powder.

[0030] b. Preparation of niobium germanate rubidium seed crystals: slowly cooling the mixed solution obtained in step a to room temperature at a cooling rate of 0.5-20° C. / h to obtain niobium germanate rubidium seed crystals by spontaneous crystallization;

[0031] c. Place the Pt crucible containing the mixed solution obtained in step a into a crystal growth furnace, fix the seed crystal obtained in step b on the seed crystal rod, place the seed crystal above the liquid level through a platinum wire, preheat the seed crystal for 15-30 minutes, and when the temperature is 2-15°C higher than the saturation point, lower the seed crystal below the solution level, keep the temperature constant for 5-20 minutes to eliminate impurities on the surface of the seed crystal, and then cool it down to the saturation point temperature at a cooling rate of 1-10°C / min;

[0032] d. Then slowly cool down at a cooling rate of 1-5℃ / day, and grow the seed crystal at a rotation speed of 10-40rpm. After the crystal grows to the required size, lift the crystal to 1-2cm above the liquid surface, then cool it to room temperature at a rate of 20-50℃ / h. Finally, open the furnace and take out the crystal to obtain a niobium rubidium germanate second-order nonlinear optical crystal.

[0033] The molar ratio of Rb2O to GeO2 in the flux Rb2O-GeO2 system is 1-5:2-8; the molar ratio of RbF to GeO2 in the RbF-GeO2 system is 1-10:1-5; the molar ratio of RbF to PbO in the RbF-PbO system is 1-10:1-20; the molar ratio of Rb2O to PbO in the Rb2O-PbO system is 5-20:1-20; the molar ratio of RbF to KF in the RbF-KF system is 5-20:1-20; the molar ratio of GeO2 to KF in the GeO2-KF system is 1-5:5-20; the molar ratio of KF to PbO to RbF in the KF-PbO-RbF system is 1-5:1-6:2-10.

[0034] The present invention provides a second-order nonlinear optical crystal of niobium rubidium germanate, which is synthesized by a high-temperature solid phase method and has a chemical formula of RbNbGe3O9. It has a second harmonic intensity similar to that of KDP in the same particle size range, a larger band gap of 3.91eV, and an infrared cutoff width of more than 5μm.

[0035] Since Rb2O, RbOH, GeO2, rubidium salts, germanium salts, PbO, KF or composite fluxes are used in the process of growing niobium rubidium germanate second-order nonlinear optical crystals, wherein the composite fluxes include one or more of Rb2O-GeO2, RbF-GeO2, RbF-PbO, Rb2O-PbO, RbF-KF, GeO2-KF or KF-PbO-RbF, it is easy to grow target crystals of larger sizes; the obtained crystals have the advantages of wide atmospheric transmission window, excellent thermal stability, large laser damage threshold, etc.

[0036] The compound niobium germanate rubidium crystal obtained by the method of the present invention can be used to prepare a frequency doubling device. At room temperature, a Nd:YAG Q-switched laser light source is used and an incident infrared light with a wavelength of 1064nm can output a green laser with a wavelength of 532nm. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] Figure 1 The X-ray diffraction pattern of the RbNbGe3O9 powder of the present invention.

[0038] Figure 2 This is the ultraviolet-visible-near-infrared diffuse reflectance spectrum and experimental band gap diagram of RbNbGe3O9 of the present invention.

[0039] Figure 3 Schematic diagram of the working principle of the nonlinear optical device made of RbNbGe3O9 crystal of the present invention, wherein 1 is the laser, 2 is the incident laser beam, 3 is the RbNbGe3O9 crystal, 4 is the generated laser beam, and 5 is the filter. DETAILED DESCRIPTION

[0040] The present invention is described in detail below with reference to the accompanying drawings and embodiments:

[0041] Embodiment 1:

[0042] According to the reaction formula: Rb2CO3+Nb2O5+6GeO2→2RbNbGe3O9+CO2↑, the compound RbNbGe3O9 is synthesized;

[0043] Rb2CO3, Nb2O5 and GeO2 are weighed in a molar ratio of 1:1:6 and put into a mortar, mixed and ground, then put into an open alumina crucible of φ60mm×60mm, placed in a muffle furnace, slowly heated to 350℃ for calcination, kept at a constant temperature for 12h to remove moisture and gas, then heated to 650℃ for calcination for 24h, taken out and ground, then placed in a muffle furnace, and heated to 930℃ for calcination for not less than 48h to prepare a single-phase polycrystalline powder of niobium germanate compound. The powder X-ray diffraction test and analysis show that the obtained sample powder X-ray diffraction spectrum is consistent with the X-ray theoretical spectrum obtained from the single crystal structure of niobium germanate RbNbGe3O9, see Appendix Figure 1 ;

[0044] The prepared compound niobium germanate rubidium RbNbGe3O9 single-phase polycrystalline powder is mixed with flux Rb2O-GeO2 in a molar ratio of 1:2, wherein the molar ratio of Rb2O to GeO2 is 1:5, and is loaded into a φ60mm×60mm platinum crucible, and the temperature is raised to 950°C and kept constant for not less than 24 hours to allow the solution to be mixed uniformly, and at the same time, Pt wire is added, and then the temperature is lowered to induce spontaneous crystallization.

[0045] The solution is slowly cooled at a cooling rate of 1-5°C / h to obtain niobium germanate rubidium seed crystals;

[0046] Growing crystals using the top seeding method: small RbNbGe3O9 grains obtained by spontaneous crystallization are used as seed crystals, and the seed crystals are fixed on the seed crystal rods using platinum wires. The seed crystals are first placed 1-3 cm above the liquid surface for preheating, and then immersed below the liquid surface when the temperature is 5-15°C higher than the saturation point, and kept for 5-20 minutes to remove surface impurities, and then quickly cooled to the saturation point temperature;

[0047] Then cool down at a rate of 1-5℃ / day, the rotation speed of the seed crystal rod is 10-40rpm, and after the growth is completed, the crystal is lifted 1-2cm above the liquid surface, cooled to room temperature at a rate of 20-50℃ / h, and then the crystal is taken out to obtain RbNbGe3O9 crystal.

[0048] The raw material rubidium carbonate in the reaction formula can be replaced by rubidium oxide, rubidium chloride, rubidium bromide, rubidium nitrate, rubidium hydroxide, rubidium sulfate or other rubidium-containing salts, niobium oxide can be replaced by niobium chloride, niobium fluoride or other niobium-containing salts, and germanium oxide can be replaced by other germanium salts.

[0049] Embodiment 2:

[0050] According to the reaction formula: 2RbNO3+Nb2O5+6GeO2→2RbNbGe3O9+2NO2↑+0.5O2↑, the compound RbNbGe3O9 is synthesized;

[0051] RbNO3, Nb2O5 and GeO2 were weighed directly in a molar ratio of 2:1:6, and the weighed raw materials were mixed with flux RbF-GeO2 in a molar ratio of 1:3, wherein the molar ratio of RbF to GeO2 was 5:1, mixed evenly, pressed, and loaded into a φ60mm×60mm Pt crucible for 10 - The mixed raw materials are heated to 920°C at a heating rate of 80°C / h and kept at this temperature for not less than 24 hours to make the solution uniformly mixed. At the same time, a Pt wire is lowered into the liquid surface and then cooled to induce spontaneous crystallization;

[0052] Slowly cooling at a cooling rate of 1-5°C / h to obtain niobium germanate rubidium seed crystals by spontaneous crystallization;

[0053] Growing crystals in compound solution: small RbNbGe3O9 grains obtained by spontaneous crystallization are used as seed crystals, and the seed crystals are fixed on seed crystal rods using platinum wires. The seed crystals are first placed 1-2 cm above the liquid surface for preheating, and then immersed below the liquid surface at a temperature 5-15°C higher than the saturation point, and kept for 5-30 minutes to remove surface impurities, and then quickly cooled to the saturation point temperature;

[0054] Then cool down at a rate of 1-5℃ / day, with the rotation speed of the seed crystal rod at 10-40rpm. After the crystal growth is completed, lift the crystal out of the liquid surface and cool it to room temperature at a cooling rate of 20-50℃ / h. Take out the crystal from the furnace to obtain RbNbGe3O9 crystal.

[0055] The raw material rubidium nitrate in the reaction formula can be replaced by rubidium oxide, rubidium chloride, rubidium bromide, rubidium hydroxide, rubidium sulfate or other rubidium-containing salts, niobium oxide can be replaced by niobium chloride, niobium fluoride or other niobium-containing salts, and germanium oxide can be replaced by other germanium salts.

[0056] Embodiment 3:

[0057] According to the reaction formula: 2RbOH+Nb2O5+6GeO2→2RbNbGe3O9+H2O↑, the compound RbNbGe3O9 is synthesized;

[0058] RbOH, Nb2O3 and GeO2 are directly weighed in a molar ratio of 2:1:6, and the weighed raw materials are mixed with flux RbF-PbO in a molar ratio of 1:1, wherein the molar ratio of RbF to PbO is 2:1, and loaded into a φ60mm×60mm platinum crucible, and the temperature is raised to 900℃, and the temperature is kept constant for not less than 24h to make the solution mixed uniformly, and Pt wire is added at the same time, and then the temperature is lowered to induce spontaneous crystallization;

[0059] The solution is slowly cooled at a cooling rate of 1-5°C / h to obtain niobium germanate rubidium seed crystals;

[0060] Growing crystals in compound solution: small RbNbGe3O9 grains obtained by spontaneous crystallization are used as seed crystals, and the seed crystals are fixed on seed crystal rods using platinum wires. The seed crystals are first placed 1-2 cm above the liquid surface for preheating treatment, and then immersed below the liquid surface when the temperature is 5-15°C higher than the saturation point, and kept for 5-20 minutes to remove surface impurities, and then quickly cooled to the saturation point temperature;

[0061] The temperature is slowly lowered at a rate of 1-3°C / day, the rotation speed of the seed crystal rod is 10-40rpm, and after the crystal growth is completed, the crystal is lifted out of the liquid surface, cooled to room temperature at a rate of 10-50°C / h, and then the crystal is taken out of the furnace to obtain RbNbGe3O9 crystal.

[0062] The raw material rubidium hydroxide in the reaction formula can be replaced by rubidium oxide, rubidium chloride, rubidium bromide, rubidium sulfate or other rubidium-containing salts, niobium oxide can be replaced by niobium chloride, niobium fluoride or other niobium-containing salts, and germanium oxide can be replaced by other germanium salts.

[0063] Embodiment 4:

[0064] According to the reaction formula: Rb2SO4+Nb2O5+6GeO2→2RbNbGe3O9+SO2↑+0.5O2↑, the compound RbNbGe3O9 is synthesized;

[0065] Weigh Rb2SO4, Nb2O5, GeO2 in a molar ratio of 1:1:6, mix the weighed raw materials with flux Rb2O-PbO in a molar ratio of 1:3, wherein the molar ratio of Rb2O to PbO is 5:3, put them into a Φ60mm×60mm platinum crucible, heat to 860℃, keep the temperature constant for not less than 24h, so that the solution is mixed evenly, and put Pt wire into it at the same time, and then cool it down to induce spontaneous crystallization;

[0066] The solution is slowly cooled at a cooling rate of 1-5°C / h to obtain niobium germanate rubidium seed crystals;

[0067] Growing crystals in compound solution: small RbNbGe3O9 grains obtained by spontaneous crystallization are used as seed crystals, and the seed crystals are fixed on seed crystal rods using platinum wires. The seed crystals are first placed 1-2 cm above the liquid surface for preheating treatment, and then immersed below the liquid surface when the temperature is 5-15°C higher than the saturation point, and kept for 5-20 minutes to remove surface impurities, and then quickly cooled to the saturation temperature;

[0068] The temperature is slowly lowered at a rate of 1-3℃ / day, the rotation speed of the seed crystal rod is 10-40rpm, and after the crystal growth is completed, the crystal is lifted out of the liquid surface, and the temperature is lowered to room temperature at a rate of 20-50℃ / h, and then the crystal is taken out of the furnace to obtain RbNbGe3O9 crystal.

[0069] The raw material rubidium sulfate in the reaction formula can be replaced by rubidium oxide, rubidium bromide, rubidium fluoride, rubidium nitrate, rubidium carbonate or other rubidium-containing salts, niobium oxide can be replaced by niobium chloride, niobium fluoride or other niobium-containing salts, and germanium oxide can be replaced by other germanium salts.

[0070] Embodiment 5:

[0071] According to the reaction formula: 2RbCl+Nb2O5+6GeO2+0.5O2→2RbNbGe3O9+Cl2↑, the compound RbNbGe3O9 is synthesized;

[0072] Weigh the raw materials of RbCl, Nb2O5 and GeO2 in a molar ratio of 2:1:6, mix the weighed raw materials with flux RbF-KF in a molar ratio of 1:4, wherein the molar ratio of RbF to KF is 2:3, put them into a φ60mm×60mm platinum crucible, heat it to 870℃, keep it at a constant temperature for not less than 24h, so that the solution is mixed evenly, and then add Pt wire, and then cool it down to induce spontaneous crystallization;

[0073] The solution is slowly cooled at a cooling rate of 1-5°C / h to obtain niobium germanate rubidium seed crystals;

[0074] Growing crystals in compound solution: small RbNbGe3O9 grains obtained by spontaneous crystallization are used as seed crystals, and the seed crystals are fixed on seed crystal rods using platinum wires. The seed crystals are first placed 1-2 cm above the liquid surface for preheating treatment, and then immersed below the liquid surface when the temperature is 5-15°C higher than the saturation point, and kept for 5-20 minutes to remove surface impurities, and then quickly cooled to the saturation point temperature;

[0075] The temperature is slowly lowered at a rate of 1-3°C / day and the rotation speed of the seed crystal rod is 10-40rpm. After the crystal growth is completed, the crystal is lifted out of the liquid surface and the temperature is lowered to room temperature at a rate of 20-50°C / h. The crystal is then taken out of the growth furnace to obtain the RbNbGe3O9 crystal.

[0076] The raw material rubidium chloride in the reaction formula can be replaced by other rubidium-containing salts such as rubidium bromide, rubidium fluoride, rubidium nitrate, rubidium carbonate, or rubidium sulfate, niobium oxide can be replaced by other niobium-containing salts such as niobium chloride or niobium fluoride, and germanium oxide can be replaced by other germanium salts.

[0077] Embodiment 6:

[0078] According to the reaction formula: 2RbBr+Nb2O5+6GeO2+0.5O2→2RbNbGe3O9+Br2↑, the compound RbNbGe3O9 is synthesized;

[0079] Weigh the raw materials of RbBr, Nb2O5 and GeO2 in a molar ratio of 2:1:6, mix the weighed raw materials with flux GeO2-KF in a molar ratio of 1:3, wherein the molar ratio of GeO2 to KF is 1:5, put them into a φ60mm×60mm platinum crucible, heat to 850℃, keep the temperature constant for not less than 24h, make the solution mixed evenly, put Pt wire into it at the same time, and then cool it down to induce spontaneous crystallization;

[0080] The solution is slowly cooled at a cooling rate of 1-5°C / h to obtain niobium germanate rubidium seed crystals;

[0081] Growing crystals in compound solution: small RbNbGe3O9 grains obtained by spontaneous crystallization are used as seed crystals, and the seed crystals are fixed on seed crystal rods using platinum wires. The seed crystals are first placed 1-2 cm above the liquid surface for preheating treatment, and then immersed below the liquid surface when the temperature is 5-15°C higher than the saturation point, and kept for 5-20 minutes to remove surface impurities, and then quickly cooled to the saturation point temperature;

[0082] The temperature is slowly lowered at a rate of 1-3°C / day, the rotation speed of the seed crystal rod is 10-40rpm, and after the crystal growth is completed, the crystal is lifted out of the liquid surface, and the temperature is lowered to room temperature at a rate of 20-50°C / h, and then the crystal is taken out of the furnace to obtain the RbNbGe3O9 crystal.

[0083] The raw material rubidium bromide in the reaction formula can be replaced by other rubidium-containing salts such as rubidium chloride, rubidium fluoride, rubidium nitrate, rubidium carbonate, or rubidium sulfate, niobium oxide can be replaced by other niobium-containing salts such as niobium chloride or niobium fluoride, and germanium oxide can be replaced by other germanium salts.

[0084] Embodiment 7:

[0085] According to the reaction formula: Rb2O+Nb2O5+6GeO2→2RbNbGe3O9, the compound RbNbGe3O9 is synthesized;

[0086] Weigh Rb2O, Nb2O5 and GeO2 in a molar ratio of 1:1:6, mix the weighed raw materials with flux KF-PbO-RbF in a molar ratio of 1:1, where the molar ratio of KF to PbO to RbF is 2:3:6, put them into a φ60mm×60mm platinum crucible, heat it to 900℃ to make the solution mix evenly, put Pt wire in at the same time, and then cool it down to induce spontaneous crystallization;

[0087] The solution is slowly cooled at a cooling rate of 1-5°C / h to obtain niobium germanate rubidium seed crystals;

[0088] Growing crystals in compound solution: small RbNbGe3O9 grains obtained by spontaneous crystallization are used as seed crystals, and the seed crystals are fixed on seed crystal rods using platinum wires. The seed crystals are first placed 1-2 cm above the liquid surface for preheating treatment, and then immersed below the liquid surface when the temperature is 5-15°C higher than the saturation point, and kept for 5-20 minutes to remove surface impurities, and then quickly cooled to the saturation point temperature;

[0089] The temperature is slowly lowered at a rate of 1-3°C / day, the rotation speed of the seed crystal rod is 10-40rpm, and after the crystal growth is completed, the crystal is lifted out of the liquid surface, and the temperature is lowered to room temperature at a rate of 20-50°C / h, and then the crystal is taken out of the furnace to obtain the RbNbGe3O9 crystal.

[0090] The raw material rubidium oxide in the reaction formula can be replaced by other rubidium-containing salts such as rubidium bromide, rubidium chloride, rubidium fluoride, rubidium nitrate, rubidium carbonate, or rubidium sulfate, niobium oxide can be replaced by other niobium-containing salts such as niobium chloride or niobium fluoride, and germanium oxide can be replaced by other germanium salts.

[0091] Example 8

[0092] Nonlinear optical devices made from RbNbGe3O9 crystals:

[0093] The RbNbGe3O9 nonlinear optical crystal obtained in Examples 1-7 can be used as a second-order nonlinear optical device by determining the crystal optical axis, orienting and processing the crystal according to the required size, angle and thickness, and polishing the light-transmitting surface.

[0094] According to the attached Figure 3 As shown, the obtained crystal is fixed at position 3. At room temperature, a Q-switched Nd:YAG laser is used as the light source. The incident wavelength is 1064nm infrared light. After the infrared light beam 2 with a wavelength of 1064nm is incident on the RbNbGe3O9 crystal, a green doubled frequency light with a wavelength of 532nm is generated. The output light beam 4 contains infrared light with a wavelength of 1064nm and green light with a wavelength of 532nm. After passing through the filter 5, a green laser with a wavelength of 532nm is obtained.

Claims

1. The present invention provides a mid-infrared niobium rubidium germanate second-order nonlinear optical crystal and its preparation and a method for making a nonlinear optical device using the crystal. The compound is prepared by a high-temperature solid-phase method, and its chemical formula is RbNbGe3O9. It has a second harmonic intensity similar to that of a KDP crystal within the same particle size range, and has a larger band gap (3.91 eV) and a wide mid-infrared transmission range, with an infrared cutoff width of more than 5 μm. The crystal is grown by a flux method, and exhibits excellent thermal and chemical stability, and can be used as a near-mid-infrared nonlinear optical crystal and applied to all-solid-state lasers.

2. The method for preparing the compound niobium rubidium germanate nonlinear optical crystal according to claim 1, characterized in that The niobium germanate rubidium second-order nonlinear optical crystal and the polycrystalline pure phase are prepared by a flux method and a high-temperature solid phase method respectively, comprising the following steps: a. Mixing a rubidium-containing compound, a niobium-containing compound and a germanium-containing compound to obtain the compound niobium germanate rubidium RbNbGe3O9 by a solid phase reaction method, wherein the molar ratio of the rubidium element in the rubidium-containing compound, the niobium element in the niobium-containing compound and the germanium element in the germanium-containing compound is 1:1:3; b. The compound niobium germanate rubidium is prepared by a high-temperature solid phase reaction method, and the specific process is as follows: the raw materials containing rubidium compound, niobium compound and germanium compound are mixed evenly, ground sufficiently, placed in a muffle furnace, pre-burned at low temperature to remove moisture and gas in the mixture, then heated and calcined, taken out and ground several times during the process, and finally cooled to room temperature to obtain the compound niobium germanate rubidium; The rubidium-containing compound includes at least one of rubidium oxide, rubidium hydroxide or a rubidium salt; the rubidium salt includes at least one of rubidium chloride, rubidium bromide, rubidium fluoride, rubidium nitrate, rubidium carbonate and rubidium sulfate; The niobium-containing compound is at least one of niobium oxide or niobium salt; the niobium salt includes at least one of niobium chloride and niobium fluoride; The germanium-containing compound is at least one of germanium oxide or germanium salt; the germanium salt includes at least one of germanium chloride and germanium bromide; Heating any obtained compound niobium germanate rubidium single-phase polycrystalline powder or a mixture of any obtained compound niobium germanate rubidium single-phase polycrystalline powder and a flux to obtain a uniform mixed solution; Or directly heating a mixture of a rubidium-containing compound, a niobium-containing compound and a germanium-containing compound or a mixture of a rubidium-containing compound, a niobium-containing compound and a germanium-containing compound and a flux to obtain a uniform mixed solution; c. Place the platinum crucible containing the mixed solution obtained in step b into a crystal growth furnace, fix one end of the seed crystal with a platinum wire and slowly lower it. When the temperature in the furnace is 5-15°C higher than the saturation point temperature, lower the other end of the seed crystal into the liquid surface to melt away surface impurities or defects, then quickly cool down to below the saturation temperature or grow at a constant temperature to prepare a niobium rubidium germanate nonlinear optical crystal.

3. The method for preparing the niobium rubidium germanate nonlinear optical crystal according to claim 2, characterized in that The molar ratio of the compound niobium rubidium germanate single-phase polycrystalline powder to the flux is 1:0-20; the flux mainly includes Rb2O, RbOH, GeO2, rubidium salt, germanium salt, PbO, KF, and composite flux, such as one or more of Rb2O-GeO2, RbF-GeO2, RbF-PbO, Rb2O-PbO, RbF-KF, GeO2-KF or KF-PbO-RbF.

4. The method for preparing the niobium rubidium germanate nonlinear optical crystal according to claim 3, characterized in that: The molar ratio of Rb2O to GeO2 in the flux Rb2O-GeO2 system is 1-5:2-8; the molar ratio of RbF to GeO2 in the RbF-GeO2 system is 1-10:1-5; the molar ratio of RbF to PbO in the RbF-PbO system is 1-10:1-20; the molar ratio of Rb2O to PbO in the Rb2O-PbO system is 5-20:1-20; the molar ratio of RbF to KF in the RbF-KF system is 5-20:1-20; the molar ratio of GeO2 to KF in the GeO2-KF system is 1-5:5-20; the molar ratio of KF to PbO to RbF in the KF-PbO-RbF system is 1-5:1-6:2-10.

5. The use of the niobium rubidium germanate nonlinear optical crystal according to claim 1, characterized in that: The niobium germanium oxide nonlinear optical crystal is used to make a frequency doubling generator, a frequency converter and an optical parametric oscillator.