Dominant security feature

By combining magnetically oriented pigment particles and cholesteric liquid crystal polymers in explicit safety features, a multi-color explicit safety feature is formed, which solves the problem of fine-tuning color shift characteristics and production complexity in the existing technology, and achieves efficient and economical Manufactured with multi-color explicit security features to enhance counterfeit protection.

CN118765236AActive Publication Date: 2024-10-11SICPA HOLDING SA
View PDF 21 Cites 0 Cited by

Patent Information

Application Number
CN202380023598.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-01
Filing Date
2023-02-22
Publication Date
2024-10-11
Estimated Expiration
2043-02-22

AI Technical Summary

Technical Problem

In the existing technology, it is difficult to fine-tune the color-shifting properties of cholesteric liquid crystal polymers, and the production process is complex, resulting in high costs and material waste, making it difficult to manufacture eye-catching multi-color explicit security features at high production speeds.

Method used

Employing explicit security features composed of free transparent materials, light-absorbing materials and cholesteric liquid crystal polymers, including a color-constant layer and an optically variable layer of magnetically oriented plate-shaped magnetic or magnetizable pigment particles, oriented and cured by a magnetic field Form an overlay to achieve the effect of presenting multiple colors at different viewing angles.

Benefits of technology

It achieves explicit security features that are easily recognized and verified through human senses without the need for external equipment, improves counterfeit protection capabilities, simplifies the production process, and reduces costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118765236A_ABST
    Figure CN118765236A_ABST
Patent Text Reader

Abstract

The present invention relates to the field of methods for producing noticeable dominant security features exhibiting color-changing properties as anti-counterfeiting means and decorative purposes on security documents or security articles. In particular, the dominant security feature exhibits a) a substrate (x10), a color constant layer (x20) comprising magnetically oriented sheet-like magnetic or magnetisable pigment particles, and an optically variable layer (x30) comprising a cholesteric liquid crystal polymer (CLCP) reflecting light in the visible spectral range, wherein the sheet-like magnetic or magnetisable pigment particles of the color constant layer (x20) have substantially the same elevation angle alpha.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of overt security features on substrates, security documents, security articles and decorative articles. In particular, the present invention provides an attractive overt security feature exhibiting color-changing properties as an anti-counterfeiting measure and for decorative purposes on a security document or security article. Background Art

[0002] With the continuous improvement of the quality of color copies and prints and attempts to protect security documents and items that do not have a reproducible effect, such as banknotes, valuable documents or cards, transportation tickets or cards, tax stickers (tax banderols) and commodity labels from counterfeiting, tampering or illegal copying, the traditional practice is to introduce various security elements into these documents and items. Typical examples of security elements include anti-counterfeiting security threads, windows, fibers, planchettes, foils, labels, holograms, watermarks, security inks containing optically variable pigments, magnetic or magnetizable thin film interference pigments, interference coated particles, thermochromic pigments, photochromic pigments, luminescent, infrared absorbing, ultraviolet absorbing or magnetic compounds.

[0003] Security features used for security documents, for example, can generally be classified as "covert" security features on the one hand and "overt" security features on the other hand. The protection provided by covert security features relies on the idea that such features are difficult to detect, typically requiring specialized instrumentation and knowledge for detection, whereas "overt" security features rely on the idea that they are easily detectable by unaided human senses, e.g. such features may be visible and / or detectable by touch, but still difficult to produce and / or reproduce. However, the effectiveness of overt security features relies heavily on their eye-catching effect and easy identification as security features, since most users, particularly those who are not aware of the security feature of the document or article secured by the security feature in advance, will in fact perform security checks based solely on the security feature if they have actual knowledge of its existence and nature.

[0004] Color-shifting optically variable security features (also referred to in the art as goniochromatic features) exhibit a color shift or color change, indicated by a change in brightness and / or chromaticity and / or hue, as the observation angle (also referred to in the art as viewing angle) varies between a grazing angle and a face angle, and are used to protect security documents and articles from counterfeiting and / or illicit duplication by common color scanning, printing and copying office equipment.

[0005] Typically, the security feature is made from an ink comprising flake-shaped multilayer interference pigments.

[0006] Other security features based on cholesteric liquid crystal materials have been developed. Materials with liquid crystal structures of chiral phases (also called cholesteric liquid crystal materials) are known and used as optically variable security features. Cholesteric liquid crystal polymers show molecular order in the form of a helical superstructure perpendicular to the longitudinal axis of their molecules. The helical superstructure provides a periodic refractive index modulation throughout the liquid crystal material, which in turn leads to selective transmission / reflection of light of a determined wavelength (interference filter effect). Cholesteric liquid crystal polymers can be obtained by arranging and orienting more than one crosslinkable substance (nematic compound) with a chiral phase. The specific situation of the helical molecular arrangement leads to the cholesteric liquid crystal material showing the property of reflecting a circularly polarized light component within a determined wavelength range, wherein the circularly polarized light can be left-handed or right-handed, depending on the direction of rotation of the molecular helix. The wavelength range reflected by the cholesteric liquid crystal polymer is determined by the geometry of its periodic refractive index modulation, i.e. the pitch of the molecular helix, as known to those skilled in the art. By varying the nature of the chiral component and the ratio of nematic and chiral compounds, and in particular by varying optional factors including temperature and solvent concentration, the helical pitch (i.e., the distance over which the helical arrangement completes a full 360° rotation) can be adjusted. The helical pitch of the material can ultimately be frozen by a crosslinking (polymerization) reaction, so that the color of the resulting cholesteric liquid crystal polymer is no longer dependent on external factors such as temperature.

[0007] US 6,423,246 discloses a security feature comprising optically variable pigments, wherein the pigments are prepared by pulverizing cholesteric liquid crystal polymer films.The disclosed pigments exhibit a color shift from a first color to a second color upon tilting the security feature.

[0008] WO 2015 / 055504 A1 discloses an optically variable security element based on a single solidified layer comprising a cholesteric liquid crystal polymer.

[0009] The color shift range of cholesteric liquid crystal polymers that can be used for security documents may be limited, and in order to increase the color gamut of the optically variable security feature, it may be advantageous to change the reflective properties and thereby increase the range of available colors. As mentioned above, the reflected light from a cholesteric liquid crystal polymer depends on the pitch of its helical structure and thereby on the nature and concentration of the chiral component. In particular, the addition of an appropriate amount of a chiral component to the precursor mixture results in a color shift change to shorter wavelengths. However, it is neither simple nor cost-effective to customize the cholesteric liquid crystal material for each specific application and each desired color shift effect during manufacturing. In addition, the fine-tuning of the color shift properties of cholesteric liquid crystal polymers is a delicate step that often results in a significant waste of time and / or material.

[0010] Therefore, there remains a need for attractive multi-color explicit security features, especially for demanding applications requiring high counterfeiting resilience, allowing easy, direct and unambiguous verification by the human eye without any external equipment or tools. The explicit security features need to be produced by a method that should be reliable, predictable in a controlled manner, easy to implement and able to operate at high production speeds. Summary of the invention

[0011] Therefore, the object of the present invention is to overcome the deficiencies of the prior art. This is achieved by providing an explicit security feature, the explicit security feature comprising:

[0012] a) a substrate (x10), wherein the substrate (x10) is made of a material selected from the group consisting of a transparent material, a light-absorbing material and a combination thereof,

[0013] b) a color-constant layer (x20) comprising magnetically oriented platelet-shaped magnetic or magnetizable pigment particles, and

[0014] c) an optically variable layer (x30) comprising a cholesteric liquid crystal polymer (CLCP) reflecting light in the visible spectral range and located on the color constant layer (x20) so as to form a first region consisting of a superposition of the optically variable layer (x30) and the color constant layer (x20);

[0015] The platelet-shaped magnetic or magnetizable pigment particles of the color constant layer (x20) have substantially the same elevation angle |α|, the value of which is between about 10° and about 45° (10°≤angle |α|≤45°), preferably between about 15° and about 40° (15°≤angle |α|≤40°); and more preferably between about 15° and about 35° (15°≤angle |α|≤35°).

[0016] The elevation angles |α| provided herein consist of average values, i) obtained using a conoscopic scattering instrument as described below, wherein the values ​​are averaged over at least about 1000 platelet-shaped magnetic or magnetizable pigment particles, or ii) obtained using a microscope as described below, wherein the values ​​are averaged over at least 10, in particular 10 to 20 platelet-shaped magnetic or magnetizable pigment particles.

[0017] The first area of ​​the overt security feature exhibits at least three different colors when observed through the optically variable layer (x30) at different viewing / observation angles, one of which is a grazing angle (e.g. 10°, 20°, 30°, etc.) and another is a face angle (approximately 90°), provided that when the substrate is transparent, the overt security feature must be set on a light-absorbing background.

[0018] The color-constant layer (x20) described herein comprises uniaxially oriented platelet-shaped magnetic or magnetizable pigment particles or comprises biaxially oriented platelet-shaped magnetic or magnetizable pigment particles, wherein the particles exhibit a metallic color, more preferably a silver color.

[0019] The optically variable layer (x30) described herein is preferably obtained from a cholesteric liquid crystal polymer precursor composition comprising one or more nematic compounds, one or more chiral dopants, one or more photoinitiators and one or more solvents.

[0020] The overt security features described herein are particularly useful for protecting security documents, security articles, and decorative articles from counterfeiting, tampering, or unauthorized copying.

[0021] Also disclosed herein are security documents, security articles and decorative articles comprising one or more of the overt security features disclosed herein, and methods for producing them, and security documents, security articles and decorative articles obtained therefrom. The method for producing the overt security features disclosed herein comprises the following steps:

[0022] a) applying a radiation-curable coating composition comprising flake-shaped magnetic or magnetizable pigment particles, said radiation-curable coating composition being in a first, liquid state, onto a surface of a substrate (x10) so as to form a layer;

[0023] b) exposing the layer obtained in step a) to magnetic field lines of a magnetic field generating device, wherein the magnetic field lines form an elevation angle |γ| with the surface of the substrate (x10), the value of the elevation angle |γ| being between about 10° and about 45° or between about 135° and about 170°, thereby orienting the platelet-shaped magnetic or magnetizable pigment particles;

[0024] c) partially simultaneously with step b) or after step b), a step of at least partially curing the layer with a curing unit, thereby at least partially fixing the position and orientation of the platelet-shaped magnetic or magnetizable pigment particles, so that the platelet-shaped magnetic or magnetizable pigment particles have the same elevation angle |α|, the elevation angle |α| is between about 10° and about 45° (10°≤angle |α|≤45°), preferably between about 15° and about 40° (15°≤angle |α|≤40°); and more preferably between about 15° and about 35° (15°≤angle |α|≤35°), thereby forming a color-consistent layer (x20),

[0025] d) applying a cholesteric liquid crystal polymer precursor composition at least partially on the color constant layer (x20) and / or at least partially on the surface of the substrate (x10),

[0026] e) heating the layer obtained in step d), and

[0027] f) Hardening the layer obtained in step e) to obtain an optically variable layer (x30).

[0028] Also described herein is a method for manufacturing a security document, security article or decorative article, which comprises a) providing a security document, security article or decorative article, and b) providing one or more explicit security features described herein so that they are included on or by the security document, security article or decorative article. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figures 1A-1E and Figure 2A-2B Several embodiments of the invention are shown schematically.

[0030] Figure 3A A platelet-shaped magnetic or magnetizable pigment particle is schematically shown with its main axis X and its main axis Y.

[0031] Figure 3B Uniaxially oriented platelet-shaped particles are schematically shown, wherein the platelet vectors (vectors parallel to the main axis X of the particles) of adjacent platelet-shaped magnetic or magnetizable pigment particles are essentially parallel to one another. Figure 3C Biaxially oriented platelet particles are schematically shown, wherein the platelet vectors (vectors parallel to the main axis X of the particles) of adjacent platelet-shaped magnetic or magnetizable pigment particles are parallel to each other, and the second platelet vectors (vectors parallel to the main axis Y of the particles) of adjacent platelet-shaped magnetic or magnetizable pigment particles are substantially parallel to each other.

[0032] Figure 4Schematically shows a cross section of a substrate (410) carrying a color-constant layer (420) comprising magnetically oriented flake-shaped magnetic or magnetizable pigment particles, wherein the flake-shaped magnetic or magnetizable pigment particles have substantially the same elevation angle |α| (i.e., the absolute values ​​of +α and -α are the same in the respective color-constant layer (x20)).

[0033] Figures 5A1-5A2 A suitable magnetic field generating device for biaxially orienting the platelet-shaped magnetic or magnetizable pigment particles contained in a layer on a substrate is schematically shown. The magnetic field generating device comprises nine magnet subassemblies (M1-M9) arranged in a row with alternating north-south magnetic directions, wherein the substrate carrying the layer comprising the platelet-shaped magnetic or magnetizable pigment particles is laid flat at an elevation angle γ and the particles are exposed to the magnetic field of the magnetic field generating device.

[0034] Figure 6 A cross section of an overt security feature of the present invention is shown, comprising a substrate (610) and an optional light absorbing background (640) (in the case where the substrate (610) is not made of more than one light absorbing material), wherein an optically variable layer (630) is above a color constant layer (620), and a method of verifying the feature by changing the viewing / observation angle β.

[0035] Figure 7 A top view of an overt security feature of the present invention is shown, comprising a substrate (710) with an optically variable layer (730) partially over a color constant layer (720), and a method of verifying the feature by varying the viewing / observation angle β. DETAILED DESCRIPTION

[0036] definition

[0037] The following definitions are intended to clarify the meaning of the terms discussed in the specification and recited in the claims.

[0038] As used herein, the indefinite article "a" means one as well as more than one and does not necessarily limit its designated noun to the singular.

[0039] As used herein, the term "at least one" is intended to define one or more than one, such as one or two or three.

[0040] As used herein, the terms "about" and "substantially" mean that the amount or value in question can be a specified certain value or some other value in the vicinity thereof. Typically, the terms "about" and "substantially" indicating a specific value are intended to indicate a range within ±5% of that value. As an example, the phrase "about 100" indicates a range of 100 ± 5, i.e., a range from 95 to 105. Typically, when the term "about" is used, it is expected that similar results or effects according to the present invention can be obtained within a range of ±5% of the specified value.

[0041] The term "substantially parallel" means at least 1 mm 2 The average deviation from parallel alignment on the surface of the coating or over at least about 100 particles is no more than 2°.

[0042] As used herein, the term "and / or" means that all or only one of the elements of the group may be present. For example, "A and / or B" means "only A, or only B, or both A and B". In the case of "only A", the term also covers the possibility that B does not exist, that is, "only A, but not B".

[0043] The term "comprising" as used herein is intended to be non-exclusive and open-ended. Thus, for example, a coating composition comprising compound A may include other compounds in addition to A. However, as a specific embodiment thereof, the term "comprising" also encompasses the more restrictive meanings of "consisting essentially of" and "consisting of", so that, for example, "comprising a mixture of A, B and optionally C" may also consist (essentially) of A and B or (essentially) of A, B and C.

[0044] The term "visible spectral range" refers to the range from 400 nm to 700 nm.

[0045] The term "coating composition" refers to any composition capable of forming a layer on a solid substrate and which can be applied preferably but not exclusively by printing methods. The coating composition comprises the flake-like magnetic or magnetizable pigment particles described herein and the binder described herein.

[0046] As used herein, the term "wet" refers to a coating that has not yet at least partially cured, for example a coating in which the platelet-shaped magnetic or magnetizable pigment particles are still able to change their position and orientation under the influence of external forces acting thereon.

[0047] The term "secure document" refers to a document that is typically protected from forgery or fraud by at least one security feature. Examples of secure documents include, but are not limited to, documents of value and commercial goods of value.

[0048] The term "security feature" is used to denote an image, pattern or graphical element that can be used for authentication purposes.

[0049] Insofar as the present description refers to “preferred” embodiments / features, combinations of these “preferred” embodiments / features are also to be regarded as disclosed, as long as this combination of “preferred” embodiments / features makes technical sense.

[0050] The overt security feature described herein comprises a substrate as described herein (x10), a color constant layer as described herein comprising magnetically oriented flake-shaped magnetic or magnetizable pigment particles (x20), and an optically variable layer as described herein comprising a cholesteric liquid crystal polymer (CLCP) that selectively reflects light in the visible spectrum (x30).

[0051] The color constant layer (x20) refers to a coating comprising magnetically oriented platelet-shaped magnetic or magnetizable pigment particles, wherein the particles are oriented by a magnetic field and wherein the oriented particles are fixed / frozen in their orientation and position (ie after curing) to form a magnetically sensitive layer.

[0052] The optically variable layer (x30) is above the color constant layer (x20) in a first area consisting of a superposition of the optically variable layer (x30) and the color constant layer (x20). Optionally, the overt security feature described herein may further comprise a second area made only of the optically variable layer (x30), wherein the second area preferably surrounds the first area described herein when viewed through the optically variable layer (x20). Figure 7 An example of an overt security feature is shown comprising a first area consisting of an indicia "A" and a second area consisting of an area surrounding the "A" indicia.

[0053] The eye-catching overt security feature described herein allows an observer to easily and conveniently identify it because the first area of ​​the overt security feature displays at least three different colors when viewed with the naked eye through the optically variable layer (x20) (as shown by the eye in the figure) at different viewing / observation angles, wherein one of the angles is a grazing angle (e.g., 10°, 20°, 30°, etc.) and another is a face angle (approximately 90°), provided that when the substrate is transparent, the overt security feature must be set on a permanent light-absorbing background.

[0054] The color shifting property of an explicit security feature comprising a cholesteric liquid crystal polymer is considered to be an explicit security feature that is easily noticeable to the public. Advantageously, anyone can easily detect, identify and / or distinguish the security feature or a security document or article comprising the security feature from its possible counterfeit using independent human senses, for example, such features can be visible and / or detectable, but still difficult to produce and / or reproduce. In addition, the property of reflecting circularly polarized light of a cholesteric liquid crystal polymer can be used as a semi-hidden feature, which is visible or detectable with the help of a light polarization filter. In other words, the property of reflecting circularly polarized light of a cholesteric liquid crystal polymer can be used as an identification tool for identifying a security feature comprising a cholesteric liquid crystal polymer or a security document, security article, or decorative article comprising the security feature.

[0055] The overt security features described herein include a substrate (x10) of a material selected from the group consisting of a transparent material, a light absorbing material, and combinations thereof.

[0056] Preferred substrates made of more than one transparent material include but are not limited to transparent polyolefins such as polyethylene (PE) and polypropylene (PP) including biaxially oriented polypropylene (BOPP), transparent polyamides, transparent polyesters such as poly(ethylene terephthalate) (PET), poly(1,4-butylene terephthalate) (PBT), poly(ethylene 2,6-naphthoate) (PEN), and transparent polyvinyl chloride (PVC), more preferably transparent polyesters such as PET.

[0057] "Light-absorbing substrate" refers to a substrate that absorbs at least 50%, preferably at least 60%, of the intensity of one or more parts of the visible part of the electromagnetic spectrum (visible spectrum). The light-absorbing substrate can be a continuous layer, or it can be a discontinuous layer in the form of a mark or pattern. Preferably, the light-absorbing substrate is a dark substrate, more preferably a black substrate. If the substrate described in this article is a light-absorbing substrate, no further additional layers or coatings are required, and the color shift characteristics of the explicit security feature can be easily observed without any machine or equipment. If the substrate is not a light-absorbing substrate, there may be an additional light-absorbing background (x40), preferably a dark background (x40), more preferably a black background (x40), wherein the dark background (x40) may be permanently or non-permanently present.

[0058] Preferred substrates made of more than one light absorbing material include, but are not limited to, those selected from the group consisting of paper or other fibrous materials (including woven and nonwoven fibrous materials), such as cellulose, paper-containing materials, glass, metals, ceramics, plastics and polymers, metallized plastics or polymers, composite materials, and mixtures or combinations of two or more thereof. Typical paper, paper-like or other fibrous materials are made from various fibers, including, but not limited to, abaca, cotton, flax, wood pulp, and blends thereof. As is well known to those skilled in the art, cotton and cotton / flax blends are preferably used for banknotes, while wood pulp is typically used for non-banknote security documents.

[0059] The light absorbing substrate may consist of a transparent substrate comprising layers (eg printer layers) made of more than one light absorbing material.

[0060] If the substrate (x10) is made of more than one transparent material, then by placing it on a non-permanent light absorbing background as described herein, the apparent color shifting properties of the overt security feature are observed.

[0061] It should be noted that these substrate materials are only used for illustrative purposes and do not limit the scope of the present invention. Generally, any substrate (which may not necessarily be flat and may be non-uniform) whose surface is insoluble or only slightly soluble in the solvent used in the cholesteric liquid crystal polymer precursor composition is a suitable substrate for the purpose of the present invention.

[0062] according to Figure 1A and 1B In one embodiment shown, the overt security feature described herein comprises a transparent substrate (x10) wherein a color constant layer (x20) and an optically variable layer (x30) are placed on the same side of said transparent substrate (x10) (see Figure 1A ) or placed on the opposite side (see Figure 1B As described herein, a non-permanent light absorbing background can be used to observe the color shifting properties of a security feature by placing the non-permanent light absorbing background on the opposite side of the optically variable layer (x30).

[0063] according to Figure 1C , 1D In another embodiment shown in FIG. 1E , the overt security feature described herein comprises a transparent substrate (x10) and a permanent light absorbing background (x40), wherein the color constant layer (x20) and the optically variable layer (x30) are placed on the same side of the transparent substrate (x10) (see FIG. 1E ). Figure 1C and 1D ) or placed on the opposite side (see Figure 1E ).

[0064] according to Figure 2AAs another embodiment shown, the overt security feature described herein comprises a light absorbing substrate (x10) wherein the color constant layer (x20) and the optically variable layer (x30) are placed on the same side of the light absorbing substrate (x10).

[0065] according to Figure 2B In another embodiment shown, the overt security feature described herein comprises a light absorbing substrate (x10) and a permanent light absorbing background (x40), wherein the color constant layer (x20) and the optically variable layer (x30) are placed on the same side of the light absorbing substrate (x10).

[0066] The optically variable layer (x30) is on top of the color constant layer (x20), thereby forming a first region as described herein. According to one embodiment, the optically variable layer (x30) is at least partially on top of the color constant layer (x20) and comprises two regions: a first region in which the optically variable layer (x30) is on top of the color constant layer (x20) (a superposition of the two layers), and a second region made of the optically variable layer (x30) alone. "On top of" is not limited to direct contact; for example and as Figure 1B As shown, the optically variable layer (x30) is at least partially on top of the color constant layer (x20), but not in direct contact, since the substrate (x10) is present between the two layers (x20 and x30).

[0067] According to e.g. Figure 1A , 1C , 1D, 2A and 2B, the optically variable layer (x30) is at least partially in direct contact with the color constant layer (x20), and both layers are located on the same side of the substrate (x10). Figure 1B and 1E In another embodiment shown, the optically variable layer (x30) is at least partially not in direct contact with the color constant layer (x20), and both layers are located on opposite sides of the substrate (x10).

[0068] The optically variable layer (x30) and the color constant layer (x20) can independently be a continuous layer or a discontinuous layer. The color constant layer (x20) and / or the optically variable layer (x30) can independently be in the form of more than one mark, wherein the mark made of the color constant layer (x20) and the mark made of the optically variable layer (x30) can have the same shape or different shapes. As used herein, the term "indicium" / "indicia" should mean a continuous and discontinuous layer consisting of a distinguishing mark or logo or pattern. Examples of marks include codes, coded marks (e.g., coded alphanumeric data, one-dimensional barcodes, two-dimensional barcodes, two-dimensional codes (QR-codes), data matrices, and IR reading codes), symbols, alphanumeric symbols, graphics, geometric patterns (e.g., circles, triangles, and regular or irregular polygons), letters, words, numbers, logos, pictures, portraits, and combinations thereof.

[0069] The overt security feature described herein comprises a color-constant layer (x20) in which platelet-shaped magnetic or magnetizable pigment particles are oriented according to a specific orientation pattern.

[0070] The thickness of the color constant layer (x20) described herein is preferably between about 5 μm and about 30 μm, preferably between about 5 μm and about 20 μm, and more preferably between about 5 μm and about 15 μm (measured by using Extramess Inductive Digital Comparator 2001 (provided by Mahr).

[0071] As described herein, the method for making an overt security feature described herein comprises a step c) of at least partially curing a layer comprising a radiation curable coating composition having particles to a second state, wherein the platelet-shaped magnetic or magnetizable pigment particles are fixed in their current position and orientation and cannot move or rotate within the layer. According to one embodiment, the step c) is performed by exposing the layer to one or more wavelengths of about 365 nm to about 470 nm, preferably about 365 nm to about 405 nm, using a UV-Vis light emitting diode (LED) curing unit.

[0072] As used herein, "at least partially solidifying the layer" means that the platelet-shaped magnetic or magnetizable pigment particles are fixed / frozen in the position and orientation they adopt and can no longer move and rotate (also known in the art as "pinning" of the particles).

[0073] As described therein, the color constant layer comprises magnetically oriented platelet-shaped magnetic or magnetizable pigment particles in the at least partially cured layer. Preferably, the platelet-shaped magnetic or magnetizable pigment particles as described herein are present in an amount of about 2 wt-% to about 25 wt-%, preferably about 3 wt-% to about 20 wt-%, more preferably about 4 wt-% to about 15 wt-%, and still more preferably about 4 wt-% to about 10 wt-%, the weight percentages being based on the total weight of the at least partially cured color constant layer. Preferably, the platelet-shaped magnetic or magnetizable pigment particles as described herein are present in an amount of about 2 wt-% to about 25 wt-%, preferably about 3 wt-% to about 20 wt-%, more preferably about 4 wt-% to about 15 wt-%, and still more preferably about 4 wt-% to about 10 wt-%, the weight percentages being based on the total weight of the radiation-curable coating as described herein.

[0074] The flaky magnetic or magnetizable pigment particles described herein are defined as having a non-isotropic reflectivity for incident electromagnetic radiation due to their non-spherical shape, wherein the cured binder material is at least partially transparent. The binder material, at least in its cured or solid state (also referred to herein as the second state), is at least partially transparent for electromagnetic radiation in a wavelength range comprised between 200 nm and 2500 nm, i.e., in a wavelength range typically referred to as the "spectrum" and including the infrared, visible and UV parts of the electromagnetic spectrum. Thus, the non-spherical magnetic or magnetizable pigment particles contained in the binder material in its hardened or solid state and their orientation-dependent reflectivity can be perceived through the binder material at some wavelengths within this range. Preferably, the cured binder material is at least partially transparent for electromagnetic radiation in a wavelength range comprised between 200 nm and 800 nm, more preferably between 400 nm and 700 nm. Here, the term "transparent" means that the transmittance of electromagnetic radiation through a 20 μm layer of the cured binder material (excluding the flake-shaped magnetic or magnetizable pigment particles, but including all other optional components of the OEL, where such components are present) present in the OEL is at least 50%, more preferably at least 60%, even more preferably at least 70% at the wavelength of interest. This can be determined, for example, by measuring the transmittance of a test piece of the hardened binder material (excluding the flake-shaped magnetic or magnetizable pigment particles) in accordance with well-established test methods such as DIN 5036-3 (1979-11). As used herein, the term "non-isotropic reflectivity" means that the proportion of incident radiation from a first angle reflected by the particles into a specific (viewing / observation) direction (a second angle) is a function of the orientation of the particles, i.e. a change in the orientation of the particles relative to the first angle may result in a reflection of different magnitudes into the viewing / observation direction. In contrast to needle-shaped pigment particles, which can be considered as one-dimensional particles, flake-shaped pigment particles have an X-axis and a Y-axis ( Figure 3A ). In other words, and if Figure 3A As shown, platelet-shaped pigment particles can be considered as two-dimensional particles due to their large aspect ratio of size, where dimensions X and Y are substantially greater than dimension Z. Platelet-shaped pigment particles are also referred to in the art as flat particles or flakes. Such pigment particles can be described as having a major axis X corresponding to the longest dimension across the pigment particle, and a second major axis Y perpendicular to X, also located within the pigment particle.

[0075] The color constant layer as described herein comprises magnetically oriented platelet-shaped magnetic or magnetizable pigment particles in the at least partially cured layer as described herein, wherein the platelet-shaped magnetic or magnetizable pigment particles have a specific orientation angle corresponding to the elevation angle |α| in the color constant layer (x20). The platelet-shaped magnetic or magnetizable pigment particles in the at least partially cured color constant layer (x20) are as described herein and as described herein and as described herein. Figure 4 The elevation angle |α| orientation shown in FIG. 1 , where |α| represents the absolute value of +α and -α. In other words, and as Figure 4 As shown, the platelet-shaped magnetic or magnetizable pigment particles in the at least partially cured color constant layer (x20) have the same angle +α or have the same angle −α.

[0076] The platelet-shaped magnetic or magnetizable pigment particles of the color constant layer (x20) have substantially the same elevation angle |α|, the value of which is between about 10° and about 45° (10°≤angle|α|≤45°), preferably between about 15° and about 40° (15°≤angle|α|≤40°); and more preferably between about 15° and about 35° (15°≤angle|α|≤35°). As described herein, the elevation angle |α| provided herein consists of an average value, which is i) obtained using a conical light scattering instrument as described below, wherein the value is averaged over at least about 1000 platelet-shaped magnetic or magnetizable pigment particles, or ii) obtained using a microscope as described below, wherein the value is averaged over at least 10, in particular 10 to 20 platelet-shaped magnetic or magnetizable pigment particles.

[0077] For example Figure 4 As shown, the platelet-shaped magnetic or magnetizable pigment particles are oriented as described above at the elevation angle α described herein. In other words, the elevation angle α is formed by the main axis X of the platelet-shaped magnetic or magnetizable pigment particles and the two-dimensional surface of the substrate (410), wherein the elevation angle |α| has the value described herein.

[0078] The orientation of the platelet-shaped magnetic or magnetizable pigment particles as described herein is obtained in step b) as described herein, wherein said orientation is performed so that said particles as described herein are uniaxially or biaxially oriented. In contrast to a uniaxial orientation in which the particles are oriented in such a way that only their major axes are constrained by the magnetic field ( Figure 3B ), biaxial orientation means orienting the particles in such a way that their two principal axes X and Y are constrained ( Figure 3C). That is, each flaky magnetic or magnetizable pigment particle can be considered to have a major axis in the plane of the pigment particle and an orthogonal minor axis in the plane of the pigment particle. The axes Y and Y of the flaky magnetic or magnetizable pigment particles are each oriented according to the magnetic field. Effectively, this results in adjacent flaky magnetic pigment particles that are spatially close to each other being substantially parallel to each other. In other words, biaxial orientation aligns the planes of the flaky magnetic or magnetizable pigment particles so that the planes of the pigment particles are oriented substantially parallel to the planes of adjacent (in all directions) flaky magnetic or magnetizable pigment particles.

[0079] For the case where the platelet-shaped magnetic or magnetizable pigment particles are e.g. Figure 3B In the embodiment shown for uniaxial orientation, the orientation of the flake-shaped pigment particles is defined by a flake vector, which is a vector parallel to the major axis X of the particle, wherein the flake vectors of adjacent flake-shaped magnetic or magnetizable pigment particles are substantially parallel to each other; that is, only the major axes X of adjacent flake-shaped magnetic or magnetizable pigment particles are substantially parallel to each other (in other words, adjacent flake-shaped magnetic or magnetizable pigment particles have substantially the same elevation angle α).

[0080] For the case where the platelet-shaped magnetic or magnetizable pigment particles are e.g. Figure 3C In the embodiment shown in Figure 1 that is biaxially oriented, the orientation of the flake-shaped pigment particles is defined by a flake vector, which is a vector parallel to the major axis X of the particle, wherein the flake vectors of adjacent flake-shaped magnetic or magnetizable pigment particles are parallel to each other and further defined by a second flake vector, which is a vector parallel to the second axis Y of the particle, wherein the flake vectors of adjacent flake-shaped magnetic or magnetizable pigment particles are parallel to each other, and the second flake vectors of adjacent flake-shaped magnetic or magnetizable pigment particles are parallel to each other. For the embodiment in which the flake-shaped magnetic or magnetizable pigment particles, for example Figure 3C In the embodiment shown in the figure which is biaxially oriented, the flake vectors of adjacent platelet-shaped magnetic or magnetizable pigment particles are parallel to each other, and not only the major axes X of adjacent platelet-shaped magnetic or magnetizable pigment particles are substantially parallel to each other, but also the secondary axes Y of adjacent platelet-shaped magnetic or magnetizable pigment particles are substantially parallel to each other. For the embodiment in which the platelet-shaped magnetic or magnetizable pigment particles are, for example, Figure 3C In the embodiment shown where biaxial orientation is performed, the platelet-shaped magnetic or magnetizable particles are essentially parallel to each other.

[0081] According to one embodiment, for example as shown in Figures 1, 2, 4 and 5, the explicit security feature described herein comprises a color constant layer (x20) having magnetically oriented flake-shaped magnetic or magnetizable pigment particles incorporated therein, wherein the flake-shaped magnetic or magnetizable pigment particles have substantially the same elevation angle |α|.

[0082] Optionally, the overt security feature described herein may include two or more regions including platelet-shaped magnetic or magnetizable pigment particles, wherein the platelet-shaped magnetic or magnetizable pigment particles in one region have substantially the same elevation angle |α| (the platelet-shaped magnetic or magnetizable pigment particles in at least the partially solidified color constant layer (x20) have the same angle +α or have the same angle -α), and the platelet-shaped magnetic or magnetizable pigment particles in the second region have substantially the same additional elevation angle |α'| (the platelet-shaped magnetic or magnetizable pigment particles in at least the partially solidified color constant layer (x20) have the same angle +α' or have the same angle -α'), the elevation angle |α| and the additional elevation angle |α'| are different from each other and / or are not coplanar. The two or more regions may consist of a single color constant layer (x20), or may consist of two or more independent color constant layers (x20, x20', etc.).

[0083] Suitable examples of the flaky magnetic or magnetizable pigment particles described herein include, but are not limited to, color-constant pigment particles comprising: a magnetic metal selected from the group consisting of cobalt (Co), iron (Fe) and nickel (Ni); a magnetic alloy of iron, manganese, cobalt, nickel or a mixture of two or more thereof; a magnetic oxide of chromium, manganese, cobalt, iron, nickel or a mixture of two or more thereof; or a mixture of two or more thereof. The term "magnetic" in relation to metals, alloys and oxides refers to ferromagnetic or ferrimagnetic metals, alloys and oxides. The magnetic oxides of chromium, manganese, cobalt, iron, nickel or a mixture of two or more thereof may be pure or mixed oxides. Examples of magnetic oxides include, but are not limited to, iron oxides such as hematite (Fe2O3), magnetite (Fe3O4), chromium dioxide (CrO2), magnetic ferrite (MFe2O4), magnetic spinel (MR2O4), magnetic hexaferrite (MFe 12 O 19 ), magnetic orthoferrite (RFeO3), magnetic garnet M3R2(AO4)3, wherein M represents a divalent metal, R represents a trivalent metal, and A represents a tetravalent metal.

[0084] Examples of the flaky magnetic or magnetizable pigment particles described herein include, but are not limited to, color-constant pigment particles comprising a magnetic layer M made of one or more of the following: a magnetic metal such as cobalt (Co), iron (Fe) or nickel (Ni); and a magnetic alloy of iron, cobalt or nickel, wherein the magnetic or magnetizable pigment particles may be a multilayer structure including one or more additional layers. Preferably, the one or more additional layers are: a layer A independently made of one or more compounds selected from the group consisting of metal fluorides such as magnesium fluoride (MgF2), silicon oxide (SiO), silicon dioxide (SiO2), titanium oxide (TiO2) and aluminum oxide (Al2O3); or a layer B independently made of one or more compounds selected from the group consisting of metals and metal alloys, preferably selected from the group consisting of reflective metals and reflective metal alloys, and more preferably selected from the group consisting of aluminum (Al), chromium (Cr) and nickel (Ni), and even more preferably aluminum (Al); or a combination of one or more layers A such as those described above and one or more layers B such as those described above. Typical examples of the flaky magnetic or magnetizable pigment particles of the above-mentioned multilayer structure include, without limitation, an A / M multilayer structure, an A / M / A multilayer structure, an A / M / B multilayer structure, an A / B / M / A multilayer structure, an A / B / M / B multilayer structure, an A / B / M / B / A multilayer structure, a B / M multilayer structure, a B / M / B multilayer structure, a B / A / M / A multilayer structure, a B / A / M / B multilayer structure, a B / A / M / B / A / multilayer structure, and a B / A / B / M / B / A / B multilayer structure, wherein layer A, magnetic layer M and layer B are selected from those described above, preferably a B / M / B multilayer structure and an A / B / M / B / A multilayer structure, wherein A is a layer of those described herein.

[0085] The platelet-shaped magnetic or magnetizable pigment particles described herein preferably exhibit a metallic color, more preferably a silver color.

[0086] The size d50 of the platelet-shaped magnetic or magnetizable pigment particles described herein is preferably between about 2 μm and about 50 μm, preferably between about 5 μm and about 30 μm (measured by direct optical granulometry).

[0087] The platelet-shaped magnetic or magnetizable pigment particles described herein may be surface treated to protect them from any degradation that may occur in radiation curable compositions and layers and / or to facilitate their incorporation into said compositions and layers; typically, corrosion inhibiting materials and / or wetting agents may be used.

[0088] The method described herein comprises the step of preparing the color constant layer (x20) described herein. The method comprises the step a) of applying a radiation curable coating composition comprising flaky magnetic or magnetizable particles described herein on the surface of the substrate (x10) described herein, the radiation curable coating composition being in a first, liquid state that allows it to be applied as a layer and being in a state that is not yet at least partially cured (i.e., wetted), wherein the pigment particles can move and rotate within the layer. Since the radiation curable coating composition described herein will be provided on the surface of the substrate (x10), the radiation curable coating composition comprises at least a binder material and magnetic or magnetizable pigment particles, wherein the composition is in a form that allows it to be processed on the desired printing or coating equipment. Preferably, the step a) is carried out by a printing method, and the printing method is more preferably selected from the group consisting of screen printing, rotary gravure printing and flexographic printing.

[0089] Depending on the printing method chosen for preparing the color constant layer (x20) and the optically variable layer (x30) of the overt security feature described herein, suitable viscosity values ​​of the radiation curable coating composition comprising platelet-shaped magnetic or magnetizable pigment particles are used: the viscosity at 25° C. for screen printing inks is between about 50 mPa s and about 3000 mPa s, the viscosity at 25° C. for flexographic printing inks is between about 50 mPa s and about 2000 mPa s, the viscosity at 25° C. for rotogravure printing inks is between about 50 mPa s and about 1000 mPa s, wherein the viscosity of security inks with viscosity values ​​between 100 mPa s and 3000 mPa s is measured using a Brookfield viscometer (model “RVDV-I Prime”), wherein the spindle and the rotation speed (rpm) are adjusted according to the following viscosity ranges: for viscosity values ​​between 100 and 500 mPa s, at 100 rpm, spindle 21; for viscosity values ​​between 500 mPa s and 2500 mPa s, spindle 22 is used; for viscosity values ​​between 100 and 500 mPa s, spindle 23 is used; for viscosity values ​​between 100 and 500 mPa s, spindle 24 is used; for viscosity values ​​between 100 and 500 mPa s, spindle 25 is used. s to 2500 mPa s, at 100 rpm, spindle 27; and for viscosity values ​​between 2500 mPa s and 3000 mPa s, at 50 rpm, spindle 27, and wherein a rotational viscometer DHR-2 from TA Instruments (with cone geometry and 40 mm diameter) was used at 25° C. and 1000 s -1 The viscosity of safety inks with viscosity values ​​between 10mPas and 100mPas can be measured at 25°C or with a DIN 4" cup.

[0090] The method described herein further comprises a step b) of exposing the layer obtained in step a) to magnetic field lines of a magnetic field generating device, wherein the magnetic field lines form an elevation angle |γ| with the surface of the substrate (x10), the value of the elevation angle |γ| being between about 10° and about 45° (10°≤|γ|≤45°), preferably between about 15° and about 40° (15°≤|γ|≤40°); and more preferably between about 15° and about 35° (15°≤|γ|≤35°), thereby orienting the flake-shaped magnetic or magnetizable pigment particles (for example by laying the substrate (x10) carrying the layer comprising the particles flat in a magnetic field, such as Fig.5A1 Step b) as described herein is carried out to uniaxially or biaxially orient the platelet-shaped magnetic or magnetizable pigment particles as described herein.

[0091] According to one embodiment, step b) is performed to uniaxially orient at least a portion of the platelet-shaped magnetic or magnetizable pigment particles described herein. Suitable magnetic field generating means for uniaxially orienting the platelet-shaped magnetic or magnetizable pigment particles described herein are not limited.

[0092] Examples of suitable magnetic field generating devices for uniaxially orienting particles are disclosed in US 7,047,883 and co-pending application PCT / EP2021 / 073863.

[0093] FIG. 5A-B of US 7,047,883 discloses a magnetic field generating device, which consists of two spaced-apart magnets 84, which are placed on a magnetic base 62 with their north poles facing the substrate. FIG. 9B of US 7,047,883 discloses a magnetic field generating device, which consists of a magnet 140, and the article is placed in a position offset relative to the magnet axis. FIG. 9C of US 7,047,883 discloses a magnetic field generating device, which consists of two magnets 142 and a magnet 142' with a rhombus cross-section, wherein the north poles of the two magnets 142 face the substrate, and the south pole of the middle magnet 142' faces the substrate. FIG. 9D of US 7,047,883 discloses a magnetic field generating device, which consists of two magnets 144 and a magnet 144' with a roof-shaped, hexagonal, circular, trapezoidal or other cross-section, wherein the north poles of the two magnets 144 face the substrate, and the south pole of the middle magnet 144' faces the substrate. FIG. 9E of US 7,047,883 discloses a magnetic field generating device consisting of five magnets, the first magnet 142 being a rhombus-shaped magnet with its north pole facing the substrate, the second magnet 146 being a rectangular magnet with its south pole facing the substrate, the third magnet 148 being a magnet with a round top with its north pole facing the substrate, the fourth magnet 150 being roof-shaped with its south pole facing the substrate, and the fifth magnet 152 also being a roof-shaped magnet with its north pole facing the substrate.

[0094] Co-pending application PCT / EP2021 / 073863 Figure 4 A1 discloses a magnetic field generating device consisting of a rod-shaped dipole magnet, and exposing particles in one or more regions (shown as dashed rectangles A) to a magnetic field of the magnetic field generating device herein (magnetic field lines are shown as lines with arrows pointing from the north pole to the south pole), wherein the magnetic field is substantially uniform, and wherein the magnetic field lines are substantially parallel to each other in the one or more regions. Co-pending application PCT / EP2021 / 073863 Figure 4 A2 discloses a magnetic field generating device consisting of an assembly including two rod-shaped dipole magnets (M1, M2) having the same magnetic orientation and an iron yoke (Y), and exposing particles in one or more regions (shown as dashed rectangles A) to a magnetic field of the magnetic field generating device (magnetic field lines are shown as lines with arrows pointing from the north pole to the south pole), wherein the magnetic field is substantially uniform and wherein the magnetic field lines are substantially parallel to each other in the one or more regions. Co-pending application PCT / EP2021 / 073863 Figure 6 AB discloses a magnetic field generating device consisting of a rectangular assembly including two rod-shaped dipole magnets (M1, M2) and two pole pieces (P1, P2), and exposing particles to a magnetic field of the magnetic field generating device (magnetic field lines are shown as lines with arrows pointing from the north pole to the south pole) in one or more regions (shown as dashed rectangles A), wherein the magnetic field is substantially uniform and wherein the magnetic field lines are substantially parallel to each other in the regions.

[0095] According to one embodiment, step b) is performed to biaxially orient the platelet-shaped magnetic or magnetizable pigment particles as described herein. Suitable magnetic field generating means for biaxially orienting the platelet-shaped magnetic or magnetizable pigment particles as described herein are not limited.

[0096] Examples of suitable magnetic field generating devices for uniaxially orienting particles are disclosed in co-pending applications PCT / EP2021073983, WO 2018 / 019594 A1, WO 2016 / 083259 A1, WO 2021 / 239607A1 and co-pending application EP2178995.3.

[0097] PCT / EP2021073983 Figure 4B1 (see also WO 2018 / 019594 A1) discloses a magnetic field generating device consisting of a linear arrangement of at least four magnets (M1-M4), wherein the at least four magnets (M1-M4) are positioned in a staggered manner or in a zigzag manner, and the particles are exposed to the magnetic field of the magnetic field generating device in one or more regions (shown as dashed rectangles A, A') (the magnetic field lines are shown as lines with arrows pointing from the north pole to the south pole), wherein the magnetic field is substantially uniform and wherein the magnetic field lines are substantially parallel to each other in the one or more regions. EP 2 157 141 A1 discloses a similar suitable magnetic field generating device in FIG. 5, wherein the magnetic field generating device consists of a linear arrangement of at least three, preferably at least four magnets, wherein the magnets are positioned in a staggered manner or in a zigzag manner. PCT / EP2021073983 Figure 4 B2 (see also WO 2018 / 019594 A1) discloses a magnetic field generating device consisting of two dipole magnets (M1, M2) with opposite magnetic directions, and exposing particles in one or more regions (shown as dashed rectangles A, A') to a magnetic field of the magnetic field generating device (magnetic field lines are shown as lines with arrows pointing from the north pole to the south pole), wherein the magnetic field is substantially uniform and wherein the magnetic field lines are substantially parallel to each other in the one or more regions. PCT / EP2021073983 Figure 4 B3 (see also WO 2018 / 019594 A1) discloses a magnetic field generating device consisting of two dipole magnets (M1, M2) having the same magnetic direction. Figure 4 As shown in B3, the flaky magnetic or magnetizable pigment particles in the coating (410) on the substrate (420) are exposed to a magnetic field (magnetic field lines are shown as lines with arrows pointing from the north pole to the south pole) of a magnetic field generating device (430) in one or more regions (shown as dashed rectangles A), wherein the magnetic field is substantially uniform, and wherein the magnetic field lines are substantially parallel to each other in the one or more regions, and wherein the substrate (420) carrying the coating (410) is arranged at an angle α as described herein in the one or more regions. PCT / EP2021073983 Figure 4 B4 (see also WO 2018 / 019594 A1) discloses a magnetic field generating device consisting of a Halbach array comprising five dipole magnets (M1-M5), and exposing particles to a magnetic field of the magnetic field generating device (magnetic field lines are shown as lines with arrows pointing from the north pole to the south pole) in one or more regions (shown as dashed parallelepiped A), wherein the magnetic field is substantially uniform and wherein the magnetic field lines are substantially parallel to each other in the one or more regions. PCT / EP2021073983 Figure 4B5 (see also WO 2016 / 083259 A1) discloses a magnetic field generating device, which consists of a Halbach cylinder assembly including four structures, each structure including a magnetic bar (M1-M4) surrounded by a magnetic wire coil (not shown), and the particles are exposed to the magnetic field of the magnetic field generating device in one or more regions (shown as a dashed rectangle A) (the magnetic field lines are shown as lines with arrows pointing from the north pole to the south pole), wherein the magnetic field is substantially uniform, and wherein the magnetic field lines are substantially parallel to each other in the one or more regions. PCT / EP2021073983 Figure 4 B6 (see also WO 2021 / 239607 A1) discloses a magnetic field generating device consisting of an assembly of eight rod-shaped dipole magnets (M1-M8), the assembly comprising: a first group comprising a first rod-shaped dipole magnet (M4) and two second rod-shaped dipole magnets (M1, M6), a second group comprising a first rod-shaped dipole magnet (M5) and two second rod-shaped dipole magnets (M3; M8), and a third rod-shaped dipole magnet (M2, M7) of the first pair, and exposing particles in one or more regions (shown as dashed rectangles A) to a magnetic field of the magnetic field generating device (magnetic field lines are shown as lines with arrows pointing from the north pole to the south pole), wherein the magnetic field is substantially uniform and wherein the magnetic field lines are substantially parallel to each other in the one or more regions. PCT / EP2021073983 Fig.5A1 -3 discloses a magnetic field generating device consisting of an assembly including nine rod-shaped dipole magnets (M1-M5) having alternating north-south magnetic directions and arranged in a row, and exposing particles to a magnetic field (magnetic field lines are shown as lines with arrows pointing from the north pole to the south pole) of the magnetic field generating device in one or more regions (shown as dashed parallelepiped A), wherein the magnetic field is substantially uniform and wherein the magnetic field lines are substantially parallel to each other in the one or more regions.

[0098] The method described herein further comprises a step c): partially simultaneously with step b) or after step b), preferably partially simultaneously with step b), a step of at least partially curing the layer with a curing unit, thereby at least partially fixing the position and orientation of the particles, so that the particles have the same elevation angle |α|, which is between about 10° and about 45° (10°≤angle |α|≤45°), preferably between about 15° and about 40° (15°≤angle |α|≤40°); and more preferably between about 15° and about 35° (15°≤angle |α|≤35°), thereby forming a color constant layer (x20) described herein. By "partially simultaneously", it is meant that the two steps are performed partially simultaneously, that is, the time for performing the respective steps partially overlaps. In the context described herein, when curing is performed partially simultaneously with the orientation step b), it must be understood that curing becomes effective after orientation, so that the particles have time to orient before the color constant layer (x20) is completely or partially cured. If step c) is performed after step b) as described herein, the time between the steps is preferably between about 0.1 seconds and about 1.5 seconds, more preferably between about 0.1 and 0.5 seconds.

[0099] According to a particularly preferred embodiment of the present invention, the radiation coating composition described herein is a UV-Vis-curable coating composition. UV-Vis curing advantageously allows a very fast curing process, and therefore significantly reduces the preparation time of the color constant layer (x20) described herein. Preferably, the UV-Vis-curable coating composition includes one or more compounds selected from the group consisting of radiation curable compounds and cationic curable compounds. The UV-Vis-curable coating composition described herein can be a mixed system and includes a mixture of one or more cationic curable compounds and one or more radiation curable compounds. Cationic curable compounds are cured by a cationic mechanism, and the cationic mechanism typically includes activation by radiation of one or more photoinitiators, and the photoinitiator releases cationic species, such as acid, and then initiates curing so that monomers and / or oligomers react and / or crosslink, thereby hardening the coating composition. Radiation curable compounds are cured by a free radical mechanism, and the free radical mechanism typically includes activation by radiation of one or more photoinitiators, thereby generating free radicals, and then initiating polymerization, thereby hardening the coating composition. Depending on the monomer, oligomer or prepolymer used to prepare the binder contained in the UV-Vis curable coating composition described herein, different photoinitiators can be used. Suitable examples of free radical photoinitiators are known to those skilled in the art, and include, but are not limited to, acetophenone, benzophenone, benzyl dimethyl ketal, α-amino ketone, α-hydroxy ketone, phosphine oxide and phosphine oxide derivatives, and mixtures of two or more thereof. Suitable examples of cationic photoinitiators are known to those skilled in the art, and include, but are not limited to, onium salts such as organic iodonium salts (e.g., diaryl iodonium salts), oxonium (e.g., triaryl oxonium salts) and sulfonium salts (e.g., triaryl sulfonium salts), and mixtures of two or more thereof. Other examples of useful photoinitiators can be found in standard textbooks such as "Chemistry & Technology of UV & EB Formulation for Coatings, Inks & Paints", Volume III, "Photoinitiators for Free Radical Cationic and Anionic Polymerization", 2nd Edition, JV Crivello & K. Dietliker, edited by G. Bradley and published jointly by John Wiley & Sons and SITA Technology Limited in 1998. It may also be advantageous to include a sensitizer along with more than one photoinitiator to achieve efficient curing.Typical examples of suitable photosensitizers include, but are not limited to, isopropyl-thioxanthone (ITX), 1-chloro-2-propoxy-thioxanthone (CPTX), 2-chloro-thioxanthone (CTX) and 2,4-diethyl-thioxanthone (DETX) and mixtures of two or more thereof. The one or more photoinitiators contained in the UV-Vis curable coating composition are preferably present in a total amount of about 0.1 wt-% to about 20 wt-%, more preferably about 1 wt-% to about 15 wt-%, the weight percentage being based on the total weight of the UV-Vis curable coating composition.

[0100] According to one embodiment, the radiation curable composition described herein is a UV-Vis LED curable composition, i.e., a composition that can be cured under exposure to one or more wavelengths between about 365 nm and about 470 nm, more preferably by exposure to 365 nm and / or 385 nm and / or 395 nm UV light emitted by a UV-LED light source. If the UV-Vis LED curable composition only includes radiation curable monomers / oligomers, the composition typically includes one or more radiation curable photoinitiators that absorb within the wavelength range and / or one or more photoinitiators that can be activated by a photosensitizer. Preferably, the photoinitiator that absorbs within the range is selected from the group consisting of phosphine oxides, phosphine oxide derivatives, thioxanthones, and mixtures thereof. If a photosensitizer is present, the photosensitizer is preferably selected from the group consisting of thioxanthones described above (which can be used as photoinitiators and photosensitizers as known to those skilled in the art), and one or more photoinitiators are preferably selected from the group consisting of phosphine oxides, phosphine oxide derivatives, α-aminoketones, benzophenones, and mixtures thereof. When using Norrish II type photoinitiators such as thioxanthone and / or benzophenone, the radiation curable composition may additionally include an amine-containing compound such as Esacure A198 (IGM Resins, CAS 1793103-51-1), Speedcure 7040 (Lambson, CAS 1182751-31-0) or an amine-modified polyether acrylate such as 80 (Allnex, CAS 143748-77-0). When the UV-LED curable composition includes cationically curable monomers (partially or entirely radiation curable monomers / oligomers), the composition preferably includes one or more iodonium salts and one or more thioxanthones, such as those described above.

[0101] The radiation curable coating composition recorded herein can further include one or more marking substances or tracers (tangant) and / or one or more machine readable materials, provided that their presence will not meaningfully affect the observation of the color shift characteristics of the dominant security features recorded herein. The material can be selected from the group consisting of magnetic materials (different from the non-spherical magnetic or magnetizable pigment particles recorded herein), luminescent materials, conductive materials and infrared absorbing materials. As used herein, the term "machine readable material" refers to a material that exhibits at least one distinguishing characteristic that is not recognizable by the naked eye and can be included in a layer to provide a method for identifying the layer or the product comprising the layer by using a specific instrument.

[0102] The radiation curable coating compositions described herein may further include one or more additives, provided that their presence does not meaningfully affect the observation of the color shift characteristics of the dominant security features described herein. The additives include, but are not limited to, compounds and materials used to adjust the physical, rheological and chemical parameters of the coating composition, such as viscosity (e.g., solvents, thickeners and surfactants), uniformity (e.g., anti-settling agents, fillers and plasticizers), foaming (e.g., defoamers), lubricity (waxes, oils), UV stability (light stabilizers), adhesion, antistatic properties, storage stability (polymerization inhibitors), etc. The additives described herein may be present in the coating composition in amounts and forms known in the art including so-called nanomaterials wherein at least one of the sizes of the additives is in the range of 1 to 1000 nm.

[0103] The overt security feature described herein comprises an optically variable layer (x30) described herein.

[0104] According to one embodiment, the optically variable layer (x30) described herein has a thickness between about 1 μm and about 10 μm, preferably between about 2 μm and about 8 μm, and more preferably between about 2 μm and about 6 μm (measured by using Extramess Inductive Digital Comparator 2001 (provided by Mahr).

[0105] Preferably, the optically variable layer (x30) is obtained from a cholesteric liquid crystal polymer precursor composition comprising at least one nematic compound, at least one chiral dopant, at least one photoinitiator and one or more solvents.

[0106] The cholesteric liquid crystal precursor composition comprises (i) one or more nematic compounds A and (ii) one or more chiral dopant compounds B, which are capable of producing a cholesteric state of the cholesteric liquid crystal precursor composition upon heating. The pitch of the obtainable cholesteric state depends on the relative proportions of the nematic compound and the chiral dopant compound. The (total) concentration of the one or more nematic compounds A used in the cholesteric liquid crystal precursor composition of the present invention is about 4 to about 30 times, preferably about 4 to about 25 times, of the (total) concentration of the one or more chiral dopant compounds B. The above-mentioned one or more chiral dopant compounds B are preferably present in an amount of about 0.1 wt-% to about 30 wt-%, more preferably about 0.1 wt-% to about 20 wt-%, and even more preferably about 3 wt-% to about 10 wt-%, the weight percentage being based on the total weight of the cholesteric liquid crystal precursor composition. The one or more nematic compounds A are preferably present in an amount of about 20 wt-% to about 50 wt-%, more preferably about 30 wt-% to about 45 wt-%, the weight percentage being based on the total weight of the cholesteric liquid crystal precursor composition.

[0107] Each of the one or more nematic compounds A and the one or more chiral dopant compounds B may include at least one compound containing at least one polymerizable group. For example, all of the one or more nematic compounds A and all of the one or more chiral dopant compounds B may include at least one polymerizable group. The at least one polymerizable group may, for example, include a group capable of participating in free radical polymerization, in particular a (preferably activated) unsaturated carbon-carbon bond, such as an acrylate having the formula H2C=CH-C(O)-O.

[0108] Nematic (precursor) compounds A suitable for cholesteric liquid crystal precursor compositions are known in the art; when used alone (i.e., without a chiral dopant compound), they themselves align in a state characterized by their birefringence. Non-limiting examples of nematic compounds A suitable for use in the present invention are described in, for example, WO 93 / 22397A1, WO 95 / 22586A1, EP 0 847432 B1, US 6,589,445, US 2007 / 0224341. The entire disclosure of these documents is hereby incorporated by reference.

[0109] A preferred class of nematic compounds A for use in the present invention includes one or more polymerizable groups per molecule that are identical or different from each other. Examples of polymerizable groups include groups that can participate in free radical polymerization, particularly groups containing carbon-carbon double or triple bonds, such as acrylate moieties, vinyl moieties or acetylenic moieties. A particularly preferred polymerizable group is an acrylate moiety.

[0110] The nematic compound A used in the present invention may further include one or more optionally substituted aromatic groups, preferably phenyl. Examples of optional substituents for the aromatic group include those described herein as examples of substituents on the benzene ring of the chiral dopant compound of formula (I), such as alkyl and alkoxy.

[0111] Examples of groups that may optionally be present to link the polymerizable group and the aromatic group (e.g., phenyl) in the nematic compound A include those exemplified herein for the chiral dopant compound B of formula (I) (including those of formula (IA) and formula (IB) described below). For example, the nematic compound A may include one or more groups of formulas (i) to (vi), which are indicated below as examples of A1 and A2 in formula (I) (and formulas (IA) and (IB)), typically bonded to an optionally substituted phenyl group.

[0112] Non-limiting specific examples of nematic compounds suitable for use in the present invention include, but are not limited to, the following compounds: 2-methoxybenzene-1,4-diylbis[4-({[4-(acryloyloxy)butoxy]carbonyl}oxy)benzoate]; 4-{[4-({[4-(acryloyloxy)butoxy]carbonyl}oxy)benzoyl]oxy}-2-methoxyphenyl 4-({[4-(acryloyloxy)butoxy]carbonyl}oxy)-2-methylbenzoate; 2-methoxybenzene-1,4-diylbis[4-({[4-(acryloyloxy)butoxy]carbonyl}oxy)-2-methyl-benzoate]; 2-methylbenzene-1,4-diylbis[4-({[4-(acryloyloxy)butoxy]carbonyl}oxy)benzoyl]oxy}-2-methoxyphenyl 4-({[4-(acryloyloxy)butoxy]carbonyl}oxy)-2-methylbenzoate 4-{[4-({[4-(acryloyloxy)butoxy]carbonyl}oxy)benzoyl]oxy}-2-methylphenyl 4-({[4-(acryloyloxy)butoxy]carbonyl}oxy)-3-methoxybenzoate; 2-methylbenzene-1,4-diylbis[4-({[4-(acryloyloxy)butoxy]carbonyl}oxy)benzoate; 2-methylbenzene-1,4-diylbis[4-({[4-(acryloyloxy)butoxy]carbonyl}oxy)-3-methoxybenzoate; 4-{[4-({[4-(acryloyloxy)butoxy]carbonyl}oxy)benzoyl]oxy}-2-methylphenyl 4-({[4-(acryloyloxy)butoxy]carbonyl}oxy)-3-methoxybenzoate Methylphenyl 4-({[4-(acryloyloxy)butoxy]carbonyl}oxy)-3,5-dimethoxybenzoate; 2-methylbenzene-1,4-diylbis[4-({[4-(acryloyloxy)butoxy]carbonyl}oxy)-3,5-dimethoxy-benzoate]; 2-methoxybenzene-1,4-diylbis[4-({[4-(acryloyloxy)butoxy]carbonyl}oxy)-3,5-dimethoxybenzoate]; 4-{[4-({[4-(acryloyloxy)butoxy]carbonyl}oxy)-3-methoxybenzoyl]oxy}-2-methoxyphenyl 4-({[4-(acryloyloxy)butoxy]carbonyl}oxy)-3,5-dimethoxybenzoic acid ester; 4-({4-[4-(acryloyloxy)butoxy]benzoyl}oxy)-3-methylphenyl 4-[4-(acryloyloxy)butoxy]-2-methylbenzoate; 4-({4-[4-(acryloyloxy)butoxy]benzoyl}oxy)-3-methylphenyl 4-[4-(acryloyloxy)butoxy]-3-methylbenzoate; 2-methylbenzene-1,4-diylbis{4-[4-(acryloyloxy)butoxy]-2-methylbenzoate}; 4-({4-[4-(acryloyloxy)butoxy]-2-methylbenzoyl}oxy)-3-methylphenyl 4-[4-(acryloyloxy)butoxy]-2,5-dimethylbenzoate;2-Methylbenzene-1,4-diylbis{4-[4-(acryloyloxy)butoxy]-2,5-dimethylbenzoate}2-Methylbenzene-1,4-diylbis{4-[4-(acryloyloxy)butoxy]benzoate}; 4-({4-[4-(acryloyloxy)butoxy]-3,5-dimethylbenzoyl}oxy)-3-methylphenyl 4-[4-(acryloyloxy)butoxy]-2,5-dimethylbenzoate; 2-Methylbenzene-1,4-diylbis{4-[4-(acryloyloxy)butoxy]-3,5-dimethylbenzoate; 2-Methoxybenzene-1,4-diylbis{4-[4-(acryloyloxy)butoxy]-3,5-dimethylbenzoate; 4-({4-[4-(acryloyloxy)butoxy]-3,5-dimethylbenzoyl}oxy)-3-methylphenyl 4-[4-(acryloyloxy)butoxy]-2,5-dimethylbenzoate 4-({4-[4-(acryloyloxy)butoxy]benzoyl}oxy)-3-methoxyphenyl 4-[4-(acryloyloxy)butoxy]-3-methylbenzoate; 4-({4-[4-(acryloyloxy)butoxy]benzoyl}oxy)-3-methoxyphenyl 4-[4-(acryloyloxy)butoxy]-2,5-dimethylbenzoate; 2-methoxybenzene-1,4-diylbis{4-[4-(acryloyloxy)butoxy]-3-methylbenzoate; 4-({4-[4-(acryloyloxy)butoxy]benzoyl}oxy)-3-methoxyphenyl 4-[4-(acryloyloxy)butoxy]-2,5-dimethylbenzoate; 2-methoxybenzene-1,4-diylbis{4-[4-(acryloyloxy)butoxy]-3-methylbenzoate 2-(4-(acryloyloxy)butoxy]-2-methoxybenzoate}; 2-methoxybenzene-1,4-diylbis{4-[4-(acryloyloxy)butoxy]-3,5-dimethoxybenzoate}; 2-methoxybenzene-1,4-diylbis{4-[4-(acryloyloxy)butoxy]-3-methoxybenzoate}; 2-ethoxybenzene-1,4-diylbis{4-[4-(acryloyloxy)butoxy]benzoate}; 2-ethoxybenzene-1,4-diylbis{4-[4-(acryloyloxy)butoxy]-2-methylbenzoate}; 2-(propan-2-yloxy)benzene-1,4-diylbis{4-[4-(acryloyloxy)butoxy]benzoate}; 4-({4-[4-(acryloyloxy)butoxy] ]benzoyl}oxy)-2-(propan-2-yloxy)phenyl 4-[4-(acryloyloxy)butoxy]-2-methylbenzoate; 2-(propan-2-yloxy)benzene-1,4-diylbis{4-[4-(acryloyloxy)butoxy]-2-methylbenzoate}; 2-(propan-2-yloxy)benzene-1,4-diylbis{4-[4-(acryloyloxy)butoxy]-2,5-dimethyl-benzoate}; 2-(propan-2-yloxy)benzene-1,4-diylbis{4-[4-(acryloyloxy)butoxy]-3,5-dimethyl-benzoate}; and 2-(propan-2-yloxy)benzene-1,4-diylbis{4-[4-(acryloyloxy)butoxy]-3,5-dimethyl-benzoate}. ;

[0113] The one or more chiral dopant compounds B used in the present invention preferably include at least one polymerizable group. Suitable examples of the one or more chiral dopant compounds B include those of formula (I):

[0114]

[0115] in:

[0116] R1, R2, R3, R4, R5, R6, R7 and R8 each independently represent a C1-C6 alkyl group and a C1-C6 alkoxy group;

[0117] A1 and A2 each independently represent a group of formula (i) to (vi):

[0118] (i)-[(CH2) y -O] z -C(O)-CH=CH2;

[0119] (ii) -C(O)-D1-O-[(CH2) y -O] z -C(O)-CH=CH2;

[0120] (iii) -C(O)-D2-O-[(CH2) y -O] z -C(O)-CH=CH2;

[0121] (iv)-[COO-(CH2) y -O] z -C(O)-CH=CH2;

[0122] (v)-C(O)-D1-O-[COO-(CH2) y -O] z -C(O)-CH=CH2;

[0123] (vi) -C(O)-D2-O-[COO-(CH2) y -O] z -C(O)-CH=CH2;

[0124] D1 represents a group of the formula

[0125]

[0126] D2 represents a group of the formula

[0127]

[0128] m, n, o, p, q, r, s, and t each independently represent 0, 1, or 2;

[0129] y represents 0, 1, 2, 3, 4, 5, or 6;

[0130] If y is equal to 0, then z is equal to 0, and if y is equal to 1-6, then z is equal to 1.

[0131] In one embodiment, the one or more chiral dopant compounds B may include one or more isomannide derivatives of formula (IA):

[0132]

[0133] in:

[0134] R1, R2, R3, R4, R5, R6, R7 and R8 each independently represent a C1-C6 alkyl group and a C1-C6 alkoxy group;

[0135] A1 and A2 each independently represent a group of formula (i) to (vi):

[0136] (i)-[(CH2) y -O] z -C(O)-CH=CH2;

[0137] (ii) -C(O)-D1-O-[(CH2)yO] z -C(O)-CH=CH2;

[0138] (iii) -C(O)-D2-O-[(CH2)yO] z -C(O)-CH=CH2;

[0139] (iv)-[COO-(CH2) y -O] z -C(O)-CH=CH2;

[0140] (v)-C(O)-D1-O-[COO-(CH2) y -O] z -C(O)-CH=CH2;

[0141] (vi) -C(O)-D2-O-[COO-(CH2) y -O] z -C(O)-CH=CH2;

[0142] D1 represents a group of the formula

[0143]

[0144] D2 represents a group of the formula

[0145]

[0146] m, n, o, p, q, r, s, and t each independently represent 0, 1, or 2;

[0147] y represents 0, 1, 2, 3, 4, 5, or 6;

[0148] If y is equal to 0, then z is equal to 0, and if y is equal to 1-6, then z is equal to 1.

[0149] In an exemplary embodiment of the compound of formula (IA) (and the compound of formula (I)), R1, R2, R3, R4, R5, R6, R7 and R8 each independently represent a C1-C6 alkyl group. In another embodiment, R1, R2, R3, R4, R5, R6, R7 and R8 in formula (IA) (and formula (I)) each independently represent a C1-C6 alkoxy group.

[0150] In another exemplary embodiment of the compounds of Formula (I) and Formula (IA), A1 and A2 each independently represent a compound of the formula -[(CH2) y -O] z -C(O)-CH=CH2; R1, R2, R3 and R4 each independently represent a C1-C6 alkyl group; and m, n, o, and p each independently represent 0, 1, or 2. In another embodiment, A1 and A2 in formula (I) and formula (IA) each independently represent a group of the formula -[(CH2) y -O] z -C(O)-CH=CH2 group; R1, R2, R3 and R4 each independently represent a C1-C6 alkoxy group; and m, n, o, and p each independently represent 0, 1, or 2.

[0151] In another embodiment of the compounds of formula (IA) (and formula (I)), A1 and A2 each independently represent a compound of the formula -C(O)-D1-O-[(CH2) y -O] z -C(O)-CH=CH2 and / or a group of the formula -C(O)-D2-O-[(CH2) y -O] z -C(O)-CH=CH2; and R1, R2, R3, R4, R5, R6, R7 and R8 each independently represent a C1-C6 alkyl group. In another embodiment, A1 and A2 in formula (IA) (and in formula (I)) each independently represent a group of the formula -C(O)-D1-O-[(CH2) y -O] z-C(O)-CH=CH2 and / or a group of the formula -C(O)-D2-O-[(CH2) y -O] z -C(O)-CH=CH2 group; and R1, R2, R3, R4, R5, R6, R7 and R8 each independently represent a C1-C6 alkoxy group.

[0152] In another embodiment of the compounds of formula (IA) (and formula (I)), A1 and A2 each independently represent a compound of the formula -C(O)-D1-O-[COO-(CH2) y -O] z -C(O)-CH=CH2 and / or a group of the formula -C(O)-D2-O-[COO-(CH2) y -O] z -C(O)-CH=CH2; and R1, R2, R3, R4, R5, R6, R7 and R8 each independently represent a C1-C6 alkyl group. In another embodiment, A1 and A2 in formula (IA) (and in formula (I)) each independently represent a group of the formula -C(O)-D1-O-[COO-(CH2) y -O] z -C(O)-CH=CH2 and / or a group of the formula -C(O)-D2-O-[COO-(CH2) y -O] z -C(O)-CH=CH2 group; and R1, R2, R3, R4, R5, R6, R7 and R8 each independently represent a C1-C6 alkoxy group.

[0153] In another embodiment, the one or more chiral dopant compounds B may include one or more isosorbide derivatives represented by formula (IB):

[0154]

[0155] in:

[0156] R1, R2, R3, R4, R5, R6, R7 and R8 each independently represent a C1-C6 alkyl group and a C1-C6 alkoxy group;

[0157] A1 and A2 each independently represent a group of formula (i) to (vi):

[0158] (i)-[(CH2)yO] z -C(O)-CH=CH2;

[0159] (ii) -C(O)-D1-O-[(CH2)yO] z -C(O)-CH=CH2;

[0160] (iii) -C(O)-D2-O-[(CH2)yO] z -C(O)-CH=CH2;

[0161] (iv)-[COO-(CH2) y -O] z -C(O)-CH=CH2;

[0162] (v)-C(O)-D1-O-[COO-(CH2) y -O] z -C(O)-CH=CH2;

[0163] (vi) -C(O)-D2-O-[COO-(CH2) y -O] z -C(O)-CH=CH2;

[0164] D1 represents a group of the formula

[0165]

[0166] D2 represents a group of the formula

[0167]

[0168] m, n, o, p, q, r, s, and t each independently represent 0, 1, or 2;

[0169] y represents 0, 1, 2, 3, 4, 5, or 6;

[0170] If y is equal to 0, then z is equal to 0, and if y is equal to 1-6, then z is equal to 1.

[0171] In one embodiment of the compound of formula (IB), R1, R2, R3, R4, R5, R6, R7 and R8 each independently represent C1-C6 alkyl; and m, n, o, and p each independently represent 0, 1, or 2. In another embodiment, R1, R2, R3, R4, R5, R6, R7 and R8 in formula (IB) each independently represent C1-C6 alkoxy; and m, n, o, and p each independently represent 0, 1, or 2.

[0172] In another embodiment of the compound of formula (IB), A1 and A2 each independently represent a compound of the formula -[(CH2) y -O] z-C(O)-CH=CH2; R1, R2, R3 and R4 each independently represent a C1-C6 alkyl group; and m, n, o, and p each independently represent 0, 1, or 2. In another embodiment, A1 and A2 in formula (IB) each independently represent a group of the formula -[(CH2) y -O] z -C(O)-CH=CH2 group; R1, R2, R3 and R4 each independently represent a C1-C6 alkoxy group; and m, n, o, and p each independently represent 0, 1, or 2.

[0173] In another embodiment of the compound of formula (IB), A1 and A2 each independently represent a compound of the formula -C(O)-D1-O-[(CH2) y -O] z -C(O)-CH=CH2 and / or a group of the formula -C(O)-D2-O-[(CH2) y -O] z -C(O)-CH=CH2; R1, R2, R3, R4, R5, R6, R7 and R8 each independently represent a C1-C6 alkyl group; and m, n, o, and p each independently represent 0, 1, or 2. In another embodiment, A1 and A2 in formula (IB) each independently represent a group of the formula -C(O)-D1-O-[(CH2) y -O] z -C(O)-CH=CH2 and / or a group of the formula -C(O)-D2-O-[(CH2) y -O] z -C(O)-CH=CH2 group; R1, R2, R3, R4, R5, R6, R7 and R8 each independently represent a C1-C6 alkoxy group; and m, n, o, and p each independently represent 0, 1, or 2.

[0174] In another embodiment of the compound of formula (IB), A1 and A2 each independently represent a compound of the formula -C(O)-D1-O-[COO-(CH2) y -O] z -C(O)-CH=CH2 and / or a group of the formula -C(O)-D2-O-[COO-(CH2) y -O] z -C(O)-CH=CH2; R1, R2, R3, R4, R5, R6, R7 and R8 each independently represent a C1-C6 alkyl group; and m, n, o, and p each independently represent 0, 1, or 2. In another embodiment, A1 and A2 in formula (IB) each independently represent a group of the formula -C(O)-D1-O-[COO-(CH2) y -O] z-C(O)-CH=CH2 and / or a group of the formula -C(O)-D2-O-[COO-(CH2) y -O] z -C(O)-CH=CH2 group; R1, R2, R3, R4, R5, R6, R7 and R8 each independently represent a C1-C6 alkoxy group; and m, n, o, and p each independently represent 0, 1, or 2.

[0175] Non-limiting examples of the chiral dopant compound B of formula (I) used in the present invention include, but are not limited to, the following compounds: 2,5-bis-O-(4-{[4-(acryloyloxy)-3-methoxybenzoyl]oxy}-3-methoxybenzoyl)-1,4:3,6-dianhydro-D-mannitol; 2-O-(4-{[4-(acryloyloxy)-3-methoxybenzoyl]oxy}-3-methoxybenzoyl)-5-O-(4-{[4-(acryloyloxy)-3-methoxybenzoyl]oxy}-benzoyl)-1,4:3,6-dianhydro-D-mannitol; 2,5-bis-O-(4-{[4-(acryloyloxy)-3-methoxybenzoyl]oxy}-benzoyl)-1,4:3,6-dianhydro-D-mannitol; ]oxy}-benzoyl)-1,4:3,6-dianhydro-D-mannitol; 2,5-bis-O-(4-{[4-(acryloyloxy)-butoxy]-benzoyl})-1,4:3,6-dianhydro-D-mannitol; 2,5-bis-O-[4-(acryloyloxy)-2-methylbenzoyl]-1,4:3,6-dianhydro-D-mannitol; 2,5-bis-O-(4-{[4-(acryloyloxy)-3-methoxybenzoyl]oxy}-benzoyl)-1,4:3,6-dianhydro-D-mannitol; 2,5-bis-O-(4-{[4-(acryloyloxy)-benzoyl]oxy}-3-methoxybenzoyl)- 1,4:3,6-dianhydro-D-mannitol; 2-O-(4-{[4-(acryloyloxy)benzoyl]oxy}-2-methoxybenzoyl)-5-O-(4-{[4-(acryloyloxy)benzoyl]oxy}-3-methoxybenzoyl)-1,4:3,6-dianhydro-D-mannitol; 2,5-bis-O-(4-{[4-(acryloyloxy)benzoyl]oxy}-2-methoxybenzoyl)-1,4:3,6-dianhydro-D-mannitol; 2-O-(4-{[4-(acryloyloxy)benzoyl]oxy}-2-methoxybenzoyl)-5-O-(4-{[4-(acryloyloxy)-2-methyl 2-O-(4-{[4-(acryloyloxy)benzoyl]oxy}-2-methoxybenzoyl)-1,4:3,6-dianhydro-D-mannitol; 2-O-(4-{[4-(acryloyloxy)benzoyl]oxy}-2-methoxybenzoyl)-5-O-(4-{[4-(acryloyloxy)-3-methylbenzoyl]oxy}-2-methoxybenzoyl)-1,4:3,6-dianhydro-D-mannitol; 2-O-(4-{[4-(acryloyloxy)benzoyl]oxy}-2-methoxybenzoyl)-5-O-(4-{[4-(acryloyloxy)-3-methylbenzoyl]oxy}-2-methoxybenzoyl)-1,4:3,6-dianhydro-D-mannitol;2-O-(4-{[4-(acryloyloxy)benzoyl]oxy}-2-methoxybenzoyl)-5-O-(4-{[4-(acryloyloxy)-2,5-dimethylbenzoyl]oxy}-2-methoxybenzoyl)-1,4:3,6-dianhydro-D-mannitol; 2-O-(4-{[4-(acryloyloxy)-2,5-dimethylbenzoyl]oxy}-2-methoxybenzoyl)-5-O-(4-{[4-(acryloyloxy)-3-methylbenzoyl]oxy}-2-methoxybenzoyl)-1,4:3,6-dianhydro-D-mannitol; 2-O-(4-{[4-(acryloyloxy)-2-methoxy-5-methylbenzoyl]oxy}-2-methoxybenzoyl benzoyl)-5-O-(4-{[4-(acryloyloxy)-3-methylbenzoyl]oxy}-2-methoxybenzoyl)-1,4:3,6-dianhydro-D-mannitol; 2-O-(4-{[4-(acryloyloxy)-2-methoxybenzoyl]oxy}-2-methoxybenzoyl)-5-O-(4-{[4-(acryloyloxy)-3-methylbenzoyl]oxy}-2-methoxybenzoyl)-1,4:3,6-dianhydro-D-mannitol; 2-O-(4-{[4-(acryloyloxy)-2-methoxybenzoyl]oxy}-2-methoxybenzoyl)-5-O-(4-{[4-(acryloyloxy)-3-methoxybenzoyl]oxy}-2-methoxybenzoyl)-1,4:3,6-dianhydro-D-mannitol; 2-O-(4-{[4-(acryloyloxy)-2-methoxybenzoyl]oxy}benzoyl)-5-O-(4-{[4-(acryloyloxy)-3-methoxybenzoyl]oxy}benzoyl)-1,4:3,6-dianhydro-D-mannitol; 2,5-bis-O-(4-{[4-(acryloyloxy)benzoyl]oxy}-3-methoxybenzoyl)-1,4:3,6-dianhydro-D-mannitol; 2-O-(4-{[4-(acryloyloxy)-2-methoxybenzoyl]oxy}-2,5-dimethylbenzoyl)-5-O-(4-{[4-(acryloyloxy)-3-methoxybenzoyl]oxy}benzoyl)-1,4:3,6-dianhydro-D-mannitol; 2-O-(4-{[4-(acryloyloxy)-2-methoxybenzoyl]oxy}-3-methylbenzoyl)-1,4:3,6-dianhydro-D-mannitol; 2-O-(4-{[4-(acryloyloxy)-2-methoxybenzoyl]oxy}-2-methylbenzoyl)-5-O-(4-{[4-(acryloyloxy)-3-methoxybenzoyl]oxy}-3-methylbenzoyl)-1,4:3,6-dianhydro-D-mannitol; 2-O-(4-{[4-(acryloyloxy)-2-methoxy-5-methylbenzoyl]oxy}-2-methylbenzoyl)-5-O-(4-{[4-(acryloyloxy)-5-methoxy-2-methylbenzoyl]oxy}-3-methylbenzoyl)-1,4:3,6-dianhydro-D-mannitol;2-O-(4-{[4-(acryloyloxy)benzoyl]oxy}-2-ethoxybenzoyl)-5-O-(4-{[4-(acryloyloxy)-3-ethoxybenzoyl]oxy}benzoyl)-1,4:3,6-dianhydro-D-mannitol; 2-O-(4-{[4-(acryloyloxy)benzoyl]oxy}-2-ethoxy-5-methylbenzoyl)-5-O-(4-{[4-(acryloyloxy)benzoyl]oxy}-3-ethoxybenzoyl]oxy}benzoyl)-1,4:3,6-dianhydro-D-mannitol; 2-O-(4-{[4-(acryloyloxy)benzoyl]oxy}-2-ethoxy-5-methylbenzoyl)-5-O-(4 -{[4-(acryloyloxy)-5-ethoxy-2-methylbenzoyl]oxy}benzoyl)-1,4:3,6-dianhydro-D-mannitol; 2-O-(4-{[4-(acryloyloxy)-3-ethoxybenzoyl]oxy}benzoyl)-5-O-(4-{[4-(acryloyloxy)-2-methylbenzoyl]oxy}-2-ethoxybenzoyl)-1,4:3,6-dianhydro-D-mannitol; 2-O-(4-{[4-(acryloyloxy)-2,5-dimethylbenzoyl]oxy}-2-ethoxybenzoyl)-5-O-(4-{[4-(acryloyloxy)-2-methylbenzoyl]oxy}-2-ethoxybenzoyl)- 1,4:3,6-dianhydro-D-mannitol; 2,5-bis-O-(4-{[4-(acryloyloxy)-2,5-dimethylbenzoyl]oxy}-2-ethoxybenzoyl)-1,4:3,6-dianhydro-D-mannitol; 2,5-bis-O-(4-{[4-(acryloyloxy)-2-ethoxybenzoyl]oxy}-2-ethoxybenzoyl)-1,4:3,6-dianhydro-D-mannitol; 2,5-bis-O-(4-{[4-(acryloyloxy)-2-methoxybenzoyl]oxy}-2-ethoxybenzoyl)-1,4:3,6-dianhydro-D-mannitol; 2,5-bis-O-(4-{[4-(acryloyloxy)-2-methoxybenzoyl]oxy}-2-ethoxybenzoyl)-1,4:3,6-dianhydro-D-mannitol; -2-ethoxybenzoyl]oxy}-2-methoxybenzoyl)-1,4:3,6-dianhydro-D-mannitol; 2,5-bis-O-(4-{[4-(acryloyloxy)-2-ethoxybenzoyl]oxy}-3-methylbenzoyl)-1,4:3,6-dianhydro-D-mannitol; 2,5-bis-O-(4-{[4-(acryloyloxy)-2-ethoxybenzoyl]oxy}-3-methoxybenzoyl)-1,4:3,6-dianhydro-D-mannitol; 2,5-bis-O-(4-{[4-(acryloyloxy)-3-methoxybenzoyl]oxy}-3-methoxybenzoyl)-1,4:3,6-dianhydro-D-glucitol;D-glucitol 1,4:3,6-dianhydro-bis[4-[[4-[[[4-[(1-oxo-2-propenyl)oxy]butoxy]carbonyl]oxy]benzoyl]oxy]benzoate]; 2,5-bis-O-(4-{[4-(acryloyloxy)benzoyl]oxy}-3-methoxybenzoyl)-1,4:3,6-dianhydro-D-glucitol; 2-O-(4-{[4-(acryloyloxy)benzoyl]oxy}-2-methoxybenzoyl)-5-O-(4-{[4-(acryloyloxy)benzoyl]oxy}-3-methoxybenzoyl)-1,4:3,6-dianhydro-D-glucitol; 2,5-bis-O-(4-{[4-(acryloyloxy)benzoyl]oxy}- 2-O-(4-{[4-(acryloyloxy)benzoyl]oxy}-2-methoxybenzoyl)-1,4:3,6-dianhydro-D-glucitol; 2-O-(4-{[4-(acryloyloxy)benzoyl]oxy}-2-methoxybenzoyl)-5-O-(4-{[4-(acryloyloxy)-2-methylbenzoyl]oxy}-2-methoxybenzoyl)-1,4:3,6-dianhydro-D-glucitol; 2-O-(4-{[4-(acryloyloxy)benzoyl]oxy}-2-methoxybenzoyl)-5-O-(4-{[4-(acryloyloxy)benzoyl]oxy}-3-methylbenzoyl]oxy}-2-methoxybenzoyl)-1,4:3,6-dianhydro-D-glucitol; 2-O-(4-{[4-(acryloyloxy)benzoyl]oxy}-2-methoxybenzoyl)-5-O-(4-{[4-(acryloyloxy)-2,5-dimethylbenzoyl]oxy}-2-methoxybenzoyl)-1,4:3,6-dianhydro-D-glucitol; 2-O-(4-{[4-(acryloyloxy)-2,5-dimethylbenzoyl]oxy}-2-methoxybenzoyl)-5-O-(4-{[4-(acryloyloxy)-3-methylbenzoyl]oxy}-2-methoxybenzoyl)-1,4:3,6-dianhydro-D-glucitol; 2-O-(4-{[4-(acryloyloxy)-2-methoxy-5-methylbenzoyl]oxy} ]oxy}-2-methoxybenzoyl)-5-O-(4-{[4-(acryloyloxy)-3-methylbenzoyl]oxy}-2-methoxybenzoyl)-1,4:3,6-dianhydro-D-glucitol; 2-O-(4-{[4-(acryloyloxy)-2-methoxybenzoyl]oxy}-2-methoxybenzoyl)-5-O-(4-{[4-(acryloyloxy)-3-methylbenzoyl]oxy}-2-methoxybenzoyl)-1,4:3,6-dianhydro-D-glucitol; 2,5-bis-O-(4-{[4-(acryloyloxy)benzoyl]oxy}-3-methoxybenzoyl)-1,4:3,6-dianhydro-D-glucitol;2-O-(4-{[4-(acryloyloxy)-2-methoxybenzoyl]oxy}-2-methoxybenzoyl)-5-O-(4-{[4-(acryloyloxy)-3-methoxybenzoyl]oxy}-2-methoxybenzoyl)-1,4:3,6-dianhydro-D-glucitol; 2-O-(4-{[4-(acryloyloxy)-2-methoxybenzoyl]oxy}benzoyl)-5-O-(4-{[4-(acryloyloxy)-3-methoxybenzoyl]oxy}benzoyl)-1,4:3,6-dianhydro-D-glucitol; 2-O-(4-{[4-(acryloyloxy)-2-methoxybenzoyl]oxy}benzoyl)}-2,5-dimethylbenzoyl)-5-O-(4-{[4-(acryloyloxy)-3-methoxybenzoyl]oxy}-3-methylbenzoyl)-1,4:3,6-dianhydro-D-glucitol; 2-O-(4-{[4-(acryloyloxy)-2-methoxybenzoyl]oxy}-2-methylbenzoyl)-5-O-(4-{[4-(acryloyloxy)-3-methoxybenzoyl]oxy}-3-methylbenzoyl)-1,4:3,6-dianhydro-D-glucitol; 2-O-(4-{[4-(acryloyloxy)-2-methoxybenzoyl]oxy}-2-methylbenzoyl)-5-O-(4-{[4-(acryloyloxy)-3-methoxybenzoyl]oxy}-3-methylbenzoyl)-1,4:3,6-dianhydro-D-glucitol; O-(4-{[4-(acryloyloxy)benzoyl]oxy}-3-methylbenzoyl)-1,4:3,6-dianhydro-D-glucitol; 2-O-(4-{[4-(acryloyloxy)benzoyl]oxy}-2-ethoxybenzoyl)-5-O-(4-{[4-(acryloyloxy)-3-ethoxybenzoyl]oxy}benzoyl)-1,4:3,6-dianhydro-D-glucitol; 2-O-(4-{[4-(acryloyloxy)benzoyl]oxy}-2-ethoxy-5-methylbenzoyl)-5-O-(4-{[4-(acryloyloxy)benzoyl]oxy}-2-ethoxy-5-methylbenzoyl) 2-O-(4-{[4-(acryloyloxy)benzoyl]oxy}-2-ethoxy-5-methylbenzoyl)-5-O-(4-{[4-(acryloyloxy)-5-ethoxy-2-methylbenzoyl]oxy}benzoyl)-1,4:3,6-dianhydro-D-glucitol; 2-O-(4-{[4-(acryloyloxy)benzoyl]oxy}-2-ethoxy-5-methylbenzoyl)-5-O-(4-{[4-(acryloyloxy)-5-ethoxy-2-methylbenzoyl]oxy}benzoyl)-1,4:3,6-dianhydro-D-glucitol; 2-O-(4-{[4-(acryloyloxy)benzoyl]oxy}benzoyl)-5-O-(4-{[4-(acryloyloxy)-2-methylbenzoyl]oxy}-2-ethoxybenzoyl)-1,4:3,6-dianhydro-D-glucitol;2-O-(4-{[4-(acryloyloxy)-2,5-dimethylbenzoyl]oxy}-2-ethoxybenzoyl)-5-O-(4-{[4-(acryloyloxy)-2-methylbenzoyl]oxy}-2-ethoxybenzoyl)-1,4:3,6-dianhydro-D-glucitol; 2,5-bis-O-(4-{[4-(acryloyloxy)-2,5-dimethylbenzoyl]oxy}-2-ethoxybenzoyl)-1,4:3,6-dianhydro-D-glucitol; 2,5-bis-O-(4-{[4-(acryloyloxy)-2-ethoxybenzoyl]oxy}-2-ethoxybenzoyl)-1,4:3,6-dianhydro-D-glucitol; 2,5-Bis-O-(4-{[4-(acryloyloxy)-2-methoxybenzoyl]oxy}-2-ethoxybenzoyl)-1,4:3,6-dianhydro-D-glucitol; 2,5-Bis-O-(4-{[4-(acryloyloxy)-2-ethoxybenzoyl]oxy}-2-methoxybenzoyl)-1,4:3,6-dianhydro-D-glucitol; 2,5-Bis-O-(4-{[4-(acryloyloxy)-2-ethoxybenzoyl]oxy}-2-methoxybenzoyl)-1,4:3,6-dianhydro-D-glucitol; 2,5-Bis-O-(4-{[4-(acryloyloxy)-2-ethoxybenzoyl]oxy}-3-methylbenzoyl)-1,4:3,6-dianhydro-D -glucitol; 2,5-bis-O-(4-{[4-(acryloyloxy)-2-ethoxybenzoyl]oxy}-3-methoxybenzoyl)-1,4:3,6-dianhydro-D-glucitol; 2,5-bis-O-[4-(acryloyloxy)benzoyl]-1,4:3,6-dianhydro-D-glucitol; 2,5-bis-O-[4-(acryloyloxy)benzoyl]-1,4:3,6-dianhydro-D-mannitol; 2,5-bis-O-(4-{[4-({[4-(acryloyloxy)-butoxy]carbonyl}oxy)benzoyl]oxy}-benzoyl)-1,4:3,6- Dianhydro-D-glucitol; 2,5-bis-O-(4-{[4-({[4-(acryloyloxy)-butoxy]carbonyl}oxy)-3-methoxybenzoyl]oxy}-benzoyl)-1,4:3,6-dianhydro-D-glucitol; 2,5-bis-O-(4-{[4-({[6-(acryloyloxy)-hexyloxy]carbonyl}oxy)benzoyl]oxy}-benzoyl)-1,4:3,6-dianhydro-D-glucitol; and 2,5-bis-O-[4-({[4-(acryloyloxy)-butoxy]carbonyl}oxy)benzoyl]-1,4:3,6-dianhydro-D-glucitol. ;

[0176] The cholesteric liquid crystal precursor composition includes one or more solvents. Suitable solvents are known to those skilled in the art and include, without limitation, low viscosity, weakly polar and aprotic organic solvents, such as methyl ethyl ketone (MEK), acetone, cyclopentanone, cyclohexanone, ethyl acetate, ethyl 3-ethoxypropionate and mixtures of two or more thereof. When present, the one or more solvents included in the cholesteric liquid crystal precursor composition are preferably present in an amount of about 30 wt-% to about 70 wt-%, more preferably about 40 to about 60 wt-%, the weight percentage being based on the total weight of the cholesteric liquid crystal precursor composition.

[0177] According to one embodiment, the cholesteric liquid crystal precursor composition described herein may further include one or more photoinitiators, and the cholesteric liquid crystal precursor composition is hardened by UV-visible light radiation during step f). Non-limiting examples of many suitable photoinitiators for the cholesteric liquid crystal precursor composition described herein include α-hydroxy ketones such as 1-hydroxy-cyclohexyl-phenyl-ketone and a mixture of 1-hydroxy-cyclohexyl-phenyl-ketone and one or more benzophenones (e.g., about 1:1), 2-hydroxy-2-methyl-1-phenyl-1-propanone, 2-hydroxy-1-[4-(2-hydroxyethoxy)phenyl]-2-methyl-1-propanone and 2-hydroxy-1-[4-[4-(1-hydroxy-2-methylpropionyl)phenoxy]phenyl]-2-methylpropan-1-one (e.g., manufactured by IGM Resins under the name ESACURE KIP 160 sold); phenylglyoxylates such as methyl benzoylformate and a mixture of 2-[2-oxo-2-phenyl-acetoxy-ethoxy]-ethyl oxy-phenyl-acetate and 2-[2-hydroxy-ethoxy]-ethyl oxy-phenyl-acetate; benzyl dimethyl ketal such as α,α-dimethoxy-α-phenylacetophenone; α-aminoketones such as 2-benzyl-2-(dimethylamino)-1-[4-(4-morpholinyl)phenyl]-butan-1-one, 2-Dimethylamino-2-(4-methyl-benzyl)-1-(4-morpholin-4-yl-phenyl)-butan-1-one and 2-methyl-1-[4-(methylthio)phenyl]-2-(4-morpholinyl)-1-propanone; phosphine oxides and phosphine oxide derivatives such as diphenyl(2,4,6-trimethylbenzoyl)-phosphine oxide; phenyl-bis(2,4,6-trimethylbenzoyl)-phosphine oxide and thioxanthone derivatives, such as those described herein. When present, the one or more photoinitiators included in the cholesteric liquid crystal precursor composition are preferably present in an amount of about 0.01 wt-% to about 10 wt-%, more preferably about 0.05 wt-% to about 7 wt-%, the weight percentages being based on the total weight of the cholesteric liquid crystal precursor composition.

[0178] The cholesteric liquid crystal precursor composition described herein may further include one or more additives, provided that the one or more additives do not adversely interfere with or hinder the formation of the helix and / or the formation of the polymer, including but not limited to compounds and materials for adjusting the physical, rheological and chemical parameters of the composition, such as uniformity (e.g., anti-settling agents and plasticizers), foaming (e.g., defoamers and degassing agents), lubricity (wax), radiation-enhancing and reducing substances, UV stability (light stabilizers), adhesion, surface properties (wetting agents, oleophobic and hydrophobic agents), etc. The additives described herein may be present in the one or more inks described herein in amounts and forms known in the art including so-called nanomaterials in which at least one of the sizes of the additives is in the range of 1 to 1000 nm. When present, the one or more additives included in the cholesteric liquid crystal precursor composition are preferably present in an amount of about 0.01 wt-% to about 5 wt-%, the weight percentage being based on the total weight of the cholesteric liquid crystal precursor composition.

[0179] The method described herein comprises a step for preparing an optically variable layer (x30) described herein. The method comprises a step d) of applying a cholesteric liquid crystal polymer precursor composition described herein on the color constant layer (x20) and / or on the surface of the substrate (x10) to form a layer. Preferably, step d) is performed by a printing method preferably selected from the group consisting of screen printing, rotogravure printing and flexographic printing, and more preferably selected from the group consisting of flexographic printing and rotogravure printing.

[0180] If the overt security feature as described herein comprises a second area made only of an optically variable layer (x30) as described herein, step d) comprises applying a cholesteric liquid crystal polymer precursor composition as described herein over the color constant layer (x20) and at least partially over the surface of the substrate (x10), thereby forming a layer.

[0181] After step d) of applying the cholesteric liquid crystal precursor composition described herein to form the layer described herein, the method comprises a step e) of heating the composition. In step e), the applied composition / layer is heated so as to bring it into a cholesteric liquid crystal state having specific optical properties. The term "specific optical properties" is understood as a liquid crystal state having a specific pitch, which selectively reflects a specific wavelength range (selective reflection band). To this end, the cholesteric liquid crystal precursor composition is heated to evaporate one or more solvents contained in the composition and promote the desired cholesteric liquid crystal state. The temperature used to evaporate the solvent and promote the formation of the liquid crystal state depends on the components of the cholesteric liquid crystal precursor composition, and is preferably about 45°C to about 150°C, more preferably about 45°C to about 120°C, and even more preferably about 50°C to about 115°C. Typically, the heating step described herein uses a suitable heating source, including but not limited to conventional heating devices, such as hot plates, ovens, hot air streams and radiation sources. The required heating time depends on several factors, such as the ingredients of the cholesteric liquid crystal precursor composition described herein, the type of heating device and the heating intensity (energy output of the heating device). Typically, the applied cholesteric liquid crystal precursor composition is heated for a time of about 1 second to about 45 seconds.

[0182] After step e) of heating as described herein, the method comprises a step f) of hardening the layer obtained in step d) to obtain the optically variable layer (x30) as described herein. Preferably, the hardening step f) is carried out by radiation comprising infrared radiation, UV-visible radiation, electron beam (E-beam) radiation, X-rays, gamma rays and ultrasonic radiation. More preferably, the hardening step f) is carried out by UV-visible (UV / VIS) light radiation. The UV-visible light radiation may be carried out in the presence of one or more photoinitiators contained in the cholesteric liquid crystal precursor composition as described herein.

[0183] The explicit security feature described herein may further include a discontinuous layer that changes the position of the selective reflection band of the optically variable layer, wherein the layer is disposed below the optically variable layer. The discontinuous layer described herein may be in the form of more than one mark, and may be made of a composition comprising more than one polymerizable monomer, each of which comprises more than one ether functional group (-C-0-C-) on each polymerizable group. WO 2015 / 067683 A1 discloses suitable resins, including organic resins (such as polyacrylates, polymethacrylates, polyvinyl ethers, polyvinyl esters, polyesters, polyethers, polyamides, polyurethanes, polycarbonates, polysulfones, phenolic resins, epoxy resins, and mixed forms of these resins), mixed inorganic / organic resins such as silicones (e.g., polyorganosiloxanes) and aqueous resins. If the discontinuous layer that changes the position of the selective reflection band of the optically variable layer is present in the explicit security feature described herein, the feature is prepared by applying and hardening / curing the discontinuous layer before applying the cholesteric liquid crystal polymer precursor composition described herein.

[0184] Also described herein are security documents, security articles, and decorative articles comprising one or more of the overt security features described herein.

[0185] Typical examples of decorative articles include, but are not limited to, luxury goods, cosmetic packaging, automotive parts, electronic / electrical products, furniture, and nail products. Optionally, the overt security features described herein may be included on a secondary substrate such as a label, and thereby transferred to the decorative article in a separate step.

[0186] Security documents include but are not limited to valuable documents and valuable commercial goods. Typical examples of valuable documents include but are not limited to banknotes, contracts, bills, checks, vouchers, stamps and tax labels, agreements, etc., identity documents such as passports, identity cards, visas, driver's licenses, bank cards, credit cards, transaction cards (transactions card), access documents (access document) or cards, admission tickets, public transportation tickets, academic diplomas or degrees (titles), etc., preferably banknotes, identity documents, authorization documents, driver's licenses and credit cards. The term "valuable commercial goods" refers to, in particular, cosmetics, functional foods, pharmaceuticals, alcoholic beverages, tobacco products, beverages or food, electrical / electronic products, fabrics or jewelry, that is, the packaging materials of the products of the products of the drugs of the legitimate version should be protected from counterfeiting and / or illegal copying to guarantee packaging. Examples of these packaging materials include but are not limited to labels such as identification brand labels, tamper-proof labels and seals. It is pointed out that the disclosed substrates, security documents and decorative articles are only given for the purpose of enumeration, without limiting the scope of the present invention.

[0187] Optionally, the overt security features described herein may be included on a secondary substrate such as a security thread, security strip, foil, label, window or tag, thereby being transferred to the security document or article in a separate step.

[0188] Also described herein is a method for manufacturing a security document, security article or decorative article, and the security documents, security articles and decorative articles obtained thereby, the method comprising a) providing a security document, security article or decorative article, and b) providing one or more explicit security features such as those described herein so that they are contained on or by the security document, security article or decorative article. For example, the method comprises the following steps: providing a security document, security article or decorative article comprising a substrate as described herein; applying a radiation-curable coating composition comprising platelet-shaped magnetic or magnetizable pigment particles as described herein on the surface of the substrate (x10) of the security document, security article or decorative article, thereby forming a layer; exposing the layer to magnetic field lines of a magnetic field generating device, thereby orienting the platelet-shaped magnetic or magnetizable pigment particles as described herein; at least partially curing the layer with a curing unit, partially simultaneously with the orienting step or after the orienting step, thereby at least partially fixing the position and orientation of the platelet-shaped magnetic or magnetizable pigment particles, so that the platelet-shaped magnetic or magnetizable pigment particles have the same elevation angle |α|, and the elevation angle |α| has a value as described herein, thereby forming a color constant layer as described herein (x20); applying a cholesteric liquid crystal polymer precursor composition as described herein; heating the layer as described herein; and hardening the layer, thereby obtaining an optically variable layer as described herein (x30).

[0189] The substrate (x10) described herein may further comprise additional security elements, such as organic and / or inorganic pigments, dyes, flakes, optically variable elements, magnetic pigments, and the like.

[0190] In order to increase durability and thus increase the cycle life of the dominant security features described herein by stain resistance or chemical resistance and cleanliness, or to modify their aesthetic appearance (e.g. optical gloss), one or more protective layers can be applied on the optically variable layer (x30). When present, one or more protective layers are typically made of protective varnishes. The protective varnish can be a radiation-curable composition, a heat-drying composition or any combination thereof. Preferably, one or more protective layers are radiation-curable compositions, more preferably UV-Vis curable compositions. The protective layer is typically applied after forming the dominant security features.

[0191] The overt security features described herein can be provided directly on the substrate (x10) on which they are to remain permanent. Alternatively, for production purposes, the overt security features can also be provided on a temporary substrate from which they are subsequently removed.

[0192] Optionally, there may be one or more adhesive layers on the side of the explicit security feature opposite to the side of the optically variable layer (x30). Therefore, one or more adhesive layers may be applied, which are applied after the hardening step f) is completed. Such products can be attached to a variety of documents or other products or articles without involving machines and printing or other methods with considerable effort. Optionally, the explicit security feature described herein can be in the form of a transfer foil, which can be applied to a document or product in a separate transfer step. For this purpose, the explicit security feature is provided with a release coating.

[0193] Due to the combination of the optically variable layer (x30) and the color constant layer (x20) as described herein with the specific orientation pattern of the magnetically oriented platelet-shaped magnetic or magnetizable pigment particles as described herein, the overt security feature as described herein allows the average person to easily and conveniently identify it with the naked eye without the need for any device by tilting the feature and observing the first area consisting of the superposition of the optically variable layer (x30) and the color constant layer (x20) as described herein, when the feature is observed through the optically variable layer (x30)) It has at least three different colors at different viewing / observation angles, provided that when the substrate is transparent, the overt security feature must be arranged on a permanently light-absorbing background.

[0194] At least one viewing / observation angle, preferably both viewing / observation angles are grazing angles, and are required to allow for easy and convenient authentication. Figure 6 and 7 Shown are different viewing / observation angles and how a substrate (x10) carrying an optically variable layer (x30), a color constant layer (x20) and an optional light absorbing background (x40) can be tilted and rotated (see steps i) to iii)) for the purpose of authenticating an overt security feature as described herein, wherein the feature is observed (as seen by the eye) through the optically variable layer (x30). Figure 7 An overt security feature comprising a first area (see marking "A") and a second area (area surrounding marking "A") as described herein is shown, wherein the shape of the color constant layer (720, letter "A") is different from the shape of the optically variable layer (730, rectangle) to better illustrate the rotation of the feature performed during step ii).

[0195] The overt security features described herein can be readily identified by their optical properties under normal lighting conditions (i.e., everyday lighting including non-directional light resulting from light diffusion or multiple reflections and directional light from the sun or artificial light sources). Direct lighting (i.e., lighting from a point source that strikes the security feature at a given angle and reflects to the observer's eye at the same angle) is best avoided because it produces specular reflections and makes color difficult / impossible to observe. Observation is preferably performed according to the following four conditions (see, for example, Figure 7 ):

[0196] Scenario A: The overt security feature is placed horizontally at arm's length and is observed at a grazing angle |β|, which corresponds approximately to the elevation angle |α| of the magnetically oriented platelet-shaped magnetic or magnetizable pigment particles in the color constant layer (x20). At this angle, the first area ( Figure 7 The "A" in the figure presents a first color (for example, blue for the following examples E1-E4), and the second area ( Figure 7 The area around "A" in the image is the same color;

[0197] The average person then tilts the substrate (x10) carrying the two layers (x20 and x30) so that the overt security feature is held vertically so as to face the observer's eye (see Figure 6-7 Step i));

[0198] Case B: The overt security feature is held vertically so as to face the observer's eye, and the viewing angle β' is now approximately 90°. At this angle, the first area appears in the second color (e.g., silver for the embodiments E1-E4 described below), and the second area appears in the third color (e.g., green for the embodiments E1-E4 described below);

[0199] The average person then tilts the substrate (x10) carrying the two layers (x20 and x30) and rotates it 180° on an axis perpendicular to the substrate (x10) so that the overt security feature is held vertically so as to face the observer's eye (see Figure 6-7 step ii)) of Figure 7 The mark "A" composed of the color constant layer (x20) is upside down due to rotation.

[0200] Case C: At this angle β', the first area exhibits a third color (e.g., green for the embodiments E1-E4 described below), and the second area exhibits the same color;

[0201] The average person then tilts and rotates the substrate (x10) carrying the two layers (x20 and x30) so that the overt security feature is held horizontally (see Figure 6-7 Step iii)) of

[0202] Situation D: The overt security feature is held horizontally and again viewed at a glancing angle β. At this angle, the first area appears the second color (eg silver for Examples E1-E4 described below) and the second area appears the first color (eg blue for Examples E1-E4 described below).

[0203] As described above, for the first region ( Figure 6 The mark "A" in the figure can be observed in at least three different colors (blue, silver, green for the following Examples E1-E4), so ordinary people can easily and conveniently identify the overt security feature by observing it at two different viewing / observation angles (β and 90°).

[0204] Alternatively, visual observation can be started from each position and each direction (i.e., clockwise or counterclockwise). However, the case A described herein is particularly easy to observe because, at the observation angle β (grazing angle), the color of the color constant layer (x20) is substantially the same as the color of the optically variable layer (x30) with the naked eye and without any device (i.e., the influence of the magnetic color particles in the color constant layer (x20) is very limited).

[0205] Example

[0206] The invention will now be described in more detail with reference to non-limiting examples.Examples E1-E4 and C1-C2 have been carried out using a coating composition comprising a flake-shaped magnetic or magnetizable pigment particle curable composition provided in Table 1 and a cholesteric liquid crystal polymer precursor composition provided in Table 2.

[0207] Table 1

[0208]

[0209] (*) For Example E4 and Comparative Example C2, pigment particles with smaller d50 values ​​were selected to ensure that the orientation of the particles was not limited by the ink layer thickness (about 25 μm).

[0210] (**) The viscosity of the composition was measured at 25° C. on a Brookfield viscometer (model “DV-IPrime”, spindle S21, 100 rpm).

[0211] By first mixing all the ingredients described in Table 1 except the magnetic particles provided in Table 1, and dispersing them at room temperature for 20 minutes using Dispermat (model LC-2) at 1500 rpm, a coating composition comprising magnetic particles was prepared. Then flaky magnetic pigment particles were added and further dispersed at room temperature for 15 minutes at 1500 rpm to obtain 100 g of coating composition. The coating composition comprising the magnetic particles of Table 1 had a viscosity that made it suitable for screen printing, rotogravure printing and flexographic printing, so the coating method used therein imitated screen printing, rotogravure printing and flexographic printing methods.

[0212] Table 2

[0213]

[0214] (*) Viscosity was measured using a DIN 4" cup at 25°C and converted to mPas using a viscosity conversion table provided by Saint Clair Systems (Washington, USA).

[0215] A cholesteric liquid crystal polymer precursor composition was prepared by pouring the solvent (cyclohexanone), LC monomer (Lumogen S250) and chiral dopant (Lumogen S750) into a 200 ml bottle and placing in an ultrasonic bath at 40°C for about 30 minutes to dissolve the ingredients in the solvent. The mixture was then poured into a Dispermat (Model LC-2), a photoinitiator was added and dispersed at 2000 rpm for 20 minutes. Finally, a surfactant (BYK 361N) was added and mixed at 1500 rpm for 5 minutes.

[0216] The cholesteric liquid crystal polymer precursor composition of Table 2 has a viscosity making it suitable for flexographic and rotogravure printing, and thus the coating method used therein simulates the flexographic and rotogravure printing methods.

[0217] When the cholesteric liquid crystal polymer precursor composition of Table 2 is heated and cured, the layer made therefrom exhibits a blue to green color shift when tilted. In other words, the optically variable layer (x30) without the color constant layer (x20) exhibits a blue to green color shift when tilted and observed between grazing angles and face angles.

[0218] For each sample, Examples E1-E4 and C1-C2 were prepared using the following method:

[0219] a) applying the coating composition comprising the magnetic particles provided in Table 1 onto a piece of transparent PET substrate (Hostaphan, 20 cm×7.5 cm, thickness: 50 μm) (x10) to form a layer (size 18 cm×4 cm), wherein said step was carried out with a semi-automatic laboratory coater (K101 Control Coater, RK Print) using a coating rod HC4 (nominal thickness 36 μm);

[0220] b) exposing the layer (x10) obtained in step a) to a magnetic field of a magnetic field generating device as described below, thereby biaxially orienting the platelet-shaped magnetic or magnetizable pigment particles; as described herein and Fig.5A1 As shown, the substrate (x10) carrying the layer (x20) is tilted to an elevation angle γ relative to the magnetic field lines;

[0221] After steps b) and c), the layer obtained in step b) is at least partially cured, thereby fixing the position and orientation of the particles so that the particles have the same elevation angle γ, which is between about 0° and about 50° as provided in Table 3, thereby forming a color-constant layer (x20), wherein the layer is exposed to a UV-LED lamp (Phoseon Firefly, 395 nm, 4 W / cm 2 ) was first cured while in contact with the magnetic field generating device for about 2 seconds, and was second cured while being removed from the magnetic field generating device using a mercury UV dryer (Technigraf Aktiprint Mini 18-2, two medium-pressure mercury lamps, total power 80 W / cm, one pass at a constant speed of 90 mm / s, corresponding to an exposure time of about 0.5 seconds); the thickness of the color constant layer (x20) thus obtained was about 25 μm;

[0222] d) applying the cholesteric liquid crystal polymer precursor composition of Table 2 (theoretical wet thickness 8 μm) on the color constant layer (x20) using the same hand coater and coating rod HC1 as described in step a) above to form a layer (size 18 cm×4 cm);

[0223] e) heating the layer obtained in step d) at a temperature of 50° C. for 30 seconds using a hot air dryer, thereby evaporating the solvent and generating a cholesteric liquid crystal state; and

[0224] f) curing the substrate (x10) carrying the color constant layer (x20) and the layer obtained in step e) by moving said substrate (x10) under the same mercury UV dryer with the same parameters as described above in step d) to obtain an optically variable layer (x30); the optically variable layer (x30) thus obtained has a thickness of about 4 μm.

[0225] A 25 μm thickness of the color constant layer (x20) was chosen to ensure that the pigment particle orientation was not restricted at the chosen d50 values ​​of the pigment particles (20 μm and 12 μm respectively), allowing comparison of the results. However, said values ​​are not preferred for end-use applications.

[0226] Examples E1-E4 and comparative examples C1-C2 comprise a first region consisting of a superposition of a color constant layer (x20) and an optically variable layer (x30).

[0227] Magnetic field generating device ( Fig.5A1 -A2)

[0228] Figure 5A1 -The magnetic assembly shown in A2 is used to orient the pigment particles biaxially. The magnetic assembly comprises nine magnet subassemblies (M1-M9), wherein each magnet assembly is made of 18 identical magnets (NdFeB N45) having a height L4 (40 mm), a width L3 (10 mm) and a thickness L5 (3 mm) (see Figure 5A2 ). Each assembly (M1-M9) is constructed by vertically stacking three groups of six magnets (i.e., each assembly (M1-M9) has a height L1=3×L4 (120 mm), a width L2=6×L5 (18 mm), and a thickness L3=10 mm). The magnetic axis of each identical magnet is parallel to its thickness (L5), and the magnets are placed together in such a way that the magnetic axis of each assembly (M1-M9) is parallel to its width (L2) and perpendicular to the plane formed by dimensions L1 and L3.

[0229] The magnet assemblies (M1-M9) are embedded in a non-magnetic bracket (not shown) made of polyoxymethylene (POM) and are arranged at a fixed interval L6 of 20 mm, with their magnetic axes perpendicular to the plane formed by the dimensions L1 (120 mm) × L7 (250 mm) of the magnetic field generating device, and alternately pointing in opposite directions, as shown in FIG. Figure 5A1 The generated magnetic field lines are substantially perpendicular to the plane L1×L7 of the magnetic field generating device, thereby generating a substantially uniform magnetic field, as long as the substrate carrying the layer including the particles moves at about half the height of the magnetic field generating device.

[0230] The substrate carrying the uncured layer including the particles is placed on a rotatable support including a polar ruler indicating the elevation angle γ between the magnetic field lines and the support, and then moved at a speed of about 10 cm / sec at half the height (L8=1 / 2L1) of the magnetic field generating device, the distance L9 between the plane L1×L7 of the magnetic field generating device and the nearest edge of the layer including the particles being about 1 cm, so that the particles are biaxially oriented so that they are substantially parallel to each other and in the plane of the generated magnetic field lines. The elevation angle γ (provided in Table 3) is set by rotating the support and accurately measuring the angle using the polar ruler.

[0231] The thickness of the color constant layer (x20) and the optically variable layer (x30) have been measured by using an Extramess InductiveDigital Comparator 2001 (supplied by Mahr).

[0232] Table 3

[0233]

[0234] a) The elevation angle values ​​are too high to be measured by a conoscopic scatterometer (the total field of view is limited to 40° and a scatterometer does not allow the use of 100% of the field of view).

[0235] Use as in WO 2019 / 038371 A1 Figure 4 A conoscopic scattering instrument (obtained from Eckhardt Optics LLC, 5430 Jefferson Ct, White Bear Lake, MN 55110; http: / / eckop.com) was used to independently obtain the measured elevation angle α of the magnetic pigment particles in the color constant layer (x20). After step d), the measured elevation angle α was obtained at about 1 mm. 2 The elevation angle α of the platelet-shaped magnetic or magnetizable pigment particles in the color constant layer (x20) is measured directly on the layer surface of , i.e. the reported value corresponds to the average value of about 1000 particles. The measured elevation angle α provided in Table 3 is the average value of about ten measurements at different positions of the color constant layer (x20).

[0236] Optical microscopy images were obtained by using a binocular microscope (Olympus BX51, magnification ×100, illuminated through the lens using an Olympus TH4-200 lighting device, camera: Nikon D7100) on microtome sections of the samples (the sectioning plane was perpendicular to the substrate surface and the coating thickness, and perpendicular to the tilt axis). The substrate (x10) carrying the color constant layer (x20) was first embedded in epoxy resin (Technicol 9461) independently, dried at room temperature for 24 hours, and then the microtome sections were cut and polished to produce samples with the following dimensions: 10 mm×10 mm×30 mm. The determination of the elevation angle α of the magnetic pigment particles was performed using the software Adobe IllustratorCC (version 23.0.2). For each elevation angle, the value of the elevation angle α reported in Table 3 was averaged over about 10 to 20 particles.

[0237] The optical properties of the thus obtained examples E1-E4 and C1-C2 have been evaluated with the naked eye without any other means and are provided in Table 4 ( Figure 6 and 7 How to observe). Examples E1-E4 and C1-C2 were observed under common lighting conditions as described above, in particular in a room illuminated by four rectangular neon lamps. A non-permanent black background (x40) (Leneta N2A-2, Leneta Company Inc. Mahwah, USA) was placed under the substrate (x10). Visual observation (represented by the eye in the figure) was performed through the optically variable layer (x30).

[0238] As described above, four conditions AD were evaluated and Figure 6-7 The following is shown in case AD:

[0239] Case A: the security feature under observation is held horizontally and visually observed at a first observation angle β (grazing angle), which corresponds approximately to the elevation angle α of the platelet-shaped magnetic or magnetizable pigment particles in the color-constant layer (x20) relative to the plane of the substrate (x10);

[0240] - Case B: the overt security feature is tilted vertically so that it now faces directly to the eye of the observer, visually observed at an observation angle β' (face angle) of about 90° to the substrate surface;

[0241] - Case C: the overt security feature is rotated 180° while remaining in the same vertical position, with the axis of rotation perpendicular to the substrate (x10), wherein the observation angle β' is the same as in Case B (face angle); and

[0242] - Case D: The overt security feature is again placed horizontally and viewed at an angle β (grazing angle).

[0243] Optionally, visual observation can be started from each position and each direction. However, case A is particularly easy to observe because the color of the first area closely matches the color of the second area at grazing angles (i.e., there is a very limited contribution from the magnetic pigment particles in the color constant layer (x20)). Therefore, it is easier to start with case A.

[0244] For Examples E1-E4 and Comparative Examples C1-C2, each case in Table 4 reports the observed color of the first region consisting of the superposition of the color constant layer (x20) and the optically variable layer (x30).

[0245] Table 4

[0246]

[0247] 1 The silver color in case B of examples E1-E3 appears slightly pink due to the reflection of the secondary color of the optically variable layer (x30).

[0248] Comparative Example C1 does not exhibit at least three different colors when viewed at different viewing / observation angles (when viewed through the optically variable layer (x30) at different viewing / observation angles).

[0249] While comparative example C2 exhibits at least three different colors when viewed at different viewing / observation angles (when viewed through the optically variable layer (x30) at different viewing / observation angles), the viewing / observation angle β (grazing angle) is too high, thus making the feature unsuitable for its simple and convenient authentication. In addition, the color at the face angle (90°) in case B is not the expected silver (examples E1-E4), but the green observed in case C.

[0250] In contrast to Comparative Examples C1-C2, Examples E1-E4 comprising a color-constant layer in which the elevation angle |α| of the platelet-shaped magnetic or magnetizable pigment particles is between about 10° and about 45° (10°≤angle |α|≤45°), preferably between about 15° and about 40° (15°≤angle |α|≤40°); and more preferably between about 15° and about 35° (15°≤angle |α|≤35°) exhibit at least three different colors (blue, silver and green) when viewed at two viewing / observation angles, wherein the viewing / observation angle β (grazing angle) is small enough to allow easy and convenient identification of the overt security feature with the naked eye without any device.

[0251] Examples E1-E4 were also observed from the color constant layer (x20) side while placing the above non-permanent black background (x40) below the optically variable layer (x30). When viewed through the color constant layer (20) and at the same different viewing / observation angles provided in Table 4, only a single color (grey) was observed.

[0252] Similar Examples E1'-E4' and Comparative Examples C1'-C2' were prepared as described above, except that the size of the optically variable layer (x30) (dimensions 18 cm x 6 cm) was larger than the size of the color constant layer (x20) (dimensions 18 cm x 4 cm); thereby forming a feature comprising a first region (dimensions: 18 x 4 cm), the first region consisting of a superposition of the color constant layer (x20) and the optically variable layer (x30) and being approximately centered on the length of the substrate (x10), and a second region comprising two zones of approximately 18 x 1 cm on each side of the first region. Upon visual observation of the above examples, the colors observed for the first region in the four cases AD were the same as described in Table 4, and the colors observed for the second region were: blue for cases A and D, and green for cases B and C. In the absence of the color constant layer (x20), in Examples E1-E4 and Comparative Examples C1-C2, the optically variable layer (x30) appeared green at the face angle, and the secondary color was red.

Claims

1. An explicit security feature comprising: a) a substrate (x10), wherein the substrate (x10) is made of a material selected from the group consisting of a transparent material, a light-absorbing material and a combination thereof, b) a color-constant layer (x20) comprising magnetically oriented, platelet-shaped magnetic or magnetizable pigment particles, c) an optically variable layer (x30) comprising a cholesteric liquid crystal polymer selectively reflecting light in the visible spectral range and located on the color constant layer (x20) so as to form a first region consisting of a superposition of the optically variable layer (x30) and the color constant layer (x20), The platelet-shaped magnetic or magnetizable pigment particles of the color constant layer (x20) have substantially the same elevation angle α, the value of the elevation angle |α| being between about 10° and about 45° (10°≤angle |α|≤45°), preferably between about 15° and about 40° (15°≤angle |α|≤40°); and more preferably between about 15° and about 35° (15°≤angle |α|≤35°).

2. An explicit security feature according to claim 1, wherein the cholesteric liquid crystal polymer of the optically variable layer (x30) is obtained from a cholesteric liquid crystal polymer precursor composition, which comprises one or more nematic compounds, one or more chiral dopants, one or more photoinitiators and one or more solvents.

3. Overt security feature according to claim 1 or 2, wherein the optically variable layer (x30) has a thickness between about 1 μm and about 10 μm, preferably between about 2 μm and about 6 μm.

4. An explicit security feature according to any one of claims 1 to 3, wherein the color constant layer (x20) is a layer obtained from a radiation curable coating composition comprising flake-like magnetic or magnetizable pigment particles, one or more radiation curable oligomers, one or more radiation curable monomers and one or more photoinitiators.

5. An overt security feature according to any one of claims 1 to 4, wherein the platelet-shaped magnetic or magnetisable pigment particles are metallic in colour.

6. An overt security feature according to claim 5 wherein the platelet-shaped magnetic or magnetisable pigment particles are silver in colour.

7. An overt security feature according to any one of claims 1 to 6, wherein the size d50 of the platelet-shaped magnetic or magnetisable pigment particles is between about 2 μm and about 50 μm.

8. An overt security feature according to any one of claims 1 to 7, wherein the platelet-shaped magnetic or magnetisable pigment particles are present in an amount of about 2 wt-% to about 25 wt-%, preferably in an amount of about 4 wt-% to about 10 wt-%, the weight percentages being based on the total weight of the colour-constant layer.

9. An overt security feature according to any one of claims 1 to 8, wherein the color-constant layer (x20) has a thickness between about 5 μm and about 30 μm, preferably between about 5 μm and about 15 μm.

10. Overt security feature according to any one of claims 1 to 9, wherein the color constant layer (x20) is in the form of more than one marking and / or the optically variable layer (x30) is in the form of more than one marking, the more than one marking being identical or different.

11. Overt security feature according to any one of claims 1 to 10, further comprising a second area made only of the optically variable layer (x30).

12. A security document, security article or decorative article comprising one or more overt security features as claimed in any one of claims 1 to 11.

13. A method of manufacturing an explicit security feature according to any one of claims 1 to 11, the method comprising the following steps: a) applying a radiation-curable coating composition comprising the flake-shaped magnetic or magnetizable pigment particles according to any one of claims 5 to 7, said radiation-curable coating composition being in a first, liquid state to form a layer, on the surface of a substrate (x10); b) exposing the layer obtained in step a) to magnetic field lines of a magnetic field generating device, wherein the magnetic field lines form an elevation angle |γ| with the surface of the substrate (x10), the value of the elevation angle |γ| being between about 10° and about 45°, thereby orienting the flake-shaped magnetic or magnetizable pigment particles; c) partially simultaneously with step b) or after step b), a step of at least partially curing the layer with a curing unit, thereby at least partially fixing the position and orientation of the platelet-shaped magnetic or magnetizable pigment particles, so that the platelet-shaped magnetic or magnetizable pigment particles have the same elevation angle α, which is between about 10° and about 45° (10°≤angle|α|≤45°), preferably between about 15° and about 40° (15°≤angle|α|≤40°); and more preferably between about 15° and about 35° (15°≤angle|α|≤35°), thereby forming a color-consistent layer (x20), d) applying a cholesteric liquid crystal polymer precursor composition at least partially on the color constant layer (x20) and / or at least partially on the surface of the substrate (x10), e) heating the layer obtained in step d), and f) Hardening the layer obtained in step e) to obtain an optically variable layer (x30).

14. The method according to claim 13, wherein the step a) is performed by a printing process selected from the group consisting of screen printing, rotogravure printing and flexographic printing, and wherein the step d) is performed by a printing process selected from the group consisting of flexographic printing and gravure printing.

15. The method according to claim 13 or 14, wherein step c) is performed by exposing the layer to one or more wavelengths between about 365 nm and about 405 nm emitted by a UV-VisLED curing unit.

Citation Information

Patent Citations

  • Polymerizable liquid-crystalline compounds

    EP0847432B1

  • Two-axial alignment of magnetic platelets

    EP2157141A1

  • Method for the Modification of Chiral Liquid-Crystal Films with the Aid of Extractants

    US20070224341A1

  • Thermostable pigments, films and effect coatings, and mixtures for their production

    US6423246B1

  • Light-reaction type optically active compound, light-reaction type chiral agent, liquid crystal composition, liquid crystal color filter, optical film, recording medium, and method of changing twist structure of liquid crystal