Composition for etching and method for manufacturing wiring board using same
By using hydrogen peroxide, sulfuric acid, azoles and other ingredients in a specific etching composition, the problem of thinning of wiring shape and loss of rectangularity during the removal of the copper seed layer is solved, and the problem of wiring shape thinning and loss of rectangularity is achieved in the SAP, M-SAP or ETS process. High-precision copper wiring pattern manufacturing in .
Patent Information
- Application Number
- CN202380022864.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-02-25
- Filing Date
- 2023-02-22
- Publication Date
- 2024-10-11
AI Technical Summary
When forming a copper wiring pattern in the prior art, the removal process of the copper seed layer easily leads to a reduction in wiring height and width, and the shape of the wiring cross section cannot maintain a rectangular shape, affecting processing accuracy.
Using an etching composition containing hydrogen peroxide, sulfuric acid, azoles or their salts, glycol ethers and halide ions, by controlling the component ratio and processing temperature, the copper seed layer can be selectively etched and the thinning of copper wiring can be suppressed. and maintain rectangularity.
In the SAP, M-SAP or ETS process, it can effectively suppress the thinning of copper wiring, maintain the rectangularity of the wiring cross-section, selectively remove the copper seed layer, and improve the precision of micron processing of copper wiring patterns.
Smart Images

Figure BDA0005002809530000031 
Figure BDA0005002809530000071 
Figure BDA0005002809530000081
Abstract
Description
Technical Field
[0001] The present invention relates to an etching composition for selectively etching a copper seed layer from a substrate having a copper wiring pattern and a copper seed layer, and a method for producing a wiring substrate using the same. Background Art
[0002] In recent years, in the manufacture of substrates for smartphones and wearable terminals, there has been a demand for processing of fine metal wiring and improvement of its precision.
[0003] As a processing method that can cope with the miniaturization of metal wiring, a semi-additive process (SAP: Semi Additive Process, hereinafter referred to as "SAP") is known to form a copper wiring pattern only in necessary parts by electrolytic copper plating. Among them, in recent years, a modified semi-additive process (M-SAP: Modified-Semi Additive Process, hereinafter referred to as "M-SAP") that can also cope with fine pitch has attracted much attention.
[0004] Regarding SAP, first, an electroless copper plating film is formed on the insulating layer, and an extremely thin electrolytic copper plating film is further formed to form a copper seed layer as required. Next, a resist pattern for forming copper wiring is formed on the copper seed layer using a photoresist, and a copper wiring pattern is formed between the resist patterns by electrolytic copper plating. Thereafter, the resist pattern is removed, and the exposed copper seed layer is removed by chemical etching, so that a fine copper wiring pattern can be formed on the insulating layer.
[0005] Regarding M-SAP, first, an electrolytic copper foil with a carrier foil is used to laminate the electrolytic copper foil on the insulating layer. Then, the electrolytic copper foil is made into an extremely thin copper layer by half etching as needed, and an electroless copper plating film is formed thereon to form a copper seed layer. Next, a resist pattern for forming copper wiring is formed on the copper seed layer, and a copper wiring pattern is formed between the resist patterns by electrolytic copper plating. Thereafter, the resist pattern is removed, and the exposed copper seed layer is removed by chemical etching, so that a fine copper wiring pattern can be formed on the insulating layer.
[0006] As described above, in SAP or M-SAP, after forming a copper wiring pattern, the copper seed layer needs to be removed. However, when the copper seed layer is removed, the height and width of the copper wiring are likely to decrease, and the shape of the wiring cross section may not maintain rectangularity.
[0007] Patent Document 1 states that an etching solution containing hydrogen peroxide and sulfuric acid as main components and azoles as additives can suppress the thinning and curling of the circuit portion when removing the copper seed layer in SAP. However, in order to further improve the processing accuracy, more selective etching of the copper seed layer is sought.
[0008] As a processing method that can cope with the miniaturization of copper wiring, an embedded trace substrate (ETS) process (hereinafter referred to as the "ETS process") is also known (Patent Document 2). However, in the case of the ETS process, after the copper wiring pattern formed on the electrolytic copper foil as the copper seed layer is buried in the resin, the electrolytic copper foil as the copper seed layer needs to be removed by etching. Depending on the etching (side etching) of the copper wiring along the side wall of the interlayer insulating resin during etching and the degree of etching on the upper surface of the copper wiring, the shape of the wiring cross section sometimes cannot maintain rectangularity. Therefore, in the ETS process, electrolytic copper foil that selectively serves as a copper seed layer is also sought.
[0009] Prior art literature
[0010] Patent Literature
[0011] Patent Document 1: Japanese Patent Application Publication No. 2006-009122
[0012] Patent Document 2: International Publication No. 2019 / 208461 Summary of the invention
[0013] Problem that the invention aims to solve
[0014] Under such circumstances, it is sought to provide an etching composition for selectively etching a copper seed layer from a substrate having a copper wiring pattern and a copper seed layer.
[0015] It should be noted that in this specification, "copper seed layer" refers to a copper thin film formed as a base layer when copper wiring is formed on an insulating layer using a plating technique, and there is no particular limitation on its formation method. The copper thin film may be, for example, an electrolytic copper foil, an electrolytic copper plating film, or an electroless copper plating film, or a combination thereof.
[0016] Solutions for solving problems
[0017] The present invention relates to the etching composition described below and a method for producing a wiring board using the same.
[0018] [1] An etching composition for selectively etching a copper seed layer from a substrate having a copper wiring pattern and a copper seed layer,
[0019] The etching composition comprises hydrogen peroxide (A), sulfuric acid (B), azoles or salts thereof (C), glycol ethers (D), halide ions (E) and water (F),
[0020] The content of hydrogen peroxide (A) is 0.1 to 10% by mass based on the total amount of the etching composition.
[0021] The content of sulfuric acid (B) is 0.5 to 5% by mass based on the total amount of the etching composition.
[0022] The ratio of hydrogen peroxide (A) to sulfuric acid (B) is 2 or more as expressed in molar ratio,
[0023] The content of the halide ion (E) is 0.01 to 3 ppm based on the total amount of the etching composition.
[0024] [2] The etching composition according to [1] above, wherein the azole is a heterocyclic compound containing a five-membered heterocyclic ring having two nitrogen atoms or a condensed heterocyclic ring thereof.
[0025] [3] The etching composition according to [2] above, wherein the azole is at least one selected from the group consisting of pyrazoles, imidazoles, and benzimidazoles.
[0026] [4] The etching composition according to [3] above, wherein the azole is one or more selected from the group consisting of compounds represented by the following formula.
[0027]
[0028] [Where R 1 , R 2 , R 3 , R 4 , R 5 and R 6 are independently a hydrogen atom, a C1-C6 alkyl group, a C6-C 10 Aryl, carboxyl, carboxyl C1-C6 alkyl, nitro, hydroxyl, C2-C7 carboxylate or halogen atom.]
[0029] [5] The etching composition according to [4], wherein the azole is at least one selected from the group consisting of imidazole, 1,2,4,5-tetramethylimidazole, 4-methyl-2-phenylimidazole, benzimidazole, 1-methylbenzimidazole, 2-methylbenzimidazole, 5-methylbenzimidazole, 2,5-dimethylbenzimidazole, 5-nitrobenzimidazole, pyrazole and 3,5-dimethylpyrazole.
[0030] [6] The etching composition according to any one of [1] to [5] above, wherein the content of the azole is 0.01 to 0.5% by mass based on the total amount of the etching composition.
[0031] [7] The etching composition according to any one of [1] to [6] above, wherein the glycol ether (D) is at least one selected from the group consisting of ethylene glycol monobutyl ether, diethylene glycol monomethyl ether, diethylene glycol monophenyl ether and dipropylene glycol monomethyl ether.
[0032] [8] The etching composition according to any one of [1] to [7] above, wherein the content of the glycol ether (D) is 0.01 to 1% by mass based on the total amount of the etching composition.
[0033] [9] The etching composition according to any one of [1] to [8] above, wherein the halide ion (E) is a chloride ion.
[0034]
[10] The etching composition according to any one of [1] to [9] above, wherein the etching rate ratio of the wiring height of the copper wiring defined by the formula (1) at a processing temperature of 30° C. is 1.2 or less.
[0035] Wiring height etching rate ratio = Δ height / seed layer thickness (1)
[0036] [Wherein, the seed layer thickness represents the thickness (μm) of the copper seed layer removed by etching, and the Δ height represents the etching thickness (μm) of the upper surface of the copper wiring removed by etching within the etching time just enough to remove the entire copper seed layer by etching.]
[0037]
[11] The etching composition according to
[10] above, wherein the etching rate ratio of the wiring width of the copper wiring defined by the formula (2) at a processing temperature of 30°C is 1.4 or less.
[0038] Wiring width etching rate ratio = Δ sheet width / seed layer thickness (2)
[0039] [Wherein, the seed layer thickness represents the thickness of the copper seed layer removed by etching (μm), and the Δ sheet width represents the value (μm) obtained by converting the lateral width of the copper wiring removed by etching into a single-side amount (1 / 2) within the etching time just enough to remove the entire copper seed layer by etching.]
[0040]
[12] The etching composition according to any one of [1] to
[11] above, wherein the copper seed layer is at least one selected from the group consisting of electrolytic copper foil, electrolytic copper plating film, and electroless copper plating film.
[0041]
[13] A method for manufacturing a wiring substrate, comprising the following steps:
[0042] Using the etching composition described in any one of [1] to
[12] above, a copper seed layer is selectively etched from a substrate having a copper wiring pattern and a copper seed layer.
[0043]
[14] The method for manufacturing a wiring board according to
[13] above, wherein the copper seed layer is at least one selected from the group consisting of an electrolytic copper foil, an electrolytic copper plating film, and an electroless copper plating film.
[0044]
[15] A method for manufacturing a wiring substrate, wherein a copper seed layer is selectively etched from a substrate having a copper wiring pattern and a copper seed layer using the etching composition described in any one of [1] to
[12] in a semi-additive process (SAP), a modified semi-additive process (M-SAP) or an embedded trace substrate process (ETS process) to form a wiring circuit.
[0045] Effects of the Invention
[0046] According to the present invention, an etching composition for selectively etching a copper seed layer from a substrate having a copper wiring pattern and a copper seed layer can be provided. The etching composition of the present invention can be suitably used in the manufacture of a wiring substrate having a wiring circuit composed of a fine copper wiring pattern in a SAP, M-SAP or ETS process, etc. According to a preferred embodiment of the present invention, it is possible to suppress the thinning of the copper wiring and maintain the rectangularity of the wiring cross section, while selectively removing the copper seed layer. BRIEF DESCRIPTION OF THE DRAWINGS
[0047] Figure 1 This is a diagram for explaining a method of manufacturing a wiring substrate in which a wiring circuit is formed by selectively etching a copper seed layer from a substrate having a copper wiring pattern and a copper seed layer in SAP.
[0048] Figure 2 This is a diagram for explaining a method for manufacturing a wiring substrate in which a wiring circuit is formed by selectively etching a copper seed layer from a substrate having a copper wiring pattern and a copper seed layer in M-SAP.
[0049] Figure 3 This is a diagram for explaining a method of manufacturing a wiring substrate in which a wiring circuit is formed by selectively etching a copper seed layer from a substrate having a copper wiring pattern and a copper seed layer in an ETS process.
[0050] Figure 4 This is a diagram showing a specific example of the evaluation criteria for the rectangularity of the copper wiring after the etching process. DETAILED DESCRIPTION
[0051] 1. Etching composition
[0052] The etching composition of the present invention is an etching composition for selectively etching a copper seed layer from a substrate having a copper wiring pattern and a copper seed layer, and is characterized in that:
[0053] comprising hydrogen peroxide (A), sulfuric acid (B), azoles or their salts (C), glycol ethers (D), halide ions (E) and water (F),
[0054] The content of hydrogen peroxide (A) is 0.1 to 10% by mass based on the total amount of the etching composition.
[0055] The content of sulfuric acid (B) is 0.5 to 5% by mass based on the total amount of the etching composition.
[0056] The ratio of hydrogen peroxide (A) to sulfuric acid (B) is 2 or more as expressed in molar ratio,
[0057] The content of the halide ion (E) is 0.01 to 3 ppm based on the total amount of the etching composition.
[0058] Hereinafter, each component will be described.
[0059] [Hydrogen peroxide (A)]
[0060] In the present invention, hydrogen peroxide (A) (hereinafter, sometimes simply referred to as component (A)) is a component that functions as an oxidizing agent for copper.
[0061] The component (A) is not particularly limited, and various grades of components for industrial use, electronic industry use, etc. can be used. Generally, it is preferred to use it in the form of an aqueous hydrogen peroxide solution from the viewpoint of availability and handling.
[0062] The content of component (A) is in the range of 0.1 to 10% by mass, preferably 0.5 to 8% by mass, more preferably 1 to 7.5% by mass, and further preferably 2 to 7% by mass, based on the total amount of the etching composition (mass basis). By making the content of component (A) within the above range, it is possible to selectively remove the copper seed layer while suppressing the thinning of the copper wiring and maintaining the rectangularity of the wiring cross section.
[0063] In addition, when a numerical range is shown in this specification, the upper limit value and the lower limit value can be appropriately combined, and the numerical range obtained by combining them is also disclosed.
[0064] [Sulfuric acid (B)]
[0065] In the present invention, sulfuric acid (B) (hereinafter, sometimes simply referred to as component (B)) is a component that functions as an etchant for copper oxidized by hydrogen peroxide (A).
[0066] The content of the component (B) is in the range of 0.5 to 5% by mass, preferably 1 to 5% by mass, more preferably 2 to 5% by mass, and further preferably 2.5 to 5% by mass, based on the total amount of the etching composition (mass basis). By making the content of the component (B) within the above range, it is possible to suppress the thinning of the copper wiring and maintain the rectangularity of the wiring cross section, while selectively removing the copper seed layer.
[0067] In the etching composition of the present invention, the ratio of hydrogen peroxide (A) to sulfuric acid (B) (component (A) / component (B)) is 2 or more, preferably 2.0 or more, more preferably 2 to 20, further preferably 2.0 to 20, further preferably 3 to 15, further preferably 3.5 to 10, and particularly preferably 3.5 to 8. By controlling the blending ratio of component (A) to component (B), it is possible to selectively remove the copper seed layer while suppressing the thinning of the copper wiring and maintaining the rectangularity of the wiring cross section.
[0068] [Azoles or their salts (C)]
[0069] In the present invention, the azole or a salt thereof (C) (hereinafter, sometimes simply referred to as component (C)) may have a function of selectively removing a copper seed layer by being adsorbed to the surface of a copper wiring.
[0070] In the present invention, azoles are heterocyclic compounds containing a five-membered heterocyclic ring or a condensed heterocyclic ring thereof having one or more nitrogen atoms, and the atoms constituting the aforementioned five-membered heterocyclic ring or condensed heterocyclic ring may have one or more substituents selected from alkyl groups, carboxyl groups, carboxyalkyl groups, nitro groups, hydroxyl groups, carboxylates, halogen atoms, etc.
[0071] Examples of azoles include pyrazoles, imidazoles, benzimidazoles, triazoles, tetrazoles, etc. Among these, from the viewpoint of being able to selectively etch a copper seed layer with respect to a copper wiring, the azole is preferably a heterocyclic compound containing a five-membered heterocyclic ring having two nitrogen atoms or a condensed heterocyclic ring thereof, and more preferably at least one selected from the group consisting of pyrazoles, imidazoles, and benzimidazoles.
[0072] It should be noted that component (C) may be a salt of an azole. The salt of an azole is not particularly limited, but is preferably an inorganic acid salt from the viewpoint of economic efficiency, and examples thereof include nitrates, sulfates, and hydrochlorides. It should be noted that when the salt of an azole is a hydrochloride, the chloride ions of the hydrochloride may function as halide ions (E).
[0073] <Pyrazoles>
[0074] The pyrazoles are not particularly limited as long as they have a pyrazole skeleton, but are preferably at least one selected from the group consisting of compounds represented by the following formula.
[0075]
[0076] [Where R 1 , R 2 , R 3 and R 4 are independently a hydrogen atom, a C1-C6 alkyl group, a C6-C 10Aryl, carboxyl, carboxyl C1-C6 alkyl, nitro, hydroxyl, C2-C7 carboxylate or halogen atom.]
[0077] It should be noted that in the present specification, "C1-C6 alkyl" refers to an alkyl group having 1 to 6 carbon atoms. Examples of the C1-C6 alkyl group include methyl, ethyl, propyl, isopropyl, n-butyl, sec-butyl, tert-butyl, pentyl, and hexyl. Among these, methyl and ethyl are preferred.
[0078] "C6~C 10 "Aryl" refers to an aromatic group having 6 to 10 carbon atoms. 10 Examples of the aryl group include phenyl, 1-naphthyl, 2-naphthyl, indenyl, biphenylyl, anthracenyl, and phenanthryl. Among these, phenyl is preferred.
[0079] "Carboxy C1-C6 alkyl" refers to an alkyl group having 1 to 6 carbon atoms and having a carboxyl group. Examples of the C1-C6 alkyl group include the same groups as above. Specific examples of the carboxy C1-C6 alkyl group include preferably carboxymethyl (-CH2-COOH) and carboxyethyl (-CH2CH2-COOH).
[0080] "C2-C7 carboxylate" refers to a group represented by -COOR (R is a C1-C6 alkyl group). Examples of the C1-C6 alkyl group include the same groups as above. Specific examples of C2-C7 carboxylate include methyl carboxylate and ethyl carboxylate.
[0081] The "halogen atom" may be any of a fluorine atom, a chlorine atom, a bromine atom and an iodine atom, and a chlorine atom and a bromine atom are particularly preferred.
[0082] In formula (a), R 1 , R 2 , R 3 and R 4 Preferably, they are each independently a hydrogen atom or a C1-C6 alkyl group.
[0083] Examples of pyrazoles include pyrazole and 3,5-dimethylpyrazole.
[0084] <Imidazoles>
[0085] The imidazoles are not particularly limited as long as they have an imidazole skeleton, but are preferably at least one selected from the group consisting of compounds represented by the following formula.
[0086]
[0087] [Where R 1 , R 2 , R 3 and R 4are independently a hydrogen atom, a C1-C6 alkyl group, a C6-C 10 Aryl, carboxyl, carboxyl C1-C6 alkyl, nitro, hydroxyl, C2-C7 carboxylate or halogen atom.]
[0088] In formula (b), R 1 , R 2 , R 3 and R 4 Preferably, they are each independently a hydrogen atom, a C1-C6 alkyl group or a phenyl group.
[0089] Examples of the imidazoles include imidazole, 1,2,4,5-tetramethylimidazole, and 4-methyl-2-phenylimidazole.
[0090] <Benzimidazoles>
[0091] The benzimidazoles are not particularly limited as long as they have a benzimidazole skeleton, but are preferably at least one selected from the group consisting of compounds represented by the following formula.
[0092]
[0093] [Where R 1 , R 2 , R 3 , R 4 , R 5 and R 6 are independently a hydrogen atom, a C1-C6 alkyl group, a C6-C 10 Aryl, carboxyl, carboxyl C1-C6 alkyl, nitro, hydroxyl, C2-C7 carboxylate or halogen atom.]
[0094] In formula (c), R 1 , R 2 , R 3 , R 4 , R 5 and R 6 Preferred are a hydrogen atom, a C1-C6 alkyl group, and a nitro group.
[0095] Examples of the benzimidazoles include benzimidazole, 1-methylbenzimidazole, 2-methylbenzimidazole, 5-methylbenzimidazole, 2,5-dimethylbenzimidazole, and 5-nitrobenzimidazole nitrate.
[0096] <Triazoles>
[0097] The triazoles are not particularly limited as long as they have a triazole skeleton, and examples thereof include 1,2,4-triazole.
[0098] <Benzotriazoles>
[0099] The benzotriazoles are not particularly limited as long as they have a benzotriazole skeleton, and examples thereof include 1H-benzotriazole and 5-methyl-1H-benzotriazole.
[0100] <Tetrazoles>
[0101] The tetrazoles are not particularly limited as long as they have a tetrazole skeleton, and examples thereof include 1H-tetrazole, 5-methyl-1H-tetrazole, 5-phenyl-1H-tetrazole, and 1,5-pentamethylenetetrazole.
[0102] Among the above, as the azole, at least one selected from the group consisting of imidazole, 1,2,4,5-tetramethylimidazole, 4-methyl-2-phenylimidazole, benzimidazole, 1-methylbenzimidazole, 2-methylbenzimidazole, 5-methylbenzimidazole, 2,5-dimethylbenzimidazole, 5-nitrobenzimidazole, pyrazole and 3,5-dimethylpyrazole is more preferred, and at least one selected from the group consisting of 4-methyl-2-phenylimidazole, benzimidazole, 1-methylbenzimidazole, 2-methylbenzimidazole, 5-methylbenzimidazole, 2,5-dimethylbenzimidazole, 5-nitrobenzimidazole and pyrazole is particularly preferred.
[0103] As described above, the component (C) may be a salt of an azole, and the component (C) is particularly preferably at least one selected from the group consisting of 4-methyl-2-phenylimidazole, benzimidazole, 1-methylbenzimidazole, 2-methylbenzimidazole, 5-methylbenzimidazole, 2,5-dimethylbenzimidazole, 5-nitrobenzimidazole nitrate and pyrazole.
[0104] (C) The component may be used alone or in combination of two or more.
[0105] The content of azoles is preferably in the range of 0.01 to 0.5 mass % (100 to 5000 ppm) based on the total amount of the etching composition (mass basis), more preferably 0.05 to 0.4 mass % (500 to 4000 ppm), further preferably 0.1 to 0.3 mass % (1000 to 3000 ppm), and particularly preferably 0.15 to 0.25 mass % (1500 to 2500 ppm). By making the content of azoles within the above range, it is possible to suppress the thinning of the copper wiring and maintain the rectangularity of the wiring cross section, and selectively remove the copper seed layer. It should be noted that when using a salt of an azole as the (C) component, the content of the azoles is calculated by converting it into the content of the azoles after removing the salt portion. When using two or more (C) components, as long as the total amount of azoles contained in them is within the above range.
[0106] [Diol ethers (D)]
[0107] In the present invention, the glycol ether (D) (hereinafter sometimes referred to as component (D)) can achieve the effect of making the amount of copper dissolved in the surface and / or on the back surface of the substrate during etching uniform. Specifically, it can achieve the effect of making the etching speed and etching amount of the copper wiring in the surface and / or on the back surface of the substrate during etching uniform. Therefore, it can achieve the effect of making the thinning degree of the copper wiring in the surface and / or on the back surface of the substrate and the rectangularity of the wiring cross section uniform.
[0108] (D) Component is not particularly limited, but is preferably at least one selected from the group consisting of ethylene glycol monobutyl ether, diethylene glycol monomethyl ether, diethylene glycol monophenyl ether, and dipropylene glycol monomethyl ether.
[0109] The content of component (D) is preferably in the range of 0.01 to 1% by mass (100 to 10000 ppm) based on the total amount of the etching composition (mass basis), more preferably in the range of 0.05 to 0.75% by mass (500 to 7500 ppm), and further preferably in the range of 0.1 to 0.5% by mass (1000 to 5000 ppm). By making the content of component (D) within the above range, it is possible to suppress the thinning of the copper wiring and maintain the rectangularity of the wiring cross section, and selectively remove the copper seed layer. In addition, according to a preferred embodiment of the present invention, by making the content of component (D) within the above range, it is not easily affected by physical conditions such as the spray pressure during the etching process. When using two or more components (D), as long as their total amount is within the above range.
[0110] [Halide ion (E)]
[0111] In the present invention, the halide ion (E) (hereinafter, sometimes simply referred to as component (E)) has a function of stabilizing the etching rate.
[0112] As the component (E), fluoride ion, chloride ion, bromide ion and iodide ion are preferred, chloride ion and bromide ion are more preferred, and chloride ion is particularly preferred.
[0113] As the supply source of component (E) (hereinafter sometimes referred to as halide ion source), there can be listed acids such as hydrochloric acid and hydrobromic acid; and salts such as sodium chloride, ammonium chloride, calcium chloride, potassium chloride, potassium bromide, sodium fluoride, potassium iodide, copper chloride, and copper bromide. Among these, at least one selected from the group consisting of hydrochloric acid and sodium chloride is preferred.
[0114] For example, when the azole or its salt (C) is a halide salt, the component (E) can be supplied from the component (C). In this case, the component (C) can also be used as a halide ion source.
[0115] In the present invention, copper dissolves when etching the copper seed layer, so copper ions may be added in advance for the purpose of suppressing the variation of the copper concentration in the etching composition. Copper chloride and copper bromide may also be used as substances having both the functions of a halide ion source and a copper ion source.
[0116] The halide ion (E) may be used alone or in combination of two or more.
[0117] The content of component (E) is in the range of 0.01 to 3 ppm based on the total amount (mass basis) of the etching composition, preferably 0.05 to 2 ppm, and more preferably 0.1 to 1 ppm. By making the content of component (E) within the above range, the etching rate can be stabilized, and in addition, the copper wiring can be suppressed from becoming thinner and the rectangularity of the wiring cross section can be maintained, and the copper seed layer can be selectively removed. When two or more halide ions (E) are used, the total amount of the components (E) derived from them can be within the above range.
[0118] [Water (F)]
[0119] The water (F) (hereinafter sometimes referred to as the (F) component) used in the present invention is not particularly limited, but is preferably water from which metal ions, organic impurities, particles, etc. have been removed by distillation, ion exchange treatment, filter treatment, various adsorption treatments, etc., and is particularly preferably pure water or ultrapure water. The content of water is not particularly limited, being the remainder of other components, but is preferably in the range of 85 to 99% by mass based on the total amount of the etching composition.
[0120] [Other ingredients]
[0121] The etching composition of the present invention may contain, in addition to the above-mentioned components, one or more kinds of additives generally used in etching compositions as necessary within a range that does not impair the effects of the above-mentioned etching composition.
[0122] Furthermore, a small amount of alkali may be added as long as the pH does not change significantly.
[0123] Furthermore, the etching composition of the present invention may contain known hydrogen peroxide stabilizers such as alcohols, phenylureas, organic carboxylic acids, and organic amine compounds, and etching rate regulators, as needed.
[0124] It should be noted that the etching solution of the present invention is preferably a dissolving solution and does not contain solid particles such as abrasive particles.
[0125] [Preparation of etching composition]
[0126] The etching composition of the present invention can be prepared by uniformly stirring and mixing the components (A), (B), (C), (D), (E), and (F) and other components added as needed. The stirring method for mixing these components is not particularly limited, and a stirring method commonly used in the preparation of etching compositions can be used.
[0127] [Application of etching composition]
[0128] The etching composition of the present invention can be used as an etching composition for selectively etching a copper seed layer from a substrate having a copper wiring pattern and a copper seed layer.
[0129] The copper seed layer to be selectively etched by the etching composition of the present invention is preferably an electrolytic copper foil, an electrolytic copper plating film, an electroless copper plating film, or a combination of two or more thereof.
[0130] It should be noted that, in this specification, “selectivity” means that the etching rate of the copper seed layer is higher than the etching rate of the copper wiring.
[0131] For example, in the present invention, the ratio of the etching rate of the copper wiring to the etching rate of the copper seed layer can be evaluated by the etching rate ratio of the wiring height and the etching rate ratio of the wiring width of the copper wiring measured at a processing temperature of 30° C. based on the etching rate of the copper seed layer. The etching rate ratio of the wiring height and the etching rate ratio of the wiring width are defined by the following formulas (1) and (2).
[0132] Wiring height etching rate ratio = Δ height / seed layer thickness (1)
[0133] Wiring width etching rate ratio = Δ sheet width / seed layer thickness (2)
[0134] [Wherein, the seed layer thickness represents the thickness of the copper seed layer removed by etching (μm), Δheight represents the etching thickness of the upper surface of the copper wiring removed by etching within the etching time that is just enough to remove the entire copper seed layer by etching (μm), and Δsheet width represents the value obtained by converting the lateral width of the copper wiring removed by etching into a single-side amount (1 / 2) within the etching time that is just enough to remove the entire copper seed layer by etching (μm).]
[0135] In the present invention, the etching rate ratio of the wiring height is preferably 1.2 or less. Furthermore, the etching rate ratio of the wiring width is preferably 1.4 or less, and more preferably 1.0 or less. In the present invention, the etching rate ratio of the wiring height preferably satisfies the above range, and more preferably, both the etching rate ratio of the wiring height and the etching rate ratio of the wiring width satisfy the above range.
[0136] For example, the etching composition of the present invention can be suitably used when removing the copper seed layer exposed along with the removal of the resist pattern after forming a copper wiring pattern in SAP or M-SAP. In addition, the etching composition of the present invention can be suitably used when removing the electrolytic copper foil as the copper seed layer in the ETS process.
[0137] According to a preferred embodiment of the present invention, by etching the copper seed layer using the etching composition of the present invention, the copper seed layer can be selectively removed while suppressing the thinning of the copper wiring and maintaining the rectangularity of the wiring cross section.
[0138] The thickness of the copper seed layer suitable for removal by the etching composition of the present invention is not particularly limited, but is usually 1.5 to 15 μm, preferably 1.5 to 10 μm, and more preferably 1.5 to 5 μm.
[0139] 2. Manufacturing method of wiring substrate
[0140] The method for manufacturing a wiring substrate of the present invention is characterized in that it includes the following steps:
[0141] The copper seed layer is selectively etched from a substrate having a copper wiring pattern and a copper seed layer using the etching composition.
[0142] The etching composition and the copper seed layer to be etched are as described in the above-mentioned “1. Etching composition”.
[0143] The use temperature of the etching composition of the present invention is not particularly limited, and is preferably a temperature of 10 to 50°C, more preferably 20 to 45°C, and further preferably 25 to 40°C. If the temperature of the etching composition is above 10°C, the etching rate becomes good, so that excellent production efficiency can be obtained. On the other hand, if the temperature of the etching composition is below 50°C, the liquid composition change can be suppressed and the etching conditions can be kept constant. By increasing the temperature of the etching solution, the etching rate increases, but it is also considered that the composition change of the etching solution (decomposition of hydrogen peroxide) is suppressed to a small extent, etc., and the optimal processing temperature can be appropriately determined.
[0144] The etching treatment time is not particularly limited, but is preferably 1 to 600 seconds, more preferably 5 to 300 seconds, further preferably 10 to 180 seconds, and particularly preferably 15 to 120 seconds. The treatment time may be appropriately selected depending on various conditions such as the treatment temperature and the treatment method.
[0145] The method of contacting the etching composition with the etching object including the copper seed layer is not particularly limited. For example, a wet etching method such as a method of contacting the etching object with the etching composition by dripping (single-wafer spinning process) or spraying the etching composition, or a method of immersing the etching object in the etching composition can be adopted. In the present invention, any method can be adopted.
[0146] The method for manufacturing a wiring substrate of the present invention is suitable for selectively etching a copper seed layer from a substrate having a copper wiring pattern and a copper seed layer to form a wiring circuit, for example in a semi-additive process (SAP), a modified semi-additive process (M-SAP) or an embedded trace substrate process (ETS process).
[0147] An example of the method for manufacturing the wiring substrate of the present invention will be described below, but the method for manufacturing the wiring substrate of the present invention is not limited thereto.
[0148] <Method for Manufacturing Wiring Substrate Using SAP>
[0149] Figure 1 This is a diagram for explaining a method for manufacturing a wiring substrate in which a wiring circuit is formed by selectively etching a copper seed layer from a substrate having a copper wiring pattern and a copper seed layer in SAP. Figure 1 In the figure, for the purpose of explanation, only necessary structures are schematically shown.
[0150] First, an insulating resin substrate (1) is prepared ( Figure 1 (a)), a through hole or a groove (1a) is formed by drilling or the like as needed ( Figure 1 Next, electroless copper plating is performed on the surface of the insulating resin substrate (1) including the inner wall of the through hole or the groove (1a) to form an electroless copper plating film (2) as a copper seed layer ( Figure 1 (c)). In addition, although not shown, an electrolytic copper plating film can be further formed on the surface of the electroless copper plating film (2). When the electrolytic copper plating film is formed, the electroless copper plating film (2) and the electrolytic copper plating film serve as a "copper seed layer".
[0151] Next, when the electroless copper plating film (2) or the electrolytic copper plating film is formed, a dry film resist (3) is formed on the surface of the electrolytic copper plating film ( Figure 1 (d)), which is then exposed and developed to form a resist pattern (3a) ( Figure 1 (e)).
[0152] Next, electrolytic copper plating is performed on the copper seed layer between the resist patterns (3a) to form an electrolytic copper plating film (4) ( Figure 1 (f)).
[0153] Next, the resist pattern (3a) is stripped off using a stripping solution to form a copper wiring pattern (4a) ( Figure 1 (g)).
[0154] Finally, by applying the etching composition of the present invention to the surface of the copper seed layer and removing the exposed portion of the copper seed layer, a wiring substrate (10) having a copper wiring pattern (4a) formed thereon can be manufactured ( Figure 1 (h)).
[0155] According to a preferred embodiment of the present invention, by using the etching composition of the present invention in SAP to etch a copper seed layer, it is possible to suppress side etching and / or upper surface etching of a copper wiring pattern (4a) and maintain the rectangularity of the wiring cross section, and selectively etch the copper seed layer, thereby manufacturing a wiring substrate (10) corresponding to wiring miniaturization.
[0156] <Method for manufacturing a wiring substrate using M-SAP>
[0157] Figure 2 This is a diagram for explaining a method for manufacturing a wiring substrate in which a wiring circuit is formed by selectively etching a copper seed layer from a substrate having a copper wiring pattern and a copper seed layer in M-SAP. Figure 2 In the figure, for the purpose of explanation, only necessary structures are shown schematically.
[0158] First, an insulating resin substrate (1) is prepared, and an electrolytic copper foil (5) is laminated using an electrolytic copper foil with a carrier foil (not shown). Figure 2 (a)). Examples of the carrier foil include aluminum foil, copper foil, stainless steel foil, resin film, resin film with a metal coating on the surface, glass plate, etc. After the carrier foil is peeled off and removed, the electrolytic copper foil (5) is half-etched as needed to form a copper thin layer (6) ( Figure 2 (b)), through holes or grooves (1a) are formed by drilling or the like as needed ( Figure 2 (c)).
[0159] Next, electroless copper plating is performed on the copper thin layer (6) including the inner wall of the through hole or the groove (1a) to form an electroless copper plating film (2) ( Figure 2 (d)). In addition, although not shown in the figure, an electrolytic copper-plated film (not shown) can be further formed on the electroless copper-plated film (2). When the electrolytic copper-plated film is not formed, the copper thin layer (6) and the electroless copper-plated film (2) are used as a "copper seed layer". When the electrolytic copper-plated film is formed, the copper thin layer (6), the electroless copper-plated film (2) and the electrolytic copper-plated film are used as a "copper seed layer".
[0160] Next, when the electroless copper plating film (2) or the electrolytic copper plating film is formed, a dry film resist (3) is formed on the surface of the electrolytic copper plating film (not shown) ( Figure 2 (e)), which is then exposed and developed to form a resist pattern (3a) ( Figure 2 (f)).
[0161] Next, electrolytic copper plating is performed on the copper seed layer between the resist patterns (3a) to form an electrolytic copper plating film (4) ( Figure 2 (g)).
[0162] Next, the resist pattern (3a) is stripped off using a stripping solution to form a copper wiring pattern (4a) ( Figure 2 (h)).
[0163] Finally, by applying the etching composition of the present invention to the surface of the copper seed layer and removing the exposed portion of the copper seed layer, a wiring substrate (10) having a copper wiring pattern (4a) formed thereon can be manufactured ( Figure 2 (i)).
[0164] According to a preferred embodiment of the present invention, by using the etching composition of the present invention in M-SAP to etch a copper seed layer, it is possible to suppress side etching and / or upper surface etching of a copper wiring pattern (4a) and selectively etch the copper seed layer, thereby manufacturing a wiring substrate (10) that can cope with miniaturization of wiring.
[0165] <Method for manufacturing wiring substrate using ETS process>
[0166] Figure 3 This is a diagram for explaining a method for manufacturing a wiring substrate in which a wiring circuit is formed by selectively etching a copper seed layer from a substrate having a copper wiring pattern and a copper seed layer in an ETS process. Figure 3 In the figure, for the purpose of explanation, only necessary structures are schematically shown.
[0167] First, an electrolytic copper foil (5) with a carrier foil (5a) is laminated on an insulating resin substrate (1). Figure 3 (a)). Examples of the carrier foil (5a) include aluminum foil, copper foil, stainless steel foil, resin film, resin film with a metal coating on the surface, and glass plate.
[0168] Next, a dry film resist is formed on the surface of the electrolytic copper foil (5), and exposure and development are performed to form a resist pattern (3a) ( Figure 3 (b)). In the ETS process, the electrolytic copper foil (5) plays the role of a copper seed layer.
[0169] Thereafter, electrolytic copper plating is performed on the exposed portion of the electrolytic copper foil (5) on which the resist pattern (3a) is not formed to form an electrolytic copper plating film (4) ( Figure 3 of (c)).
[0170] Next, the resist pattern (3a) is peeled off using a stripping solution to form a copper wiring pattern (4a) composed of copper wirings ( Figure 3 of (d)).
[0171] Next, the obtained structure is turned over, and the copper wiring pattern (4a) is embedded in the interlayer insulating resin (7) ( Figure 3 of (e)). As the interlayer insulating resin (7), there is no particular limitation as long as it is a resin generally used for manufacturing printed circuit boards.
[0172] Thereafter, the insulating resin substrate (1) and the carrier foil (5a) are peeled off ( Figure 3 of (f)), and finally, the electrolytic copper foil (5) is etched back using the etching composition of the present invention, and a printed circuit board (10) in which the copper wiring pattern (4a) is embedded can be obtained ( Figure 3 of (g)).
[0173] According to a preferred embodiment of the present invention, by etching the electrolytic copper foil (copper seed layer) using the etching composition of the present invention in the ETS process, it is possible to both suppress the occurrence of side etching of the copper wiring pattern (4a) along the side wall of the interlayer insulating resin (7) and / or etching of the upper surface and maintain the rectangularity of the wiring cross section, and selectively etch the electrolytic copper foil (5), and a printed circuit board (10) corresponding to wiring miniaturization can be manufactured.
[0174] Examples
[0175] Next, the present invention will be described in more detail using examples and comparative examples, but the present invention is not limited to these examples at all.
[0176] <Examples 1 to 24>
[0177] (1) Preparation of etching composition
[0178] Each component is mixed and stirred according to the composition ratio described in Table 1A to make a uniform state, and an etching composition is prepared.
[0179] [Table 1A]
[0180]
[0181] (2) Evaluation samples
[0182] <Evaluation samples in M - SAP (Examples 1 to 13, Examples 15 to 24, Comparative Examples 1 to 9)>
[0183] Operate as follows to prepare evaluation samples of the etching compositions of Examples 1 to 13, Examples 15 to 24, and Comparative Examples 1 to 9.
[0184] First, laminate an ultra-thin copper foil with a carrier foil, "Micro Thin18EX" (manufactured by Mitsui Mining & Smelting Co., Ltd.), having an electrolytic copper foil with a thickness of 3 μm, such that the electrolytic copper foil side contacts an insulating resin substrate (separator core).
[0185] Next, peel off the carrier foil, and perform electroless copper plating (0.6 μm) and electrolytic copper plating (3.4 μm) on the exposed electrolytic copper foil such that the total thickness becomes 4 μm to form a copper seed layer with a thickness of 7 μm.
[0186] Thereafter, laminate a dry film resist on the copper seed layer, and expose the dry film resist according to a wiring design of line / space (L / S) = 45 / 15 μm. Develop the exposed dry film resist using an aqueous sodium carbonate solution to form a resist pattern.
[0187] Next, perform electrolytic copper plating on the exposed portion of the copper seed layer not covered with the resist to form an electrolytic copper plating film such that the wiring height becomes 20 μm.
[0188] Thereafter, use a dry film stripper "R-100S" (manufactured by Mitsubishi Gas Chemical Company, Inc.) to peel off the resist pattern, and obtain a substrate (evaluation sample) having a copper wiring formed on the copper seed layer.
[0189] The width of the copper wiring in the evaluation sample is 43.8 μm, and the height of the copper wiring from the upper surface of the copper seed layer is 21.3 μm.
[0190] <Evaluation sample (Example 14) in the ETS process>
[0191] Operate as follows to prepare an evaluation sample of the etching composition of Example 14.
[0192] First, laminate an ultra-thin copper foil with a carrier foil, "MT18SD-H-T5" (manufactured by Mitsui Mining & Smelting Co., Ltd.), having an electrolytic copper foil with a thickness of 5 μm, such that the carrier foil side contacts a separator core with a thickness of 100 μm (base material: "HL-832NSF") (manufactured by Mitsubishi Gas Chemical Company, Inc.).
[0193] Next, laminate a dry film resist on the surface of the electrolytic copper foil, and expose the dry film resist according to a wiring design of line / space (L / S) = 10 / 10 μm. Develop the exposed dry film resist using an aqueous sodium carbonate solution to form a resist pattern.
[0194] Next, electrolytic copper plating was performed on the exposed portion of the electrolytic copper foil (copper seed layer) not covered with the resist to form an electrolytic copper plated film so that the wiring height would be 10 μm.
[0195] Thereafter, the resist pattern was peeled off using a dry film stripping liquid "R-100S" (manufactured by Mitsubishi Gas Chemical Co., Ltd.), thereby forming copper wiring on the electrolytic copper foil.
[0196] Next, the obtained structure was turned over and laminated in a manner that the copper wiring was embedded in the prepreg "GHPL-830NS SH65" (manufactured by Mitsubishi Gas Chemical Co., Ltd.). It should be noted that as the outer layer copper foil laminated on the prepreg on the side opposite to the copper wiring used when laminating the copper wiring on the prepreg, an ultra-thin copper foil "MT18Ex" (manufactured by Mitsui Mining and Smelting Co., Ltd.) with a carrier foil having an electrolytic copper foil with a thickness of 5 μm was used in a manner that the electrolytic copper foil became the prepreg side.
[0197] Thereafter, the separate core and the carrier foil are peeled off to produce a substrate having an electrolytic copper foil on the surface and in which copper wiring is embedded.
[0198] The obtained substrate had copper wiring formed at a pitch of 20 μm and a wiring width of 10 to 10.5 μm.
[0199] (3) Etching treatment
[0200] The sample for evaluation was etched using the etching composition prepared in (1) above at a treatment temperature of 30° C. using a spray etching machine. The spray pressure was set to 0.05 MPa in Example 4 and 0.15 MPa in other examples and comparative examples. The etching endpoint was observed using an optical microscope (“MX-63L” manufactured by Olympus Corporation) and was set to the time point when the residual copper of the copper seed layer between the copper wirings disappeared (just etching time).
[0201] The evaluation sample was removed from the etching composition, and washed by immersing in ultrapure water for 10 seconds, immersing in 5 mass % sulfuric acid for 10 seconds, and immersing in ultrapure water for 10 seconds. The evaluation sample was removed from the ultrapure water and dried by blowing nitrogen.
[0202] (4) Evaluation of the Width and Height of Copper Wiring after Etching
[0203] The wiring width and height of the copper wiring after etching of each evaluation sample of the example and comparative example were measured from the wiring cross-sectional direction using SEM ("S-3700" manufactured by Hitachi High-Technologies Corporation) and evaluated according to the following criteria.
[0204] <Width>
[0205] ◎: 30μm or more
[0206] ○: 25 μm or more and less than 30 μm
[0207] ×: less than 25 μm
[0208] <Height>
[0209] ◎: 20μm or more
[0210] ×: less than 20 μm
[0211] (5) Evaluation of rectangularity of copper wiring after etching
[0212] The wiring cross section of the copper wiring after etching was observed by SEM ("S-3700" manufactured by Hitachi High-Technologies Corporation), and the rectangularity of the wiring cross-sectional shape was visually evaluated. The rectangularity was evaluated according to the following criteria.
[0213] <Rectangularity>
[0214] ◎: Maintain rectangularity
[0215] 0: Slightly trapezoidal, but rectangular
[0216] ×: Trapezoidal, unable to maintain rectangular shape, or undercut or side etching
[0217] It should be noted that specific examples of evaluation criteria for the cases of SAP, M-SAP and ETS process are shown in Figure 4 .
[0218] (6) Evaluation of Etching Rate of Copper Seed Layer
[0219] The etching rate (ER, μm / min) of the copper seed layer was calculated by dividing the thickness (μm) of the copper seed layer by the exact etching time (min).
[0220] (7) Evaluation of etching rate ratio
[0221] The etching rate ratio of the wiring width and the etching rate ratio of the wiring height were calculated according to the following formula, and evaluated according to the following criteria.
[0222] Wiring height etching rate ratio = Δ height / seed layer thickness (1)
[0223] Wiring width etching rate ratio = Δ sheet width / seed layer thickness (2)
[0224] <Etching speed ratio of wiring height>
[0225] ◎: 1.2 or less
[0226] ×: more than 1.2
[0227] <Etching speed ratio of wiring width>
[0228] ◎: 1.0 or less
[0229] ○: more than 1.0 and less than 1.4
[0230] ×: more than 1.4
[0231] The results are shown in Table 1B. In addition, the comprehensive evaluation was set as the lowest evaluation among the evaluation items.
[0232] [Table 1B]
[0233]
[0234] Comparative Examples 1 to 9
[0235] The etching composition was prepared in the same manner as in Example except that the composition ratio was set to that described in Table 2A. The evaluation sample was used for etching treatment, and the shape (width, height, and rectangularity) of the copper wiring after the etching treatment, the etching rate, and the etching rate ratio were evaluated.
[0236] [Table 2A]
[0237]
[0238] The results are shown in Table 2B. In addition, the comprehensive evaluation was set as the lowest evaluation among the evaluation items.
[0239] [Table 2B]
[0240]
[0241] As shown in the above results, by using the etching composition of the present invention, it is possible to selectively remove the copper seed layer while suppressing the thinning of the copper wiring and maintaining the rectangularity of the wiring cross section (Examples 1 to 24).
[0242] On the other hand, when the components (A) and (B) are not included, etching is not performed (Comparative Example 1). When only the components (A) and (B) are included or when the component (C) is not included, the wiring height is greatly reduced and the copper seed layer cannot be selectively etched (Comparative Examples 2 and 3).
[0243] In the case where the (E) component is not included, the wiring width and wiring height are greatly reduced, and the copper seed layer cannot be selectively etched (Comparative Example 4). In addition, when the content of the (E) component exceeds the specified range, the wiring height is greatly reduced, and the copper seed layer cannot be selectively etched (Comparative Example 5).
[0244] When the (A) component / (B) component ratio was less than the predetermined range, the copper seed layer could not be selectively etched (Comparative Examples 6 and 7).
[0245] When the (D) component is not contained and the (A) component / (B) component is less than the prescribed range, the rectangular property cannot be maintained (Comparative Example 8).
[0246] In addition, when the (D) component and the (E) component were not contained and the (A) component / (B) component was less than the prescribed range, the wiring height was significantly reduced and the rectangularity could not be maintained (Comparative Example 9).
[0247] Description of Reference Numerals
[0248] 1 Insulating resin substrate
[0249] 1a Through hole or groove
[0250] 2 Electroless copper plating
[0251] 3 Dry Film Resist
[0252] 3a Resist pattern
[0253] 4 Electrolytic copper plating
[0254] 4a Copper wiring pattern
[0255] 5 Electrolytic copper foil
[0256] 5a Carrier foil
[0257] 6 Copper thin layer
[0258] 7. Interlayer insulation resin
[0259] 10 Wiring substrate or printed circuit board
Claims
1. An etching composition for selectively etching a copper seed layer from a substrate having a copper wiring pattern and a copper seed layer, The etching composition comprises hydrogen peroxide (A), sulfuric acid (B), azoles or salts thereof (C), glycol ethers (D), halide ions (E) and water (F), The content of hydrogen peroxide (A) is 0.1 to 10% by mass based on the total amount of the etching composition. The content of sulfuric acid (B) is 0.5 to 5% by mass based on the total amount of the etching composition. The ratio of hydrogen peroxide (A) to sulfuric acid (B) is 2 or more as expressed in molar ratio, The content of the halide ion (E) is 0.01 to 3 ppm based on the total amount of the etching composition.
2. The etching composition according to claim 1, in, Azoles are heterocyclic compounds containing a five-membered heterocyclic ring or a condensed heterocyclic ring thereof having two nitrogen atoms.
3. The etching composition according to claim 2, in, The azole is at least one selected from the group consisting of pyrazoles, imidazoles, and benzimidazoles.
4. The etching composition according to claim 3, in, The azoles are one or more selected from the group consisting of compounds represented by the following formula: In the formula, R 1 , R 2 , R 3 , R 4 , R 5 and R 6 are independently hydrogen atoms, C 1 ~C 6 Alkyl, C 6 ~C 10 Aryl, Carboxyl, Carboxyl C 1 ~C 6 Alkyl, nitro, hydroxyl, C 2 ~C 7 carboxylate or a halogen atom.
5. The etching composition according to claim 4, in, The azole is at least one selected from the group consisting of imidazole, 1,2,4,5-tetramethylimidazole, 4-methyl-2-phenylimidazole, benzimidazole, 1-methylbenzimidazole, 2-methylbenzimidazole, 5-methylbenzimidazole, 2,5-dimethylbenzimidazole, 5-nitrobenzimidazole, pyrazole and 3,5-dimethylpyrazole.
6. The etching composition according to any one of claims 1 to 5, in, The content of the azoles is 0.01 to 0.5% by mass based on the total amount of the etching composition.
7. The etching composition according to any one of claims 1 to 6, in, The glycol ether (D) is at least one selected from the group consisting of ethylene glycol monobutyl ether, diethylene glycol monomethyl ether, diethylene glycol monophenyl ether, and dipropylene glycol monomethyl ether.
8. The etching composition according to any one of claims 1 to 7, in, The content of the glycol ether (D) is 0.01 to 1% by mass based on the total amount of the etching composition.
9. The etching composition according to any one of claims 1 to 8, in, The halide ion (E) is a chloride ion.
10. The etching composition according to any one of claims 1 to 9, in, The etching rate ratio of the wiring height of the copper wiring defined by the formula (1) at a processing temperature of 30° C. is 1.2 or less. Wiring height etching rate ratio = Δ height / seed layer thickness (1) In formula (1), the seed layer thickness represents the thickness (μm) of the copper seed layer removed by etching, and the Δ height represents the etching thickness (μm) of the upper surface of the copper wiring removed by etching within the etching time just enough to remove the entire copper seed layer by etching.
11. The etching composition according to claim 10, in, The etching rate ratio of the wiring width of the copper wiring defined by the formula (2) at a processing temperature of 30° C. is 1.4 or less. Wiring width etching rate ratio = Δ sheet width / seed layer thickness (2) In formula (2), the seed layer thickness represents the thickness of the copper seed layer removed by etching (μm), and the Δ sheet width represents the value (μm) obtained by converting the lateral width of the copper wiring removed by etching into a single-sided amount (1 / 2) within the etching time required to remove the entire copper seed layer by etching.
12. The etching composition according to any one of claims 1 to 11, in, The copper seed layer is at least one selected from the group consisting of an electrolytic copper foil, an electrolytic copper plating film, and an electroless copper plating film.
13. A method for manufacturing a wiring substrate, comprising the following steps: A copper seed layer is selectively etched from a substrate having a copper wiring pattern and a copper seed layer using the etching composition according to any one of claims 1 to 12.
14. The method for manufacturing a wiring substrate according to claim 13, in, The copper seed layer is at least one selected from the group consisting of an electrolytic copper foil, an electrolytic copper plating film, and an electroless copper plating film.
15. A method for manufacturing a wiring substrate, in, In a semi-additive process (SAP), a modified semi-additive process (M-SAP) or an embedded trace substrate process (ETS process), a copper seed layer is selectively etched from a substrate having a copper wiring pattern and a copper seed layer using the etching composition described in any one of claims 1 to 12 to form a wiring circuit.
Citation Information
Patent Citations
Etching liquid for copper foils, method for producing printed wiring board using said etching liquid for copper foils, etching liquid for electrolytic copper layers, and method for producing copper pillar said etching liquid for electrolytic copper layers
WO2019208461A1
Mirror finish etching liquid for copper and copper alloy
JP2005015860A