Grain boundary diffusion process for neodymium-iron-boron magnet
Spraying technology is used to apply heavy rare earth and light rare earth diffusing agents on the surface of NdFeB magnets in zones, which solves the problems of low heavy rare earth diffusion rate and high cost in the existing grain boundary diffusion process, and improves the coercive force and thickness of the magnet. Suitable for the production of high-performance magnets.
Patent Information
- Application Number
- CN202411066408.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-05
- Publication Date
- 2024-10-11
AI Technical Summary
In the existing grain boundary diffusion process, the diffusion rate of the heavy rare earth diffusing agent is low, resulting in poor coercivity improvement effect. At the same time, the process cost is high, and the thickness of most magnets is less than 4mm, which makes it difficult to meet the requirements of high-performance NdFeB magnets. High temperature requirements.
Spraying technology is used to coat heavy rare earth diffusing agents and light rare earth diffusing agents on the surface of NdFeB magnets in zones. Vacuum heat treatment is used to improve grain boundary diffusion efficiency, reduce the amount of heavy rare earths and increase the coercive force of the magnet.
It effectively increases the coercive force and thickness of the magnet, reduces the amount of heavy rare earths, is suitable for the production of high-temperature resistant magnets required in large motors and generators, and reduces process costs.
Smart Images

Figure CN118762919A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of rare earth magnetic materials, and in particular to a grain boundary diffusion process for neodymium iron boron magnets. Background Art
[0002] Since its introduction, the grain boundary diffusion technology has developed very rapidly because it can significantly improve the coercivity, save heavy rare earths, and greatly save material costs. At present, the maturity of the grain boundary diffusion technology has been used to evaluate the advancement of a NdFeB enterprise in the industry. Grain boundary diffusion technology is a major technological innovation in the sintered NdFeB permanent magnet industry in the 21st century. While achieving high coercivity and high magnetic energy product, it significantly reduces the use of heavy rare earth elements. Through the grain boundary diffusion technology, the coercivity and maximum magnetic energy product of sintered magnet products have achieved new breakthroughs. With the development of strategic emerging fields, the demand for high-performance NdFeB magnets will continue to grow. This puts forward a more urgent need and higher requirements for grain boundary diffusion technology.
[0003] The existing grain boundary diffusion process uses heavy rare earth diffusers to perform grain boundary diffusion treatment on the magnet surface. Heavy rare earth oxides have good stability, but because their melting point is higher than 2000°C, their diffusion rate is low. In addition, it is difficult for heavy rare earth (HRE) atoms to separate from the oxide and enter the 2:14:1 phase, and the coercive force improvement effect is poor. At the same time, heavy rare earth metals are expensive, and the large-scale use of heavy rare earth metals greatly increases the process cost. Therefore, a new type of grain boundary diffusion process for NdFeB magnets is needed that can not only improve the diffusion efficiency of heavy rare earth diffusers but also combine the advantages of light rare earths, which can further improve the performance of NdFeB magnets while reducing process costs. Summary of the invention
[0004] The purpose of the present invention is to provide a grain boundary diffusion process for NdFeB magnets to solve the problems of low diffusion rate of heavy rare earth and high process cost in the background technology.
[0005] A grain boundary diffusion process for NdFeB magnets, characterized by comprising the following steps:
[0006] Step 1, cutting a sintered NdFeB magnet that does not contain heavy rare earth elements and light rare earth elements into a magnet sample of 10 mm×10 mm×3-10 mm, wherein the Z-axis length is 3-10 mm;
[0007] Step 2, cleaning and drying the surface of the sintered NdFeB magnet sample;
[0008] Step 3, using spraying technology to apply heavy rare earth diffusant and light rare earth diffusant on the surface in different areas;
[0009] Step 4: subjecting the magnet in step 3 to a vacuum heat treatment grain boundary diffusion process to obtain a high coercive force sintered NdFeB magnet.
[0010] Furthermore, in step 2, the surface of the sintered NdFeB magnet sample is first cleaned by grinding with sandpaper of 400, 800, 1200, 1600, 2000, and 3000 meshes, and then ultrasonically cleaned with distilled water for 8-10 minutes and with anhydrous ethanol for 3-5 minutes.
[0011] Furthermore, in step 2, the drying treatment adopts heat preservation drying, the temperature is 60-100° C., and the heat preservation time is 25-30 minutes.
[0012] Furthermore, in step 3, during spraying, the muzzle is 6-10 cm away from the surface of the magnet sample, the angle between the muzzle and the surface of the magnet sample is 70-90°, and the movement speed of the spray gun is 40-60 cm / min.
[0013] Furthermore, in step 3, the heavy rare earth diffusant is coated on the eight vertices and edge portions of the magnetic pole surface of the magnet, and the light rare earth diffusant is coated on the core portion of the magnetic pole surface.
[0014] Furthermore, in step 3, the heavy rare earth diffusant is composed of a heavy rare earth metal compound, a solvent, and a binder, and the mass proportions of the heavy rare earth metal compound, the solvent, and the binder are 40-60%: 30-40%: 5-10%.
[0015] Furthermore, the heavy rare earth metal compound is one or more oxides of micron-sized heavy rare earth elements such as Dy and Tb, the solvent is industrial alcohol with a concentration of ≥99.8%, and the additive is a binder.
[0016] Furthermore, in step 3, the light rare earth diffuser is composed of a light rare earth metal compound, a solvent, and a binder, and the mass proportions of the light rare earth metal compound, the solvent, and the additive are 40-60%: 30-40%: 5-10% respectively.
[0017] Furthermore, the light rare earth metal compound is one or more oxides of micron-sized light rare earth elements such as Pr, Nd, Ce, etc., the solvent is industrial alcohol with a concentration of ≥99.8%, and the additive is a binder.
[0018] Compared with the prior art, the present invention has the following beneficial effects:
[0019] 1. For magnets with complex shapes or large sizes, there are always areas that are most susceptible to demagnetization, and magnetization reversal starts first at some weak locations. In the present invention, while the heavy rare earth diffuser focuses on strengthening the easily demagnetized locations of the magnet, the light rare earth diffuser can also provide more low-melting-point liquid phases to promote the grain boundary diffusion of the heavy rare earth. This grain boundary diffusion method can further improve the coercive force of the magnet while reducing the amount of heavy rare earth used.
[0020] 2. In actual production of the present invention, the diffusion depth of the elements is limited. When the thickness of the magnet increases, the diffusion along the Z axis cannot improve the coercive force of the magnet well. This phenomenon is particularly obvious when the thickness of the magnet is greater than 10 mm. Therefore, in current industrial production, the thickness of most magnets treated by grain boundary diffusion is less than 4 mm, and rarely exceeds 8 mm. The use of spraying technology to coat the surface with heavy rare earth diffusants and light rare earth diffusants can effectively increase the thickness of the diffused magnet, which is required for the production of high temperature resistant magnets in large motors and generators. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 This is a flow chart of a grain boundary diffusion process for NdFeB magnets according to an embodiment of the present application. DETAILED DESCRIPTION
[0022] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0023] Example 1
[0024] See also Figure 1 , a grain boundary diffusion process for NdFeB magnets, comprising the following steps:
[0025] Step 1, cutting a sintered NdFeB magnet that does not contain heavy rare earth elements and light rare earth elements into 10 mm×10 mm×3 mm, wherein the Z-axis length is 3 to 10 mm;
[0026] Step 2, cleaning and drying the surface of the sintered NdFeB magnet sample;
[0027] Step 3, using spraying technology to apply heavy rare earth diffusant and light rare earth diffusant on the surface partition, wherein during spraying, the muzzle is 10 cm away from the surface of the magnet sample, the angle between the muzzle and the surface of the magnet sample is 90°, and the movement speed of the spray gun is 40 cm / min;
[0028] Step 4: subjecting the magnet in step 3 to a vacuum heat treatment grain boundary diffusion process to obtain a high coercive force sintered NdFeB magnet.
[0029] Example 2
[0030] A grain boundary diffusion process for NdFeB magnets, the process flow of which is the same as that of Example 1, except that in step 1, the sintered NdFeB magnets are cut into 10 mm×10 mm×6 mm pieces, and the other components and parameters remain unchanged.
[0031] Example 3
[0032] A grain boundary diffusion process for NdFeB magnets, the process flow of which is the same as that of Example 1, except that in step 1, the sintered NdFeB magnets are cut into 10 mm×10 mm×10 mm pieces, and the other components and parameters remain unchanged.
[0033] Example 4
[0034] A grain boundary diffusion process for NdFeB magnets, the process flow of which is the same as that of Example 1, except that during spraying in step 3, the muzzle is 8 cm away from the surface of the magnet sample, the angle between the muzzle and the surface of the magnet sample is 80°, and the movement speed of the spray gun is 50 cm / min.
[0035] Example 5
[0036] A grain boundary diffusion process for NdFeB magnets, the process flow of which is the same as that of Example 1, except that during spraying in step 3, the muzzle is 6 cm away from the surface of the magnet sample, the angle between the muzzle and the surface of the magnet sample is 70°, and the movement speed of the spray gun is 60 cm / min.
[0037] Comparative Example 1
[0038] A grain boundary diffusion process for NdFeB magnets, the process flow of which is the same as that of Example 1, except that a heavy rare earth diffusion agent is coated on the surface by spraying technology in step 3, and the other components and parameters remain unchanged.
[0039] Comparative Example 2
[0040] A grain boundary diffusion process for NdFeB magnets, the process flow of which is the same as that of Example 1, except that in step 3, a heavy rare earth diffusant and a light rare earth diffusant are sequentially coated on the surface, and the other components and parameters remain unchanged.
[0041] Comparative Example 3
[0042] A grain boundary diffusion process for NdFeB magnets, the process flow of which is the same as that of Example 1, except that a double layer of heavy rare earth element Dy and heavy rare earth element Tb is sequentially coated on the surface of the capture 3, and the other components and parameters remain unchanged.
[0043] Comparative Example 4
[0044] A grain boundary diffusion process for NdFeB magnets, the process flow of which is the same as that of Example 2, except that a heavy rare earth diffusion agent is coated on the surface by spraying technology in step 3, and the other components and parameters remain unchanged.
[0045] Comparative Example 5
[0046] A grain boundary diffusion process for NdFeB magnets, the process flow of which is the same as that of Example 3, except that the important spraying technology in step 3 is used to coat the surface with a heavy rare earth diffusing agent, and the other components and parameters remain unchanged.
[0047] The magnet properties of the above different embodiments and comparative examples were tested at 25° C. The test results are shown in Table 1.
[0048] Table 1
[0049]
[0050]
[0051] In actual production, the diffusion depth of elements is limited. When the thickness of the magnet increases, the diffusion along the Z axis cannot improve the coercive force of the magnet well. This phenomenon is particularly obvious when the thickness of the magnet is 10 mm. Therefore, in current industrial production, the thickness of most magnets treated by grain boundary diffusion is less than 4 mm, and rarely exceeds 8 mm. It can be seen from Examples 1-3 and Comparative Examples 4-5 that the thickness of the diffused magnet can be effectively increased by coating the surface with heavy rare earth diffusants and light rare earth diffusants using spraying technology.
[0052] It can be seen from Examples 1 and 4-5 that when heavy rare earth diffusants and light rare earth diffusants are coated on the surface in partitions using spraying technology, the spray gun is 10 cm away from the product surface, the muzzle is at a 90° angle to the surface of the magnet sample, and the spray gun moves at a speed of 40 cm / min, the performance of the magnet is better.
[0053] It can be seen from Example 1 and Comparative Examples 1-3 that coating the heavy rare earth diffusant and the light rare earth diffusant on the surface in different areas by spraying technology can reduce the amount of heavy rare earth and further improve the coercive force of the magnet.
[0054] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprises" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.
[0055] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A grain boundary diffusion process for NdFeB magnets, It is characterized in that The following steps are involved: Step 1, cutting a sintered NdFeB magnet that does not contain heavy rare earth elements and light rare earth elements into magnet samples of 10 mm×10 mm×3-10 mm, wherein the Z-axis length is 3-10 mm; Step 2, cleaning and drying the surface of the sintered NdFeB magnet sample; Step 3, using spraying technology to apply heavy rare earth diffusant and light rare earth diffusant on the surface in different areas; Step 4: subjecting the magnet in step 3 to a vacuum heat treatment grain boundary diffusion process to obtain a high coercive force sintered NdFeB magnet.
2. A grain boundary diffusion process for NdFeB magnets according to claim 1, It is characterized in that In the step 2, the surface of the sintered NdFeB magnet sample is first cleaned by grinding with sandpaper of 400, 800, 1200, 1600, 2000, and 3000 meshes, and then ultrasonically cleaned with distilled water for 8-10 minutes and with anhydrous ethanol for 3-5 minutes; in the step 2, the drying treatment adopts heat preservation drying at a temperature of 60-100° C. and a heat preservation time of 25-30 minutes.
3. The grain boundary diffusion process for NdFeB magnets according to claim 1, It is characterized in that In step 3, during spraying, the muzzle is 6-10 cm away from the surface of the magnet sample, the angle between the muzzle and the surface of the magnet sample is 70-90°, and the movement speed of the spray gun is 40-60 cm / min.
4. The grain boundary diffusion process for NdFeB magnets according to claim 1, It is characterized in that In the step 3, the heavy rare earth diffuser is coated on the eight vertices and edge portions of the magnetic pole surface of the magnet, and the light rare earth diffuser is coated on the core portion of the magnetic pole surface.
5. The grain boundary diffusion process for NdFeB magnets according to claim 1, It is characterized in that In step 3, the heavy rare earth diffuser is composed of a heavy rare earth metal compound, a solvent, and a binder, and the mass proportions of the heavy rare earth metal compound, the solvent, and the additive are 40-60%: 30-40%: 5-10% respectively.
6. A grain boundary diffusion process for NdFeB magnets according to claim 6, It is characterized in that The heavy rare earth metal compound is one or more oxides of micron-sized heavy rare earth elements such as Dy and Tb, the solvent is industrial alcohol with a concentration of ≥99.8%, and the additive is a binder.
7. The grain boundary diffusion process for NdFeB magnets according to claim 1, It is characterized in that In step 3, the light rare earth diffuser is composed of a light rare earth metal compound, a solvent, and a binder, and the mass proportions of the light rare earth metal compound, the solvent, and the binder are 40-60%: 30-40%: 5-10% respectively.
8. A grain boundary diffusion process for NdFeB magnets according to claim 8, It is characterized in that The light rare earth metal compound is one or more oxides of micron-sized light rare earth elements such as Pr, Nd, and Ce, the solvent is industrial alcohol with a concentration of ≥99.8%, and the additive is a binder.
9. The grain boundary diffusion process for NdFeB magnets according to claim 1, It is characterized in that In step 3, the vacuum heat treatment grain boundary diffusion process parameters are: vacuum degree of single temperature zone tube furnace: 5.5-6×10 -4 Pa, diffusion temperature: 850-1000℃, diffusion time: 6-8h, annealing temperature: 500-700℃, annealing time: 4-6h.
10. A neodymium iron boron magnet, It is characterized in that Prepared by the process described in any one of claims 1 to 10.