Preparation method of ternary metal phosphide CoNiMn-P porous hollow nanosheet electrode material
The preparation of porous hollow ternary metal phosphide CoNiMn-P nanosheet electrode materials is simplified through mixed solvent-assisted etching and atmosphere phosphating. It solves the problem of complicated preparation methods in the existing technology and achieves efficient preparation and excellent electrochemical performance. chemical properties.
Patent Information
- Application Number
- CN202410774794.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-17
- Publication Date
- 2024-10-11
AI Technical Summary
The preparation methods of existing porous hollow ternary metal phosphide electrode materials are complicated, resulting in long production cycles and limiting the application of the materials.
The mixed solvent-assisted etching method was used to in-situ convert Co-MOF into CoNiMn-OH hollow nanosheet arrays, and the porous hollow ternary metal phosphide CoNiMn-P nanosheets were synthesized through the atmosphere phosphating method. By adjusting the mixed solvent concentration and phosphating temperature to control the morphology and structure of the product, simplifying the preparation process.
Efficient preparation of porous hollow CoNiMn-P nanosheet electrode materials was achieved, providing more active sites, improving charge transfer speed and mechanical stability, and showing excellent electrochemical performance and high specific capacity.
Smart Images

Figure CN118762936A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of electrochemical energy storage, and specifically relates to a preparation method of a porous hollow ternary metal phosphide CoNiMn-P nanosheet electrode material and a nickel-cobalt-manganese synergistic energy storage mechanism. Background Art
[0002] In the field of energy storage and conversion, the development of electrode materials has always been one of the research hotspots. With the growing demand for renewable energy, how to improve the performance of energy storage devices such as supercapacitors has become a key issue. In recent years, porous nanomaterials have attracted widespread attention due to their high specific surface area and excellent electrochemical properties. Among them, ternary metal phosphides have attracted much attention due to their superior performance compared to single and binary metal phosphides, while metal phosphides with porous hollow structures have shown great application potential due to their unique structure and excellent conductivity. For example, Lei et al. reported high-capacity and high-energy-density Zn-Ni-Co-P phosphide nanowire arrays grown on nickel foam. The electrode has a high charge-discharge rate of 10 A·g -1 The following shows 1111 C·g -1 The capacity retention rate after 10,000 cycles is 92.68%. Saleh et al. used electrodeposition and low temperature PH 3 Ternary metal manganese nickel alloy-cobalt phosphide (MNCPs) was synthesized by plasma to improve the electrochemical performance. -1 When the temperature is 1690.0 C·g -1 It can be seen that the multi-metal phosphide material has a higher specific capacity and exhibits metallic properties and high conductivity.
[0003] Materials Today Energy 34(2023)101287 Fe-Ni-Co-P nanoneedles were coated on reduced graphene oxide (rGO) (Fe-Ni-Co-P / rGO) using atomic layer deposition technology. The synergistic effect between the large specific surface area of rGO and the high specific capacity of TMP improves the electrode reaction kinetics by fully exposing the active sites of Fe-Ni-Co-P / rGO and shortening the ion / electron transport path. However, the preparation method of this electrode material is relatively complicated and requires multiple steps to complete, which usually leads to a long sample preparation cycle, limiting the production and application of electrode materials.
[0004] In the synthesized porous hollow electrode materials, the mixed solvent-assisted etching method has significant advantages in the preparation of nanomaterials. It can accurately control the surface morphology and structure during the etching process, while reducing local unevenness during the etching process. The material maintains a stable structure with Co-MOF as the skeleton. The atmosphere phosphating method is carried out under a controlled environment, which can effectively avoid the introduction of impurities. The prepared phosphide nanomaterials have high purity and quality. The two-dimensional nanosheet array material grown in situ on a conductive substrate avoids the dead volume and high resistance of the powder electrode material. The chemical composition of the phosphide can be precisely controlled by adjusting the atmosphere and reaction temperature to obtain materials with specific properties, thereby significantly improving the material preparation efficiency and shortening the production cycle. Summary of the invention
[0005] The present invention adopts a mixed solvent assisted etching method to in-situ transform Co-MOF into a CoNiMn-OH hollow nanosheet array, and then synthesizes a porous hollow ternary metal phosphide CoNiMn-P nanosheet by an atmosphere phosphating method. The morphology and structure of the product can be controlled by changing the concentration of the mixed solvent and the phosphating temperature. The structure of the porous hollow CoNiMn-P is slightly curled on the basis of the hollow triangular nanosheet CC / CoNiMn-OH, and a certain connection is formed between the nanosheets. Its unique structure can provide more active sites, which not only helps the rapid transfer of charges, but also improves the mechanical stability of the electrode, thereby showing excellent electrochemical performance.
[0006] In order to solve the above technical problems, the present invention adopts the following technical method: Based on a method for preparing a porous hollow ternary metal phosphide CoNiMn-P nanosheet electrode material, the present invention first prepares a Co-MOF nanosheet array grown in situ on a carbon cloth (CC) at room temperature, puts the CC / Co-MOF into a mixed solvent of N,N-dimethylformamide and anhydrous ethanol, and then adds 10 mL of 1.4 mM Ni(NO 3 ) 2 6H 2 O and 1.4 mM MnCl 2 ·4H 2 O solution, and then transferred into an 80 mL high-pressure reactor and reacted at 90 °C for 2 h to obtain hollow CoNiMn-OH nanosheets grown on carbon cloth. 2 PO 2 ·H 2 O was placed upstream of the tube furnace, and the prepared hollow CoNiMn-OH nanosheets grown on carbon cloth were placed downstream of the tube furnace and mixed with NaH 2 PO 2 ·H2 O is 3 cm away, at N 2 The temperature was raised to 500 °C at a heating rate of 2 °C / min under atmospheric conditions and maintained for 2 h to obtain CoNiMn-P porous hollow nanosheet electrode material grown on carbon cloth.
[0007] The obtained CC / CoNiMn-P nanosheet electrode material is prepared on N 2 The process is carried out within a controllable range, avoiding the introduction of impurities. The average thickness of CC / CoNiMn-P nanosheets is 300-350 nm, and the quality of the prepared electrode is controlled to be 1.8-2.2 mg. The controllable atmosphere phosphating method plays a vital role in the quality of the electrode, avoiding the cumbersome preparation method. Due to the above advantages, the electrode has a current density of 1 A·g -1 When the single electrode specific capacity reaches 2247.2 F·g -1 . BRIEF DESCRIPTION OF THE DRAWINGS
[0008] Figure 1 3 is the XRD curve of the CC / CoNiMn-P nanosheet electrode material prepared in Example 1.
[0009] Figure 2 This is a scanning electron microscope image of the CC / CoNiMn-OH nanosheet electrode material prepared in Example 1.
[0010] Figure 3 This is a scanning electron microscope image of the CC / CoNiMn-P nanosheet electrode material prepared in Example 1.
[0011] Figure 4 This is the cyclic voltammetry curve of the CC / CoNiMn-P nanosheet electrode material prepared in Example 1.
[0012] Figure 5 1 is the charge and discharge curve of the CC / CoNiMn-P nanosheet electrode material prepared in Example 1. DETAILED DESCRIPTION
[0013] The technical scheme and effects of the present invention are further described below in conjunction with the embodiments. However, the specific methods, formulations and descriptions used are not intended to limit the present invention.
[0014] Example 1: First, a Co-MOF nanosheet array grown in situ on carbon cloth (CC) was prepared at room temperature. CC / Co-MOF was placed in a mixed solvent of N,N-dimethylformamide and anhydrous ethanol. After ultrasonic-assisted etching for 10 min, 10 mL of 1.4 mM Ni(NO 3 ) 2 6H 2O and 1.4 mM MnCl 2 ·4H 2 O solution, and then transferred into an 80 mL high-pressure reactor and reacted at 90 °C for 2 h to obtain hollow CoNiMn-OH nanosheets grown on carbon cloth. 2 PO 2 ·H 2 O was placed upstream of the tube furnace, and the prepared hollow CoNiMn-OH nanosheets grown on carbon cloth were placed downstream of the tube furnace and mixed with NaH 2 PO 2 ·H 2 O is 3 cm away, at N 2 The temperature was raised to 500°C at a heating rate of 2°C / min under atmospheric conditions and maintained for 2 h to obtain CoNiMn-P porous hollow nanosheet electrode material grown on carbon cloth.
[0015] Example 2: First, a Co-MOF nanosheet array grown in situ on carbon cloth (CC) was prepared at room temperature. CC / Co-MOF was placed in a mixed solvent of N,N-dimethylformamide and anhydrous ethanol. After ultrasonic-assisted etching for 10 min, 5 mL of 0.7 mM Ni(NO 3 ) 2 6H 2 O and 0.7 mM MnCl 2 ·4H 2 O solution, and then transferred into an 80 mL high-pressure reactor and reacted at 90 °C for 2 h to obtain hollow CoNiMn-OH nanosheets grown on carbon cloth. 2 PO 2 ·H 2 O was placed upstream of the tube furnace, and the prepared hollow CoNiMn-OH nanosheets grown on carbon cloth were placed downstream of the tube furnace and mixed with NaH 2 PO 2 ·H 2 O is 3 cm away, at N 2 The temperature was raised to 500°C at a heating rate of 2°C / min under atmospheric conditions and maintained for 2 h to obtain CoNiMn-P porous hollow nanosheet electrode material grown on carbon cloth.
[0016] Example 3: First, a Co-MOF nanosheet array grown in situ on carbon cloth (CC) was prepared at room temperature. CC / Co-MOF was placed in a mixed solvent of N,N-dimethylformamide and anhydrous ethanol. After ultrasonic-assisted etching for 10 min, 15 mL of 2.1 mM Ni(NO 3 ) 2 6H2 O and 2.1 mM MnCl 2 ·4H 2 O solution, and then transferred into an 80 mL high-pressure reactor and reacted at 90 °C for 2 h to obtain hollow CoNiMn-OH nanosheets grown on carbon cloth. 2 PO 2 ·H 2 O was placed upstream of the tube furnace, and the prepared hollow CoNiMn-OH nanosheets grown on carbon cloth were placed downstream of the tube furnace and mixed with NaH 2 PO 2 ·H 2 O is 3 cm away, at N 2 The temperature was raised to 500°C at a heating rate of 2°C / min under atmospheric conditions and maintained for 2 h to obtain CoNiMn-P porous hollow nanosheet electrode material grown on carbon cloth.
[0017] Example 4: First, a Co-MOF nanosheet array grown in situ on carbon cloth (CC) was prepared at room temperature. CC / Co-MOF was placed in a mixed solvent of N,N-dimethylformamide and anhydrous ethanol. After ultrasonic-assisted etching for 10 min, 10 mL of 1.4 mM Ni(NO 3 ) 2 6H 2 O and 1.4 mM MnCl 2 ·4H 2 O solution, and then transferred into an 80 mL high-pressure reactor and reacted at 90 °C for 2 h to obtain hollow CoNiMn-OH nanosheets grown on carbon cloth. 2 PO 2 ·H 2 O was placed upstream of the tube furnace, and the prepared hollow CoNiMn-OH nanosheets grown on carbon cloth were placed downstream of the tube furnace and mixed with NaH 2 PO 2 ·H 2 O is 3 cm away, at N 2 The temperature was raised to 450°C at a heating rate of 2°C / min under atmospheric conditions and maintained for 2 h to obtain CoNiMn-P porous hollow nanosheet electrode material grown on carbon cloth.
[0018] Example 5: First, a Co-MOF nanosheet array grown in situ on carbon cloth (CC) was prepared at room temperature. CC / Co-MOF was placed in a mixed solvent of N,N-dimethylformamide and anhydrous ethanol. After ultrasonic-assisted etching for 10 min, 10 mL of 1.4 mM Ni(NO 3 )2 6H 2 O and 1.4 mM MnCl 2 ·4H 2 O solution, and then transferred into an 80 mL high-pressure reactor and reacted at 90 °C for 2 h to obtain hollow CoNiMn-OH nanosheets grown on carbon cloth. 2 PO 2 ·H 2 O was placed upstream of the tube furnace, and the prepared hollow CoNiMn-OH nanosheets grown on carbon cloth were placed downstream of the tube furnace and mixed with NaH 2 PO 2 ·H 2 O is 5 cm away, at N 2 The temperature was raised to 550°C at a heating rate of 2°C / min under atmospheric conditions and maintained for 2 h to obtain CoNiMn-P porous hollow nanosheet electrode material grown on carbon cloth.
[0019] Example 6: First, a Co-MOF nanosheet array grown in situ on carbon cloth (CC) was prepared at room temperature. CC / Co-MOF was placed in a mixed solvent of N,N-dimethylformamide and anhydrous ethanol. After ultrasonic-assisted etching for 10 min, 10 mL of 1.4 mM Ni(NO 3 ) 2 6H 2 O and 1.4 mM MnCl 2 ·4H 2 O solution, and then transferred into an 80 mL high pressure reactor and reacted at 90 °C for 2 h to obtain hollow CoNiMn-OH nanosheets grown on carbon cloth. 2 PO 2 ·H 2 O was placed upstream of the tube furnace, and the prepared hollow CoNiMn-OH nanosheets grown on carbon cloth were placed downstream of the tube furnace and mixed with NaH 2 PO 2 ·H 2 O is 7 cm away, at N 2 The temperature was raised to 650°C at a heating rate of 2°C / min under atmospheric conditions and maintained for 2 h to obtain CoNiMn-P porous hollow nanosheet electrode material grown on carbon cloth.
[0020] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.
Claims
1. Ternary metal phosphide CoNiMn-P porous hollow nanosheet electrode material, It is characterized in that The skeleton of the CoNiMn-P nanoelectrode material is derived from Co-MOF nanosheets grown in situ on carbon cloth and etched hollow structure CoNiMn-OH nanosheets. The phosphated CoNiMn-P electrode material is in the shape of a thin-walled hollow porous triangle as a whole.
2. Preparation method of ternary metal phosphide CoNiMn-P porous hollow nanosheet electrode material, It is characterized in that The process comprises the following steps: firstly, preparing an in-situ grown Co-MOF nanosheet array on carbon cloth (CC) at room temperature, placing CC / Co-MOF in a mixed solvent of N,N-dimethylformamide and anhydrous ethanol, and then adding 5-15 mL of 0.7-2.1 mM Ni(NO 3 ) 2 6H 2 O and 0.7-2.1 mM MnCl 2 ·4H 2 O solution, and then transferred into an 80 mL high-pressure reactor and reacted at 90 °C for 2 h to obtain hollow CoNiMn-OH nanosheets grown on carbon cloth. 2 PO 2 ·H 2 O was placed upstream of the tube furnace, and the prepared hollow CoNiMn-OH nanosheets grown on carbon cloth were placed downstream of the tube furnace and mixed with NaH 2 PO 2 ·H 2 O is 3-7 cm away, at N 2 Under atmospheric conditions, the temperature was raised to 450-650 °C at a heating rate of 2 °C / min and maintained for 2 h to obtain CoNiMn-P porous hollow nanosheet electrode material grown on carbon cloth. CC / CoNiMn-P retained the triangular morphology relative to CC / CoNiMn-OH, but its surface became rough, which increased the rapid charge transfer. At the same time, the phosphated electrode material combined the synergistic effect of the three transition metals, effectively solving the problem of poor cycle stability of phosphides.