Preparation method and application of silicon-based lithium niobate ferroelectric single crystal film vibration sensor
By combining PECVD, magnetron sputtering and photolithography processes in the preparation of silicon-based lithium niobate ferroelectric single crystal thin film vibration sensors, the temperature and chemical stability problems of traditional sensors in high radiation environments are solved, and the sensor is realized in Stable operation in space orbit and high-frequency micro-vibration measurement capabilities.
Patent Information
- Application Number
- CN202411237493.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-05
- Publication Date
- 2024-10-11
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing piezoelectric vibration sensors have poor temperature stability and chemical stability in high radiation and harsh environments, and cannot operate stably in space orbit for a long time. In particular, there is a risk of performance degradation and failure when processing vibration signals.
The preparation method of the silicon-based lithium niobate ferroelectric single crystal thin film vibration sensor is adopted. The SiO2 thin film layer is deposited by the PECVD method, the metal electrode is processed by the magnetron sputtering process, the LiNbO3 piezoelectric layer and Si substrate are etched by the photolithography process, and combined with the ion beam Etching and reactive ion etching processes form the structure of the peripheral frame, cantilever beam and mass block to achieve efficient piezoelectric conversion.
The sensor maintains good piezoelectric characteristics and radiation resistance in extreme environments. It is suitable for high-frequency micro-vibration testing and space exploration. It provides stable vibration signal monitoring and fault diagnosis capabilities, reduces costs and improves yield.
Smart Images

Figure CN118765154A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of semiconductor device processing and manufacturing, and in particular to a preparation method and application of a silicon-based lithium niobate ferroelectric single crystal thin film vibration sensor. Background Art
[0002] The progress of science and technology in the 21st century has made deep space exploration an important field, which is directly related to the space resources needed for the sustainable development of mankind in the future. As people's exploration of space continues to deepen, the performance requirements of electronic devices in aerospace systems are also increasing. In space, factors such as high-energy particles, cosmic rays and radio frequency interference may cause damage to the electronic components of spacecraft, affecting their reliability and life. These radiation environments may cause satellites to be affected by total dose effects, single particle effects and charge and discharge effects. Therefore, micro-nano sensor devices will face the challenge of high-intensity radiation, including short-wavelength, high-energy electromagnetic radiation, especially gamma rays and X-rays, as well as high-energy particles. This may cause damage to spacecraft materials, devices and structures, resulting in performance degradation or even failure. The harsh space environment may make the performance of traditional silicon-based materials unstable, and devices that have not been treated with radiation resistance cannot obtain high-resolution sensing signals through in-situ measurement methods. At present, the failure and false alarm of environmental parameter sensor devices have become common technical problems in the field of deep space exploration in various countries. The technical barriers of micro-nano sensor devices in irradiated environments urgently need to be solved.
[0003] Common types of vibration sensors today include piezoresistive, capacitive, optical, and piezoelectric. Piezoresistive vibration sensors have simple structures and processing processes, but low sensitivity and high temperature sensitivity; capacitive vibration sensors have good DC performance and high sensitivity, but are easily interfered by electromagnetic waves; optical vibration sensors are resistant to electromagnetic interference noise and have high sensitivity, but are difficult to integrate with output circuits, and the cost of test equipment is very high; piezoelectric vibration sensors have high sensitivity, large dynamic range, and are durable, but have poor DC response. In order to adapt to the space exploration environment, it is necessary to select functional electronic components that can operate stably on orbit for a long time. In particular, for situations where vibration signals within a certain frequency range need to be processed, priority should be given to devices that are passive, miniaturized, compatible with integrated circuit chips, and able to withstand harsh environments such as space radiation and large-scale temperature fluctuations. In comparison, piezoelectric vibration sensors can better meet the above requirements.
[0004] Common piezoelectric materials include lead zirconate titanate (PZT), lead zinc niobate (PZN), lithium niobate (LiNbO 3 ), barium titanate (BaTiO 3) and polyvinylidene fluoride (PVDF). Piezoelectric materials realize the mutual conversion of electrical energy and mechanical energy based on the piezoelectric effect. When mechanical pressure or stress is applied to a piezoelectric material, the material will produce polarization, thereby generating a voltage on its surface. This phenomenon is called the positive piezoelectric effect. In contrast to the positive piezoelectric effect, the inverse piezoelectric effect means that when an electric field is applied to a piezoelectric material, the material will undergo mechanical deformation, that is, mechanical strain will be generated along the direction of the electric field. As a commonly used piezoelectric material, lithium niobate has many advantages that make it popular. First, it has a high piezoelectric coefficient, which means that it has high efficiency when converting mechanical energy into electrical energy or vice versa. Secondly, lithium niobate exhibits good temperature stability and chemical stability, which enables it to maintain stable performance in various harsh environmental conditions, especially low temperature and irradiation environments, and has a long service life. In addition, lithium niobate is usually prepared in the form of a single crystal with a uniform structure and performance distribution, which enables lithium niobate to achieve high-precision piezoelectric applications. Summary of the invention
[0005] In order to solve the problem that the existing piezoelectric vibration sensors have poor temperature stability and chemical stability and cannot adapt to use in harsh environmental conditions such as space radiation, the present invention provides a preparation method and application of a silicon-based lithium niobate ferroelectric single crystal thin film vibration sensor.
[0006] The present invention is realized by the following technical scheme: a method for preparing a silicon-based lithium niobate ferroelectric single crystal thin film vibration sensor, wherein the structure of the prepared silicon-based lithium niobate ferroelectric single crystal thin film vibration sensor is as follows: a peripheral frame, a cantilever beam and a mass block, wherein the peripheral frame is rectangular in top view, and the layer structure of the peripheral frame is as follows from bottom to top: a first SiO 2 Thin film layer, Si substrate, second SiO 2 Thin film layer, LiNbO 3 The piezoelectric layer, the inner side of the short side of the outer frame is connected to one end of the cantilever beam, and the other end of the cantilever beam is connected to the mass block, the mass block is square in top view, the cantilever beam is rectangular in top view, and the side length of the mass block is greater than the width of the cantilever beam. The layer structure of the mass block and the cantilever beam is the same, and the layer structure from bottom to top is: Si substrate, second SiO 2 Thin film layer, LiNbO 3 The piezoelectric layer, the top surface of the cantilever beam is also provided with a metal electrode I and a metal electrode II, wherein one end of the metal electrode I is located at the inner edge of the outer frame, and the other end is directly opposite to the metal electrode II, and the other end of the metal electrode II extends to the top of the mass block; the preparation method comprises the following steps: Step 1: Si-LiNbO 3 The bonded wafer is cleaned and the Si-LiNbO 3 The first SiO2 is deposited on the back of the bond wafer using PECVD 2Thin film layer, used for hard mask of deep silicon process; Step 2: Processing metal electrodes on the upper surface of the product in step 1 by using magnetron sputtering process; Step 3: Use a photolithography process to mark the pattern of the metal electrode on the product of step 2, and use an ion beam etching process to etch the metal electrode to etch out the metal electrode I and metal electrode II on the upper surface; Step 4: Use photolithography to mark the cantilever beam, mass block and peripheral frame of the product in step 3, and use ion beam etching to complete the LiNbO 3 The piezoelectric layer is etched and the second SiO 2 Etching of thin film layers; Step 5: According to the pattern marked in step 4, the pattern mark is deepened by using a photolithography process, and a deep silicon etcher is used to complete the etching of the front Si substrate by using a deep reactive ion etching process; Step 6: Use photolithography to mark the pattern on the back of the product in step 5, and etch the first SiO2 on the back by anisotropic oxidation etching process. 2 A thin film layer is formed to form a cavity; a deep silicon etcher is used to etch the back Si substrate using a deep reactive ion etching process to release the device, thereby forming an external frame, a cantilever beam and a mass block. The silicon-based lithium niobate ferroelectric single crystal thin film vibration sensor is completed. The prepared silicon-based lithium niobate ferroelectric single crystal thin film vibration sensor is an improved piezoelectric vibration sensor.
[0007] Further, in step 1, a first SiO 2 The growth rate of the thin film is 0.5 μm / h; the first SiO 2 The cleaning process before the thin film layer is as follows: 3 The bonding wafer is acid-washed, alkaline-washed and rinsed with deionized water several times, and blown dry with nitrogen to make the surface clean.
[0008] Further, in step 2, in LiNbO 3 A 20nm thick Cr layer and a 200nm thick Au layer are grown on the surface of the piezoelectric layer by magnetron sputtering process.
[0009] Further, in step 3, during the photolithography process, Si-LiNbO 3 The bond wafer surface was spin-coated with AZ 6130 positive photoresist. The mask used was a positive plate. The pattern shape matched the shape of the metal electrodes I and II on the top of the vibration sensor. The parameters used were: 3000r / min and 4000r / min were used for photoresist spin coating, and pre-baking was performed on a 100℃ baking table for 1 minute. The exposure dose was 200mJ / cm2 , developed with a developer formed by AZ 400K and water in a volume ratio of 1:4 for 28 seconds, and post-baked on a 120°C baking table for 15 minutes; the ion beam etching process used an ion beam etcher, set the energy of Ar ions to 500eV, the gas flux to 5, and the ion beam etching rate to 25nm / min.
[0010] Further, in step 4, in Si-LiNbO 3 The bond wafer surface was spin-coated with AZ 4620 positive photoresist. The mask used was a positive mask. The pattern shape matched the shape of the vibration sensor cantilever beam, mass block and peripheral frame. The low speed was set to 1000r / min for 120s and the high speed was set to 3000r / min for 5s. The surface was pre-baked on a 100℃ baking table for 2min, followed by photolithography. The exposure dose was set to 400mJ / cm 2 , developed in a developer solution of AZ 400K and water in a volume ratio of 1:3 for 71 seconds, and then used an oxygen plasma glue process to remove the residual glue on the surface, and then used a 120°C baking table for 15 minutes. 3 The bonded wafer was fixed on the tray of the ion beam etcher, the Ar flux was set to 5, the etching rate was set to 1.25 μm / h, and the LiNbO 3 Etching of the piezoelectric layer. Etching was stopped until a colored halo appeared. The subsequent reactive ion etching process used an RIE etcher, and the gas introduced was SF 4 , the etching rate is 16.7nm / min.
[0011] Further, in step 5, during the photolithography process, the mask in step 4 is used to form a Si-LiNbO 3 The front side of the bond wafer was sprayed with AZ 4620 positive photoresist for 4 cycles, and pre-baked for 150s on a 100℃ baking table with an exposure dose of 400mJ / cm 2 , developed with a developer formed by AZ 400K and water in a volume ratio of 1:3 for 107 seconds, and after patterning, an oxygen plasma degumming machine was used to remove the floating glue remaining on the surface; finally, post-baking was performed on a 120°C baking table for 15 minutes; a deep silicon etcher was used to etch the Si substrate to a thickness of 70μm, 50~55loops were etched, and the etching rate was 1.4μm / loop.
[0012] Furthermore, in step 6, during the photolithography process, the mask used is a positive mask, the pattern shape matches the shape of the outer frame of the vibration sensor, AZ 4620 photoresist is sprayed for 8 cycles, and the photoresist is baked on a 100°C baking table for 270 seconds, and the exposure dose is set to 800mJ / cm 2, developed for 120 seconds in a developer solution composed of AZ 400K and water in a volume ratio of 1:2. If the development is insufficient, the development time is extended. The residual floating glue is removed using an oxygen plasma degumming machine. Then, it is post-baked on a 100°C baking table for 30 minutes. The Si-LiNbO 3 The bonded wafer was hardened on a 100℃ baking table for 1 hour; the first SiO 2 The thin film layer was patterned with an etching rate of 350nm / min and an etching time of 342s. The Si substrate was etched using a deep silicon etcher with an etching thickness of 423μm and an etching rate of 1.2μm / loop until all devices were released.
[0013] Preferably, in step 3 to step 6, cleaning and nitrogen drying are performed after each step is completed to ensure that there is no glue, water, or oil when entering the next step, and the cleaning reagent solution used is concentrated H 2 SO 4 , H 2 O 2 Solution, NH 4 One or more of (OH) solution, acetone, anhydrous ethanol and deionized water.
[0014] After the above steps, the prepared silicon-based lithium niobate ferroelectric single crystal thin film vibration sensor has a Si substrate thickness of 493 μm for the outer frame, a Si substrate thickness of 70 μm for the mass block and the cantilever beam, and a second SiO 2 The thickness of the film layer is 2μm; LiNbO 3 The thickness of the piezoelectric layer is 5 μm; the top view size of the cantilever beam is 1860 μm in length and 470 μm in width; and the top view side length of the mass block is 600 μm.
[0015] The present invention discloses a method for preparing a silicon-based lithium niobate ferroelectric single crystal thin film vibration sensor, by Si-LiNbO 3 The bonding wafer is formed by using magnetron sputtering, photolithography and ion beam etching to prepare the required marking pattern and metal electrode on its upper surface; and the LiNbO 3 Piezoelectric layer and second SiO 2 Preparation of thin film layer; Use deep silicon etcher to complete the front Si substrate etching using deep reactive ion etching process; Finally, on Si-LiNbO 3After the back of the bonding sheet is subjected to the photolithography process, an AOE etcher is used to etch the back cavity, and a deep silicon etcher is used to complete the preparation and release of the device. The silicon-based lithium niobate ferroelectric single crystal thin film vibration sensor prepared by this method has a cantilever beam as the main functional element. It is processed and prepared based on the MEMS process. Since lithium niobate can maintain good piezoelectric properties in a wide temperature range and has good radiation resistance. Therefore, this silicon-based lithium niobate ferroelectric single crystal thin film vibration sensor has potential application value for equipment fault diagnosis and vibration signal monitoring in extreme environments; the sensor can be well used in high-frequency micro-vibration testing, space exploration or electron irradiation.
[0016] Compared with the prior art, the present invention has the following beneficial effects: the preparation method and application of a silicon-based lithium niobate ferroelectric single crystal thin film vibration sensor provided by the present invention, the prepared silicon-based lithium niobate ferroelectric single crystal thin film vibration sensor is an improved piezoelectric vibration sensor, which has a simple structure, is easy to integrate and has a low cost, and can meet the test in an irradiation environment. The present invention is processed and prepared based on the MEMS process. On the basis of compatibility, a deep silicon etcher is used to etch the Si substrate, thereby improving the yield of the process. The preparation method of the present invention is reasonably designed, the manufacturing process is simple, and the yield is high. As a passive and irradiation-resistant detection device, this silicon-based lithium niobate ferroelectric single crystal thin film vibration sensor is conducive to long-distance signal transmission and is suitable for high-frequency micro-vibration test environments. It provides powerful assistance for vibration information collection and equipment abnormality detection in extreme environments such as low temperature and irradiation. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1 The present invention is a flow chart of the preparation method of the silicon-based lithium niobate ferroelectric single crystal thin film vibration sensor.
[0018] Figure 2 The present invention is a process flow diagram of the silicon-based lithium niobate ferroelectric single crystal thin film vibration sensor.
[0019] Figure 3 It is a schematic diagram of the structure of the silicon-based lithium niobate ferroelectric single crystal thin film vibration sensor of the present invention.
[0020] Figure 4 for Figure 3 Cross-sectional view at DD in the middle.
[0021] Figure 5 The injection rates of the silicon-based lithium niobate ferroelectric single crystal thin film vibration sensor before and after irradiation are 1.37E10 e / cm²·s, 4.11E10 e / cm²·s and 1.0117E11 e / cm²·s LiNbO 3 XRD pattern of the piezoelectric layer.
[0022] Figure 6 The frequency response curves of the silicon-based lithium niobate ferroelectric single crystal thin film vibration sensor of the present invention before and after irradiation.
[0023] Figure 7 The graphs are curves showing the change of output charge with acceleration before and after irradiation of the silicon-based lithium niobate ferroelectric single crystal thin film vibration sensor of the present invention.
[0024] Figure 8 The invention discloses a sinusoidal wave variation law of the output charge of the silicon-based lithium niobate ferroelectric single crystal thin film vibration sensor before and after irradiation.
[0025] The markings in the figure are as follows: 1-peripheral frame, 2-cantilever beam, 3-mass block, 41-metal electrode I, 42-metal electrode II. DETAILED DESCRIPTION
[0026] The present invention is further described below in conjunction with specific embodiments.
[0027] A method for preparing a silicon-based lithium niobate ferroelectric single crystal thin film vibration sensor. The structure of the prepared silicon-based lithium niobate ferroelectric single crystal thin film vibration sensor is as follows: Figure 3 and Figure 4 As shown in the figure: the structure of the prepared silicon-based lithium niobate ferroelectric single crystal thin film vibration sensor is as follows: it includes an outer frame 1, a cantilever beam 2 and a mass block 3. The outer frame 1 is rectangular when viewed from above. The layer structure of the outer frame 1 is as follows from bottom to top: the first SiO 2 Thin film layer, Si substrate, second SiO 2 Thin film layer, LiNbO 3 The inner side of the short side of the outer frame 1 is connected to one end of the cantilever beam 2, and the other end of the cantilever beam 2 is connected to the mass block 3. The mass block 3 is square in top view, and the cantilever beam 2 is rectangular in top view. The side length of the mass block 3 is greater than the width of the cantilever beam 2. The layer structure of the mass block 3 and the cantilever beam 2 is the same, and the layer structure from bottom to top is: Si substrate, second SiO 2 Thin film layer, LiNbO 3 The piezoelectric layer, the top surface of the cantilever beam 2 is also provided with a metal electrode I41 and a metal electrode II42, wherein one end of the metal electrode I41 is located at the inner edge of the outer frame 1, and the other end is directly opposite to the metal electrode II42, and the other end of the metal electrode II42 extends to the top of the mass block 3; the preparation method flow is as follows Figure 1 and Figure 2 As shown, the following steps are included: Step 1: Si-LiNbO 3 The bonded wafer is cleaned and the Si-LiNbO 3 The first SiO is deposited on the back of the bond wafer using PECVD 2Thin film layer, used for deep silicon process hard mask; specifically: 1-1: Si-LiNbO 3 The bond pad is placed in concentrated H 2 SO 4 The solution was pickled at 150°C and then washed with H 2 O 2 and NH 4 The mixed solution of (OH) was alkaline washed at 80°C, followed by several deionized water washes to remove residual acid and alkali substances on the surface and the residual water stains on the surface were blown dry with a nitrogen gun; 1-2: In Si-LiNbO 3 The back of the bond wafer is deposited with a 2 μm thick first SiO 2 Thin film layer, the growth rate of the film is 0.5 μm / h; 1-3: For Si-LiNbO 3 The bonding wafer was cleaned with acetone, anhydrous ethanol and deionized water, and the residual water stains on the surface were blown dry with a nitrogen gun.
[0028] Step 2: Use magnetron sputtering technology to process metal electrodes on the upper surface of the product in step 1; specifically: 2-1: In LiNbO 3 A 20nm thick Cr layer and a 200nm thick Au layer are grown on the surface of the piezoelectric layer by magnetron sputtering. The Cr layer is used as an adhesion layer to enhance the LiNbO 3 The adhesion between the piezoelectric layer and the Au layer facilitates charge collection.
[0029] Step 3: Use a photolithography process to mark the pattern of the metal electrode on the product of step 2, and use an ion beam etching process to etch the metal electrode to etch out the metal electrode I 41 and the metal electrode II 42 on the upper surface; specifically: 3-1: Using a mask containing a marking pattern and a metal electrode pattern, first 3 The bond wafer surface was spin-coated with AZ 6130 positive photoresist. The mask used was a positive plate. The pattern shape matched the shape of the metal electrode Ⅰ41 and the metal electrode Ⅱ42 on the top of the vibration sensor. The high speed was 3000r / min for 30s, and then 4000r / min for 5s. Then, it was pre-baked on a 100℃ baking table for 1min. The photolithography process was performed using EVG 620, and the exposure dose was 200mJ / cm 2 After the exposure is completed, the photoresist is developed in a solution of AZ 400K and water in a volume ratio of 1:4 for about 28 seconds to complete the preparation of the photolithography pattern, and the residual glue on the surface is removed by oxygen plasma. The photoresist is post-baked on a baking table at 120°C for 15 minutes to evaporate the water in the photoresist. 3-2: Si-LiNbO 3 The bonded wafer is pasted on the tray of the ion beam etcher, the energy of the Ar ions is set to 500eV, the gas flux is set to 5, and the ion beam etching rate is 25nm / min (it takes about 8min to etch). 3-3: Etching of Si-LiNbO with acetone, anhydrous ethanol and deionized water 3 The bonding wafer is cleaned and the residual water stains on the surface are blown dry with a nitrogen gun.
[0030] Step 4: Use photolithography to mark the cantilever beam 2, mass block 3 and peripheral frame 1 of the product in step 3, and use ion beam etching to complete the LiNbO 3 The piezoelectric layer is etched and the second SiO 2 Etching of thin film layers; specifically: 4-1: First in Si-LiNbO 3 The bonding wafer surface was spin-coated with AZ 4620 positive photoresist. The mask used was a positive mask. The pattern shape matched the shape of the vibration sensor cantilever beam 2, the mass block 3 and the peripheral frame 1. The low speed was set to 1000r / min for 120s, and the high speed was set to 3000r / min for 5s. The surface was pre-baked on a 100℃ baking table for 2min, and then the photolithography process was carried out. EVG 620 was used for the photolithography process, and the exposure dose was set to 400mJ / cm 2 , develop in a solution of AZ 400K and water in a volume ratio of 1:3 for about 71 seconds, use oxygen plasma glue process to remove the residual glue on the surface, and use a 120℃ drying table for 15 minutes to evaporate the surface moisture; 4-2: Si-LiNbO 3 The bonded wafer is fixed on the tray of the ion beam etcher, the etching rate is 1.25μm / h, the Ar flux is set to 5, and the etching is stopped until a colored halo appears; it takes about 4 hours to complete the etching of 5μm thickness. The machine is stopped every half an hour to observe the etching situation. First, the temperature difference between the low temperature tray and the high temperature generated by the high energy ion bombardment during the etching process is large, which will cause LiNbO 3 The chip breaks due to uneven heating, and secondly, it prevents the high temperature ion bombardment from causing glue paste; 4-3: After step 4-2, Si-LiNbO 3 The bonded wafer is subjected to reactive ion etching process using RIE etcher and SF 4 Gas, etching rate is 16.7nm / min; 4-4: After etching, Si-LiNbO 3The bonding wafers were placed in acetone, anhydrous ethanol and deionized water for degumming and cleaning, and the residual water stains on the surface were blown dry with a nitrogen gun; then the etching height was measured using a step profiler. Based on the above process operation, Si-LiNbO 3 The height difference between the bond pads is about 7μm (LiNbO 3 The thickness of the piezoelectric layer is 5 μm, and the second SiO 2 The thickness of the film layer is 2 μm).
[0031] Step 5: According to the pattern marked in step 4, the pattern mark is deepened by using a photolithography process, and a deep silicon etcher is used to complete the etching of the front Si substrate by using a deep reactive ion etching process; specifically: 5-1: During the photolithography process, use the mask in step 4 to 3 The front side of the bond wafer was sprayed with AZ4620 positive photoresist for 4 cycles, and then pre-baked on a 100℃ baking table for 150s, followed by photolithography. EVG 620 was used for photolithography, and the exposure dose was set to 400mJ / cm 2 , then developed in a solution of AZ 400K and water in a volume ratio of 1:3 for 107s, and after patterning, an oxygen plasma stripper was used to remove the floating glue remaining on the surface, and finally post-baked on a baking table at 120°C for 15min. After this step was completed, the thickness of the sprayed photoresist was measured using a step profiler and recorded; 5-2: The thickness of the Si substrate is 70 μm using a deep silicon etcher, which requires about 50 to 55 loops and an etching rate of 1.4 μm / loop; 5-3: Repeat the cleaning and drying work in step 4-4, and then use the step profiler to measure the Si-LiNbO 3 The height difference on the front side of the bonding wafer (the height difference should be as equal to 77μm as possible). If the height difference is less than 77μm, steps 5-1 and 5-2 need to be repeated until the etching height is approximately equal to 77μm.
[0032] Step 6: Use photolithography to mark the pattern on the back of the product in step 5, and etch the first SiO2 on the back by anisotropic oxidation etching process. 2 The thin film layer is formed into a cavity; a deep silicon etcher is used to etch the back Si substrate using a deep reactive ion etching process to complete the device release, thereby forming an external frame 1, a cantilever beam 2 and a mass block 3. The silicon-based lithium niobate ferroelectric single crystal thin film vibration sensor is prepared, specifically as follows: 6-1: During the photolithography process, the mask used is a positive plate, and the pattern shape matches the shape of the vibration sensor outer frame 1. 3The back of the bond wafer was sprayed with AZ 4620 photoresist for 8 cycles, followed by pre-baking for 270 seconds on a 100°C baking table. The lithography process was performed using EVG 620, with an exposure dose of 800 mJ / cm 2 , develop for 120 seconds in a developer with a volume ratio of AZ 400K to water of 1:2, observe whether the pattern is graphical, if the development is insufficient, extend the development time appropriately, use an oxygen plasma glue machine to remove the floating glue remaining on the surface, and bake on a 100℃ drying table for 30 minutes; 6-2: Using AZ 4620 photoresist to 3 The etched area on the front side of the bond wafer is filled and dried on a 100°C baking table for 1 hour, which is the hardening process; 6-3: Use AOE etcher to complete the first layer of SiO on the back 2 For patterning of the thin film layer, the etching rate is 350nm / min, and it takes 342s to etch; 6-4: Use a deep silicon etcher to etch the Si substrate to a thickness of 423 μm. The etching process should be slow and the etching rate is about 1.2 μm / loop until all devices are released; 6-5: Use anhydrous ethanol to clean the device and complete the device preparation process.
[0033] Figure 2 The process of preparing the silicon-based lithium niobate ferroelectric single crystal thin film vibration sensor in the embodiment of the present application is to deposit a 2 μm thick first SiO 2 The thin film layer is prepared by magnetron sputtering, photolithography and ion beam etching processes to prepare the required marking pattern and metal electrode, and the LiNbO 3 Piezoelectric layer and second SiO 2 Etching of the thin film layer; using a deep silicon etcher to etch the front Si substrate. Finally, etching the back cavity and using a deep silicon etcher to release the device. Figure 3 Schematic diagram of the structure of the silicon-based lithium niobate ferroelectric single crystal thin film vibration sensor in this application. The prepared silicon-based lithium niobate ferroelectric single crystal thin film vibration sensor has a Si substrate thickness of 493 μm for the peripheral frame 1; a Si substrate thickness of 70 μm for the mass block 3 and the cantilever beam 2; and a second SiO 2 The thickness of the film layer is 2μm; LiNbO 3 The thickness of the piezoelectric layer is 5 μm; the top view size of the cantilever beam 2 is 1860 μm in length and 470 μm in width; and the side length of the mass block 3 is 600 μm.
[0034] This embodiment tests the prepared silicon-based lithium niobate ferroelectric single crystal thin film vibration sensor, and the test process is as follows: Step S1: Use an electron accelerator to irradiate the prepared device. In this embodiment, the total irradiation dose is set to 2MGy. Then different injection rates are set: 1.37E10 e / cm²·s, 4.11E10 e / cm²·s and 1.0117E11 e / cm²·s. The irradiation time is shortened as the injection rate increases, and is 2968s, 1048s and 424s respectively.
[0035] Step S2: Test the samples before and after irradiation, as follows: Use ACT2000 (Zhongyuan Micro Instrument) standard vibration table to test. Load the sample with vibration shock, select multiple frequency points within the frequency range of 20Hz-2400Hz and apply acceleration of different g values to perform fixed frequency test.
[0036] Figure 5 LiNbO2 is a silicon-based lithium niobate ferroelectric single crystal thin film vibration sensor based on LiNbO2 at different injection rates before and after irradiation. 3 XRD pattern of the piezoelectric layer. The results show that at an injection rate of 1.37E10 e / cm²·s, LiNbO 3 The peak diffraction angle of the piezoelectric layer is the same as that when not irradiated, which is 34.82°. When the injection rate is 4.11E10 e / cm²·s, the peak diffraction angle shifts to the right by 0.04° to 34.86°, with a change rate of only 0.114%. When the injection rate is 1.0117E11e / cm²·s, the peak diffraction angle shifts to the right by 0.08° to 34.9°, with a change rate of only 0.229%. Even under maximum irradiation, the change in diffraction angle is very limited, so electron irradiation has little effect on LiNbO 3 The effect of the piezoelectric layer can be neglected. Figure 6 The frequency response curves of the samples at different injection rates before and after irradiation in this embodiment are shown in Figure 1. The results show that different irradiations have almost no effect on the output charge of the test samples at different frequencies. Figure 7 The curves of output charge variation with acceleration at different injection rates before and after irradiation of this embodiment when the operating frequency is 2400 Hz show that the effect of irradiation on the variation of output charge with acceleration is very small. Figure 8 When f=2200Hz and Acc=10g, the sinusoidal change law of the output charge before and after irradiation in this embodiment shows that their waveforms are consistent. This has important application value for deep space exploration.
[0037] The silicon-based lithium niobate ferroelectric single crystal thin film vibration sensor obtained in the embodiment of the present application has a small structural size, good radiation resistance, and can achieve good output performance in the frequency band of 20-2400Hz. It can solve the deficiencies of traditional vibration sensor devices in radiation resistance and low-temperature working time, and meet the needs of long-term stable high-frequency micro-vibration measurement in high-resolution earth observation for deep space exploration devices. In summary, this embodiment can well prepare a vibration sensor based on silicon-based lithium niobate ferroelectric single crystal thin film, and the prepared sensor has the ability to measure vibration signals under irradiation, wide frequency range and micro-vibration environment, which solves the performance disadvantages of existing sensors in high-frequency, high-radiation applications and weak vibration environments. The silicon-based lithium niobate ferroelectric single crystal thin film vibration sensor prepared in this embodiment can be used in a wide frequency range and irradiation environment, has high charge sensitivity and good charge output capability, and can still maintain relatively good piezoelectric properties in harsh environments. It can adapt well to space exploration environments, solves some technical barriers of micro-nano sensor devices in irradiation environments, and can be used in equipment fault diagnosis, vibration signal monitoring, high-frequency micro-vibration testing, space exploration or electron irradiation; it has important scientific significance.
[0038] The scope of protection claimed by the present invention is not limited to the above specific embodiments. For those skilled in the art, the present invention may have various deformations and changes. Any modifications, improvements and equivalent substitutions made within the concept and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing a silicon-based lithium niobate ferroelectric single crystal thin film vibration sensor, Features: The structure of the prepared silicon-based lithium niobate ferroelectric single crystal thin film vibration sensor is: comprising an outer frame (1), a cantilever beam (2) and a mass block (3); the outer frame (1) is rectangular in top view, and the layer structure of the outer frame (1) is as follows from bottom to top: a first SiO 2 Thin film layer, Si substrate, second SiO 2 Thin film layer, LiNbO 3 The piezoelectric layer, the inner side of the short side of the outer frame (1) is connected to one end of the cantilever beam (2), the other end of the cantilever beam (2) is connected to a mass block (3), the mass block (3) is square in a top view, the cantilever beam (2) is rectangular in a top view, and the side length of the mass block (3) is greater than the width of the cantilever beam (2), the mass block (3) and the cantilever beam (2) have the same layer structure, and the layer structure from bottom to top is: Si substrate, second SiO 2 Thin film layer, LiNbO 3 The piezoelectric layer, the top surface of the cantilever beam (2) is also provided with a metal electrode I (41) and a metal electrode II (42), wherein one end of the metal electrode I (41) is located at the inner edge of the outer frame (1), and the other end is directly opposite to the metal electrode II (42), and the other end of the metal electrode II (42) extends to the top of the mass block (3); the preparation method comprises the following steps: Step 1: Si-LiNbO 3 The bonded wafer is cleaned and the Si-LiNbO 3 The first SiO2 is deposited on the back of the bond wafer using PECVD 2 Thin film layer, used for hard mask of deep silicon process; Step 2: Processing metal electrodes on the upper surface of the product in step 1 by using magnetron sputtering process; Step 3: using a photolithography process to mark the pattern of the metal electrode on the product of step 2, and using an ion beam etching process to etch the metal electrode to etch out the metal electrode I (41) and the metal electrode II (42) on the upper surface; Step 4: Use photolithography to mark the cantilever beam (2), mass block (3) and peripheral frame (1) of the product of step 3, and use ion beam etching to complete the LiNbO 3 The piezoelectric layer is etched and the second SiO 2 Etching of thin film layers; Step 5: According to the pattern marked in step 4, the pattern mark is deepened by using a photolithography process, and a deep silicon etcher is used to complete the etching of the front Si substrate by using a deep reactive ion etching process; Step 6: Use photolithography to mark the pattern on the back of the product in step 5, and etch the first SiO2 on the back by anisotropic oxidation etching process. 2 The thin film layer is formed into a cavity; a deep silicon etcher is used to etch the back Si substrate using a deep reactive ion etching process to release the device, thereby forming an external frame (1), a cantilever beam (2) and a mass block (3), and the silicon-based lithium niobate ferroelectric single crystal thin film vibration sensor is completed.
2. The method for preparing a silicon-based lithium niobate ferroelectric single crystal thin film vibration sensor according to claim 1, Features: In step 1, a first SiO layer with a thickness of 2 μm is deposited by PECVD. 2 The growth rate of the thin film is 0.5 μm / h; the first SiO 2 The cleaning process before the thin film layer is as follows: 3 The bonding wafer is acid-washed, alkaline-washed and rinsed with deionized water several times, and blown dry with nitrogen to make the surface clean.
3. The method for preparing a silicon-based lithium niobate ferroelectric single crystal thin film vibration sensor according to claim 2, Features: In step 2, LiNbO 3 A 20nm thick Cr layer and a 200nm thick Au layer are grown on the surface of the piezoelectric layer by magnetron sputtering.
4. The method for preparing a silicon-based lithium niobate ferroelectric single crystal thin film vibration sensor according to claim 3, Features: In step 3, during the photolithography process, Si-LiNbO 3 The bonding wafer surface was spin-coated with AZ 6130 positive photoresist. The mask used was a positive plate. The pattern shape matched the shape of the metal electrode Ⅰ (41) and the metal electrode Ⅱ (42) on the top of the vibration sensor. The parameters used were: 3000 r / min and 4000 r / min were used for photoresist spin coating, and pre-baking was performed on a 100°C baking table for 1 minute. The exposure dose was 200 mJ / cm 2 , developed with a developer formed by AZ 400K and water in a volume ratio of 1:4 for 28 seconds, and post-baked on a 120°C baking table for 15 minutes; the ion beam etching process used an ion beam etcher, set the energy of Ar ions to 500eV, the gas flux to 5, and the ion beam etching rate to 25nm / min.
5. The method for preparing a silicon-based lithium niobate ferroelectric single crystal thin film vibration sensor according to claim 4, Features: In step 4, in Si-LiNbO 3 The bonding wafer surface was spin-coated with AZ 4620 positive photoresist. The mask plate used was a positive plate. The pattern shape matched the shape of the vibration sensor cantilever beam (2), the mass block (3) and the peripheral frame (1). The low speed was set to 1000 r / min for 120 s, and the high speed was set to 3000 r / min for 5 s. The surface was then pre-baked on a 100°C baking table for 2 minutes, and then photolithography was performed. The exposure dose was set to 400 mJ / cm 2 , developed in a developer solution of AZ 400K and water in a volume ratio of 1:3 for 71 seconds, and then used an oxygen plasma glue process to remove the residual glue on the surface, and then used a 120°C baking table for 15 minutes. 3 The bonded wafer was fixed on the tray of the ion beam etcher, the Ar flux was set to 5, the etching rate was set to 1.25 μm / h, and the LiNbO 3 Etching of the piezoelectric layer. Etching was stopped until a colored halo appeared. The subsequent reactive ion etching process used an RIE etcher, and the gas introduced was SF 4 , the etching rate is 16.7nm / min.
6. The method for preparing a silicon-based lithium niobate ferroelectric single crystal thin film vibration sensor according to claim 5, Features: In step 5, during the photolithography process, the mask plate in step 4 is used to form a Si-LiNbO 3 The front side of the bond wafer was sprayed with AZ 4620 positive photoresist for 4 cycles, and pre-baked for 150s on a 100℃ baking table with an exposure dose of 400mJ / cm 2 , developed with a developer formed by AZ 400K and water in a volume ratio of 1:3 for 107 seconds, and after patterning, an oxygen plasma degumming machine was used to remove the floating glue remaining on the surface; finally, post-baking was performed on a 120°C baking table for 15 minutes; a deep silicon etcher was used to etch the Si substrate to a thickness of 70μm, 50~55loops were etched, and the etching rate was 1.4μm / loop.
7. The method for preparing a silicon-based lithium niobate ferroelectric single crystal thin film vibration sensor according to claim 6, Features: In step 6, during the photolithography process, the mask used is a positive mask, the pattern shape matches the shape of the vibration sensor outer frame (1), AZ 4620 photoresist is sprayed for 8 cycles, and the photoresist is baked on a 100°C baking table for 270 seconds, and the exposure dose is set to 800mJ / cm 2 , developed for 120 seconds in a developer solution composed of AZ 400K and water in a volume ratio of 1:
2. If the development is insufficient, the development time is extended. The residual floating glue is removed using an oxygen plasma degumming machine. Then, it is post-baked on a 100°C baking table for 30 minutes. The Si-LiNbO 3 The bonded wafer was hardened on a 100℃ baking table for 1 hour; the first SiO 2 The thin film layer was patterned with an etching rate of 350nm / min and an etching time of 342s. The Si substrate was etched using a deep silicon etcher with an etching thickness of 423μm and an etching rate of 1.2μm / loop until all devices were released.
8. The method for preparing a silicon-based lithium niobate ferroelectric single crystal thin film vibration sensor according to claim 7, Features: From step 3 to step 6, each step is cleaned and dried with nitrogen to ensure that there is no glue, water or oil when entering the next step. The cleaning reagent solution used is concentrated H 2 SO 4 , H 2 O 2 Solution, NH 4 One or more of (OH) solution, acetone, anhydrous ethanol and deionized water.
9. The method for preparing a silicon-based lithium niobate ferroelectric single crystal thin film vibration sensor according to claim 8, Features: The prepared silicon-based lithium niobate ferroelectric single crystal thin film vibration sensor has a Si substrate thickness of 493 μm for the outer frame (1); a Si substrate thickness of 70 μm for the mass block (3) and the cantilever beam (2); and a second SiO 2 The thickness of the film layer is 2μm; LiNbO 3 The thickness of the piezoelectric layer is 5 μm; the top-view dimensions of the cantilever beam (2) are 1860 μm in length and 470 μm in width; and the top-view side length of the mass block (3) is 600 μm.
10. Application of a silicon-based lithium niobate ferroelectric single crystal thin film vibration sensor prepared by the method for preparing a silicon-based lithium niobate ferroelectric single crystal thin film vibration sensor as described in any one of claims 1 to 9 in equipment fault diagnosis, vibration signal monitoring, high-frequency micro-vibration testing, space exploration or electron irradiation.
Citation Information
Patent Citations
D15-mode ferroelectric single crystal film piezoelectric vibration sensor and preparation method thereof
CN114665006A
Silicon-based lithium niobate piezoelectric vibration sensor based on transmission beam structure and preparation method of silicon-based lithium niobate piezoelectric vibration sensor
CN116887662A
Actuator structure
WO2003049209A1