Synthesis, blocking and dispersion of high refractive index nanocrystals and nanocomposite materials
Through the core-shell structure and inorganic passivation treatment of TiO2 nanocrystals, the problems of photocatalytic activity and thermal stability are solved, achieving high refractive index and stable nanocomposites suitable for optical and catalytic applications.
Patent Information
- Application Number
- CN202280092273.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2021-12-21
- Filing Date
- 2022-12-20
- Publication Date
- 2024-10-11
AI Technical Summary
Existing TiO2 nanocrystals are too active under photocatalytic and high-temperature conditions, leading to the decomposition of surface organic matter, causing polymer defects such as powdering and yellowing, and lack of stable high-refractive index materials.
TiO2 and ZrO2 nanocrystals with core-shell structure are used to reduce photocatalytic activity and improve thermal stability by forming metal oxide shells and inorganic passivation treatments, and disperse them in solvents, monomers, oligomers or polymers In, use capping agents and inorganic passivators for treatment to improve dispersion and stability.
The stability and high refractive index of TiO2 nanocrystals under high temperature and light conditions are achieved, reducing photocatalytic activity, extending the service life of the material and improving optical transparency.
Smart Images

Figure CN118765339A_ABST
Abstract
Description
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS
[0002] This application claims priority to U.S. application No. 63 / 292,197. Technical Field
[0003] This application claims the benefit of U.S. Provisional Application No. 63 / 292,197, filed on December 21, 2021, the entire contents of which are incorporated herein by reference.
[0004] In various embodiments, the present application describes the preparation of metal oxide nanocrystals having photocatalytically stable and thermally stable capped ZrO and TiO shells, and dispersions thereof in monomers, oligomers and / or polymers, and the resulting nanocomposite films. These nanocrystals are highly monodisperse, with nanocrystal sizes ranging from 3 to 100 nm. Dispersions of these nanocrystals are formed in various solvents, monomers, oligomers and / or polymers. These dispersions typically have high loading, high transmittance and low viscosity. The resulting formulations incorporating these nanocrystals and a matrix material are typically highly stable and result in nanocomposites having a high refractive index, are low absorbing, exhibit little change in absorbance upon thermal or UV treatment, and are optically transparent at visible wavelengths with very little or no scattering. Background Art
[0005] Titanium dioxide (TiO2), or titanium dioxide, is one of the most widely used versatile ceramic materials due to its unique physical and chemical properties, combined with its abundance and non-toxicity. Due to its numerous properties, including a high refractive index and (UV) light absorption, TiO2 is commercially produced in millions of tons and is commonly found in pigments, paints, sunscreens, and coatings. In addition to its traditional applications, titanium dioxide is being investigated for numerous applications, including optoelectronics, photovoltaics, catalysis, fuel cells, batteries, smart windows, sensors, and self-cleaning surfaces.
[0006] Titanium dioxide, particularly subnanometer-sized particles, has attracted significant interest in optical applications due to its high refractive index. The two crystalline phases of titanium oxide, anatase and rutile, have refractive indices of 2.55 and 2.76, respectively. When combined with monomers, oligomers, or polymers, these metal oxides exhibit high transparency and a high refractive index. However, TiO2 particles are excellent UV absorbers. The energy band gaps of anatase and rutile are 3.23 eV and 3.06 eV, respectively. Due to this large band gap, TiO2 is photochemically active. When exposed to high-energy wavelengths, electrons are excited from the valence band to the conduction band, generating electron-hole pairs. These electron-hole pairs diffuse to the surface of the TiO2 to generate free radical species, which can then be detrimental to surface organic matter, causing its breakdown. This decomposition of surface organic matter leads to the decomposition of the polymer, resulting in defects such as chalking and yellowing.
[0007] As the demand for higher refractive index materials increases, the need for photochemically and thermally stable TiO2 becomes critical. Due to the limited choice of available organic materials, inorganic-organic nanocomposites remain the only option to achieve this higher refractive index requirement. Summary of the Invention
[0008] The present disclosure provides a method for preparing TiO2 nanocrystals with reduced photocatalytic activity and thermal stability at higher temperatures.
[0009] The present disclosure provides a method for preparing TiO2 and ZrO2 nanocrystals, wherein the TiO2 and ZrO2 nanocrystals include a crystalline core forming a nanocrystal having a core-shell structure and a thin shell of a metal oxide. The shell material includes but is not limited to silicon dioxide, zirconium dioxide, hafnium dioxide, niobium oxide, aluminum oxide, tantalum oxide, barium titanium oxide, cerium oxide, or any combination thereof.
[0010] The present disclosure includes a method for end-capping core-shell nanocrystals with a crystalline core and a metal oxide shell / coating. The core-shell nanocrystals are separated and / or purified, and end-capped with at least one end-capping agent to produce at least part of the end-capped nanocrystals. The at least part of the end-capped nanocrystals can be further purified and / or separated according to the method of the present disclosure. In the method of the present disclosure, the nanocrystals and the end-capped nanocrystals can be dispersed in a material that comprises a solvent, a monomer, a polymer or some combination thereof.
[0011] The present disclosure also includes the TiO that is coated with metal oxide shell / coating and ZrO nanocrystal carries out surface passivation and the method for further processing with at least one inorganic passivating agent.Before or after carrying out end-capping with at least one end-capping agent, core-shell nanocrystal of the present disclosure is processed with at least one inorganic passivating agent.According to the method of the present disclosure, the at least partially end-capped nanocrystal that obtains through inorganic processing is further purified and / or separated.In the method of the present disclosure, nanocrystal and end-capped nanocrystal are dispersed in the material that comprises solvent, polymer or its some combination.
[0012] The present disclosure includes a method for passivating TiO2 and ZrO2 nanocrystals without shells with at least one inorganic passivating agent. The TiO2 and ZrO2 nanocrystals of the present disclosure are optionally treated with at least one inorganic passivating agent before or after capping. The inorganically treated at least partially capped nanocrystals are further purified and / or separated according to the method of the present disclosure. In the method of the present disclosure, the nanocrystals and the capped nanocrystals are dispersed in a material comprising a solvent, a polymer, or some combination thereof.
[0013] The present disclosure also includes dispersions and formulations of core-shell nanocrystals having a core metal oxide and at least one shell metal oxide outer shell. These dispersions can be in solvents and formulations that contain monomers, oligomers, and / or polymers in addition to other additives.
[0014] The disclosure also comprises the nanocomposite material that contains matrix and nanocrystal, and said matrix and nanocrystal are for example mixed, stirred or dispersed.Prepared according to the nanocomposite material of the present disclosure by for example the precursor of nanocrystal and matrix material or matrix is carried out UV curing, thermosetting, melt blending, in-situ polymerization and / or solvent mixing.Nanocrystal comprises ZrO Nanocrystal, TiO One or more in nanocrystal and the core-shell nanocrystal.
[0015] The present disclosure includes methods for evaluating the photocatalytic activity and thermal stability of TiO2 nanocrystals embedded in a polymer matrix.
[0016] The present disclosure also provides exemplary embodiments, such as those set forth in the Examples section, listed embodiments 1-42, and claims 1-62 herein.
[0017] It is to be understood that the foregoing summary and the following detailed description are exemplary and explanatory only and are not restrictive of the invention herein. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1: Exemplary intensity versus particle size DLS plot of 5 wt % inorganically passivated capped titanium oxide nanocrystals with ZrO2 shells as described in Example 6 in PGMEA, showing an average particle size of 37.15 nm.
[0019] Figure 2 : Exemplary volume versus particle size DLS plot of 5 wt % inorganically passivated capped titanium oxide nanocrystals containing ZrO2 shells as described in Example 6 in PGMEA, showing an average particle size of 25.46 nm.
[0020] Figure 3 : An exemplary TEM image of titanium oxide nanocrystals with a ZrO2 shell described in Example 6, showing an average particle size of less than 20 nm and the presence of Zr and Ti atoms in the same particles.
[0021] Figure 4a 、 Figure 4b and Figure 4c : Exemplary optical transmittance of a 1 micron thick spin-coated nanocomposite comprising at least partially end-capped TiO2 nanocrystals having a ZrO2 shell and the acrylic monomer described in Example 19, wherein: (a) nanocrystals of Example 5, (b) nanocrystals of Example 6, and (c) nanocrystals of Example 7, when continuously exposed to a 450 nm wavelength for 1000 h.
[0022] Table Description
[0023] Table 1: Discoloration rating of TiO2 nanocrystals with and without ZrO2 shells before capping and without inorganic treatment upon exposure to UV irradiation and accelerated baking steps.
[0024] Table 2: Discoloration rating of at least partially capped TiO2 nanocrystals without any metal oxide shell and subjected to different inorganic treatments upon exposure to UV irradiation and accelerated baking steps.
[0025] Table 3: Discoloration levels of at least partially capped TiO2 with and without a ZrO2 shell and / or inorganic treatment when heated to different temperatures.
[0026] Table 4: Optical properties of nanocomposites prepared using the formulation described in Example 19.
[0027] Table 5: Nanocomposites prepared by the process described in Example 19 after continuous exposure to 320-390 nm wavelength for 158 h (average intensity 4 mW / cm 2 ) when the optical properties.
[0028] Table 6: Nanocomposites prepared by the process described in Example 19 after continuous exposure to 405 nm wavelength for 148 h (average intensity 25 mW / cm 2 ) when the optical properties.
[0029] Table 7: Nanocomposites prepared by the process described in Example 19 after continuous exposure to 450 nm wavelength for 1000 h (average intensity 16 mW / cm 2 ) when the optical properties.
[0030] Table 8a: Summary of formulation compositions and properties. Includes samples with titanium dioxide nanocrystals and titanium dioxide-zirconia nanocrystals.
[0031] Table 8c: Optical properties of the nanocomposite material described in Example 21 upon exposure to UVA light for 72 h.
[0032] Table 8d: Optical properties of the nanocomposite material described in Example 21 upon exposure to QUV accelerated weathering testing for 72 h.
[0033] Table 9a: Summary of formulation composition and viscosity described in Example 22.
[0034] Table 9b: Optical properties of the nanocomposite material on a glass substrate described in Example 22 upon exposure to 405 nm light for 150 h.
[0035] Table 10a: Viscosity and optical properties of the nanocomposites prepared using the formulation described in Example 23
[0036] Table 10b: Optical properties of the nanocomposite material described in Example 23 upon exposure to QUV accelerated weathering testing for 72 h.
[0037] Table 10c: Optical properties of the nanocomposite material described in Example 23 upon continuous exposure to 405 nm wavelength for 148 h DETAILED DESCRIPTION
[0038] The zirconium oxide and titanium oxide nanocrystals used in the various treatments disclosed herein can generally be prepared by a solvothermal process, in which a precursor of titanium oxide or zirconium oxide is mixed or dissolved in at least one solvent and allowed to react for a certain period of time. In some cases, pressure and / or heating are applied. Optionally, the resulting TiO2 or ZrO2 nanocrystals are separated and purified by sedimentation, centrifugation, filtration, and other separation methods known in the art. In the solvothermal process, the solvent is not water. When water is used as the majority solvent, the synthesis method is referred to as a hydrothermal synthesis. In the solvothermal synthesis of TiO2 and ZrO2 nanocrystals, adding a small amount of water as a reactant rather than as a solvent to the reaction mixture provides better control over particle size and size distribution than reactions carried out without the addition of water. Exemplary useful methods for the synthesis, capping, and dispersion of TiO2 and ZrO2 nanocrystals herein include those described in International Application Nos. PCT / US2011 / 057822 (published as WO 2012 / 058271) and PCT / US2019 / 062439 (published as WO 2020 / 106860), the contents of each of which are incorporated herein by reference in their entirety.
[0039] The precursor of titanium oxide nanocrystals is generally selected from one or more of the following: alkoxides, such as titanium methoxide (Ti(OCH3)4), titanium ethoxide (Ti(OCH2CH3)4), titanium n-propoxide (Ti(OCH2CH2CH3)4), titanium isopropoxide (Ti(OCH(CH3)2)4), titanium n-butoxide (Ti(OCH2CH2CH2CH3)4); acetylacetonates, such as titanium oxyacetylacetonate (TiO(CH3COCH4)4); C OCH3)2); halides such as titanium chloride (TiCl4); and mixed halides and alkoxides such as triisopropoxytitanium chloride (TiCl(OCH(CH3)2)3), chlorotributoxytitanium (TiCl(OCH2CH2CH2CH3)3), or dichlorodiethoxide titanium (TiCl2(OCH2CH3)2) or other organometallic compounds.
[0040] The precursor of the zirconium oxide nanocrystals is generally selected from one or more of the following: alkoxides, such as zirconium methoxide (Zr(OCH3)4), zirconium ethoxide (Zr(OCH2CH3)4), zirconium n-propoxide (Zr(OCH2CH2CH3)4), zirconium isopropoxide (Zr(OCH(CH3)2)4), zirconium n-butoxide (Zr(OCH2CH2CH2CH3)4); acetylacetonates, such as zirconium oxyacetylacetonate (ZrO(CH3COCH4)4); COCH3)2); halides, such as zirconium chloride (ZrCl4); and mixed halides and alkoxides, such as triisopropoxytitanium zirconium chloride (ZrCl(OCH(CH3)2)3), chlorotributoxyzirconium (ZrCl(OCH2CH2CH2CH3)3), or diethyl zirconium dichloride (ZrCl2(OCH2CH3)2) or other organometallic compounds.
[0041] Examples of solvents for synthesizing the disclosed nanocrystals generally include one or more of the following: alcohols such as benzyl alcohol, phenol, oleyl alcohol, butanol, propanol, isopropanol, ethanol, butoxyethanol, butoxypropanol, methanol, 2-(isopentyloxy)ethanol, 2-propoxy-propanol (PnP), 2-(hexyloxy)ethanol; ethers and cyclic ethers such as tetrahydrofuran, dimethyl ether, ethyl ether, dibutyl ether, propylene glycol monomethyl ether (PGME), diethylene glycol butyl ether, dipropylene glycol methyl ether (DPGME), diethylene glycol monomethyl ether (DPG ... Methyl ether and diethylene glycol monoethyl ether; glycols such as diethylene glycol, dipropylene glycol; ketones and cyclic ketones such as acetone; esters such as propylene glycol methyl ether acetate (PGMEA), ethyl lactate (EL), methyl acetate, ethyl acetate, butyl acetate, ethylene glycol monobutyl ether acetate, diethylene glycol monobutyl ether acetate, diethylene glycol monoethyl ether acetate, butoxyethyl acetate, ethyl acetate, 2-(2-butoxyethoxy)ethyl acetate; aromatic compounds such as benzene, toluene; and water and any combination or mixture thereof.
[0042] The titanium oxide or zirconium oxide of the present disclosure is typically coated with an outer shell comprising at least one metal oxide. The method for applying the outer oxide shell typically involves converting a precursor of the oxide shell to surround the zirconium oxide or titanium oxide nanocrystals. Examples of oxides used as shell materials include, but are not limited to, silicon dioxide, zirconium dioxide, hafnium dioxide, niobium oxide, aluminum oxide, tantalum oxide, barium titanium oxide, cerium oxide, or any combination thereof. The process comprises mixing or suspending the optionally separated and purified TiO2 or ZrO2 nanocrystals in a solvent and adding at least one precursor of the shell metal oxide to the solution. The solution is then reacted for a period of time to promote the reaction between the core metal oxide and the shell oxide precursor. Heat and / or pressure are optionally applied during the reaction. This produces core-shell structured nanocrystals. The core-shell structured nanocrystals are optionally separated and purified.
[0043] Examples of precursors of oxide shells on TiO2 or ZrO2 nanocrystals include, but are not limited to, metal alkoxides, metal oxyhalides, metal halides, metals or any combination thereof. The metal alkoxide is a metal alkoxide such as a metal alkoxide having the formula M(OR)4, a metal alkoxide having the formula M(OR) x G yor a combination thereof; wherein M can be Ce, Zr, Si, Hf, NB, Al, Ta, Ti, Ba, each R group can independently be an alkyl group (e.g., C1-C6 alkyl) or a substituted alkyl group, each occurrence of the G group is independently a halogen (e.g., Cl), wherein x is an integer from 0 to 4, and y is an integer from 0 to 4, provided that x + y is 4. Examples of precursors of the shell metal oxide include, but are not limited to, zirconium oxychloride, titanium oxychloride, hafnium oxychloride, sodium aluminate, aluminum isopropoxide, ethyl orthosilicate, methyl orthosilicate, cerium chloride, cerium carbonate, or any combination thereof.
[0044] Optionally, a base or acid is present to promote the conversion of the shell metal oxide precursor to an oxide shell on the TiO2 or ZrO2 nanocrystals. Examples of bases or acids disclosed herein include, but are not limited to, trimethylammonium hydroxide, triethylammonium hydroxide, nitric acid, ammonium hydroxide, triethylamine, polyethyleneimine, citric acid, hydrochloric acid, benzoic acid, acetic acid, or trifluoroacetic acid.
[0045] Examples of solvents for promoting the conversion of the shell metal oxide precursor to an oxide shell on the TiO 2 or ZrO 2 nanocrystals include, but are not limited to, water, PGMEA, PGME, ethanol, methanol, isopropanol, benzyl alcohol, or any combination thereof.
[0046] Examples of solvents used for purification include, but are not limited to, water, THF, acetone, heptane, toluene, PGMEA, PGME, ethanol, methanol, isopropanol, or any combination thereof.
[0047] Optionally, a base or acid is present to facilitate neutralization of excess acid or base present during purification. Examples of bases or acids of the present disclosure include, but are not limited to, trimethylammonium hydroxide, triethylammonium hydroxide, nitric acid, ammonium hydroxide, triethylamine, polyethyleneimine, citric acid, hydrochloric acid, benzoic acid, acetic acid, or trifluoroacetic acid.
[0048] The production of sub-nanometer sized nanocrystals often results in agglomeration, which causes scattering and loss of transparency in the resulting nanocomposite. The key to producing well-dispersed nanocomposites is to use nanocrystals that have not aggregated before starting to mix with the matrix or medium. One way to achieve non-aggregating nanocrystals is to control the surface chemistry of the nanocrystals by introducing ligand ions or molecules called capping agents. These capping agents are added to the surface of the nanocrystals to create a new effective surface of the nanocrystal. The effective surface is the surface of the shell that is created by complete or partial surface coverage with the capping agent. The chemistry of the effective surface can be specifically tailored to create a chemical environment that is different from the actual or initial surface of the nanocrystal, which promotes dispersion while preventing or reducing aggregation.
[0049] In some embodiments, the surface of the core-shell structured titanium oxide or zirconium oxide nanocrystals of the present disclosure is capped with at least one capping agent. The capping process includes suspending the core-shell structured nanocrystals that have been optionally separated and purified in a capping solvent and adding the capping agent to the solution, which is called a reaction mixture. The reaction mixture is allowed to react for a period of time. Heat and / or pressure are optionally applied during the reaction. Optionally, a base or acid is added to the solution to promote the reaction. Optionally, a second capping agent is added to the reaction mixture and allowed to react for a period of time. Heat and / or pressure are optionally applied during the reaction. The resulting capped product is optionally separated and purified to produce at least partially capped core-shell structured nanocrystals. Optionally, the separated and purified at least partially capped core-shell structured nanocrystals are dried and then dispersed in a solvent.
[0050] In one embodiment, the at least partially end-capped core-shell nanocrystals of the present disclosure can be further treated with an inorganic passivating agent. The treatment process includes suspending the isolated and purified synthesized core-shell nanocrystals in an end-capping solvent and adding an end-capping agent to the solution. Heat and / or pressure are optionally applied during the reaction, and the solution is allowed to react for a period of time. A base or acid is optionally added to the solution to promote the reaction. After the set reaction time period, at least one inorganic passivating agent is added to the solution. Heat and / or pressure are optionally applied during the reaction. The resulting product is optionally separated and purified to produce inorganically treated at least partially end-capped synthesized core-shell nanocrystals. Optionally, the end-capped inorganically treated material is separated, purified, dried, and then dispersed in a solvent.
[0051] In another embodiment, the surface of the core-shell titanium oxide or zirconium oxide nanocrystals of the present disclosure is treated with an inorganic passivating agent before being capped with at least one capping agent. The treatment process generally includes suspending the core-shell nanocrystals, which have been optionally separated and purified, in a solvent and adding at least one inorganic passivating agent to the suspension. The suspension is mixed for a period of time. Thereafter, the nanocrystals are separated, purified, and resuspended in a capping solvent. At least one capping agent is added to the suspension and allowed to react for a period of time. Heat and / or pressure are optionally applied during the reaction. Optionally, a base or acid is added to the solution to promote the reaction. Optionally, a second capping agent is added to the reaction mixture and allowed to react for a period of time. Heat and / or pressure are optionally applied during the reaction. The resulting capped product is optionally separated and purified to produce inorganically treated at least partially capped core-shell nanocrystals. Optionally, the inorganically treated, separated and purified at least partially capped core-shell nanocrystals are dried and then dispersed in a solvent.
[0052] Examples of suitable capping agents include, but are not limited to, silanes, alcohols, compounds containing phosphoric acid groups, or compounds containing carboxylic acid groups. Examples of silanes of the present disclosure include, but are not limited to, methyltrimethoxysilane, ethyltrimethoxysilane, n-propyltrimethoxysilane, n-propyltriethoxysilane, n-octyltrimethoxysilane, n-octyltriethoxysilane, phenyltrimethoxysilane, dodecyltrimethoxysilane, m-, p-ethylphenethyltrimethoxysilane, 2-[methoxy(polyethyleneoxy)propyl]-trimethoxysilane, methoxy(trivinyloxy)propyltrimethoxysilane, 3-aminopropyltrimethoxysilane, 3-mercaptopropyltrimethoxysilane, 3-(methacryloyloxy)propyltrimethoxysilane, 3-(acryloyloxy)propyltrimethoxysilane, 3-isocyanatopropyltriethoxysilane, 3-isocyanatopropyltrimethoxysilane, and 3-glycidoxypropyltrimethoxysilane, vinyltrimethoxysilane, allyltrimethoxysilane, 1
[00145] In some embodiments, the present invention includes but is not limited to: -hexenyltrimethoxysilane, 1-octenyltrimethoxysilane, N-phenylaminopropyltrimethoxysilane, 3-(4-pyridylethyl)thiopropyltrimethoxysilane, N-(3-trimethoxysilylpropyl)pyrrole, 2-(3-trimethoxysilylpropylthio)thiophene, (3-trimethoxysilylpropyl)diethylenetriamine, phenyltrimethoxysilane, ((chloromethyl)phenylethyl)trimethoxysilane, 2-(diphenylphosphino)ethyltriethoxysilane, 4-phenylbutyltrimethoxysilane, 2-phenylethyltrimethoxysilane, 4-biphenyltriethoxysilane, N-[3-(trimethoxysilyl)propyl]allylamine, 3-mercaptopropyltrimethoxysilane, 8-glycidoxyoctyltrimethoxysilane, (3-glycidoxypropyl)trimethoxysilane, ethyl orthosilicate, or any combination thereof.
[0053] Examples of alcohols include, but are not limited to, heptanol, hexanol, octanol, benzyl alcohol, phenol, ethanol, propanol, butanol, oleyl alcohol, dodecanol, octadecyl alcohol, and triethylene glycol monomethyl ether, or any combination thereof.
[0054] Examples of phosphoric acid group-containing capping agents include, but are not limited to, (2-{2-[2-methoxy-ethoxy]-ethoxy}-ethyl)phosphonic acid, (6-{2-[2-(2-methoxy-ethoxy)-ethoxy]-ethoxy}-hexyl)phosphonic acid, 11-acryloyloxyundecylphosphonic acid, or any combination thereof.
[0055] Examples of compounds containing a carboxylic acid group include, but are not limited to, octanoic acid, acetic acid, propionic acid, 2-[2-(2-methoxyethoxy)ethoxy]acetic acid, oleic acid, benzoic acid, stearic acid, trifluoroacetic acid, biphenyl-4-carboxylic acid, 2-(2-methoxyethoxy)acetic acid, methacrylic acid, mono-2-(methacryloyloxy)ethylsuccinate, or any combination thereof.
[0056] Optionally, the silane capping agent can form a second outer metal oxide layer comprising silicon dioxide that encapsulates the titanium oxide or zirconium oxide nanocrystals comprising the first metal oxide shell. Examples of first metal oxide shell materials include, but are not limited to, silicon dioxide, zirconium dioxide, hafnium dioxide, niobium oxide, aluminum oxide, tantalum oxide, barium titanium oxide, cerium oxide, or any combination thereof.
[0057] Optionally, the silane capping agent can be mixed with an outer metal oxide shell material to form a shell comprising a mixture of silicon dioxide and other metal oxides encapsulating the titanium oxide or zirconium oxide nanocrystals. Examples of other metal oxide shell materials include, but are not limited to, silicon dioxide, zirconium dioxide, hafnium dioxide, niobium oxide, tantalum oxide, aluminum oxide, barium titanium oxide, cerium oxide, or any combination thereof.
[0058] Examples of blocked solvents include, but are not limited to, alcohols such as benzyl alcohol, phenol, oleyl alcohol, butanol, propanol, isopropanol, ethanol, butoxyethanol, butoxypropanol, methanol; ethers and cyclic ethers such as tetrahydrofuran, dimethyl ether, ethyl ether, dibutyl ether, propylene glycol monomethyl ether (PGME), diethylene glycol butyl ether, dipropylene glycol methyl ether (DPGME), diethylene glycol monomethyl ether, and diethylene glycol monoethyl ether; glycols such as diethylene glycol, dipropylene glycol; ketones and cyclic ketones such as acetone; esters such as propylene glycol methyl ether acetate (PGMEA), ethyl lactate (EL), methyl acetate, ethyl acetate, butyl acetate, ethylene glycol monobutyl ether acetate, diethylene glycol monobutyl ether acetate, diethylene glycol monoethyl ether acetate, butoxyethyl acetate, ethyl acetate, 2-(2-butoxyethoxy)ethyl acetate; aromatic compounds such as benzene, toluene; and water, and any combination or mixture thereof.
[0059] Examples of bases or acids of the present disclosure include, but are not limited to, trimethylammonium hydroxide, triethylammonium hydroxide, nitric acid, ammonium hydroxide, triethylamine, polyethyleneimine, citric acid, hydrochloric acid, benzoic acid, acetic acid, or trifluoroacetic acid.
[0060] Examples of solvents used for purification include, but are not limited to, water, THF, acetone, heptane, toluene, isopropyl alcohol, propylene glycol methyl ether acetate (PGMEA), propylene glycol monomethyl ether (PGME), ethanol, methanol, toluene, benzyl alcohol, or any combination thereof.
[0061] Examples of solvents for dispersion include, but are not limited to, THF, acetone, heptane, benzyl alcohol, phenol, oleyl alcohol, butanol, propanol, isopropanol, ethanol, butoxyethanol, butoxypropanol, methanol, tetrahydrofuran, dimethyl ether, ethyl ether, dibutyl ether, propylene glycol monomethyl ether (PGME), diethylene glycol butyl ether, dipropylene glycol methyl ether (DPGME), diethylene glycol monomethyl ether and diethylene glycol monoethyl ether, diethylene glycol, dipropylene glycol, acetone; esters such as propylene glycol methyl ether acetate (PGMEA), ethyl lactate (EL), methyl acetate, ethyl acetate, butyl acetate, ethylene glycol monobutyl ether acetate, diethylene glycol monobutyl ether acetate, diethylene glycol monoethyl ether acetate, butoxyethyl acetate, ethyl acetate, 2-(2-butoxyethoxy)ethyl acetate, benzene, toluene, and water, and any combination or mixture thereof.
[0062] Examples of inorganic passivating agents include, but are not limited to, sodium polyphosphate, lithium nitrate, sodium hypochlorite, sodium hypophosphite, sodium phosphite, lithium chloride, sodium nitrate, sodium chloride, sodium aluminum phosphate, sodium hexametaphosphate, or any combination thereof.
[0063] Optionally, an inorganic passivating agent can be bound to the outer metal oxide layer of the titanium oxide or zirconium oxide nanocrystals.
[0064] In another embodiment, the titanium oxide or zirconium oxide of the present disclosure is treated with an inorganic passivating agent before being coated with an outer metal oxide shell. The treatment process generally includes suspending the titanium oxide or zirconium oxide, which has been optionally separated and purified, in a solvent and adding at least one inorganic passivating agent to the suspension. The suspension is mixed for a period of time. Thereafter, the nanocrystals treated with the inorganic passivating agent are separated, purified, and resuspended in a solvent for coating. The method for coating the outer oxide shell generally includes converting a precursor of the oxide shell to surround the zirconium oxide or titanium oxide nanocrystals. The coating process includes mixing or suspending the TiO2 or ZrO2 nanocrystals, which have been optionally separated and purified, in a solvent and adding at least one precursor of the shell metal oxide to the solution. The solution is then reacted for a period of time to promote the reaction between the TiO2 or ZrO2 nanocrystals and the shell oxide precursor. Heat and / or pressure are optionally applied during the reaction. This produces synthesized inorganically treated core-shell nanocrystals. The synthesized inorganically treated core-shell nanocrystals are optionally separated and purified.
[0065] In some embodiments, the surface of the inorganically treated core-shell structured titanium oxide or zirconium oxide nanocrystals disclosed herein is capped with at least one capping agent. The capping process includes suspending the optionally separated and purified core-shell structured nanocrystals in a capping solvent and adding the capping agent to a solution called a reaction mixture. The reaction mixture is allowed to react for a period of time. Heat and / or pressure are optionally applied during the reaction. Optionally, a base or acid is added to the solution to promote the reaction. Optionally, a second capping agent is added to the reaction mixture and allowed to react for a period of time. Heat and / or pressure are optionally applied during the reaction. The resulting capped product is optionally separated and purified to produce at least partially capped core-shell structured nanocrystals. Optionally, the inorganically treated, separated and purified at least partially capped core-shell structured nanocrystals are dried and then dispersed in a solvent.
[0066] Examples of inorganic passivating agents include, but are not limited to, sodium polyphosphate, lithium nitrate, sodium hypochlorite, sodium hypophosphite, sodium phosphite, lithium chloride, sodium nitrate, sodium chloride, sodium aluminum phosphate, aluminum hypophosphite, sodium hexametaphosphate, calcium hypophosphite, or any combination thereof.
[0067] Examples of solvents for inorganic treatment include, but are not limited to, benzyl alcohol, phenol, oleyl alcohol, butanol, propanol, isopropanol, ethanol, butoxyethanol, butoxypropanol, methanol, and water, and any combination or mixture thereof.
[0068] Examples of oxides used as shell materials include, but are not limited to, silicon dioxide, zirconium dioxide, hafnium dioxide, niobium oxide, aluminum oxide, tantalum oxide, barium titanium oxide, cerium oxide, or any combination thereof.
[0069] Examples of precursors of the shell metal oxide include, but are not limited to, zirconium oxychloride, titanium oxychloride, and hafnium oxychloride, cerium chloride, cerium carbonate, or any combination thereof.
[0070] Examples of bases or acids present to promote the conversion of the shell metal oxide precursor to the oxide shell on the TiO2 or ZrO2 nanocrystals include, but are not limited to, trimethylammonium hydroxide, triethylammonium hydroxide, nitric acid, ammonium hydroxide, triethylamine, polyethyleneimine, citric acid, hydrochloric acid, benzoic acid, acetic acid, or trifluoroacetic acid. Examples of solvents used to promote the conversion of the shell metal oxide precursor to the oxide shell on the TiO2 or ZrO2 nanocrystals include, but are not limited to, water, PGMEA, PGME, ethanol, methanol, benzyl alcohol, or any combination thereof.
[0071] Examples of solvents used for purification include, but are not limited to, water, THF, acetone, heptane, toluene, PGMEA, PGME, ethanol, methanol, toluene, or any combination thereof.
[0072] Optionally, a base or acid is present to facilitate neutralization of excess acid or base present during purification. Examples of bases or acids disclosed herein include, but are not limited to, trimethylammonium hydroxide, triethylammonium hydroxide, nitric acid, ammonium hydroxide, triethylamine, polyethyleneimine, citric acid, hydrochloric acid, benzoic acid, acetic acid, or trifluoroacetic acid.
[0073] Examples of blocked solvents include, but are not limited to, alcohols such as benzyl alcohol, phenol, oleyl alcohol, butanol, propanol, isopropanol, ethanol, butoxyethanol, butoxypropanol, methanol; ethers and cyclic ethers such as tetrahydrofuran, dimethyl ether, ethyl ether, dibutyl ether, propylene glycol monomethyl ether (PGME), diethylene glycol butyl ether, dipropylene glycol methyl ether (DPGME), diethylene glycol monomethyl ether, and diethylene glycol monoethyl ether; glycols such as diethylene glycol, dipropylene glycol; ketones and cyclic ketones such as acetone; esters such as propylene glycol methyl ether acetate (PGMEA), ethyl lactate (EL), methyl acetate, ethyl acetate, butyl acetate, ethylene glycol monobutyl ether acetate, diethylene glycol monobutyl ether acetate, diethylene glycol monoethyl ether acetate, butoxyethyl acetate, ethyl acetate, 2-(2-butoxyethoxy)ethyl acetate; aromatic compounds such as benzene, toluene; and water, and any combination or mixture thereof.
[0074] Examples of capping agents include, but are not limited to, silanes, alcohols, compounds containing phosphoric acid groups, or compounds containing carboxylic acid groups. Examples of silanes of the present disclosure include, but are not limited to, methyltrimethoxysilane, ethyltrimethoxysilane, n-propyltrimethoxysilane, n-propyltriethoxysilane, n-octyltrimethoxysilane, n-octyltriethoxysilane, phenyltrimethoxysilane, dodecyltrimethoxysilane, m-, p-ethylphenethyltrimethoxysilane, 2-[methoxy(polyethyleneoxy)propyl]-trimethoxysilane, methoxy(trivinyloxy)propyltrimethoxysilane, 3-aminopropyltrimethoxysilane, 3-mercaptopropyltrimethoxysilane, 3-(methacryloyloxy)propyltrimethoxysilane, 3-(acryloyloxy)propyltrimethoxysilane, 3-isocyanatopropyltriethoxysilane, 3-isocyanatopropyltrimethoxysilane, and 3-glycidoxypropyltrimethoxysilane, vinyltrimethoxysilane, allyltrimethoxysilane, 1
[00145] In some embodiments, the present invention includes but is not limited to: -hexenyltrimethoxysilane, 1-octenyltrimethoxysilane, N-phenylaminopropyltrimethoxysilane, 3-(4-pyridylethyl)thiopropyltrimethoxysilane, N-(3-trimethoxysilylpropyl)pyrrole, 2-(3-trimethoxysilylpropylthio)thiophene, (3-trimethoxysilylpropyl)diethylenetriamine, phenyltrimethoxysilane, ((chloromethyl)phenylethyl)trimethoxysilane, 2-(diphenylphosphino)ethyltriethoxysilane, 4-phenylbutyltrimethoxysilane, 2-phenylethyltrimethoxysilane, 4-biphenyltriethoxysilane, N-[3-(trimethoxysilyl)propyl]allylamine, 3-mercaptopropyltrimethoxysilane, 8-glycidoxyoctyltrimethoxysilane, (3-glycidoxypropyl)trimethoxysilane, ethyl orthosilicate, or any combination thereof.
[0075] Examples of alcohols include, but are not limited to, heptanol, hexanol, octanol, benzyl alcohol, phenol, ethanol, propanol, butanol, oleyl alcohol, dodecanol, octadecyl alcohol, and triethylene glycol monomethyl ether, or any combination thereof.
[0076] Examples of phosphoric acid group-containing capping agents include, but are not limited to, (2-{2-[2-methoxy-ethoxy]-ethoxy}-ethyl)phosphonic acid, (6-{2-[2-(2-methoxy-ethoxy)-ethoxy]-ethoxy}-hexyl)phosphonic acid, 11-acryloyloxyundecylphosphonic acid, or any combination thereof.
[0077] Examples of compounds containing a carboxylic acid group include, but are not limited to, octanoic acid, acetic acid, propionic acid, 2-[2-(2-methoxyethoxy)ethoxy]acetic acid, oleic acid, benzoic acid, stearic acid, trifluoroacetic acid, biphenyl-4-carboxylic acid, 2-(2-methoxyethoxy)acetic acid, methacrylic acid, mono-2-(methacryloyloxy)ethylsuccinate, or any combination thereof.
[0078] Examples of the base or acid include, but are not limited to, trimethylammonium hydroxide, triethylammonium hydroxide, nitric acid, ammonium hydroxide, triethylamine, polyethyleneimine, citric acid, hydrochloric acid, benzoic acid, acetic acid, or trifluoroacetic acid.
[0079] Examples of solvents used for purification include, but are not limited to, water, THF, acetone, heptane, toluene, propylene glycol methyl ether acetate (PGMEA / PGA), propylene glycol monomethyl ether (PGME), ethanol, methanol, toluene, benzyl alcohol, or any combination thereof.
[0080] Examples of solvents for dispersion include, but are not limited to, THF, acetone, heptane, benzyl alcohol, phenol, oleyl alcohol, butanol, propanol, isopropanol, ethanol, butoxyethanol, butoxypropanol, methanol, tetrahydrofuran, dimethyl ether, ethyl ether, dibutyl ether, propylene glycol monomethyl ether (PGME), diethylene glycol butyl ether, dipropylene glycol methyl ether (DPGME), diethylene glycol monomethyl ether and diethylene glycol monoethyl ether, diethylene glycol, dipropylene glycol, acetone; esters such as propylene glycol methyl ether acetate (PGMEA), ethyl lactate (EL), methyl acetate, ethyl acetate (ETA), butyl acetate, ethylene glycol monobutyl ether acetate, diethylene glycol monobutyl ether acetate, diethylene glycol monoethyl ether acetate, butoxyethyl acetate, ethyl acetate, 2-(2-butoxyethoxy)ethyl acetate, benzene, toluene, and water, and any combination or mixture thereof.
[0081] Optionally, the silane capping agent can form a second outer metal oxide layer comprising silicon dioxide that encapsulates the titanium oxide or zirconium oxide nanocrystals comprising the first metal oxide shell. Examples of first metal oxide shell materials include, but are not limited to, silicon dioxide, zirconium dioxide, hafnium dioxide, niobium oxide, aluminum oxide, tantalum oxide, barium titanium oxide, cerium oxide, or any combination thereof.
[0082] Optionally, a silane capping agent can be mixed with an outer metal oxide shell material to form a shell comprising a mixture of silicon dioxide and other metal oxides encapsulating the titanium oxide or zirconium oxide nanocrystals. Examples of other metal oxide shell materials include, but are not limited to, silicon dioxide, zirconium dioxide, hafnium dioxide, niobium oxide, tantalum oxide, aluminum oxide, barium titanium oxide, or any combination thereof.
[0083] Optionally, an inorganic passivating agent can be bound to the outer metal oxide layer of the titanium oxide or zirconium oxide nanocrystals.
[0084] In another embodiment, the titanium oxide or zirconium oxide of the present disclosure without any shell is treated with an inorganic passivating agent and then capped. The treatment process generally includes suspending the titanium oxide or zirconium oxide that has been optionally separated and purified in a solvent and adding at least one inorganic passivating agent to the suspension. The suspension is mixed for a period of time. Thereafter, the inorganically treated nanocrystals are separated, purified and resuspended in a capping solvent. At least one capping agent is added to the suspension and allowed to react for a period of time. Heat and / or pressure are optionally applied during the reaction. Optionally, a base or acid is added to the solution to promote the reaction. Optionally, a second capping agent is added to the reaction mixture and allowed to react for a period of time. Heat and / or pressure are optionally applied during the reaction. The resulting capped product is optionally separated and purified to produce inorganically treated at least partially capped nanocrystals. Optionally, the inorganically treated, separated and purified at least partially capped nanocrystals are dried and then dispersed in a solvent.
[0085] Examples of inorganic passivating agents include, but are not limited to, sodium polyphosphate, lithium nitrate, sodium hypochlorite, sodium hypophosphite, sodium phosphite, lithium chloride, sodium nitrate, sodium chloride, sodium aluminum phosphate, aluminum hypophosphite, sodium hexametaphosphate, calcium hypophosphite, or any combination thereof.
[0086] Examples of solvents for inorganic treatment include, but are not limited to, benzyl alcohol, phenol, oleyl alcohol, butanol, propanol, isopropanol, ethanol, butoxyethanol, butoxypropanol, methanol, and water, and any combination or mixture thereof.
[0087] Examples of solvents used for purification include, but are not limited to, water, THF, acetone, heptane, toluene, PGMEA, PGME, ethanol, methanol, toluene, or any combination thereof.
[0088] Optionally, a base or acid is present to facilitate neutralization of excess acid or base present during purification. Examples of bases or acids of the present disclosure include, but are not limited to, trimethylammonium hydroxide, triethylammonium hydroxide, nitric acid, ammonium hydroxide, hydrochloric acid, benzoic acid, acetic acid, or trifluoroacetic acid.
[0089] Examples of blocked solvents include, but are not limited to, alcohols such as benzyl alcohol, phenol, oleyl alcohol, butanol, propanol, isopropanol, ethanol, butoxyethanol, butoxypropanol, methanol; ethers and cyclic ethers such as tetrahydrofuran, dimethyl ether, ethyl ether, dibutyl ether, propylene glycol monomethyl ether (PGME), diethylene glycol butyl ether, dipropylene glycol methyl ether (DPGME), diethylene glycol monomethyl ether, and diethylene glycol monoethyl ether; glycols such as diethylene glycol, dipropylene glycol; ketones and cyclic ketones such as acetone; esters such as propylene glycol methyl ether acetate (PGMEA), ethyl lactate (EL), methyl acetate, ethyl acetate (ETA), butyl acetate, ethylene glycol monobutyl ether acetate, diethylene glycol monobutyl ether acetate, diethylene glycol monoethyl ether acetate, butoxyethyl acetate, ethyl acetate, 2-(2-butoxyethoxy)ethyl acetate; aromatic compounds such as benzene, toluene; and water, and any combination or mixture thereof.
[0090] Examples of suitable capping agents include, but are not limited to, silanes, alcohols, compounds containing phosphoric acid groups, or compounds containing carboxylic acid groups. Examples of silanes of the present disclosure include, but are not limited to, methyltrimethoxysilane, ethyltrimethoxysilane, n-propyltrimethoxysilane, n-propyltriethoxysilane, n-octyltrimethoxysilane, n-octyltriethoxysilane, phenyltrimethoxysilane, dodecyltrimethoxysilane, m-, p-ethylphenethyltrimethoxysilane, 2-[methoxy(polyethyleneoxy)propyl]-trimethoxysilane, methoxy(trivinyloxy)propyltrimethoxysilane, 3-aminopropyltrimethoxysilane, 3-mercaptopropyltrimethoxysilane, 3-(methacryloyloxy)propyltrimethoxysilane, 3-(acryloyloxy)propyltrimethoxysilane, 3-isocyanatopropyltriethoxysilane, 3-isocyanatopropyltrimethoxysilane, and 3-glycidoxypropyltrimethoxysilane, vinyltrimethoxysilane, allyltrimethoxysilane, 1
[00145] In some embodiments, the present invention includes but is not limited to: -hexenyltrimethoxysilane, 1-octenyltrimethoxysilane, N-phenylaminopropyltrimethoxysilane, 3-(4-pyridylethyl)thiopropyltrimethoxysilane, N-(3-trimethoxysilylpropyl)pyrrole, 2-(3-trimethoxysilylpropylthio)thiophene, (3-trimethoxysilylpropyl)diethylenetriamine, phenyltrimethoxysilane, ((chloromethyl)phenylethyl)trimethoxysilane, 2-(diphenylphosphino)ethyltriethoxysilane, 4-phenylbutyltrimethoxysilane, 2-phenylethyltrimethoxysilane, 4-biphenyltriethoxysilane, N-[3-(trimethoxysilyl)propyl]allylamine, 3-mercaptopropyltrimethoxysilane, 8-glycidoxyoctyltrimethoxysilane, (3-glycidoxypropyl)trimethoxysilane, ethyl orthosilicate, or any combination thereof.
[0091] Examples of alcohols include, but are not limited to, heptanol, hexanol, octanol, benzyl alcohol, phenol, ethanol, propanol, butanol, oleyl alcohol, dodecanol, octadecyl alcohol, and triethylene glycol monomethyl ether, or any combination thereof.
[0092] Examples of phosphoric acid group-containing capping agents include, but are not limited to, (2-{2-[2-methoxy-ethoxy]-ethoxy}-ethyl)phosphonic acid, (6-{2-[2-(2-methoxy-ethoxy)-ethoxy]-ethoxy}-hexyl)phosphonic acid, 11-acryloyloxyundecylphosphonic acid, or any combination thereof.
[0093] Examples of compounds containing a carboxylic acid group include, but are not limited to, octanoic acid, acetic acid, propionic acid, 2-[2-(2-methoxyethoxy)ethoxy]acetic acid, oleic acid, benzoic acid, stearic acid, trifluoroacetic acid, biphenyl-4-carboxylic acid, 2-(2-methoxyethoxy)acetic acid, methacrylic acid, mono-2-(methacryloyloxy)ethylsuccinate, or any combination thereof.
[0094] Examples of the base or acid include, but are not limited to, trimethylammonium hydroxide, triethylammonium hydroxide, nitric acid, ammonium hydroxide, triethylamine, polyethyleneimine, citric acid, hydrochloric acid, benzoic acid, acetic acid, or trifluoroacetic acid.
[0095] Examples of solvents used for purification include, but are not limited to, water, THF, acetone, heptane, toluene, propylene glycol methyl ether acetate (PGMEA), propylene glycol monomethyl ether (PGME), ethanol, methanol, toluene, benzyl alcohol, or any combination thereof.
[0096] Examples of solvents for dispersion include, but are not limited to, THF, acetone, heptane, benzyl alcohol, phenol, oleyl alcohol, butanol, propanol, isopropanol, ethanol, butoxyethanol, butoxypropanol, methanol, tetrahydrofuran, dimethyl ether, ethyl ether, dibutyl ether, propylene glycol monomethyl ether (PGME), diethylene glycol butyl ether, dipropylene glycol methyl ether (DPGME), diethylene glycol monomethyl ether and diethylene glycol monoethyl ether, diethylene glycol, dipropylene glycol, acetone; esters such as propylene glycol methyl ether acetate (PGMEA), ethyl lactate (EL), methyl acetate, ethyl acetate (ETA), butyl acetate, ethylene glycol monobutyl ether acetate, diethylene glycol monobutyl ether acetate, diethylene glycol monoethyl ether acetate, butoxyethyl acetate, ethyl acetate, 2-(2-butoxyethoxy)ethyl acetate, benzene, toluene, and water, and any combination or mixture thereof.
[0097] Optionally, the silane capping agent may form an outer metal oxide layer comprising silica encapsulating the titania or zirconia nanocrystals.
[0098] Optionally, an inorganic passivating agent can be bound to the outer metal oxide layer of the titanium oxide or zirconium oxide nanocrystals.
[0099] Synthesis Technology of TiO2 and ZrO2 Nanocrystals
[0100] Exemplary methods for synthesizing, capping, and dispersing TiO2 and ZrO2 nanocrystals herein include those described in International Application Nos. PCT / US2011 / 057822 (published as WO 2012 / 058271) and PCT / US2019 / 062439 (published as WO 2020 / 106860), the contents of each of which are incorporated herein by reference in their entirety.
[0101] In one exemplary method, titanium oxide nanocrystals are prepared by a solvothermal process from a mixture of titanium (IV) butoxide, water, and benzyl alcohol in an inert atmosphere in a sealed autoclave. The ratio of titanium (IV) butoxide to water ranges from 1:0.1 to 1:10, such as 1:0.1-1:05, 1:0.5-1:1, 1:1-1:1.5, 1:1.5-1:2, 1:2-1:2.5, 1:2.5-1:3, 1:3-1:3.5, 1:3.5 to 1:4, 1:4-1:4.5, 1:4.5-1:5, 1:5-1:5.5, 1:5.5-1:6, 1:6-1:6.5, 1:6.5-1:7, 1:7-1:7.5, 1:7.5-1:8, 1:8-1:8.5, 1:8.5-1:9, 1:9-1:9.5 or 1:9.5-1:10. The ratio of titanium (IV) butoxide to benzyl alcohol ranges from 1:0.1 to 1:100, such as 1:0.1-1:5, 1:5-1:10, 1:10-1:15, 1:15-1:20, 1:20-1:25, 1:25-1:30, 1:30-1:35, 1:35-1:40, 1:40-1:45, 1:45-1:50, 1:50-1:55, 1:55-1:60, 1:60-1:65, 1:65-1:70, 1:70-1:75, 1:75-1:80, 1:80-1:85, 1:85-1:90, 1:90-1:95, or 1:95-1:100. The reaction mixture is heated to a temperature of 140-300°C, such as 140-150, 150-160, 160-170, 170-180, 180-190, 190-200, 200-210, 210-220, 220-230, 230-240, 240-250, 250-260, 260-270, 270-280, 280-290, or 290-300°C at a heating rate of 0.1-5°C / min, such as 0.1-0.5, 0.5-1, 1-1.5, 1.5-2, 2-2.5, 2.5-3, 3-3.5, 2.5-4, 4-4.5, or 4.5-5°C / min. In case the reaction mixture reaches desired temperature, the temperature is kept for 1-120 min, such as 1-10, 10-20, 20-30, 30-40, 40-50, 50-60, 60-70, 70-80, 80-90, 90-100 or 100-120 min. After the reactor is cooled to room temperature, collect the white milky solution of synthetic TiO nanocrystalline. The pressure of the reaction reaches 50 to 150 psi.
[0102] In one exemplary method, zirconium oxide nanocrystals are prepared by a solvothermal process from a mixture of zirconium (IV) butoxide, water, and benzyl alcohol in an inert atmosphere in a sealed autoclave. The ratio of zirconium (IV) butoxide to water ranges from 1:0.1 to 1:10, such as 1:0.1-1:05, 1:0.5-1:1, 1:1-1:1.5, 1:1.5-1:2, 1:2-1:2.5, 1:2.5-1:3, 1:3-1:3.5, 1:3.5-1:4, 1:4-1:4.5, 1:4.5-1:5, 1:5-1:5.5, 1:5.5-1:6, 1:6-1:6.5, 1:6.5-1:7, 1:7-1:7.5, 1:7.5-1:8, 1:8-1:8.5, 1:8.5-1:9, 1:9-1:9.5, or 1:9.5-1:10. The ratio of zirconium (IV) butoxide to benzyl alcohol ranges from 1:0.1 to 1:100, such as 1:0.1-1:5, 1:5-1:10, 1:10-1:15, 1:15-1:20, 1:20-1:25, 1:25-1:30, 1:30-1:35, 1:35-1:40, 1:40-1:45, 1:45-1:50, 1:50-1:55, 1:55-1:60, 1:60-1:65, 1:65-1:70, 1:70-1:75, 1:75-1:80, 1:80-1:85, 1:85-1:90, 1:90-1:95, or 1:95-1:100. The reaction mixture is heated to a temperature of 140-350°C, such as 140-150, 150-160, 160-170, 170-180, 180-190, 190-200, 200-210, 210-220, 220-230, 230-240, 240-250, 250-260, 260-270, 270-280, 280-290 or 290-300°C or 300-350°C at a heating rate of 0.1-5°C / min, such as 0.1-0.5, 0.5-1, 1-1.5, 1.5-2, 2-2.5, 2.5-3, 3-3.5, 2.5-4, 4-4.5 or 4.5-5°C / min. In case the mixture reaches the desired temperature, the temperature is maintained for 1-120 min, such as 1-10, 10-20, 20-30, 30-40, 40-50, 50-60, 60-70, 70-80, 80-90, 90-100 or 100-120 min. After the reactor is cooled to room temperature, the white milky solution of synthetic ZrO nanocrystals is collected. The pressure of the reaction reaches 100 to 500 psi.
[0103] Core-shell coating process
[0104] In one exemplary method, the slurry is stirred at 100-9000 rpm, such as 100-500, 500-1000, 100-1500, 1500-2000, 2000-2500, 2500-3000 rpm, 3000-3500, 3500-4000, 4000-4500, 4500-5000, 5000-5500, 5500-6000, 6000-6500, 6 The reaction mixture is centrifuged at 500-7000, 7000-7500, 7500-8000, 8000-8500, or 8500-9000 rpm for 0-60 min, such as 0-5, 5-10, 10-15, 15-20, 30-25, 25-30, 30-35, 35-40, 40-45, 45-50, 50-55, or 55-60 min to obtain TiO2 or ZrO2 nanocrystals from the reaction mixture. The supernatant is then decanted, and the purified TiO2 or ZrO2 nanocrystals form a wet cake at the bottom of the centrifuge bottle. The solvent is added to the wet cake, and the centrifugation step is repeated 1-10 times, such as 1-2, 2-3, 3-4, 4-5, 5-6, 6-7, 7-8, 8-9, or 9-10 times. The wet cake is dispersed in the solvent at 5-50% by weight of wet cake to solvent, such as 5, 10, 15, 20, 25, 30, 35, 40, 45 or 50% by weight of wet cake to solvent. At least one shell metal oxide precursor is added to the nanocrystal suspension at 0.1-500% by weight of the precursor relative to the wet cake, such as 0.1-5%, 5-10%, 10-15%, 15-20%, 20-25%, 25%-30%, 30%-35%, 35%-40%, 40%-45%, 45%-50%, 50%-55%, 55%-60%, 60%-70%, 70%-80%, 80%-90%, 90%-100%, 100%-110%, 110%-120%, 120%-130%, 130%-140%, 140%-150%, 150%-200%, 200%-300%, or 300%-500% by weight of the precursor relative to the wet cake. The mixture is then heated to 50-130° C., such as 50-60, 60-70, 70-80, 80-90, 90-100, 100-110, 110-120, or 120-130° C. for 1-400 h, such as 1-10, 10-20, 20-30, 30-40, 40-50, 50-60, 60-70, 70-80, 80-90, 90-100, 100-120, 120-150, 150-200, 200-250, 250-300, 300-350, or 340-400 h. Upon completion, the reaction mixture is cooled to room temperature.At least one other precursor of the second and subsequent shell metal oxides can be added simultaneously with the first shell metal oxide precursor or after heating the first precursor for a period of time.The heating and / or application of pressure can be repeated after the addition of the second shell material.
[0105] The titanium oxide or zirconium oxide nanocrystals having at least one shell oxide coating are purified by precipitating the nanocrystals from a reaction mixture using a solvent or solvent mixture to form an emulsion suspension at 100-9000 rpm, such as 100-500, 500-1000, 100-1500, 1500-2000, 2000-2500, 2500-3000 rpm, 3000-3500, 3500-4000, 4000-4500, 4500-5000, 5000-5500, 5500-6000, 6000-6000 The method comprises the steps of: centrifuging the titanium dioxide or zirconium oxide nanocrystals at 500, 6500-7000, 7000-7500, 7500-8000, 8000-8500 or 8500-9000 rpm for 0-60 min, such as 0-5, 5-10, 10-15, 15-20, 30-25, 25-30, 30-35, 35-40, 40-45, 45-50, 50-55 or 55-60 min. The supernatant is then decanted to form a wet cake of the titanium oxide or zirconium oxide with a purified core-shell structure at the bottom of the centrifuge bottle. The solvent is added to the wet cake, and the centrifugal step is repeated 1-10 times, such as 1-2, 2-3, 3-4, 4-5, 5-6, 6-7, 7-8, 8-9 or 9-10 times, to produce the titanium oxide or zirconium oxide nanocrystals with a purified core-shell structure. Optionally, a base or acid is present to facilitate neutralization of any excess acid or base present.
[0106] End-capping of core-shell TiO2 or ZrO2
[0107] In an exemplary method, purified core-shell TiO2 or ZrO2 nanocrystals are capped with at least one capping agent in a solvent. The purified core-shell titanium oxide nanocrystals obtained as a wet cake are dispersed in a solvent selected for capping in a round-bottom flask. The capping solvent is dispersed in an amount of 5-80% by weight relative to the wet cake, such as 5%, 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50%, 55%, 60%, 65%, 70%, 75% or 80% relative to the solvent. At least one capping agent is added to the wet cake at 0.1-100% by weight of the capping agent relative to the wet cake, such as 0.1-5%, 5-10%, 10-15%, 15-20%, 20-25%, 25%-30%, 30%-35%, 35%-40%, 40%-45%, 45%-50%, 50%-55%, 55%-60%, 60%-70%, 70%-80%, 80%-90%, 90%-100% by weight of the capping agent relative to the wet cake. The suspension is mixed at 25-60° C., such as 25° C., or 30° C., or 35° C., or 40° C., or 45° C., or 50° C., or 55° C., or 60° C. for 5 min to 3 h, such as 5 min, 10 min, 15 min, 20 min, 25 min, or 30 min, 45 min, 1 h, 2 h, or 3 h. The base is added to the suspension at 5-30% by weight of the wet cake relative to the solvent, such as 5%, 10%, 15%, 20%, 25%, or 30% by weight of the wet cake relative to the solvent. The suspension is heated at 50-130°C, such as 50-60, 60-70, 70-80, 80-90, 90-100, 100-110, 110-120 or 120-130°C, for 15-300 min, such as 15-30 min, 30-60 min, 60-90 min, 90-120 min, 120-150 min, 150-180 min, 180-210 min, 210-240 min, 240-270 min or 270-300 min.
[0108] In some embodiments, the second capping agent is added to the reaction mixture at 0.1-100% by weight of the capping agent relative to the wet cake, such as 0.1-5%, 5-10%, 10-15%, 15-20%, 20-25%, 25%-30%, 30%-35%, 35%-40%, 40%-45%, 45%-50%, 50%-55%, 55%-60%, 60%-70%, 70%-80%, 80%-90%, or 90%-100% by weight of the capping agent relative to the wet cake. The suspension is heated at 50-130°C, such as 50-60, 60-70, 70-80, 80-90, 90-100, 100-110, 110-120, 120-130°C for a further 15-300 min, such as 15-30 min, 30-60 min, 60-90 min, 90-120 min, 120-150 min, 150-180 min, 180-210 min, 210-240 min, 240-270 min or 270-300 min.
[0109] In some embodiments, after the first or second capping agent addition step, an inorganic passivating agent is added to the reaction mixture at 0.1-50% by weight of the inorganic passivating agent relative to the wet cake, such as 0.1-5%, 5-10%, 10-15%, 15-20%, 20-25%, 25%-30%, 30%-35%, 35%-40%, 40%-45%, or 45%-50% by weight of the inorganic passivating agent relative to the wet cake. The suspension is heated at 50-130°C, such as 50-60, 60-70, 70-80, 80-90, 90-100, 100-110, 110-120 or 120-130°C for a further 15-300 min, such as 15-30 min, 30-60 min, 60-90 min, 90-120 min, 120-150 min, 150-180 min, 180-210 min, 210-240 min, 240-270 min or 270-300 min.
[0110] The reaction mixture is then cooled to room temperature to provide the nanocrystals of at least part end-blocked core-shell structure. Through repeated precipitation in solvent or solvent combination to remove excessive end-capping agent and other by-products, the nanocrystals of end-blocked core-shell structure are purified. Through with the solvent of 0.1: 1-3: 1 and reaction mixture weight ratio, such as 0.1: 1-1: 1, 1: 1-1.25: 1, 1.25: 1-1.5: 1, 1.5: 1-1.75: 1, 1.75: 1-2: 1, 2: 1-2.25: 1, 2.25: 1-2.5: 1, 2.5: 1-2.75: 1 or 2.75: 1-3: 1 solvent and mixture weight ratio, add the solvent or solvent combination that is called anti-solvent, from reaction mixture, precipitate the nanocrystals of end-blocked core-shell structure. Anti-solvent is a solvent or solvent combination that is incompatible with nanocrystals and causes nanocrystals to be precipitated out from solution that is incompatible with nanocrystals. The precipitate is centrifuged at 100-9000 rpm, such as 100-500, 500-1000, 100-1500, 1500-2000, 2000-2500, 2500-3000 rpm, 3000-3500, 3500-4000, 4000-4500, 4500-5000, 5000-5500, 5500-6000, 6000 The supernatant is decanted and discarded. The solid collected from the centrifugation step is then dispersed in a solvent compatible with the end-capped nanocrystals. The dispersed solid is then precipitated with an antisolvent at an antisolvent to solvent weight ratio of 0.1:1-3:1, such as 0.1:1-1:1, 1:1-1.25:1, 1.25:1-1.5:1, 1.5:1-1.75:1, 1.75:1-2:1, 2:1-2.25:1, 2.25:1-2.5:1, 2.5:1-2.75:1, or 2.75:1-3:1.By rotating the machine at 100-9000 rpm, such as 100-500, 500-1000, 100-1500, 1500-2000, 2000-2500, 2500-3000 rpm, 3000-3500, 3500-4000, 4000-4500, 4500-5000, 5000-5500, 5500-6000, 6000-6500 The precipitate is collected by centrifugation at 0, 6500-7000, 7000-7500, 7500-8000, 8000-8500 or 8500-9000 rpm for 0-60 min, such as 0-5, 5-10, 10-15, 15-20, 30-25, 25-30, 30-35, 35-40, 40-45, 45-50, 50-55, 55-60 min. The resulting supernatant is decanted and discarded. If necessary, the process is repeated. The solid is then placed in a vacuum oven to dry overnight.
[0111] The dried solids are redispersed in a 1:1 ratio of solid to solvent (such as PGMEA, PGME, ETA or ethanol) to produce a 50 wt% loaded dispersion. The resulting dispersion is filtered through a 0.45 micron absolute or nominal filter and then through a 0.2 micron absolute or nominal filter.
[0112] Inorganic treatment of core-shell TiO2 or ZrO2 followed by end-capping
[0113] In the present disclosure, terms such as inorganic treatment, inorganic passivation, alkali metal compound treatment, and inorganic salt are used interchangeably and refer to a process of treating the core metal oxide or core-shell metal oxide nanocrystals before or after capping with at least one compound selected from the group consisting of sodium polyphosphate, lithium nitrate, sodium hypochlorite, sodium hypophosphite, sodium phosphite, lithium chloride, sodium nitrate, sodium chloride, sodium aluminum phosphate, aluminum hypophosphite, sodium hexametaphosphate, calcium hypophosphite, or any hydrate thereof, or any combination thereof.
[0114] In an exemplary method, purified core-shell TiO2 or ZrO2 nanocrystals are treated with an inorganic passivating agent before end-capping. The purified core-shell nanocrystals obtained as a wet cake are dispersed in a solvent selected for inorganic treatment in a round-bottom flask. The wet cake is dispersed in the solvent at a ratio of 5-80% by weight relative to the solvent, such as 5%, 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50%, 60%, 70% or 80% relative to the solvent by weight to obtain a white slurry. At least one inorganic passivating agent is added to the slurry at 0.1-100% by weight of the inorganic passivating agent relative to the wet cake, such as 0.1-5%, 5-10%, 10-15%, 15-20%, 20-25%, 25%-30%, 30%-35%, 35%-40%, 40%-45%, 45%-50%, 50%-55%, 55%-60%, 60%-70%, 70%-80%, 80%-90% or 90%-100% by weight of the inorganic passivating agent relative to the wet cake. The slurry is mixed for 0.1-12 h, such as 0.1-1 h, 1-2 h, 2-3 h, 3-4 h, 4-5 h, 5-6 h, 6-7 h, 7-8 h, 8-9 h, 9-10 h, 10-11 h or 11-12 h at 25-60 ° C, such as 25 ° C, or 30 ° C, or 35 ° C, or 40 ° C, or 45 ° C, or 50 ° C, or 55 ° C or 60 ° C. The treated nanocrystals are collected from the slurry by centrifugation. The slurry is stirred at 100-9000 rpm, such as 100-500, 500-1000, 100-1500, 1500-2000, 2000-2500, 2500-3000 rpm, 3000-3500, 3500-4000, 4000-4500, 4500-5000, 5000-5500, 5500-6000, 6000 The supernatant is decanted and discarded. The solid collected by the centrifugation step is suspended in a solvent or solvent combination and centrifuged again. This process is repeated twice. The resulting solid is suspended in the solvent selected for end-capping in a round-bottom flask. The wet cake is dispersed in the capping solvent at 5-80 wt % of the wet cake relative to the solvent, for example, 5, 10, 15, 20, 25, 30, 35, 40, 45, 50, 60, 70 or 80 wt % of the wet cake relative to the solvent.The first capping agent is added to the nanocrystal suspension at 0.1-100% by weight of the capping agent relative to the wet cake, such as 0.1-5%, 5-10%, 10-15%, 15-20%, 20-25%, 25%-30%, 30%-35%, 35%-40%, 40%-45%, 45%-50%, 50%-55%, 55%-60%, 60%-70%, 70%-80%, 80%-90%, or 90%-100% by weight of the capping agent relative to the wet cake. The suspension is mixed at 25-60° C., such as 25° C., or 30° C., or 35° C., or 40° C., or 45° C., or 50° C., or 55° C., or 60° C. for 5 min to 3 h, such as 5 min, 10 min, 15 min, 20 min, 25 min, or 30 min, 45 min, 1 h, 2 h, or 3 h. The base is added to the suspension at 5-30% by weight of wet cake relative to solvent, such as 5%, 10%, 15%, 20%, 25% or 30% by weight of wet cake relative to solvent. The suspension is heated at 50-300°C, such as 50-60, 60-70, 70-80, 80-90, 90-100, 100-110, 110-120, 120-130°C, for 15-30 min, 30-60 min, 60-90 min, 90-120 min, 120-150 min, 150-180 min, 180-210 min, 210-240 min, 240-270 min or 270-300 min.
[0115] In some embodiments, the second capping agent is added to the reaction mixture at 0.1-100% by weight of the capping agent relative to the wet cake, such as 0.1-5%, 5-10%, 10-15%, 15-20%, 20-25%, 25%-30%, 30%-35%, 35%-40%, 40%-45%, 45%-50%, 50%-55%, 55%-60%, 60%-70%, 70%-80%, 80%-90%, or 90%-100% by weight of the capping agent relative to the wet cake. The suspension is heated at 50-130°C, such as 50-60, 60-70, 70-80, 80-90, 90-100, 100-110, 110-120, 120-130°C for a further 15-300 min, such as 15-30 min, 30-60 min, 60-90 min, 90-120 min, 120-150 min, 150-180 min, 180-210 min, 210-240 min, 240-270 min or 270-300 min.
[0116] In some embodiments, after the first or second capping agent addition step, an inorganic passivating agent is added to the reaction mixture at 0.1-50% by weight of the inorganic passivating agent relative to the wet cake, such as 0.1-5%, 5-10%, 10-15%, 15-20%, 20-25%, 25%-30%, 30%-35%, 35%-40%, 40%-45%, or 45%-50% by weight of the inorganic passivating agent relative to the wet cake. The suspension is heated at 50-130°C, such as 50-60, 60-70, 70-80, 80-90, 90-100, 100-110, 110-120 or 120-130°C for a further 15-300 min, such as 15-30 min, 30-60 min, 60-90 min, 90-120 min, 120-150 min, 150-180 min, 180-210 min, 210-240 min, 240-270 min or 270-300 min.
[0117] The reaction mixture is then cooled to room temperature to provide the nanocrystals of inorganically treated core-shell structure of at least part of the end-blocking. By repeatedly precipitating in a solvent or solvent composition to remove excessive end-capping agent and other by-products, the nanocrystals of inorganically treated core-shell structure of the end-blocking are purified. By adding a solvent or solvent composition that is called an anti-solvent to the solvent and mixture weight ratio of 0.1:1-3:1, such as 0.1:1-1:1, 1:1-1.25:1, 1.25:1-1.5:1, 1.5:1-1.75:1, 1.75:1-2:1, 2:1-2.25:1, 2.25:1-2.5:1, 2.5:1-2.75:1 or 2.75:1-3:1, the nanocrystals of inorganically treated core-shell structure of the end-blocking are precipitated from the reaction mixture. Anti-solvent is a solvent or solvent composition that is incompatible with the nanocrystals and causes the nanocrystals to be precipitated out from the solution that is a nanocrystal. The precipitate is centrifuged at 100-9000 rpm, such as 100-500, 500-1000, 100-1500, 1500-2000, 2000-2500, 2500-3000 rpm, 3000-3500, 3500-4000, 4000-4500, 4500-5000, 5000-5500, 5500-6000, 6000 The supernatant is decanted and discarded. The solid collected from the centrifugation step is then dispersed in a solvent compatible with the end-capped nanocrystals. The dispersed solid is then precipitated with an antisolvent at an antisolvent to solvent weight ratio of 0.1:1-3:1, such as 0.1:1-1:1, 1:1-1.25:1, 1.25:1-1.5:1, 1.5:1-1.75:1, 1.75:1-2:1, 2:1-2.25:1, 2.25:1-2.5:1, 2.5:1-2.75:1, or 2.75:1-3:1.By rotating the machine at 100-9000 rpm, such as 100-500, 500-1000, 100-1500, 1500-2000, 2000-2500, 2500-3000 rpm, 3000-3500, 3500-4000, 4000-4500, 4500-5000, 5000-5500, 5500-6000, 6000-6500 The precipitate is collected by centrifugation at 0, 6500-7000, 7000-7500, 7500-8000, 8000-8500 or 8500-9000 rpm for 0-60 min, such as 0-5, 5-10, 10-15, 15-20, 30-25, 25-30, 30-35, 35-40, 40-45, 45-50, 50-55, 55-60 min. The resulting supernatant is decanted and discarded. If necessary, the process is repeated. The solid is then placed in a vacuum oven to dry overnight.
[0118] The dried solids are redispersed in a 1:1 ratio of solid to solvent (such as PGMEA, PGME, ETA or ethanol) to produce a 50 wt% loaded dispersion. The resulting dispersion is filtered through a 0.45 micron absolute or nominal filter and then through a 0.2 micron absolute or nominal filter.
[0119] Inorganic treatment of nanocrystals without shell structure followed by core-shell process
[0120] In one exemplary method, purified TiO or ZrO nanocrystals (without other metal oxide shells) are treated with an inorganic passivating agent prior to coating with the metal oxide. The purified nanocrystals obtained as a wet cake are dispersed in a solvent selected for the inorganic treatment in a round-bottom flask. The wet cake is dispersed in the solvent at 5-80% by weight of the wet cake relative to the solvent, such as 5%, 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50%, 60%, 70% or 80% by weight of the wet cake relative to the solvent to obtain a white slurry. At least one inorganic passivating agent is added to the slurry at 0.1-100% by weight of the inorganic passivating agent relative to the wet cake, such as 0.1-5%, 5-10%, 10-15%, 15-20%, 20-25%, 25%-30%, 30%-35%, 35%-40%, 40%-45%, 45%-50%, 50%-55%, 55%-60%, 60%-70%, 70%-80%, 80%-90% or 90%-100% by weight of the inorganic passivating agent relative to the wet cake. The slurry is mixed for 0.1-12 h, such as 0.1-1 h, 1-2 h, 2-3 h, 3-4 h, 4-5 h, 5-6 h, 6-7 h, 7-8 h, 8-9 h, 9-10 h, 10-11 h or 11-12 h at 25-60 ° C, such as 25 ° C, or 30 ° C, or 35 ° C, or 40 ° C, or 45 ° C, or 50 ° C, or 55 ° C or 60 ° C. The treated nanocrystals are collected from the slurry by centrifugation. The slurry is stirred at 100-9000 rpm, such as 100-500, 500-1000, 100-1500, 1500-2000, 2000-2500, 2500-3000 rpm, 3000-3500, 3500-4000, 4000-4500, 4500-5000, 5000-5500, 5500-6000, 6000 The supernatant is decanted and discarded. The solid collected by the centrifugation step is suspended in a solvent or solvent combination and centrifuged again. This process is repeated twice. The resulting solid or wet cake is suspended in a solvent selected for the oxide shell formation process.
[0121] For the coating process, the wet cake is dispersed in the solvent at 5-50% by weight of wet cake to solvent, such as 5%, 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45% or 50% by weight of wet cake to solvent. The at least one shell metal oxide precursor is added to the nanocrystal suspension at 0.1-500% by weight of the precursor relative to the wet cake, such as 0.1-5%, 5-10%, 10-15%, 15-20%, 20-25%, 25%-30%, 30%-35%, 35%-40%, 40%-45%, 45%-50%, 50%-55%, 55%-60%, 60%-70%, 70%-80%, 80%-90%, 90%-100%, 100%-110%, 110%-120%, 120%-130%, 130%-140%, 140%-150%, 150%-200%, 200%-300%, or 300%-500% by weight of the precursor relative to the wet cake. The mixture is then heated to 50-130° C., such as 50-60, 60-70, 70-80, 80-90, 90-100, 100-110, 110-120, 120-130° C., for 1-400 h, such as 1-10, 10-20, 20-30, 30-40, 40-50, 50-60, 60-70, 70-80, 80-90, 90-100, 100-120, 120-150, 150-200, 200-250, 250-300, 300-350, or 340-400 h. Upon completion, the reaction mixture is cooled to room temperature.
[0122] The inorganically treated nanocrystals having at least one oxide shell are purified by precipitating the nanocrystals from the reaction mixture using a solvent or solvent mixture to form an emulsion suspension at 100-9000 rpm, such as 100-500, 500-1000, 100-1500, 1500-2000, 2000-2500, 2500-3000 rpm, 3000-3500, 3500-4000, 4000-4500, 4500-5000, 5000-5500, 5500-6000, 6000-6500, 6500-7000, 7000-75 ... The nanocrystal of inorganic treatment is prepared by centrifuging at least one of the following precipitates: 1) a nanocrystal of inorganic treatment and 2) a nanocrystal of inorganic treatment having an inorganic core-shell structure and a nanocrystal of inorganic treatment having an inorganic core-shell structure. The nanocrystal of inorganic treatment is prepared by centrifuging at least one of the following precipitates: 1) a nanocrystal of inorganic treatment and 2) a nanocrystal of inorganic treatment having an inorganic core-shell structure and a nanocrystal of inorganic treatment having an inorganic core-shell structure. The nanocrystal of inorganic treatment is prepared by centrifuging at least one of the following precipitates: 1) a nanocrystal of inorganic treatment and 2) a nanocrystal of inorganic treatment having an inorganic core-shell structure and a nanocrystal of inorganic treatment having an inorganic core-shell structure. The nanocrystal of inorganic treatment is prepared by centrifuging at least one of the following precipitates: 1) a nanocrystal of inorganic treatment and 2) a nanocrystal of inorganic treatment having an inorganic core-shell structure and a nanocrystal of inorganic treatment having an inorganic core-shell structure.
[0123] Optionally, a base or acid is present to facilitate neutralization of any excess acid or base present.
[0124] In some embodiments, the nanocrystals from this process are at least partially capped with a capping agent according to the process described in "Capping of Core-Shell Synthesized TiO2 or ZrO2".
[0125] End-capping of inorganically treated nanocrystals (non-core-shell)
[0126] In an exemplary method, purified TiO2 or ZrO2 nanocrystals (without a metal oxide shell) are treated with an inorganic passivating agent prior to coating with a metal oxide. The purified nanocrystals obtained as a wet cake are dispersed in a solvent selected for the inorganic treatment in a round-bottom flask. The wet cake is dispersed in the solvent at a ratio of 5-80% by weight of the wet cake relative to the solvent, such as 5%, 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50%, 60%, 70% or 80% by weight of the wet cake relative to the solvent to obtain a white slurry. At least one inorganic passivating agent is added to the slurry at 0.1-100% by weight of the inorganic passivating agent relative to the wet cake, such as 0.1-5%, 5-10%, 10-15%, 15-20%, 20-25%, 25%-30%, 30%-35%, 35%-40%, 40%-45%, 45%-50%, 50%-55%, 55%-60%, 60%-70%, 70%-80%, 80%-90% or 90%-100% by weight of the inorganic passivating agent relative to the wet cake. The slurry is mixed for 0.1-12 h, such as 0.1-1 h, 1-2 h, 2-3 h, 3-4 h, 4-5 h, 5-6 h, 6-7 h, 7-8 h, 8-9 h, 9-10 h, 10-11 h, or 11-12 h at 25-35 ° C, such as 25 ° C or 30 ° C or 35 ° C. The treated nanocrystals are collected from the slurry by centrifugation. The slurry is stirred at 100-9000 rpm, such as 100-500, 500-1000, 100-1500, 1500-2000, 2000-2500, 2500-3000 rpm, 3000-3500, 3500-4000, 4000-4500, 4500-5000, 5000-5500, 5500-6000, 6000 The nanocrystals are centrifuged at 6500-6500, 6500-7000, 7000-7500, 7500-8000, 8000-8500, or 8500-9000 rpm for 0-60 min, such as 0-5, 5-10, 10-15, 15-20, 30-25, 25-30, 30-35, 35-40, 40-45, 45-50, 50-55, or 55-60 min. The resulting supernatant is decanted and discarded. The solid collected by the centrifugation step is suspended in a solvent or solvent combination and centrifuged again. This process is repeated twice. The resulting solid or wet cake is suspended in a solvent selected for end-capping in a round-bottom flask. The nanocrystals from this process are at least partially end-capped with an end-capping agent according to the process described in "End-capping of Core-Shell Structured TiO2 or ZrO2".
[0127] Core-shell structured TiO2 and ZrO2 nanocrystals
[0128] The crystallinity of the nanocrystals described in this disclosure was analyzed by X-ray powder diffraction. The XRD patterns of the titanium oxide and zirconium oxide nanocrystals including the metal oxide shells matched the original anatase and tetragonal phases, respectively, indicating that the shelling and capping processes had not altered the original phases.
[0129] The at least partially capped titanium dioxide nanocrystals of the present disclosure comprising a metal oxide shell and / or treated with an inorganic passivating agent have an average particle size of less than 30 nm as measured by TEM. Preferably, the particle size is 1-4 nm, or 4-6 nm, or 6-8 nm, or 8-10 nm, or 10-12 nm, or 12-14 nm, or 14-16 nm, or 16-18 nm, or 18-20 nm, or 20-25 nm, or 25-30 nm as measured by TEM.
[0130] The at least partially capped zirconium oxide nanocrystals of the present disclosure comprising a metal oxide shell and / or treated with an inorganic passivating agent have an average particle size of less than 30 nm as measured by TEM. Preferably, the particle size is 1-4 nm, or 4-6 nm, or 6-8 nm, or 8-10 nm, or 10-12 nm, or 12-14 nm, or 14-16 nm, or 16-18 nm, or 18-20 nm, or 20-25 nm, or 25-30 nm as measured by TEM.
[0131] The present disclosure provides at least partially capped titanium dioxide nanocrystals comprising a metal oxide shell and / or treated with an inorganic passivating agent, wherein the metal oxide shell has a thickness of less than 5 nm as measured by TEM. Preferably, the shell has a thickness of 0.05-0.1 nm, 0.1-0.2 nm, 0.2-0.3 nm, 0.3-0.4 nm, 0.4-0.5 nm, 0.5-0.6 nm, 0.6-0.7 nm, 0.7-0.8 nm, 0.8-0.9 nm, 0.9-1.0 nm, 1.0-1.2 nm, 1.2-1.4 nm, 1.4-1.6 nm, 1.6-1.8 nm, 1.8-2. 0nm, 2.0-2.2nm, 2.2-2.4nm, 2.4-2.6nm, 2.6-2.8nm, 2.8-3.0nm, 3.0-3.2nm, 3.2-3.4nm, 3.4- 3.6nm, 3.6-3.8nm, 3.8-4.0nm, 4.0-4.2nm, 4.2-4.4nm, 4.4nm-4.6nm, 4.6-4.8nm, 4.8-5.0nm.
[0132] The present disclosure provides at least partially capped zirconium oxide nanocrystals comprising a metal oxide shell and / or treated with an inorganic passivating agent, wherein the metal oxide shell has a thickness of less than 5 nm as measured by TEM. Preferably, the shell has a thickness of 0.05-0.1 nm, 0.1-0.2 nm, 0.2-0.3 nm, 0.3-0.4 nm, 0.4-0.5 nm, 0.5-0.6 nm, 0.6-0.7 nm, 0.7-0.8 nm, 0.8-0.9 nm, 0.9-1.0 nm, 1.0-1.2 nm, 1.2-1.4 nm, 1.4-1.6 nm, 1.6-1.8 nm, 1.8-2. 0nm, 2.0-2.2nm, 2.2-2.4nm, 2.4-2.6nm, 2.6-2.8nm, 2.8-3.0nm, 3.0-3.2nm, 3.2-3.4nm, 3.4- 3.6nm, 3.6-3.8nm, 3.8-4.0nm, 4.0-4.2nm, 4.2-4.4nm, 4.4nm-4.6nm, 4.6-4.8nm, 4.8-5.0nm.
[0133] In some embodiments, the at least partially capped titanium or zirconium oxide nanocrystals of the present disclosure comprising a metal oxide shell and / or treated with an inorganic passivating agent can be characterized in that the core metal oxide has a narrow particle size distribution characterized by: 1) a D90:D10 ratio of less than 5, preferably less than 3, or less than 2, such as from about 1.1 to about 2, from about 1.5 to about 2, from about 1.2 to about 1.8, from about 1.2 to about 3, or from about 1.5 to about 3; 2) a D90:D50 ratio of less than 3, preferably less than 2, or less than 1.5, such as from about 1.1 to about 2, from about 1.5 to about 2, from about 1.2 to about 1.5; and / or 3) a D50:D10 ratio of less than 3, preferably less than 2, or less than 1.5, such as from about 1.1 to about 2, from about 1.5 to about 2, from about 1.2 to about 1.5
[0134] In some embodiments, the at least partially capped titanium or zirconium oxide nanocrystals of the present disclosure comprising a metal oxide shell and / or treated with an inorganic passivating agent can be characterized in that the core-shell metal oxide has a narrow particle size distribution characterized by: 1) a D90:D10 ratio of less than 5, preferably, less than 3, or less than 2, such as from about 1.1 to about 2, from about 1.5 to about 2, from about 1.2 to about 1.8, from about 1.2 to about 3, or from about 1.5 to about 3; 2) a D90:D50 ratio of less than 3, preferably, less than 2, or less than 1.5, such as from about 1.1 to about 2, from about 1.5 to about 2, from about 1.2 to about 1.5; and / or 3) a D50:D10 ratio of less than 3, preferably, less than 2, or less than 1.5, such as from about 1.1 to about 2, from about 1.5 to about 2, from about 1.2 to about 1.5.
[0135] In some embodiments, the at least partially capped core-shell nanocrystals and / or nanocrystals treated with an inorganic passivating agent of the present disclosure can be characterized by an atomic ratio of shell metal oxide to core metal oxide of less than 0.1, less than 0.2, less than 0.3, less than 0.4, less than 0.5, less than 0.6, less than 0.7, less than 0.8, less than 0.9, less than 1, less than 2, or less than 3 as measured by SEM EDX.
[0136] In some embodiments, the at least partially capped titanium dioxide nanocrystals of the present disclosure comprising a ZrO2 shell and / or treated with an inorganic passivating agent can be characterized in that the atomic ratio of Zr / Ti of the core TiO2 nanocrystal having a shell of ZrO2 material is less than 0.1, less than 0.2, less than 0.3, less than 0.4, less than 0.5, less than 0.6, less than 0.7, less than 0.8, less than 0.9, less than 1, less than 2, or less than 3 as measured by SEM EDX.
[0137] In some embodiments, the at least partially capped titanium dioxide nanocrystals of the present disclosure comprising a metal oxide shell and / or treated with an inorganic passivating agent can be characterized in that the metal oxide shell comprises ZrO 2 and fully or partially encapsulates the TiO 2 core.
[0138] In some embodiments, the at least partially capped zirconium dioxide nanocrystals of the present disclosure comprising a metal oxide shell and / or treated with an inorganic passivating agent can be characterized in that the metal oxide shell comprises ZrO 2 and fully or partially encapsulates the ZrO 2 core.
[0139] In some embodiments, the at least partially capped titanium dioxide nanocrystals of the present disclosure comprising a metal oxide shell and / or treated with an inorganic passivating agent may be characterized in that the shell metal oxide comprises ZrO2 and encapsulates one or more core TiO2 nanocrystals to form a single particle.
[0140] In some embodiments, the at least partially capped zirconium dioxide nanocrystals of the present disclosure comprising a metal oxide shell and / or treated with an inorganic passivating agent may be characterized in that the shell metal oxide comprises ZrO2 and encapsulates one or more core ZrO2 nanocrystals to form a single particle.
[0141] In some embodiments, the at least partially capped titanium dioxide nanocrystals of the present disclosure comprising a metal oxide shell and / or treated with an inorganic passivating agent can be characterized in that the metal oxide shell comprises a ZrO2 material that can be crystalline or amorphous.
[0142] In some embodiments, the at least partially capped zirconium dioxide nanocrystals of the present disclosure comprising a metal oxide shell and / or treated with an inorganic passivating agent can be characterized in that the metal oxide shell comprises a ZrO2 material that can be crystalline or amorphous.
[0143] In some embodiments, the nanocrystals of the present disclosure have a core-shell structure comprising a core and an outer shell, wherein the core is a TiO nanocrystal and is at least partially encapsulated by an outer shell comprising a metal oxide and / or treated with an inorganic passivating agent, and additionally exhibit UV stability. When exposed to UV radiation at 320 nm or higher, or 340 nm or higher, or 365 nm or higher, or 390 nm or higher, or 405 nm or higher, or 450 nm or higher, or 500 nm or higher for 1-2 min, 2-5 min, 5-10 min, or 10-30 min, or 30-60 min, or 1-2 h, 2 h, 3 h, 4 h, 5 h, 6 h, 8 h, 9 h, 10 h, 15 h, 20 h, 30 h, 35 h, 365 nm or higher, or 390 nm or higher, or 405 nm or higher, or 450 nm or higher, or 500 nm or higher When the optical properties and refractive index of the TiO nanocrystals comprising the metal oxide shells vary less than those of the nanocrystals without the oxide shells for a period of 1-8 hours, 8-48 hours, 48-72 hours, 72-100 hours, 100-200 hours, 200-300 hours, 300-400 hours, 400-500 hours, 500-600 hours, 600-700 hours, 700-800 hours, 800-900 hours, 900-1000 hours or more, the optical properties and refractive index of the TiO nanocrystals comprising the metal oxide shells vary less than those of the nanocrystals without the oxide shells. When the b* of the film comprising the core-shell nanocrystals is measured using a haze meter before and after UV exposure, the nanocrystals exhibit a b* variation of less than 5%, less than 10%, less than 15%, less than 20%, less than 30%, less than 40% or less than 50%. For films less than 1 micron thick, or 1-2 microns thick, or 2-4 microns thick, or 4-6 microns thick, or 6-8 microns thick, or 8-10 microns thick, or 10-20 microns thick, or 20-30 microns thick, the nanocrystals exhibit a change in refractive index at 520 nm of less than 0.001, or less than 0.002, or less than 0.004, or less than 0.006, or less than 0.008, or less than 0.01, or ... 0.012, or less than 0.015, or less than 0.018, or less than 0.02, or less than 0.022, or less than 0.025, or less than 0.028, or less than 0.03, or less than 0.035, or less than 0.04, or less than 0.045, or less than 0.05, or less than 0.055, or less than 0.06, or less than 0.065, or less than 0.07, or less than 0.075, or less than 0.08, or less than 0.085, or less than 0.09, or less than 0.095, or less than 0.1.For films less than 1 micron thick, or 1-2 microns thick, or 2-4 microns thick, or 4-6 microns thick, or 6-8 microns thick, or 8-10 microns thick, or 10-20 microns thick, or 20-30 microns thick comprising these nanocrystals, the nanocrystals also exhibit a percent change in film thickness of less than 0.1, or less than 0.2, or less than 0.3, or less than 0.4, or less than 0.5, or less than 0.6, or less than 0.7, or less than 0.8, or less than 0.9, or less than 1.0, or less than 1.5, or less than 2.0, or less than 2.5, or less than 3.0, or less than 3.5, or less than 4.0, or less than 4.5, or less than 5, or less than 10, or less than 15, or less than 16, or less than 17, or less than 18, or less than 19, or less than 20, or less than 21, or less than 22, or less than 23, or less than 24, or less than 25, or less than 26, or less than 27, or less than 28, or less than 29, or less than 30, or less than 31, or less than 32, or less than 33, or less than 34, or less than 35, or less than 36, or less than 37, or less than 38, or less than 39, or less than 40, or less than 41, or less than 42, or less than 43, or less than 44, or less than 45, or less than 46, or less than 47, or less than 48, or less than 49, or less than 51, or less than 52, or less less than 20, or less than 25, or less than 50, and the % haze change is less than 0.001, or less than 0.002, or less than 0.004, or less than 0.006, or less than 0.008, or less than 0.01, or less than 0.012, or less than 0.015, or less than 0.018, or less than 0.02, or less than 0.022, or less than 0.025, or less than 0.028, or less than 0.03, or less than 0.035, or less than 0.04, or less than 0.045, or less than 0.05, or less than 0.055, or less than 0.06, or less than 0.065, or less than 0.07, or less than 0.075, or less than 0.08, or less than 0.085, or less than 0.09, or less than 0.095, or less than 0.1.
[0144] In some embodiments, the core-shell nanocrystals of the present disclosure comprising a metal oxide shell and / or treated with an inorganic passivating agent comprising TiO nanocrystals also exhibit thermal stability. When exposed to a temperature below 120°C, or 120°C-175°C, or 175°C-200°C, or 200°C-250°C, or 250°C-300°C, or above 300°C for more than 5 minutes, or more than 10 minutes, or more than 30 minutes, or more than 60 minutes, or more than 120 minutes under air, nitrogen, or vacuum, the core-shell nanocrystals experience less discoloration than nanocrystals without oxide shells or inorganic treatments. On a discoloration scale of 0-6, where "0" represents no discoloration and "6" represents the most discoloration (such as brown), the nanocrystals exhibit discoloration of 0-1, 1-2, or 2-3 compared to nanocrystals without shells / inorganic treatments that exhibit a discoloration of "6."
[0145] TiO2 nanocrystal dispersion
[0146] The present disclosure provides a composition comprising a dispersion or at least one monomer of end-capped titanium oxide or zirconium oxide nanocrystals and end-capped core-shell TiO and ZrO nanocrystals comprising a metal oxide shell and end-capped titanium dioxide or zirconium oxide nanocrystals and core-shell nanocrystals treated with an inorganic passivating agent in a solvent. The end-capped nanocrystals are present in the solvent in an amount less than 10% by weight of the total dispersion, or 10% to 20% by weight, or 20% to 30% by weight, or 30% to 40% by weight, or 40% to 50% by weight, or 50% to 60% by weight, or 60% to 70% by weight, or 70% to 80% by weight, or 80% to 90% by weight, or 90% to 95% by weight. Solvents include alcohols such as benzyl alcohol, phenol, oleyl alcohol, butanol, propanol, isopropanol, ethanol, butoxyethanol, butoxypropanol, methanol, 2-(isopentyloxy)ethanol, 2-propoxy-propanol (PnP), 2-(hexyloxy)ethanol; ethers and cyclic ethers such as tetrahydrofuran, dimethyl ether, ethyl ether, dibutyl ether, propylene glycol monomethyl ether (PGME), diethylene glycol butyl ether, dipropylene glycol methyl ether (DPGME), diethylene glycol monomethyl ether and diethylene glycol monoethyl ether; glycols such as: Diethylene glycol, dipropylene glycol; ketones and cyclic ketones, such as acetone; esters, such as propylene glycol methyl ether acetate (PGMEA), ethyl lactate (EL), methyl acetate, ethyl acetate (ETA), butyl acetate, ethylene glycol monobutyl ether acetate, diethylene glycol monobutyl ether acetate, diethylene glycol monoethyl ether acetate, butoxyethyl acetate, ethyl acetate, 2-(2-butoxyethoxy)ethyl acetate; aromatic compounds, such as benzene, toluene; and water, and any combination or mixture thereof.
[0147] A common technique for characterizing the size and size distribution of nanocrystals in dispersions is dynamic light scattering (DLS). DLS typically measures nanocrystals dispersed in a liquid that is transparent to the measurement wavelength. In this technique, a liquid sample with an appropriate concentration is kept in a plastic, glass, or fused silica sample cell, a laser beam is scattered from the liquid sample, and the time dependence of the scattered laser light as a result of the Brownian motion of the nanocrystals is measured, and the size and size distribution of the nanocrystals can be calculated. The result is typically a size distribution of nanocrystals with equivalent diameter as the x-axis and the y-axis representing the scattering intensity, the volume of scattered nanocrystals, or the number of scattered nanocrystals. The measured size typically includes the size of the nanocrystals, the size of the thin layer (solvent shell) of the capping agent and / or solvent groups and / or precursor groups along with the solvent, so the actual nanocrystal size is typically smaller than the size measured by DLS. In this disclosure, unless otherwise noted as "measured by DLS," all references to nanocrystal size and size distribution refer to the nanocrystal size as measured by TEM, and not the nanocrystal size plus capping agent and / or solvent groups and / or precursor groups or the nanocrystal plus capping agent and / or solvent groups and / or precursor groups plus solvent shell. D9999 is defined as the particle size at which 99.99% of the particles in the dispersion are measured to be smaller than the reported value (in nanometers) measured by volume. There are a variety of DLS spectrometers available, and each vendor typically develops its own proprietary methods and algorithms, and the results may not be interchangeable. The model specifically used to acquire the data in this disclosure was the Malvern Zetasizer Nano SDLS.
[0148] Typical DLS measurements of particle size and size distribution by intensity or volume of nanocrystal dispersions are taken when there are 5 wt% nanocrystals in the solvent.
[0149] The capped titanium oxide or zirconium oxide nanocrystals and any of the core-shell structured and / or inorganically treated TiO2 and ZrO2 nanocrystals described in the present disclosure have an average particle size, measured by intensity, of less than 100 nm when dispersed at 5 wt % in a solvent as measured by dynamic light scattering. Preferably, the particle size is 1-4 nm, or 4-6 nm, or 6-8 nm, or 8-10 nm, or 10-12 nm, or 12-14 nm, or 14-16 nm, or 16-18 nm, or 18-20 nm, or 20-25 nm, or 25-30 nm, or 30-35 nm, or 35-40 nm, or 40-45 nm, or 45-50 nm, or 50-55 nm, or 55-60 nm, or 60-65 nm, or 65-70 nm, or 75-80 nm, or 80-85 nm, or 85-90 nm, or 90-95 nm, or 95-100 nm, as measured by DLS.
[0150] The capped titanium oxide or zirconium oxide nanocrystals and any of the core-shell structured and / or inorganically treated TiO2 and ZrO2 nanocrystals described in the present disclosure have an average particle size by volume of less than 100 nm when dispersed at 5 wt % in a solvent as measured by dynamic light scattering. Preferably, the particle size is 1-4 nm, or 4-6 nm, or 6-8 nm, or 8-10 nm, or 10-12 nm, or 12-14 nm, or 14-16 nm, or 16-18 nm, or 18-20 nm, or 20-25 nm, 25-30, or 30-35 nm, or 35-40 nm, or 40-45 nm, or 45-50 nm, or 50-55 nm, or 55-60 nm, or 60-65 nm, or 65-70 nm, or 75-80 nm, or 80-85 nm, or 85-90 nm, or 90-95 nm, or 95-100 nm, as measured by DLS.
[0151] The capped titanium oxide, zirconium oxide nanocrystals, core-shell nanocrystals, inorganically treated nanocrystals, core-shell structured and inorganically treated nanocrystals described in the present disclosure have a D9999 measured by volume of <500 nm when dispersed in a solvent at 5 wt % as measured by dynamic light scattering. Preferably, the D9999 is <20, <30, <40, <50, <60, <70, <<80, <90, <100, <110, <120, <130, <140, <150, <160, <170, <180, <190, <200, <220, <150, <240, <260, <280, <300, <400 or <500 nm as measured by DLS.
[0152] In one embodiment, the disclosed at least partially capped core-shell nanocrystals comprising a core TiO2 or ZrO2 nanocrystal and a metal oxide shell comprising ZrO2 and / or treated with an inorganic passivating agent have a narrow particle size distribution characterized by: D9999 <20, <30, <40, <50, <60, <70, <80, <90, <100, <110, <120, <130, <140, <150, <160, <170, <180, <190, <200.
[0153] A common technique for characterizing the % solids, % inorganics, and % organics in a nanocrystal dispersion or nanocrystal formulation is thermogravimetric analysis (TGA). A nanocrystal formulation in the present disclosure is any dispersion comprising any of the capped nanocrystals described in the present disclosure, monomers, oligomers, polymers, and other additives. Optionally, the formulation will contain a solvent or a combination of solvents. In this technique, the nanocrystal dispersion or nanocrystal-polymer nanocomposite is held in a crucible and heated from room temperature to approximately 800° C. while the weight is monitored. The organic solvent, polymer, and capping agent will decompose at elevated temperatures, typically at varying temperatures, leaving only the inorganic nanocrystals. The relative weight percentages of the various components in the original sample can be obtained. TGA results typically produce a graph with temperature as the x-axis and relative weight percentages as the y-axis. A variety of TGA instruments are available, all based on similar principles, and when properly operated, the results are interchangeable. The model specifically used to acquire the data in the present disclosure is the TA Instrument TGA Q500.
[0154] The dispersions of the present disclosure were analyzed using a TA Instrument Q500 thermogravimetric analyzer (TGA) to determine the organic content, inorganic content, and solids content of the capped nanocrystal dispersions. The mass percentage relative to the initial mass at 200° C. (M200° C.) was considered the capped nanocrystals present in the dispersion, and the mass percentage relative to the initial mass at 700° C. (M700° C.) was considered the inorganic portion of the capped nanocrystals, i.e., the inorganic solids content. The organic content of the capped nanocrystals was defined as the difference between the mass percentages at 200° C. and 700° C. divided by the mass percentage at 200° C., i.e., % organic matter = (M200° C. - M700° C.) / M200° C.
[0155] The formulations of the present disclosure were analyzed using a TA Instrument Q500 thermogravimetric analyzer (TGA). TGA was run when the nanocrystal dispersion was in a solvent with a boiling point <200° C. to determine the organic content of the end-capped nanocrystals. The mass percentage relative to the initial mass at 200° C. was considered the end-capped nanocrystals, and the weight percentage relative to the initial mass at 700° C. was considered the inorganic portion of the end-capped nanocrystals, i.e., the inorganic solids content. The organic percentage (%Org) of the end-capped nanocrystals was defined as the difference between the mass percentages at 200° C. (M200° C.) and 700° C. (M700° C.) divided by the mass percentage at 200° C.:
[0156] %Org=(M200℃-M700℃) / M200℃x 100%
[0157] For nanocomposites or formulations, the percent solids (%S) is calculated from the inorganic content of the nanocomposite and the organic content of the capped nanocrystals measured in the solvent:
[0158] %S=M700℃ / (100%-%Org)x100%
[0159] The solids content of the dispersions of the present disclosure comprising capped titanium oxide, zirconium oxide nanocrystals, core-shell TiO2 and ZrO2 nanocrystals comprising metal oxide shells, and inorganically treated nanocrystals is typically 0-93%, such as 0-10%, or 10-20%, or 20-30%, or 30-40%, or 40-50%, or 50-60%, or 60-70%, or 70-80%, or 80-90%, or 90-93%, as measured by TGA.
[0160] The inorganic solids content of the dispersions of the present disclosure comprising capped titanium oxide, zirconium oxide nanocrystals, core-shell TiO2 and ZrO2 nanocrystals comprising metal oxide shells, and inorganically treated nanocrystals is typically 0-93%, such as 0-10%, or 10-20%, or 20-30%, or 30-40%, or 40-50%, or 50-60%, or 60-70%, or 70-80%, or 80-90%, or 90-93%, as measured by TGA.
[0161] The organic content of the dispersions of the present disclosure comprising capped titanium oxide, zirconium oxide nanocrystals, core-shell TiO2 and ZrO2 nanocrystals comprising metal oxide shells, and inorganically treated nanocrystals is typically 0-25%, such as 0-5%, or 5-10%, or 10-15%, or 15-20%, or 20-25%, or less than 5%, or less than 8% or less than 10%, less than 12%, or less than 14% or less than 16%, less than 18%, or less than 20%, or less than 20%, less than 25%, of the capped nanocrystals as measured by TGA.
[0162] The organic content of the capped titanium oxide, zirconium oxide nanocrystals, core-shell TiO2 and ZrO2 nanocrystals including metal oxide shells, and inorganically treated nanocrystals is typically 0-25% of the capped nanocrystals, such as 0-5%, or 5-10%, or 10-15%, or 15-20%, or 20-25%, or less than 5%, or less than 8% or less than 10%, less than 12%, or less than 14% or less than 16%, less than 18%, or less than 20% or less than 20%, less than 25%, as measured by TGA.
[0163] The titanium or zirconium oxide nanocrystals and core-shell TiO2 and ZrO2 nanocrystals of the present disclosure dispersed in a solvent, monomer, polymer, or as a formulation can be stable for at least 1 week, 2 weeks, 3 weeks, 4 weeks, 3 months, or at least 5 months, or at least 6 months, or at least 7 months, or at least 8 months, or at least 9 months, or at least 10 months, or at least 11 months, or at least 1 year, or at least 2 years, or at least 3 years when the dispersion is stored at a temperature in the range of 18-25°C without intentionally shaking or mixing the dispersion.
[0164] Preparation components and properties
[0165] The present disclosure provides a kind of solvent-containing and / or solvent-free, nano-imprintable, ink-jet and spin-coated, high transparency, high RI preparation, it comprises and is dispersed in monomer, oligomer, polymer or its mixture and comprises metal oxide shell layer and / or is handled with inorganic passivating agent at least partially end-capped titanium dioxide or zirconium oxide nanocrystal.Described preparation optionally comprises solvent, curing agent, tackifier, wetting agent, leveling agent, dispersant, viscosity modifier, organic dopant and antioxidant.These preparations make production have nanocomposite material and thin film coating of high refractive index and high optical transparency become possibility.
[0166] Acrylic monomers, oligomers and / or polymers of the disclosed formulations may include benzyl (meth)acrylate (BA and BMA), trimethylolpropane tri(meth)acrylate (TMPTA and TMPTMA), trimethylolpropane ethoxylate tri(meth)acrylate (EOTMPTA and EOTMPTMA), 1,6-hexanediol di(meth)acrylate (HDDA and HDDMA), di(ethylene glycol) di(meth)acrylate (DEGDA and DEGDMA), ethylene glycol diacrylate, 1,3-diglycerol Ester diacrylate, tripropylene glycol diacrylate, 1,6-hexanediol ethoxylate diacrylate, ethylene glycol phenyl ether (meth)acrylate (PEA and PEMA), 2-hydroxy-3-phenoxypropyl acrylate (HPPA), 2-hydroxy-3-phenoxypropyl methacrylate (HPPMA), 2-phenoxybenzyl methacrylate (PBA), biphenyl methacrylate (BPMA), isobornyl acrylate (IBA), 2-phenylphenol methacrylate (PPMA), isobutyl acrylate (IBA), 2-phenylethyl acrylate (2-PEA), 2-(phenylthio)ethyl acrylate (PTEA), tris(2-hydroxyethyl)isocyanurate triacrylate (THEICTA or M370), bisphenol A glycerate dimethacrylate, acrylic acid esters (OPPEOA), 9,9-bis[4-(2-acryloyloxyethoxy)phenyl]fluorene or bisfluorene diacrylate in OPPEOA (HR6042), bisphenol A ethoxylate diacrylate, bisphenol A propoxylate diacrylate, bisphenol F ethoxylate (2E O / phenol) diacrylate, bisphenol A glycerate diacrylate, bisphenol A ethoxylate dimethacrylate, ethoxy (4) bisphenol A diacrylate (SR-601), bisphenol A ethoxylate diacrylate (SR-349), tris(2-acryloyloxy)ethyl} isocyanurate, tricyclodecane dimethanol diacrylate, cresol novolac epoxy acrylate (CN112C60), tri(ethylene glycol) diacrylate, ethylene glycol diacrylate, poly(ethylene glycol) diacrylate, 1,3-diglycerate diacrylate and combinations thereof.
[0167] In some preferred embodiments, the monomers, oligomers and / or polymers may be selected from 2-phenylethyl acrylate (2-PEA), biphenyl methacrylate (BPMA), 2-phenoxybenzyl acrylate (PBA), trimethylolpropane tri(meth)acrylate (TMPTA and TMPTMA), tris(2-hydroxyethyl)isocyanurate triacrylate (THEICTA), 9,9-bis[4-(2-acryloyloxyethoxy)phenyl]fluorene or bisfluorene diacrylate in OPPEOA (HR6042), and combinations thereof.
[0168] The vinyl monomers, oligomers and / or polymers of the formulations of the present disclosure may include N-vinyl pyrrolidone (NVP), phenyl norbornene, styrene (STY), 4-methylstyrene, 4-vinylanisole, divinylbenzene, or combinations thereof.
[0169] The capped nanocrystals are present in the monomer in an amount less than 10 wt %, or 10 wt % to 20 wt %, or 20 wt % to 30 wt %, or 30 wt % to 40 wt %, or 40 wt % to 50 wt %, or 50 wt % to 60 wt %, or 60 wt % to 70 wt %, or 70 wt % to 80 wt %, or 80 wt % to 90 wt %, or 90 wt % to 95 wt % of the total weight of the monomer, oligomer, and polymer.
[0170] The formulations of the present disclosure optionally contain an organic dopant to increase the refractive index of the film or coating. Organic dopants, if present, include phenanthrene (PhA), 9-cyanophenanthrene, triphenylmethane, benzoquinoline, 9-vinylcarbazole, and combinations thereof.
[0171] The curing agent of the formulation of the present disclosure generally includes a photopolymerization initiator. Any photopolymerization initiator can be used, provided that it does not limit the optical and physical properties of the nanocomposite material, as long as it can generate reactive species, such as free radicals with light energy (UV). Examples of photopolymerization initiator curing agents include: amines such as P115, or benzophenone and its derivatives such as P39, benzophenone, SpeedCure BEM (Lambson USA Ltd, Rutherford, CT, USA) or an organic phosphine such as diphenyl (2,4,6-trimethylbenzoyl)-phosphine oxide (TPO), 819 or 184 (BASF USA, Florham Park, NJ, USA). The formulation comprises a single photopolymerization initiator or any combination thereof. Although the formulations described herein focus on the use of UV radiation for curing, thermal curing is entirely possible with an appropriate thermal initiator, such as 2,2-azobis(2-methylpropionitrile) (AIBN).
[0172] It is known to those skilled in the art that in certain cases a combination of more than one curing agent is advantageous.
[0173] The amount of curing agent of the formulations of the present disclosure is typically in an amount of less than 0.5% of the total weight of the monomers, oligomers and / or polymers, or 0.5%-1% of the total weight of the monomers, oligomers and / or polymers, or 1%-2% of the total weight of the monomers, oligomers and / or polymers, or 2%-3% of the total weight of the monomers, oligomers and / or polymers, or 3%-4% of the total weight of the monomers, oligomers and / or polymers, or 4%-5% of the total weight of the monomers, oligomers and / or polymers, or 5%-6% of the total weight of the monomers, oligomers and / or polymers, or 6%-7% of the total weight of the monomers, oligomers and / or polymers, or 7%-8% of the total weight of the monomers, oligomers and / or polymers, or 8%-15% of the total weight of the monomers, oligomers and / or polymers.
[0174] The adhesion promoter, if present, is selected from organometallic compounds such as organofunctional silanes, or from functionalized monomers and oligomers. Some suitable organofunctional silane adhesion promoters contain amino or methacryloxy groups. Exemplary silane adhesion promoters include, but are not limited to, 3-aminopropyltriethoxysilane, 3-[(methacryloyloxy)propyl]trimethoxysilane, ureidopropyltrimethoxysilane, and trimethoxy[3-(methylamino)propyl]silane, AP3000 (Dow Chemical). Functionalized monomer and oligomer adhesion promoters include, but are not limited to, CN820, CN146 (Sartomer Americas, Exton, PA, USA), SR9051, SR9053 (Sartomer Americas, Exton, PA, USA), and Ebecryl 171 (Allnex USA Inc., Wallingford, CT, USA).
[0175] The viscosity increasing agent of the formulations of the present disclosure may be present in an amount of less than 0.5% by weight of the monomers, oligomers and / or polymers, or 0.5-1% by weight of the monomers, oligomers and / or polymers, or 1-5% by weight of the monomers, oligomers and / or polymers, or 5-10% by weight of the monomers, oligomers and / or polymers, or 10-15% by weight of the monomers, oligomers and / or polymers, or 15-30% by weight of the monomers, oligomers and / or polymers.
[0176] In some embodiments, there is a surfactant that can be used as a wetting agent, leveling agent, defoamer and dispersant to reduce the surface tension of the formulation, thereby improving the flow properties of the formulation, thereby producing a more uniform dry coating surface. The surfactant is nonionic, anionic or a combination thereof. Representative examples of suitable wetting agents include, but are not limited to, silicone surfactants such as BYK-331, BYK-333, BYK-377, BYK-378 (BYK Chemie, GMBH); and fluorosurfactants such as Novec 4430, Novec 4432 and Novec 4434 (3M, St.Paul, MN, USA) and Capstone FS-3100 (The Chemours Company, Wilmington, DE, USA).
[0177] Examples of leveling agents (if present) are polyacrylate compounds such as BYK-352, BYK-353, BYK-356, and BYK-361N; aralkyl-modified polymethylalkylsiloxanes such as BYK-322, BYK-323, and BYK-350 (BYK Chemie, GMBH), and polyether-modified acryl-functional siloxanes such as BYK-UV3530. Examples of dispersants include, but are not limited to, polyalkylene glycols and their esters, polyoxyalkylenes, polyol ester oxyalkylene addition products, alcohol oxyalkylene addition products, sulfonic acid esters, sulfonic acid salts, carboxylic acid esters, carboxylic acid salts, alkylamide oxyalkylene addition products, alkylamines, and the like, and these may be used alone or as a mixture of two or more. Examples of commercial dispersants include, but are not limited to, DISPERBYK-101, DISPERBYK-130, DISPERBYK-140, DISPERBYK-160, DISPERBYK-161, DISPERBYK-162, DISPERBYK-163, DISPERBYK-164, DISPERBYK-165, DISPERBYK-166, DISPERBYK-170, DISPERBYK-171, DISPERBYK-182, DISPERBYK-2000, DISPERBYK-2001 (BYK Chemie, GMBH), Solsperse 32000, Solsperse 36000, Solsperse 28000, Solsperse 20000, Solsperse 41000 and Solsperse 45000 (Lubrizol, Wickliffe, OH, USA).
[0178] In some embodiments, to improve wetting properties, the amount of surfactant in the formulations of the present disclosure is less than 0.05% by weight of the total formulation, or 0.05-0.1% by weight of the total formulation, or 0.1-0.5% by weight of the total formulation, or 0.5-1% by weight of the total formulation, or 1-2% by weight of the total formulation, or 2-5% by weight of the total formulation. To aid dispersion, the amount of surfactant in the formulations of the present disclosure varies depending on the material being dispersed. The amount of dispersant is less than 3% by weight of the material being dispersed, or 3-5% by weight of the material being dispersed, or 5-10% by weight of the material being dispersed, or 10-20% by weight of the material being dispersed, or 20-40% by weight of the material being dispersed, or 40-60% by weight of the material being dispersed, or 60-80% by weight of the material being dispersed, or 80-100% by weight of the material being dispersed, or 100-150% by weight of the material being dispersed.
[0179] The antioxidants of the formulations of the present disclosure, if present, may include at least one primary antioxidant. The primary antioxidant is typically selected from sterically hindered phenols such as Irganox 1010, Irganox 1076, 1076, 2450, or phenolic phosphites, such as 1680, or a phosphine compound such as Irgaphos 168 (BASF USA, Florham Park, NJ, USA), or an aromatic secondary amine or hindered amine such as Song 6220 (Songwon Americas, Friendswood, TX, USA).
[0180] The formulations of the present disclosure optionally contain UV absorbers, such as TINUVIN 405 (T405), solid triazine-based UV absorbers for coatings, and Tinuvin 400. The amount of UV absorber in the formulations of the present disclosure is typically less than 0.5% by weight of the total formulation, or 0.5% to 1% by weight of the total formulation, or 1% to 2% by weight of the total formulation, or 2% to 3% by weight of the total formulation, or 3% to 4% by weight of the total formulation, or 4% to 5% by weight of the total formulation, or 5% to 6% by weight of the total formulation, or 6% to 7% by weight of the total formulation, or 7% to 8% by weight of the total formulation, or 8% to 10% by weight of the total formulation.
[0181] The formulations of the present disclosure optionally contain at least one secondary antioxidant. The secondary antioxidant is preferably selected from compounds comprising at least one unit formed by a sulfur atom attached to two carbon atoms. Representative examples of secondary antioxidants are di(tert-butyl)hydroxyphenylaminobisoctylthiotriazine and Irganox PS800 (BASF USA, Florham Park, NJ, USA).
[0182] The amount of antioxidant of the presently disclosed formulations is typically less than 0.5% by weight of the total formulation, or 0.5% to 1% by weight of the total formulation, or 1% to 2% by weight of the total formulation, or 2% to 3% by weight of the total formulation, or 3% to 4% by weight of the total formulation, or 4% to 5% by weight of the total formulation, or 5% to 6% by weight of the total formulation, or 6% to 7% by weight of the total formulation, or 7% to 8% by weight of the total formulation, or 8% to 10% by weight of the total formulation.
[0183] The formulations of the present disclosure may also contain plasticizers, tougheners, thickeners, diluents, dispersants or softeners, or other functional additives.
[0184] Optionally, the formulations of the present disclosure further comprise a solvent. The choice of solvent depends entirely on the at least partially capped titanium dioxide or zirconium oxide comprising a metal oxide shell and / or treated with an inorganic passivating agent, and the selected monomers, oligomers, and polymers of the formulation. Examples of solvents ranging from low boiling points to high boiling points include alcohols, glycols, methyl acetate, ethyl acetate, esters, ketones, glycol ethers, glycol esters such as propylene glycol monomethyl ether acetate (PGMEA), propylene glycol monomethyl ether (PGME), ethylene glycol monobutyl ether acetate, diethylene glycol monobutyl ether acetate, diethylene glycol butyl ether, diethylene glycol monoethyl ether acetate, dipropylene glycol methyl ether acetate, butoxyethanol, butoxypropanol, ethoxyethyl acetate, butoxyethyl acetate, 2-(isopentyloxy)ethanol, 2-(hexyloxy)ethanol, diethylene glycol, diethanol monomethyl ether, diethylene glycol monoethyl ether, triethylene glycol, triethylene glycol monomethyl ether, dipropylene glycol, dipropylene glycol monomethyl ether and dipropylene glycol monoethyl ether, ethyl acetate, THF, acetone, and any combination thereof.
[0185] The amount of solvent in the formulations of the present disclosure is less than 0.5% by weight of the total formulation, or 0.5% to 1% by weight of the total formulation, or 1% to 2% by weight of the total formulation, or 2% to 3% by weight of the total formulation, or 3% to 4% by weight of the total formulation, or 4% to 5% by weight of the total formulation, or 5% to 6% by weight of the total formulation, or 6% to 7% by weight of the total formulation, or 7% to 8% by weight of the total formulation, or 8% to 10% by weight of the total formulation. 0 wt %, or 10 wt %-20 wt % of the total formulation, or 20 wt %-30 wt % of the total formulation, or 30 wt %-40 wt % of the total formulation, or 40 wt %-50 wt % of the total formulation, or 50 wt %-60 wt % of the total formulation, or 60 wt %-70 wt % of the total formulation, or 70 wt %-80 wt % of the total formulation, or 80 wt %-90 wt % of the total formulation, or 90 wt %-95 wt % of the total formulation.
[0186] Preparation properties
[0187] The solids content of the formulations of the present disclosure as measured by TGA is typically 0-93%, such as 0-10%, or 10-20%, or 20-30%, or 30-40%, or 40-50%, or 50-60%, or 60-70%, or 70-80%, or 80-90%, or 90-93%.
[0188] The inorganic content of the formulations of the present disclosure is typically 0-93%, such as 0-10%, or 10-20%, or 20-30%, or 30-40%, or 40-50%, or 50-60%, or 60-70%, or 70-80%, or 80-90%, or 90-93%, as measured by TGA.
[0189] The capped nanocrystals of the disclosed formulations comprise less than 10% by weight of the total formulation, or 10% to 20% by weight of the total formulation, or 20% to 30% by weight of the total formulation, or 30% to 40% by weight of the total formulation, or 40% to 50% by weight of the total formulation, or 50% to 60% by weight of the total formulation, or 60% to 70% by weight of the total formulation, or 70% to 80% by weight of the total formulation, or 80% to 90% by weight of the total formulation, or 90% to 93% by weight of the total formulation.
[0190] The capped nanocrystals of the nanocomposite of the present disclosure comprise less than 10 wt % of the total nanocomposite, or 10 wt % to 20 wt % of the total nanocomposite, or 20 wt % to 30 wt % of the total nanocomposite, or 30 wt % to 40 wt % of the total nanocomposite, or 40 wt % to 50 wt % of the total nanocomposite, or 50 wt % to 60 wt % of the total nanocomposite, or 60 wt % to 70 wt % of the total nanocomposite, or 70 wt % to 80 wt % of the total nanocomposite, or 80 wt % to 90 wt % of the total nanocomposite, or 90 wt % to 93 wt % of the total nanocomposite.
[0191] One common technique for characterizing the optical transmittance and absorbance of nanocrystal formulations and / or nanocomposites is UV-Vis spectrophotometry (UV-Vis). The UV-Vis technique measures the light transmitted by a sample relative to incident light in the wavelength range of 200 nm to 900 nm.
[0192] The transmittance of a sample at a given wavelength is defined as: Where I is the transmitted light intensity and I0 is the incident light intensity, both at the same wavelength. The sample absorbance at a given wavelength is defined as:
[0193]
[0194] The absorbance of a sample at a given wavelength, or optical density (OD), is defined as:
[0195]
[0196] Reference samples are often used to remove the influence of other materials in the sample. For thin film samples, which often involve multiple reflections, modeling and algorithms can be applied to obtain the actual transmittance, absorptance, and absorbance.
[0197] In order to measure the nanocrystal preparation, usually sample is remained in plastics, glass or the fused silica sample cell with 10mm light path.Contrast comprises the reference thing measurement sample of the identical solvent, monomer, polymer that uses in the dispersion that is remained in identical or same type of sample cell, to remove the influence from cuvette and solvent, monomer, polymer.In order to measure nanocrystal polymer nanocomposite material, nanocomposite material is spin-cast on glass or fused silica wafer to form uniform film, can contrast comprise identical wafer and / or be spin-cast on the reference thing measurement sample of the identical polymer on the wafer with same thickness, to remove the influence from wafer and polymer.Can use modeling and algorithm to obtain accurate transmittance, absorptivity and the absorbance of nanocomposite material.
[0198] There are a variety of UV-Vis spectrophotometers available, all based on the same principles and, when operated properly, the results are interchangeable. The model specifically used to acquire the data in this disclosure was a Perkin Elmer Lambda 850.
[0199] The transmittance at 450 nm of the formulation of the present disclosure comprising any of the at least partially capped titanium oxide nanocrystals and / or inorganically treated nanocrystals comprising metal oxide shells as described herein is between 99% and 95%, or between 95% and 90%, or between 90% and 85%, or between 85% and 80%, or between 80% and 75%, or between 75% and 70%, when measured in a sample cell having a path length of 1 cm. %, 70%-65%, or 65%-60%, or 60%-55%, or 55%-50%, or 50%-45%, or 45%-40%, or 40%-35%, or 35%-30%, or 30%-25%, or 25%-20%, or 20%-15%, or 15%-10%, 10%-5%, or 5%-3%, or 3%-2%, or 2%-1%.
[0200] The transmittance at 500 nm of the formulation of the present disclosure comprising any of the at least partially capped titanium oxide nanocrystals and / or inorganically treated nanocrystals comprising metal oxide shells as described herein is between 99% and 95%, or between 95% and 90%, or between 90% and 85%, or between 85% and 80%, or between 80% and 75%, or between 75% and 70%, when measured in a sample cell having a path length of 1 cm. %, 70%-65%, or 65%-60%, or 60%-55%, or 55%-50%, or 50%-45%, or 45%-40%, or 40%-35%, or 35%-30%, or 30%-25%, or 25%-20%, or 20%-15%, or 15%-10%, 10%-5%, or 5%-3%, or 3%-2%, or 2%-1%.
[0201] The transmittance at 450 nm of the formulations of the present disclosure comprising any of the at least partially capped zirconium oxide nanocrystals and / or inorganically treated nanocrystals comprising metal oxide shells as described herein is between 99% and 95%, or between 95% and 90%, or between 90% and 85%, or between 85% and 80%, or between 80% and 75%, or between 75% and 70%, when measured in a sample cell having a path length of 1 cm. %, 70%-65%, or 65%-60%, or 60%-55%, or 55%-50%, or 50%-45%, or 45%-40%, or 40%-35%, or 35%-30%, or 30%-25%, or 25%-20%, or 20%-15%, or 15%-10%, 10%-5%, or 5%-3%, or 3%-2%, or 2%-1%.
[0202] The transmittance at 500 nm of the formulations of the present disclosure comprising any of the at least partially capped zirconium oxide nanocrystals and / or inorganically treated nanocrystals comprising metal oxide shells as described herein is between 99% and 95%, or between 95% and 90%, or between 90% and 85%, or between 85% and 80%, or between 80% and 75%, or between 75% and 70%, when measured in a sample cell having a path length of 1 cm. %, 70%-65%, or 65%-60%, or 60%-55%, or 55%-50%, or 50%-45%, or 45%-40%, or 40%-35%, or 35%-30%, or 30%-25%, or 25%-20%, or 20%-15%, or 15%-10%, 10%-5%, or 5%-3%, or 3%-2%, or 2%-1%.
[0203] The formulations disclosed herein have adjustable viscosities, and / or viscosities that can be controlled by one or more components of the formulation. Parameters that can control the viscosity of the formulation include, but are not limited to, the average length and molecular weight of the monomers, oligomers, and / or polymers; as well as the presence and concentration of solvents, the presence and concentration of thickeners (i.e., viscosity-modifying components), the particle size of the components present in the formulation, temperature, and combinations thereof.
[0204] The formulations described herein may also have a viscosity between about 1 cp and about 1000 cp, such as about 1 cP-2 cP, about 2 cP-5 cP, about 5 cP-10 cP, about 10 cP-15 cP, about 15 cP-20 cP, about 20 cP-25 cP, about 25 cP-30 cP, about 30 cP-40 cP, about 40 cP-50 cP, about 50 cP-60 cP, about 60 cP-75 cP, about 75 cP-100 cP, about 100 cP-20 ...0 cP-250 cP, about 250 cP-300 cP, about 300 cP-400 cP, about 400 cP-500 cP, about 500 cP-600 cP, about 600 cP-75 cP, about 750 cP-100 cP, about 100 cP-200 cP, about 200 cP- The viscosity can be adjusted within the range of 100cP-500cP, or about 500cp-1000cp, or about 1000cp-2000cp, about 2000cp-3000cp, or about 3000cp-4000cp, or about 4000cp-5000cp, or about 5000cp-6000cp, or about 6000cp-7000cp, or about 7000cp-8000cp, or about 8000cp-9000cp, or about 9000cp-10000cp, or >10000cp.
[0205] Preparation of the present disclosure is stable and surpasses 1 week or surpasses 2 weeks or surpasses 3 weeks or surpasses 6 weeks or surpasses 8 weeks or surpasses 3 months or surpasses 6 months or surpasses 12 months or surpasses 36 months, and wherein viscosity does not significantly increase.End-capped nanocrystal does not have visible precipitation, and the variation of preparation viscosity is less than 1% or less than 2% or less than 3% or less than 4% or less than 5% or less than 10% or less than 20% or less than 30% or less than 40%.In addition, the transmittance of preparation changes less than 0.5%, less than 1% or less than 2% or less than 3% or less than 4% or less than 5% or less than 10% or less than 20% or less than 30% or less than 40% (450nm).
[0206] Formulations for inkjet printing applications are highly resistant to wetting the inkjet nozzle faceplate and exhibit appropriate wettability to the desired substrate. A liquid wets a specific solid surface, and once the liquid reaches equilibrium, a contact angle is established. Very low contact angle values are typically less than 10°, indicating high wettability of the liquid to the surface. High wettability allows for uniform coatings. Contact angles greater than 45° indicate partial or no wetting. Such conditions are likely to result in irregular surfaces and potentially flexographic printing, and generally indicate high surface tension liquids on low surface energy surfaces.
[0207] For inkjet printing applications, the disclosed formulations are jet-stable for more than 1 hour, more than 8 hours, more than 1 day, or more than 1 week without a significant increase in viscosity. The formulations do not solidify by drying or curing to cause clogging of the printhead nozzles.
[0208] Method for preparing solvent-free or solvent-containing formulations
[0209] 1. A method for preparing a solvent-free formulation comprising a direct dispersion (direct dispersion of nanocrystals in a medium), wherein at least partially capped nanocrystals of the present disclosure are separated from a solvent and dried under vacuum until the solvent content is less than 5% to form dried nanocrystals; and the dried nanocrystals of at least partially capped oxide nanocrystals are mixed in at least one monomer, oligomer, polymer, or mixture thereof by soaking, stirring, rapid mixing, microfluidization, or other mixing methods.
[0210] Method 1 may further comprise filtering the formulation to remove agglomerates or other contaminants.
[0211] 2. Another method for preparing a solvent-free formulation comprises mixing a dry powder of at least partially capped oxide nanocrystals of the present disclosure in at least one solvent by soaking, stirring, rapid mixing, microfluidization or other mixing methods to provide a nanocrystal solvent dispersion; mixing the dispersion with at least one monomer, oligomer and / or polymer or mixture or monomers, oligomers and / or polymers to provide a solvent-containing formulation; and removing the solvent by evaporation or other solvent removal method such as rotary evaporation.
[0212] Method 2 may further comprise filtering the formulation, with or without solvent, to remove agglomerates or other contaminants.
[0213] The amount of solvent remaining in the final solvent-free formulation may be referred to as residual solvent. In a solvent-free formulation, the residual solvent is typically less than 10% of the total formulation, preferably less than 5%.
[0214] The solvent for Method 2 includes ethyl acetate (ETA), methyl ethyl ketone or other low boiling point solvents.
[0215] 3. A method for preparing a solvent-containing formulation comprising mixing a dry powder of at least partially capped oxide nanocrystals of the present disclosure in at least one solvent by soaking, stirring, rapid mixing, microfluidization or other mixing methods to provide a nanocrystal solvent dispersion; and mixing the dispersion with at least one monomer, oligomer and / or polymer or mixture or monomers, oligomers and / or polymers to provide a solvent-containing formulation.
[0216] Nanocomposites
[0217] The nanocomposite is a film, coating, layer, or crystal on a substrate or a freestanding structure. The present disclosure provides a nanocomposite comprising a mixture of at least partially capped titanium dioxide or zirconium oxide nanocrystals comprising a metal oxide shell and / or nanocrystals treated with an inorganic passivating agent and a polymerizable matrix, wherein the capped nanocrystals are present in the nanocomposite in an amount of 20-95% by weight of the nanocomposite.
[0218] The inorganic solids content of the nanocomposite coatings or films of the present disclosure was analyzed using a TA instrument Q500 thermogravimetric analyzer (TGA). The procedure was the same as previously described. The percentage relative to the initial mass at 700° C. was considered the inorganic portion of the formulation, i.e., the solids content.
[0219] The nanocomposite coatings of the present disclosure have an inorganic solids content of 0.1-10% as measured by TGA, or 10-20% as measured by TGA, or 20-30% as measured by TGA, or 30-40% as measured by TGA, or 40-50% as measured by TGA, or 50-60% as measured by TGA, or 60-70% as measured by TGA, or 70-80% as measured by TGA, or 80-90% as measured by TGA, or 90-93% as measured by TGA.
[0220] The nanocomposite film has a medium to high degree of cure, good adhesion to the expected substrate and good film uniformity. The disclosed end-capped nanocrystals keep dispersiveness or keep no agglomeration in polymer or monomer matrix. This type of physical characteristic of the disclosed material not only reduces light scattering, but also improves processability.
[0221] The transmittance of the film according to the present disclosure can be a normal transmittance measured with a Perkin-Elmer UV-Vis Lambda 850 spectrophotometer, wherein the film is coated on an optically transparent substrate, such as a fused silica or glass substrate, and a blank substrate of the same type and thickness is used as a reference. The ripples in the spectrum are the result of interference between the incident and reflected light, which generally indicates high film quality, i.e., high smoothness, high uniformity, and high transparency.
[0222] For films less than 20 microns thick, the Perkin-Elmer UV-Vis Lambda The nanocomposites of the present disclosure have a high light transmittance of 99.9%-99%, or 99%-98%, or 98%-97%, or 97%-96%, or 96%-95%, or 95%-90%, or 90%-85%, or 85%-80%, 80%-75%, or 75%-70%, or 70%-65%, or 65%-60%, or 60%-55%, or 55%-50%, or 50%-45%, or 45%-40%, or 40%-35%, or 35%-30%, or 30%-25%, or 25%-20%, or 20%-15%, or 15%-10%, as measured on a Spectrophotometer with an 850 spectrophotometer at 400 nm. The transmittance of films according to the present disclosure is the normal transmittance measured with a Perkin-Elmer UV-Vis Lambda 850 spectrophotometer, where the nanocomposite film is coated on an optically transparent substrate, such as a fused silica or glass substrate, and a blank substrate of the same type and thickness is used as a reference.
[0223] For films less than 20 microns thick, the Perkin-Elmer UV-Vis Lambda The nanocomposites of the present disclosure have a high light transmittance of 99.9%-99%, or 99%-98%, or 98%-97%, or 97%-96%, or 96%-95%, or 95%-90%, or 90%-85%, or 85%-80%, 80%-75%, or 75%-70%, or 70%-65%, or 65%-60%, or 60%-55%, or 55%-50%, or 50%-45%, or 45%-40%, or 40%-35%, or 35%-30%, or 30%-25%, or 25%-20%, or 20%-15%, or 15%-10%, as measured on a Spectrophotometer with an 850 spectrophotometer at 450 nm.
[0224] For films less than 20 microns thick, the Perkin-Elmer UV-Vis Lambda The nanocomposites of the present disclosure have a high light transmittance of 99.9%-99%, or 99%-98%, or 98%-97%, or 97%-96%, or 96%-95%, or 95%-90%, or 90%-85%, or 85%-80%, 80%-75%, or 75%-70%, or 70%-65%, or 65%-60%, or 60%-55%, or 55%-50%, or 50%-45%, or 45%-40%, or 40%-35%, or 35%-30%, or 30%-25%, or 25%-20%, or 20%-15%, or 15%-10%, as measured on a Spectrophotometer with an 850 spectrophotometer at 650 nm.
[0225] The nanocomposites of the present disclosure have high light transmittance of 99.9%-99%, or 99%-98%, or 98%-97%, or 97%-96%, or 96%-95%, or 95%-90%, or 90%-85%, or 85%-80%, 80%-75%, or 75%-70%, or 70%-65%, or 65%-60%, or 60%-55%, or 55%-50%, or 50%-45%, or 45%-40%, or 40%-35%, or 35%-30%, or 30%-25%, or 25%-20%, or 20%-15%, or 15%-10%, as measured by a Perkin-Elmer UV-Vis Lambda 850 spectrophotometer at 400 nm for films less than 1 micron thick.
[0226] For films less than 1 micron thick, the Perkin-Elmer UV-Vis Lambda The nanocomposites of the present disclosure have a high light transmittance of 99.9%-99%, or 99%-98%, or 98%-97%, or 97%-96%, or 96%-95%, or 95%-90%, or 90%-85%, or 85%-80%, 80%-75%, or 75%-70%, or 70%-65%, or 65%-60%, or 60%-55%, or 55%-50%, or 50%-45%, or 45%-40%, or 40%-35%, or 35%-30%, or 30%-25%, or 25%-20%, or 20%-15%, or 15%-10%, as measured on a Spectrophotometer with an 850 spectrophotometer at 450 nm.
[0227] For films less than 1 micron thick, the Perkin-Elmer UV-Vis Lambda The nanocomposites of the present disclosure have a high light transmittance of 99.9%-99%, or 99%-98%, or 98%-97%, or 97%-96%, or 96%-95%, or 95%-90%, or 90%-85%, or 85%-80%, 80%-75%, or 75%-70%, or 70%-65%, or 65%-60%, or 60%-55%, or 55%-50%, or 50%-45%, or 45%-40%, or 40%-35%, or 35%-30%, or 30%-25%, or 25%-20%, or 20%-15%, or 15%-10%, as measured on a Spectrophotometer with an 850 spectrophotometer at 650 nm.
[0228] When the nanocrystal loading is 0.1-10%, or 10-20%, or 20-30%, or 30-40%, or 40-50%, or 50-60%, or 60-70%, or 70-80%, or 80-90%, or 90-93%; for films less than 20 microns thick, the nanocrystals were prepared by a Perkin-Elmer UV-Vis Lambda The nanocomposites of the present disclosure have a high light transmittance of 99.9%-99%, or 99%-98%, or 98%-97%, or 97%-96%, or 96%-95%, or 95%-90%, or 90%-85%, or 85%-80%, 80%-75%, or 75%-70%, or 70%-65%, or 65%-60%, or 60%-55%, or 55%-50%, or 50%-45%, or 45%-40%, or 40%-35%, or 35%-30%, or 30%-25%, or 25%-20%, or 20%-15%, or 15%-10%, as measured on a Spectrophotometer with an 850 spectrophotometer at 450 nm.
[0229] When the nanocrystal loading is 0.1-10%, or 10-20%, or 20-30%, or 30-40%, or 40-50%, or 50-60%, or 60-70%, or 70-80%, or 80-90%, or 90-93%; for films less than 1 micron thick, the nanocrystals were prepared by a Perkin-Elmer UV-Vis Lambda The nanocomposites of the present disclosure have a high light transmittance of 99.9%-99%, or 99%-98%, or 98%-97%, or 97%-96%, or 96%-95%, or 95%-90%, or 90%-85%, or 85%-80%, 80%-75%, or 75%-70%, or 70%-65%, or 65%-60%, or 60%-55%, or 55%-50%, or 50%-45%, or 45%-40%, or 40%-35%, or 35%-30%, or 30%-25%, or 25%-20%, or 20%-15%, or 15%-10%, as measured on a Spectrophotometer with an 850 spectrophotometer at 450 nm.
[0230] When the nanocrystal loading is 0.1-10%, or 10-20%, or 20-30%, or 30-40%, or 40-50%, or 50-60%, or 60-70%, or 70-80%, or 80-90%, or 90-93%; for films less than 20 microns thick, the nanocrystals were prepared by a Perkin-Elmer UV-Vis Lambda The nanocomposites of the present disclosure have a high light transmittance of 99.9%-99%, or 99%-98%, or 98%-97%, or 97%-96%, or 96%-95%, or 95%-90%, or 90%-85%, or 85%-80%, 80%-75%, or 75%-70%, or 70%-65%, or 65%-60%, or 60%-55%, or 55%-50%, or 50%-45%, or 45%-40%, or 40%-35%, or 35%-30%, or 30%-25%, or 25%-20%, or 20%-15%, or 15%-10%, as measured on a Spectrophotometer with an 850 spectrophotometer at 520 nm.
[0231] When the nanocrystal loading is 0.1-10%, or 10-20%, or 20-30%, or 30-40%, or 40-50%, or 50-60%, or 60-70%, or 70-80%, or 80-90%, or 90-93%; for films less than 1 micron thick, the nanocrystals were prepared by a Perkin-Elmer UV-Vis Lambda The nanocomposites of the present disclosure have a high light transmittance of 99.9%-99%, or 99%-98%, or 98%-97%, or 97%-96%, or 96%-95%, or 95%-90%, or 90%-85%, or 85%-80%, 80%-75%, or 75%-70%, or 70%-65%, or 65%-60%, or 60%-55%, or 55%-50%, or 50%-45%, or 45%-40%, or 40%-35%, or 35%-30%, or 30%-25%, or 25%-20%, or 20%-15%, or 15%-10%, as measured on a Spectrophotometer with an 850 spectrophotometer at 520 nm.
[0232] A common technique for characterizing the color of nanocomposite materials is to use a colorimetric spectrophotometer to quantify the intensity of the red wavelength, green wavelength and blue wavelength transmitted through the nanocomposite material, wherein the light intensity of each wavelength is multiplied by the illuminant to obtain the X, Y, Z color values known as CIE color coordinates. The color coordinates reported in this disclosure are measured using the Vista haze meter of Hunterlab, which converts the CIE X, Y, Z color coordinates into a three-dimensional rectangular color space by a series of equations to provide L*, a*, b* color space values. In color space, "L*" is located on the "y-axis" and represents the brightness of the sample, "a*" is the "x-axis" and represents a red-green offset, and "b*" represents a blue-yellow offset and is located on the "z-axis". Typically, when nanocomposite materials degrade, the color changes from transparent or white to yellow, and this variation is measured according to the variation of "b*". In addition, the degradation of the film in all aspects of color space can be monitored by calculating ΔE* from ΔL*, a* and b*.
[0233] ΔE*=[(L* 最终 -L* 初始 ) 2 +(a* 最终 -a* 初始 ) 2 +(b* 最终 -b* 初始 ) 2 ] 1 / 2
[0234] In addition to color, Hunterlab's Vista Haze Meter is used to quantify the haze or clarity of optically clear nanocomposites.
[0235] Nanocomposite materials of the present disclosure have very low b* usually, and this shows that the painted minimum of film, and for the film less than 1 micron thickness, measured by Hunterlab Vista haze meter, b* is in the scope of 0.01-0.05 or 0.05-0.1 or 0.1-0.5 or 0.5-1.0 or 1.0-1.5 or 1.5-2.0.The haze value and the b* value of nanocomposite materials may be subject to the influence of RI mismatch and film thickness between substrate type, substrate haze, substrate and the film.For example, the nanocomposite materials made of same formulations demonstrate b* and the haze higher than when being coated on the glass substrate when being coated on the PET substrate.Unless otherwise stated, the b* value reported is for the film on the glass substrate.
[0236] The nanocomposites of the present disclosure generally have very low % haze, which indicates high clarity of the film, and for films less than 1 micron thick, the % haze is in the range of 0.0-0.02, or 0.02-0.04, or 0.04-0.06, or 0.06-0.08, or 0.08-0.1, or 0.1-0.14, or 0.14-0.18, or 0.18-0.20, or 0.20-0.25, or 0.25-0.30, or 0.30-0.35, or 0.35-0.40, or 0.40-0.45, or 0.45-0.50 as measured by a Hunterlab Vista haze meter.
[0237] The nanocomposites of the present disclosure generally have very low b*, which indicates minimal coloration of the film, and for films less than 20 microns thick, the b* is in the range of 0.01-0.05, or 0.05-0.1, or 0.1-0.5, or 0.5-1.0, or 1.0-1.5, or 1.5-2.0, 2.0-2.5, or 2.5-3.0 as measured by a Hunterlab Vista haze meter.
[0238] The nanocomposites of the present disclosure generally have very low b*, which indicates minimal coloration of the film, and are in the range of 0.01-0.05, or 0.05-0.1, or 0.1-0.5, or 0.5-1.0, or 1.0-1.5, or 1.5-2.0, 2.0-2.5, or 2.5-3.0, or 3.0-3.5, or 3.5-4.0, or 4.0-4.5, or 4.5-5.0 for films less than 20 microns thick coated on a PET substrate as measured by a Hunterlab Vista haze meter.
[0239] The nanocomposites of the present disclosure typically have very low % haze, which indicates high clarity of the film, and for films less than 20 microns thick, the % haze is in the range of 0.0-0.02, or 0.02-0.04, or 0.04-0.06, or 0.06-0.08, or 0.08-0.1, or 0.1-0.14, or 0.14-0.18, or 0.18-0.20, or 0.20-0.25, or 0.25-0.30, or 0.30-0.35, or 0.35-0.40, or 0.40-0.45, or 0.45-0.50 as measured by a Hunterlab Vista haze meter.
[0240] A common technique for characterizing the measured refractive index is to use a Metricon Model 2010 / M Prism Coupler. Using a Metricon Model 2010 / M Prism Coupler equipped with 448nm and 635nm laser beams, it is possible to calculate an estimated refractive index for the same material at a third wavelength. The calculation of the refractive index at 550nm is based on the 2-term version of the Cauchy equation:
[0241]
[0242] The A and B parameters depend on the RI values measured at specific wavelengths, which are chosen to be 448 and 635 nm. By expressing the parameters A and B in terms of RI (448 nm) and RI (635 nm), the following equation allows the calculation of RI (550 nm):
[0243]
[0244] The same equation can be used to calculate RI values for other wavelengths.
[0245] Another way to measure refractive index is by ellipsometer. With an ellipsometer, the refractive index can be measured as a function of wavelength. Some refractive index measurements were performed using a JA Woollam M2000 ellipsometer.
[0246] The nanocomposites of the present disclosure typically have a RI of 1.54-1.56, 1.56-1.58, 1.58-1.60, 1.60-1.62, or 1.62-1.64, 1.64-1.66, or 1.66-1.68, or 1.68-1.70, or 1.70-1.72, or 1.72-1.74, or 1.74-1.76, or 1.76-1.78, or 1 .78-1.80, or 1.80-1.82, or 1.82-1.84, or 1.84-1.86, or 1.86-1.88, or 1.88-1.90, or 1.90-1.92, or 1.92-1.94, or 1.94-1.96, or 1.96-1.98, or 1.98-2.00, or 2.00-2.02, or 2.02-2.04, or 2.04-2.06 , or 2.06-2.08, or 2.08-2.10, or 2.10-2.12, or 2.12-2.14, or 2.14-2.16, or 2.16-2.18, or 2.18-2.20, or 2.20-2.22, or 2.22-2.24, or 2.24-2.26, or 2.26-2.28, or 2.28-2.30, or 2.30-2.32, or 2.32-2 or 2.54-2.56, or 2.56-2.58, or 2.58-2.60.
[0247] The nanocomposites of the present disclosure typically have a RI of 1.54-1.56, 1.56-1.58, 1.58-1.60, 1.60-1.62, or 1.62-1.64, 1.64-1.66, or 1.66-1.68, or 1.68-1.70, or 1.70-1.72, or 1.72-1.74, or 1.74-1.76, or 1.76-1.78, or 1 .78-1.80, or 1.80-1.82, or 1.82-1.84, or 1.84-1.86, or 1.86-1.88, or 1.88-1.90, 1.90-1.92, or 1.92-1.94, or 1.94-1.96, or 1.96-1.98, or 1.98-2.00, or 2.00-2.02, or 2.02-2.04, or 2.04-2.06, or 2.06-2.08, or 2.08-2.10, or 2.10-2.12, or 2.12-2.14, or 2.14-2.16, or 2.16-2.18, or 2.18-2.20, or 2.20-2.22, or 2.22-2.24, or 2.24-2.26, or 2.26-2.28, or 2.28-2.30, or 2.30-2.32, or 2.32-2 or 2.54-2.56, or 2.56-2.58, or 2.58-2.60.
[0248] The nanocomposites of the present disclosure typically have a RI of 1.54-1.56, 1.56-1.58, 1.58-1.60, 1.60-1.62, or 1.62-1.64, 1.64-1.66, or 1.66-1.68, or 1.68-1.70, or 1.70-1.72, or 1.72-1.74, or 1.74-1.76, or 1.76-1.78, or 1 .78-1.80, or 1.80-1.82, or 1.82-1.84, or 1.84-1.86, or 1.86-1.88, or 1.88-1.90, 1.90-1.92, or 1.92-1.94, or 1.94-1.96, or 1.96-1.98, or 1.98-2.00, or 2.00-2.02, or 2.02-2.04, or 2.04-2.06, or 2.06-2.08, or 2.08-2.10, or 2.10-2.12, or 2.12-2.14, or 2.14-2.16, or 2.16-2.18, or 2.18-2.20, or 2.20-2.22, or 2.22-2.24, or 2.24-2.26, or 2.26-2.28, or 2.28-2.30, or 2.30-2.32, or 2.32-2 or 2.54-2.56, or 2.56-2.58, or 2.58-2.60.
[0249] The nanocomposites of the present disclosure typically have a RI of 1.54-1.56, 1.56-1.58, 1.58-1.60, 1.60-1.62, or 1.62-1.64, 1.64-1.66, or 1.66-1.68, or 1.68-1.70, or 1.70-1.72, or 1.72-1.74, or 1.74-1.76, or 1.76-1.78, or 1 .78-1.80, or 1.80-1.82, or 1.82-1.84, or 1.84-1.86, or 1.86-1.88, or 1.88-1.90, 1.90-1.92, or 1.92-1.94, or 1.94-1.96, or 1.96-1.98, or 1.98-2.00, or 2.00-2.02, or 2.02-2.04, or 2.04-2.06, or 2.06-2.08, or 2.08-2.10, or 2.10-2.12, or 2.12-2.14, or 2.14-2.16, or 2.16-2.18, or 2.18-2.20, or 2.20-2.22, or 2.22-2.24, or 2.24-2.26, or 2.26-2.28, or 2.28-2.30, or 2.30-2.32, or 2.32-2 or 2.54-2.56, or 2.56-2.58, or 2.58-2.60.
[0250] The nanocomposites of the present disclosure typically have hardness values of 100-150 MPa, or 150-200 MPa, or 200-250 MPa, 250-300 MPa, or 300-350 MPa, or 350-400 MPa, as measured by nanoindentation.
[0251] The nanocomposites of the present disclosure typically have modulus values of 3.0-3.5 GPa, or 3.5-4.0 GPa, or 4.0-4.5 GPa, 4.5-5.0 GPa, 5.0-5.5 GPa, 5.5-6.0 GPa, 6.0-6.5 GPa, 6.5-7.0 GPa, 7.0-7.5 GPa, 7.5-8.0 GPa, 8.0-8.5 GPa, 8.5-9.0 GPa, 9.0-9.5 GPa, 9.5-10.0 GPa, or 10.0-15.0 GPa, as measured by nanoindentation.
[0252] The nanocomposites of the present disclosure additionally exhibit thermal stability at temperatures below 120°C, or 120-175°C, or 175-200°C, or 200-250°C, or 250-300°C, or 300-400°C. Thermal stability is measured by placing the nanocomposite in air, nitrogen or vacuum at a specified temperature for 10s-5min, or 5-10min, or 10-30min, or 30-60min, or 60-120min, or longer than 120min without visually observable coloration, cracking or delamination, and a change in b* of less than 1%, or less than 5%, or less than 10%, or less than 15%, or less than 20%, or less than 25%, or less than 50% of the initial b* as measured by a Hunterlab Vista haze meter for films less than 1 micron thickness, or less than 2 microns thickness, or less than 3 microns thickness, or less than 4 microns thickness, or less than 5 microns thickness, or less than 10um thickness, or 5-10um thickness, or 1-2um thickness, or less than 1um thickness, or >10um thickness.
[0253] The nanocomposites of the present disclosure additionally exhibit thermal stability at temperatures below 120°C, or 120-175°C, or 175-200°C, or 200-250°C, or 250-300°C, or 300-400°C. Thermal stability is measured by placing the nanocomposite in air, nitrogen or vacuum at a specified temperature for 10s-5min, or 5-10min, or 10-30min, or 30-60min, or 60-120min, or longer than 120min without visually observable coloration, cracking or delamination, and the % haze change is less than 1%, or less than 5%, or less than 10%, or less than 15%, or less than 20%, or less than 25%, or less than 50% of the initial haze for a film of 1 micron thickness, or less than 2 microns thickness, or less than 3 microns thickness, or less than 4 microns thickness, or less than 5 microns thickness, or less than 10um thickness, or 5-10um thickness, or 1-2um thickness, or less than 1um thickness, or >10um thickness as measured by a Hunterlab Vista haze meter.
[0254] The nanocomposites of the present disclosure additionally exhibit thermal stability at temperatures below 120°C, or 120-175°C, or 175-200°C, or 200-250°C, or 250-300°C, or 300-400°C. Thermal stability is measured by placing the nanocomposite in air, nitrogen or vacuum at a specified temperature for 10s-5min, or 5-10min, or 10-30min, or 30-60min, or 60-120min, or longer than 120min without visually observable coloration, cracking or delamination, and for a film of 1 micron thickness, or less than 2 microns thickness, or less than 3 microns thickness, or less than 4 microns thickness, or less than 5 microns thickness, or less than 10um, or 5-10um thickness, or 1-2um thickness, or less than 1um thickness, or >10um thickness, a decrease in transmittance of less than 10%, a decrease in transmittance of less than 20%, a decrease in transmittance of less than 30%, a decrease in transmittance of less than 40%, or a decrease in transmittance of less than 50% at 400nm as measured by a PerkinElmer UV-Vis Lambda 850 spectrophotometer.
[0255] In various embodiments, the present disclosure relates to various properties of the nanocrystals, dispersions, formulations and / or nanocomposites herein. In view of the present disclosure, unless otherwise specified or contrary to the context, these properties are measured according to industry standards known to those of ordinary skill in the art. In addition, unless otherwise specified or contrary to the context, when two or more test methods for a given nanocrystal, dispersion, formulation, or nanocomposite provide different results for a stated property, it is understood that such given nanocrystal, dispersion, formulation, or nanocomposite is considered to be within the range defined herein (e.g., claims, enumerated embodiments, etc.) as long as (1) the result is within the range or definition described for the property of the nanocrystal, dispersion, formulation, or nanocomposite under one test method according to the relevant method shown in the Examples section herein; for example, such one test method can be validated using the exemplary compositions in the Examples section herein, which should provide results that are the same as the results reported herein within the experimental error generally accepted by those of ordinary skill in the art; or (2) if the relevant method is not shown in the Examples section, the result is within the range or definition described for the property of the nanocrystal, dispersion, formulation, or nanocomposite under any test method acceptable to those of ordinary skill in the art in view of this disclosure.
[0256] QUV accelerated weathering test:
[0257] In some embodiments, the disclosed core-shell nanocrystals, both inorganically treated and non-inorganically treated, dispersions, formulations, and nanocomposites exhibit low photocatalytic activity when exposed to UV irradiation. The Q Lab QUV accelerated weathering tester uses a commercial device with controlled irradiance. The QUV weathering test has two components, a UV step and a humidity step. For step 1, the UV is at 0.89 mW / cm 2 The film used in the QUV test was deposited on a glass substrate or a PET substrate supported by a glass substrate. The sample was inserted into the sample holder with the film side down and loaded into the QUV accelerated weathering tester. The refractive index and film thickness of the sampler were measured using a Metricon Model 2010 / M prism coupler, and the color and haze parameters were measured using a HunterLab haze meter. Measurements were taken before and after exposure to calculate the changes in optical properties due to the weathering test.
[0258] UVA:
[0259] For the UVA setup, two 250-watt UV-A flood lamps (320-390 nm range) were set up with a height difference of 15 cm from the circular rotating sample stage, so that the bulbs and fixtures were as close to each other as possible. The 2.5-inch glass substrates with thin films were then organized in a radial manner, starting from a point below the bulb and moving around the circle, avoiding the center of the rotating plate to ensure that all films were equally exposed to the UV-A bulbs when the stage rotated. The bulb intensity was checked before each 72-h run.
[0260] Place the film on a tray, face down, allowing the UV-A wavelengths to pass through the glass substrate and then reach the film. To begin the test, place the film on a rotating plate in the orientation specified above, turn on the lamp, and run the test for 72-158 hours. Since the lamp will heat up, if necessary, the lamp can be turned off for 1 hour every 12-24 hours, but the total exposure time should be 72 hours. Maintain an average intensity of 4mW / cm 2 .
[0261] After the test, the refractive index and film thickness of the sample were measured using a Metricon Model 2010 / M prism coupler, and the color and haze parameters were measured using a HunterLab haze meter. Measurements were taken before and after exposure to calculate changes in optical properties due to the weathering test.
[0262] In some embodiments, the light stability of the nanocomposite material of the present invention to 405nm and 450nm wavelengths was also tested. This device is similar to the described UVA test device, comprises a lamp of the desired wavelength and a flat aluminum tray placed on a turntable. The lamp is suspended above 6-12 inches above the horizontal surface of the coated substrate. The film or the nanocomposite material coated on the substrate such as glass, silicon chip or the plastic substrate such as PET is placed flat on the aluminum tray so that the film surface is upward. The aluminum tray is rotated at a slow speed then, while the film is exposed to the light for the required duration. The nanocomposite material is exposed to 405nm (average intensity is 25mW / cm 2 ) and 450nm (average intensity of 16mW / cm 2 ) wavelength for 148h (total UV dosage is 13000J / cm 2 ) and 1000h (total UV dosage is 57600J / cm 2 ). Optical properties of the nanocomposite film properties such as b*, % haze, RI and film thickness were measured and recorded before and after total exposure.
[0263] In some embodiments, the nanocomposites of the present disclosure exhibit low photocatalytic activity when exposed to UV light at wavelengths of 320-390 nm, or 390-420 nm, or 420-450 nm, or greater than 450 nm, and thus have high photostability. Photocatalytic stability is measured by: 2 .s, or 1.0-2.0mJ / cm 2 .s, or 2.0-3.0mJ / cm 2 .s, or 3.0-4.0mJ / cm 2 .s, or 4.0-5.0mJ / cm 2 .s, or 5.0-8.0mJ / cm 2 .s, or 8.0-10.0mJ / cm 2 .s, or 10.0-12.0mJ / cm 2 .s, or 12.0-14.0mJ / cm 2 .s, or 14.0-16.0mJ / cm 2 .s, or 16.0-18.0mJ / cm 2 .s, or 18.0-20.0mJ / cm 2 .s, or 20.0-25.0mJ / cm 2 .s, or 25.0-30.0mJ / cm 2 .s, or 30.0-35.0mJ / cm 2 .s, or 35.0-40.0mJ / cm 2.s, or 40.0-45.0mJ / cm 2 .s, or 45.0-50.0mJ / cm 2 s, or more, to a specified exposure wavelength for 30 seconds or more, 1 minute or more, 2 minutes or more, 3 minutes or more, 4 minutes or more, 5 minutes or more, or 10 minutes or more, or 30 minutes or more, or 60 minutes or more, or 2 hours or more, or 6 hours or more, or 12 hours or more, or 24 hours or more, or 48 hours or more, or 72 hours or more, or 100 hours or more, or 120 hours or more, or 158 hours or more, or 192 hours or more, or 240 hours or more, or 288 hours or more, or 336 hours or more, or 384 hours or more, or 432 hours or more, or 500 hours or more, or 600 hours or more, or 700 hours or more, or 800 hours or more, or 900 hours or more, or 1000 hours or more, without visually observable coloration, cracking, or delamination and passing Hunterlab For films less than 1 micron thick, or 1-5um thick, or 5-10um thick, or 10-20um thick, as measured by a Vista haze meter, the change in b* is less than 1%, or less than 5%, or less than 10%, or less than 15%, or less than 20%, or less than 25%, less than 30%, less than 40%, or less than 50% of the initial b*.
[0264] In some embodiments, the nanocomposites of the present disclosure exhibit low photocatalytic activity upon UV exposure at wavelengths of 320-390 nm, or 390-420 nm, or 420-450 nm, or greater than 450 nm, and thus have high photostability. Photocatalytic stability is measured by: 2 .s, or 1.0-2.0mJ / cm 2 .s, or 2.0-3.0mJ / cm 2 .s, or 3.0-4.0mJ / cm 2 .s, or 4.0-5.0mJ / cm 2 .s, or 5.0-8.0mJ / cm 2 .s, or 8.0-10.0mJ / cm 2 .s, or 10.0-12.0mJ / cm 2 .s, or 12.0-14.0mJ / cm 2 .s, or 14.0-16.0mJ / cm 2 .s, or 16.0-18.0mJ / cm 2 .s, or 18.0-20.0mJ / cm 2 .s, or 20.0-25.0mJ / cm 2.s, or 25.0-30.0mJ / cm 2 .s, or 30.0-35.0mJ / cm 2 .s, or 35.0-40.0mJ / cm 2 .s, or 40.0-45.0mJ / cm 2 .s, or 45.0-50.0mJ / cm 2 s, or more, to a specified exposure wavelength for 30 seconds or more, 1 minute or more, 2 minutes or more, 3 minutes or more, 4 minutes or more, 5 minutes or more, or 10 minutes or more, or 30 minutes or more, or 60 minutes or more, or 2 hours or more, or 6 hours or more, or 12 hours or more, or 24 hours or more, or 48 hours or more, or 72 hours or more, or 96 hours or more, or 120 hours or more, or 158 hours or more, or 192 hours or more, or 240 hours or more, or 288 hours or more, or 336 hours or more, or 384 hours or more, or 432 hours or more, or 500 hours or more, or 600 hours or more, or 700 hours or more, or 800 hours or more, or 900 hours or more, or 1000 hours or more, without visually observable coloration, cracking, or delamination and passing Hunterlab The change in % haze is less than 1%, or less than 5%, or less than 10%, or less than 15%, or less than 20%, or less than 25%, less than 30%, less than 40%, or less than 50% of the initial haze for films less than 1 micron thick, or 1-5um thickness, or 5-10um thickness, or 10-20um thickness, as measured by a Vista haze meter. These films also exhibit a decrease in transmittance of less than 10%, a decrease in transmittance of less than 20%, a decrease in transmittance of less than 30%, a decrease in transmittance of less than 40%, or a decrease in transmittance of less than 50% at 400nm, or 450nm, or 520nm, or 550nm for films less than 1 micron thick, or 1-5um thickness, or 5-10um thickness, or 10-20um thickness, as measured by a Perkin-Elmer UV-Vis-Lambda 850 spectrophotometer.
[0265] In some embodiments, the nanocomposites of the present disclosure exhibit low photocatalytic activity upon UV exposure at wavelengths of 320-390 nm, or 390-420 nm, or 420-450 nm, or greater than 450 nm, and thus have high photostability. Photocatalytic stability is measured by: 2 .s, or 1.0-2.0mJ / cm 2 .s, or 2.0-3.0mJ / cm 2 .s, or 3.0-4.0mJ / cm 2 .s, or 4.0-5.0mJ / cm 2.s, or 5.0-8.0mJ / cm 2 .s, or 8.0-10.0mJ / cm 2 .s, or 10.0-12.0mJ / cm 2 .s, or 12.0-14.0mJ / cm 2 .s, or 14.0-16.0mJ / cm 2 .s, or 16.0-18.0mJ / cm 2 .s, or 18.0-20.0mJ / cm 2 .s, or 20.0-25.0mJ / cm 2 .s, or 25.0-30.0mJ / cm 2 .s, or 30.0-35.0mJ / cm 2 .s, or 35.0-40.0mJ / cm 2 .s, or 40.0-45.0mJ / cm 2 .s, or 45.0-50.0mJ / cm 2 s, or more, for 30 seconds or more, 1 minute or more, 2 minutes or more, 3 minutes or more, 4 minutes or more, 5 minutes or more, or 10 minutes or more, or 30 minutes or more, or 60 minutes or more, or 2 hours or more, or 6 hours or more, or 12 hours or more, or 24 hours or more, or 48 hours or more, or 72 hours or more, or 96 hours or more, or 120 hours or more, or 158 hours or more, or 192 hours or more, or 240 hours or more, or 288 hours or more, or 336 hours or more, or 384 hours or more, or 432 hours or more, or 500 hours or more, or 600 hours or more, or 700 hours or more, or 800 hours or more, or 900 hours or more, or 1000 hours or more, wherein the refractive index does not change significantly, and wherein for less than 1 A film of micrometer thickness, or 1-5um thickness, or 5-10um thickness, or 10-20um thickness, with a refractive index variation of less than 0.001, or less than 0.002, or less than 0.004, or less than 0.006, or less than 0.008, or less than 0.01, or less than 0.012, or less than 0.015, or less than 0.018, or less than 0.02, or less than 0.022 at 520nm , or less than 0.025, or less than 0.028, or less than 0.03, or less than 0.035, or less than 0.04, or less than 0.045, or less than 0.05, or less than 0.055, or less than 0.06, or less than 0.065, or less than 0.07, or less than 0.075, or less than 0.08, or less than 0.085, or less than 0.09, or less than 0.095, or less than 0.1.
[0266] In some embodiments, the nanocomposites of the present disclosure exhibit low photocatalytic activity upon UV exposure at wavelengths of 390-420 nm, or 420-450 nm, or greater than 450 nm, and thus have high photostability. Photocatalytic stability is measured by: 2 .s, or 1.0-2.0mJ / cm 2 .s, or 2.0-3.0mJ / cm 2 .s, or 3.0-4.0mJ / cm 2 .s, or 4.0-5.0mJ / cm 2 .s, or 5.0-8.0mJ / cm 2 .s, or 8.0-10.0mJ / cm 2 .s, or 10.0-12.0mJ / cm 2 .s, or 12.0-14.0mJ / cm 2 .s, or 14.0-16.0mJ / cm 2 .s, or 16.0-18.0mJ / cm 2 .s, or 18.0-20.0mJ / cm 2 .s, or 20.0-25.0mJ / cm 2 .s, or 25.0-30.0mJ / cm 2 .s, or 30.0-35.0mJ / cm 2 .s, or 35.0-40.0mJ / cm 2 .s, or 40.0-45.0mJ / cm 2 .s, or 45.0-50.0mJ / cm 2s, or more, to a specified exposure wavelength for 30 seconds or more, 1 minute or more, 2 minutes or more, 3 minutes or more, 4 minutes or more, 5 minutes or more, or 10 minutes or more, or 30 minutes or more, or 60 minutes or more, or 2 hours or more, or 6 hours or more, or 12 hours or more, or 24 hours or more, or 48 hours or more, or 72 hours or more, or 96 hours or more, or 120 hours or more, or 158 hours or more, or 192 hours or more, or 240 hours or more, or 288 hours or more, or 336 hours or more, or 384 hours or more, or 432 hours or more, or 500 hours or more, or 600 hours or more, or 700 hours or more, or 800 hours or more, or 900 hours or more, or 1000 hours or more, without visually observable coloration, cracking, or delamination and passing Hunterlab The change in % haze is less than 1%, or less than 5%, or less than 10%, or less than 15%, or less than 20%, or less than 25%, less than 30%, less than 40%, or less than 50% of the initial haze for films less than 1 micron thick, or 1-5um thickness, or 5-10um thickness, or 10-20um thickness, as measured by a Vista haze meter. These films also exhibit a decrease in transmittance of less than 10%, a decrease in transmittance of less than 20%, a decrease in transmittance of less than 30%, a decrease in transmittance of less than 40%, or a decrease in transmittance of less than 50% at 400nm, or 450nm, or 520nm, or 550nm for films less than 1 micron thick, or 1-5um thickness, or 5-10um thickness, or 10-20um thickness, as measured by a Perkin-Elmer UV-Vis-Lambda 850 spectrophotometer.
[0267] In some embodiments, the nanocomposites of the present disclosure exhibit low photocatalytic activity upon UV exposure at wavelengths of 390-420 nm, or 420-450 nm, or greater than 450 nm, and thus have high photostability. Photocatalytic stability is measured by: 2 .s, or 1.0-2.0mJ / cm 2 .s, or 2.0-3.0mJ / cm 2 .s, or 3.0-4.0mJ / cm 2 .s, or 4.0-5.0mJ / cm 2 .s, or 5.0-8.0mJ / cm 2 .s, or 8.0-10.0mJ / cm 2 .s, or 10.0-12.0mJ / cm 2 .s, or 12.0-14.0mJ / cm 2 .s, or 14.0-16.0mJ / cm 2 .s, or 16.0-18.0mJ / cm2 .s, or 18.0-20.0mJ / cm 2 .s, or 20.0-25.0mJ / cm 2 .s, or 25.0-30.0mJ / cm 2 .s, or 30.0-35.0mJ / cm 2 .s, or 35.0-40.0mJ / cm 2 .s, or 40.0-45.0mJ / cm 2 .s, or 45.0-50.0mJ / cm 2 s, or more ... The film has a thickness of 1-5 μm, 5-10 μm, or 10-20 μm, and the refractive index at 520 nm varies by less than 0.001, less than 0.002, less than 0.004, less than 0.006, less than 0.008, less than 0.01, less than 0.012, less than 0.015, less than 0.018, less than 0.02, or less than 0.022, or less than 0.025, or less than 0.028, or less than 0.03, or less than 0.035, or less than 0.04, or less than 0.045, or less than 0.05, or less than 0.055, or less than 0.06, or less than 0.065, or less than 0.07, or less than 0.075, or less than 0.08, or less than 0.085, or less than 0.09, or less than 0.095, or less than 0.1.
[0268] A method for preparing nanocomposite materials
[0269] The present disclosure provides methods for preparing nanocomposites using the formulations of the present disclosure. Nanocomposite films comprising cured or partially cured formulations of the present disclosure are described herein. The nanocomposites are cured or partially cured by UV or thermal curing techniques known to those of ordinary skill in the art.
[0270] The present disclosure provides a nanocomposite film as described herein, wherein the film is prepared by spin coating, slot die coating, screen printing, inkjet printing, dip coating, drawbar coating, roll-to-roll printing, spray coating, embossing, nanoimprinting, molding, or any combination thereof.
[0271] Device
[0272] The present disclosure provides an LED, an organic LED, a micro-LED, a touch screen, a display, a sensor, an augmented reality lens, a virtual reality lens, an optical lens, or a solar cell device comprising an active component, wherein the active component comprises or contains the nanocomposite material of the present disclosure.
[0273] Preferred embodiments include the following embodiments 1-42:
[0274] 1. A nanocrystal having a core-shell structure, comprising a core and a shell, wherein the core is at least partially encapsulated by the shell, wherein the core comprises a core metal oxide and the shell comprises a shell metal oxide, wherein the core metal oxide is characterized in that it has an average particle size greater than 3 nm but less than 50 nm as measured by TEM; and the shell is characterized in that it has a thickness of 0.1 nm to 5 nm as measured by TEM, wherein the core metal oxide and the shell metal oxide are the same or different.
[0275] 2. The nanocrystal of embodiment 1, wherein the atomic ratio of the shell metal oxide to the core metal oxide as measured by SEM EDX is less than 3, such as less than 0.1, less than 0.2, less than 0.3, less than 0.4, less than 0.5, less than 0.6, less than 0.7, less than 0.8 nm, less than 0.9, less than 1, less than 2, or less than 3. Preferably, the atomic ratio of the shell metal oxide to the core metal oxide is less than 0.5.
[0276] 3. The nanocrystals of any of embodiments 1 and 2, wherein the core metal oxide and core-shell metal oxide nanocrystals have a narrow particle size distribution characterized by: 1) a D90:D10 ratio of less than 5, preferably less than 3, or less than 2, such as from about 1.1 to about 2, from about 1.5 to about 2, from about 1.2 to about 1.8, from about 1.2 to about 3, or from about 1.5 to about 3; 2) a D90:D50 ratio of less than 3, preferably less than 2, or less than 1.5, such as from about 1.1 to about 2, from about 1.5 to about 2, from about 1.2 to about 1.5; and / or 3) a D50:D10 ratio of less than 3, preferably less than 2, or less than 1.5, such as from about 1.1 to about 2, from about 1.5 to about 2, from about 1.2 to about 1.5.
[0277] 4. The nanocrystal of any one of embodiments 1-3, comprising a core and / or core-shell treated with an inorganic passivating agent, wherein the inorganic passivating agent comprises at least one of sodium polyphosphate, lithium nitrate, sodium hypochlorite, sodium hypophosphite, sodium phosphite, lithium chloride, sodium nitrate, sodium chloride, sodium aluminum phosphate, sodium hexametaphosphate, or any combination thereof. Preferably, the inorganic passivating agent comprises NaH PO .
[0278] 5. The nanocrystals of any one of embodiments 1-4, comprising at least partially end-capped nanocrystals, wherein the at least partially end-capped nanocrystals are end-capped with at least one end-capping agent selected from the group consisting of methyltrimethoxysilane, ethyltrimethoxysilane, n-propyltrimethoxysilane, n-propyltriethoxysilane, n-octyltrimethoxysilane, n-octyltriethoxysilane, phenyltrimethoxysilane, dodecyltrimethoxysilane, m-, p-ethylphenethyltrimethoxysilane, 2-[methoxy(polyethyleneoxy)propyl]-trimethoxysilane, methoxy(trivinyloxy)propyltrimethoxysilane, 3-amino trimethoxysilane, 3-mercaptopropyltrimethoxysilane, 3-(methacryloyloxy)propyltrimethoxysilane, 3-(acryloyloxy)propyltrimethoxysilane, 3-isocyanatopropyltriethoxysilane, 3-isocyanatopropyltrimethoxysilane, and 3-glycidoxypropyltrimethoxysilane, vinyltrimethoxysilane, allyltrimethoxysilane, 1-hexenyltrimethoxysilane, 1-octenyltrimethoxysilane, N-phenylaminopropyltrimethoxysilane, 3-(4-pyridylethyl)thiopropyltrimethoxysilane, N-(3-trimethoxysilylpropyl)pyrrole, 2-(3 -trimethoxysilylpropylthio)thiophene, (3-trimethoxysilylpropyl)diethylenetriamine, phenyltrimethoxysilane, ((chloromethyl)phenylethyl)trimethoxysilane, 2-(diphenylphosphino)ethyltriethoxysilane, 4-phenylbutyltrimethoxysilane, 2-phenylethyltrimethoxysilane, 4-biphenyltriethoxysilane, N-[3-(trimethoxysilyl)propyl]allylamine, 3-mercaptopropyltrimethoxysilane, 8-glycidoxyoctyltrimethoxysilane, (3-glycidoxypropyl)trimethoxysilane, ethyl orthosilicate, heptanol, hexanol, octanol, benzyl alcohol, phenol, ethyl alcohol, propanol, butanol, oleyl alcohol, dodecanol, octadecanol and triethylene glycol monomethyl ether, (2-{2-[2-methoxy-ethoxy]-ethoxy}-ethyl)phosphonic acid, (6-{2-[2-(2-methoxy-ethoxy)-ethoxy]-ethoxy}-hexyl)phosphonic acid, 11-acryloyloxyundecylphosphonic acid, octanoic acid, acetic acid, propionic acid, 2-[2-(2-methoxyethoxy)ethoxy]acetic acid, oleic acid, benzoic acid, stearic acid, trifluoroacetic acid, biphenyl-4-carboxylic acid, 2-(2-methoxyethoxy)acetic acid, methacrylic acid, mono-2-(methacryloyloxy)ethyl succinate, or any combination thereof.Preferably, the end-capping agent is methyltrimethoxysilane, phenyltrimethoxysilane, m-, p-ethylphenethyltrimethoxysilane, 2-[methoxy(polyethyleneoxy)propyl]-trimethoxysilane, methoxy(trivinyloxy)propyltrimethoxysilane, 3-aminopropyltrimethoxysilane, 3-mercaptopropyltrimethoxysilane, 3-(methacryloyloxy)propyltrimethoxysilane, 3-(acryloyloxy)propyltrimethoxysilane, vinyltrimethoxysilane, allyltrimethoxysilane, (2-{2-[2-methoxy-ethoxy]-ethoxy}-ethyl)phosphonic acid, (6-{2-[2-(2-methoxy-ethoxy)-ethoxy]-ethoxy}-hexyl)phosphonic acid, 11-acryloyloxyundecylphosphonic acid, 2-[2-(2-methoxyethoxy)ethoxy]acetic acid, or any combination thereof.
[0279] 6. The nanocrystals of embodiment 5, wherein the organic content of the at least partially end-capped nanocrystals is less than 25%, such as less than 5%, or between 5% and 8%, or between 8% and 10%, or between 10% and 12%, or between 12% and 14%, or between 14% and 16%, or between 16% and 18%, or between 18% and 20% of the at least partially end-capped nanocrystals.
[0280] 7. The nanocrystal of any one of embodiments 1-6, wherein the core metal oxide comprises titanium dioxide, zirconium dioxide, and / or barium titanate, and wherein the shell metal oxide comprises silicon dioxide, zirconium dioxide, hafnium dioxide, niobium oxide, aluminum oxide, tantalum oxide, barium titanium oxide, cerium oxide, or any combination thereof.
[0281] 8. The nanocrystal of any one of embodiments 1-6, wherein the core metal oxide comprises TiO2, and the shell metal oxide comprises silicon dioxide, zirconium dioxide, hafnium dioxide, niobium oxide, aluminum oxide, tantalum oxide, cerium oxide, barium titanium oxide, or any combination thereof.
[0282] 9. The nanocrystal of any one of embodiments 1-6, wherein the core metal oxide comprises TiO2, and the shell metal oxide comprises silica, zirconia, ceria, or any combination thereof.
[0283] 10. The nanocrystals of any one of embodiments 1-9 exhibit low photocatalytic activity, as measured by a change in b* before and after UV exposure of a 1 μm thick film comprising the core-shell structure using a haze meter, the b* being less than 50%, such as less than 1%, or less than 5%, or less than 10%, or less than 15%, or less than 20%, or less than 25%, less than 30%, less than 40%, or less than 50%; and a change in refractive index before and after exposure of a film comprising the core-shell nanocrystals to UV at a light intensity of 4 mW / cm2 at or above 320-390 nm using a prism coupler or ellipsometer, the change in refractive index being less than 0.08, such as less than 0.01, less than 0.02, less than 0.03, less than 0.04, less than 0.05, less than 0.06, or less than 0.07.
[0284] 11. The nanocrystals of any one of embodiments 1-9 exhibit low photocatalytic activity, as measured by a change in b* before and after UV exposure of a 1 μm thick film comprising the core-shell structure using a haze meter, the change in b* being less than 50%, such as less than 1%, or less than 5%, or less than 10%, or less than 15%, or less than 20%, or less than 25%, less than 30%, less than 40%, or less than 50%; and a photocatalytic activity of less than 100 μm when measured at 16 mW / cm2 using a prism coupler or ellipsometer. 2 1000h under UV light of 450nm or above or 25mW / cm 2 The change in refractive index is measured by the change in refractive index before and after exposure to UV at 405 nm or higher for 148 h at a light intensity of less than 0.01, less than 0.02, less than 0.03, less than 0.04, less than 0.05, less than 0.06, less than 0.07.
[0285] 12. The nanocrystal of any one of embodiments 10-11, wherein the core metal oxide is titanium oxide, the shell metal oxide comprises zirconium oxide, and the nanocrystals have an average particle size of less than 30 nm as measured by TEM; wherein the atomic ratio of the shell Zr to the core Ti as measured by SEM EDX is less than 3, such as less than 0.1, less than 0.2, less than 0.3, less than 0.4, less than 0.5, less than 0.6, less than 0.7, less than 0.8 nm, less than 0.9, less than 1, less than 2, less than 3.
[0286] 13. The capped nanocrystal of any one of embodiments 5-12, wherein the particle size distribution of the nanocrystals is characterized by a D9999 of less than 500 nm when measured by dynamic light scattering (DLS) based on the volume of 5 wt% of the nanocrystals dispersed in a solvent.
[0287] 14. A method for preparing core-shell structured TiO2 nanocrystals, wherein the core-shell TiO2 nanocrystals include a core comprising TiO2 nanocrystals and a shell comprising a shell metal oxide, the method comprising converting a precursor of the shell metal oxide into the shell metal oxide that at least partially encapsulates the core comprising TiO2 nanocrystals in a solvent, wherein the conversion comprises 1) mixing the precursor of the shell metal oxide into a reaction mixture of the solvent and the core comprising TiO2 nanocrystals, and 2) heating the reaction mixture at a reaction temperature, such as about 90°C, for a period of time to provide the shell metal oxide that at least partially encapsulates the core comprising TiO2 nanocrystals.
[0288] 15. The method of embodiment 14, wherein the converting comprises 1) adding the precursor of the shell metal oxide directly or mixing the precursor of the shell metal oxide in water to the reaction mixture of the solvent and the core comprising TiO2 nanocrystals, and 2) heating the reaction mixture at a reaction temperature of about 50°C to about 90°C for about 10 minutes to about 7 days, preferably about 1 hour to 24 hours, to form the shell metal oxide that at least partially encapsulates the core comprising TiO2 nanocrystals.
[0289] 16. The method of any of embodiments 14-15, wherein the shell metal oxide comprises zirconium oxide, and wherein the precursor of the zirconium dioxide is a zirconium alkoxide, such as a zirconium alkoxide having the formula Zr(OR)4, a zirconium alkoxide having the formula Zr(OR) x G y The invention also provides a compound or combination thereof, or a zirconium oxyhalide or zirconium halide, wherein each R group can independently be an alkyl group (e.g., C1-C6 alkyl) or a substituted alkyl group, and each occurrence of the G group is independently a halogen (e.g., Cl), wherein x is an integer from 0 to 4, and y is an integer from 0 to 4, provided that x + y is 4; zirconium oxyhalide is preferred. The atomic ratio of Zr / Ti of the core TiO2 nanocrystal and the shell ZrO2 is less than 3, such as less than 0.1, less than 0.2, less than 0.3, less than 0.4, less than 0.5, less than 0.6, less than 0.7, less than 0.8, less than 0.9, less than 1, less than 2, or less than 3 as measured by SEM EDX. Preferably, the atomic ratio of Zr / Ti of the core TiO2 nanocrystal and the shell ZrO2 is less than 1.
[0290] 17. The method of any one of embodiments 14-16, wherein the solvent comprises one or more solvents selected from benzyl alcohol, phenol, oleyl alcohol, butanol, propanol, isopropanol, ethanol, butoxyethanol, butoxypropanol, methanol, 2-(isopentyloxy)ethanol, 2-propoxy-propanol (PnP), 2-(hexyloxy)ethanol, tetrahydrofuran, dimethyl ether, ethyl ether, dibutyl ether, propylene glycol monomethyl ether (PGME), diethylene glycol butyl ether, dipropylene glycol methyl ether (DPGME), diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol, dipropylene glycol, acetone, propylene glycol methyl ether acetate (PGMEA), ethyl lactate (EL), methyl acetate, ethyl acetate, butyl acetate, ethylene glycol monobutyl ether acetate, diethylene glycol monoethyl ether acetate, butoxyethyl acetate, ethyl acetate, 2-(2-butoxyethoxy)ethyl acetate, benzene, toluene, and water. Preferably, the solvent comprises water.
[0291] 18. The method of any one of embodiments 14-17, wherein the core-shell structured TiO nanocrystals have an average particle size of about 3 nm to about 50 nm as measured by TEM, or 4 nm to 30 nm as measured by TEM. Preferably, the core-shell nanocrystals having the shell comprising the shell metal oxide have a shell thickness of 0.1 nm to 5 nm as measured by TEM. Preferably, the shell of at least one metal oxide material on the TiO nanocrystals completely or partially encapsulates the TiO nanocrystals. Additionally, the shell comprises the shell metal oxide in crystalline and / or amorphous form. The core-shell TiO2 nanocrystals prepared according to the methods of embodiments 14-18 have a narrow particle size distribution, characterized by: 1) a D90:D10 ratio of less than 5, preferably less than 3, or less than 2, such as from about 1.1 to about 2, from about 1.5 to about 2, from about 1.2 to about 1.8, from about 1.2 to about 3, or from about 1.5 to about 3; 2) a D90:D50 ratio of less than 3, preferably less than 2, or less than 1.5, such as from about 1.1 to about 2, from about 1.5 to about 2, from about 1.2 to about 1.5; and / or 3) a D50:D10 ratio of less than 3, preferably less than 2, or less than 1.5, such as from about 1.1 to about 2, from about 1.5 to about 2, from about 1.2 to about 1.5.
[0292] 19. A method for capping a core-shell TiO nanocrystal having a core comprising a TiO nanocrystal with a shell comprising ZrO, comprising reacting the nanocrystal of any one of embodiments 1-5 with a first capping agent in a first capping solvent to produce a first at least partially capped core-shell TiO nanocrystal. The capping agent is methyltrimethoxysilane, ethyltrimethoxysilane, n-propyltrimethoxysilane, n-propyltriethoxysilane, n-octyltrimethoxysilane, n-octyltriethoxysilane, phenyltrimethoxysilane, dodecyltrimethoxysilane, m-, p-ethylphenethyltrimethoxysilane, 2-[methoxy(polyethyleneoxy)propyl]-trimethoxysilane, methoxy(trivinyloxy)propyltrimethoxysilane, 3-aminopropyltrimethoxysilane, 3-mercaptopropyltrimethoxysilane, 3-(methacryloyloxy)propyltrimethoxysilane, 3-(acryloyloxy)propyltrimethoxysilane )propyltrimethoxysilane, 3-isocyanatopropyltriethoxysilane, 3-isocyanatopropyltrimethoxysilane, and 3-glycidoxypropyltrimethoxysilane, vinyltrimethoxysilane, allyltrimethoxysilane, 1-hexenyltrimethoxysilane, 1-octenyltrimethoxysilane, N-phenylaminopropyltrimethoxysilane, 3-(4-pyridylethyl)thiopropyltrimethoxysilane, N-(3-trimethoxysilylpropyl)pyrrole, 2-(3-trimethoxysilylpropylthio)thiophene, (3-trimethoxysilylpropyl)diethylenetriamine , phenyltrimethoxysilane, ((chloromethyl)phenylethyl)trimethoxysilane, 2-(diphenylphosphino)ethyltriethoxysilane, 4-phenylbutyltrimethoxysilane, 2-phenylethyltrimethoxysilane, 4-biphenyltriethoxysilane, N-[3-(trimethoxysilyl)propyl]allylamine, 3-mercaptopropyltrimethoxysilane, 8-glycidoxyoctyltrimethoxysilane, (3-glycidoxypropyl)trimethoxysilane, ethyl orthosilicate, heptanol, hexanol, octanol, benzyl alcohol, phenol, ethanol, propanol, butanol, oleyl alcohol, dodecanol, octadecyl alcohol and triethylamine one or more of glycol monomethyl ether, (2-{2-[2-methoxy-ethoxy]-ethoxy}-ethyl)phosphonic acid, (6-{2-[2-(2-methoxy-ethoxy)-ethoxy]-ethoxy}-hexyl)phosphonic acid, 11-acryloyloxyundecylphosphonic acid, octanoic acid, acetic acid, propionic acid, 2-[2-(2-methoxyethoxy)ethoxy]acetic acid, oleic acid, benzoic acid, stearic acid, trifluoroacetic acid, biphenyl-4-carboxylic acid, 2-(2-methoxyethoxy)acetic acid, methacrylic acid, mono-2-(methacryloyloxy)ethyl succinate, or any combination thereof.Preferably, the end-capping agent is methyltrimethoxysilane, phenyltrimethoxysilane, m-, p-ethylphenethyltrimethoxysilane, 2-[methoxy(polyethyleneoxy)propyl]-trimethoxysilane, methoxy(trivinyloxy)propyltrimethoxysilane, 3-aminopropyltrimethoxysilane, 3-mercaptopropyltrimethoxysilane, 3-(methacryloyloxy)propyltrimethoxysilane, 3-(acryloyloxy)propyltrimethoxysilane, vinyltrimethoxysilane, allyltrimethoxysilane, (2-{2-[2-methoxy-ethoxy]-ethoxy}-ethyl)phosphonic acid, (6-{2-[2-(2-methoxy-ethoxy)-ethoxy]-ethoxy}-hexyl)phosphonic acid, 11-acryloyloxyundecylphosphonic acid, 2-[2-(2-methoxyethoxy)ethoxy]acetic acid, or any combination thereof.
[0293] 20. A nanocrystal dispersion comprising at least partially capped core-shell nanocrystals comprising a core metal oxide with an outer shell comprising a shell metal oxide, at least one capping agent, and a dispersion medium, wherein the core metal oxide is characterized by having an average particle size greater than 3 nm but less than 50 nm as measured by TEM or DLS, and the shell is characterized by having a thickness of 0.1 nm to 5 nm as measured by TEM or DLS; and wherein the at least partially capped core-shell nanocrystals are present in an amount greater than 10%, or greater than 20%, or greater than 30%, or greater than 40%, or greater than 50%, or greater than 60%, or greater than 70%, or greater than 80% by weight of the dispersion.The at least partially capped core-shell structured nanocrystals are capped with at least one capping agent, wherein the at least one capping agent is selected from methyltrimethoxysilane, ethyltrimethoxysilane, n-propyltrimethoxysilane, n-propyltriethoxysilane, n-octyltrimethoxysilane, n-octyltriethoxysilane, phenyltrimethoxysilane, dodecyltrimethoxysilane, m, p-ethylphenethyltrimethoxysilane, 2-[methoxy(polyethyleneoxy)propyl]-trimethoxysilane, methoxy(trivinyloxy)propyltrimethoxysilane, 3-aminopropyltrimethoxysilane, 3-mercaptopropyltrimethoxysilane , 3-(methacryloyloxy)propyltrimethoxysilane, 3-(acryloyloxy)propyltrimethoxysilane, 3-isocyanatopropyltriethoxysilane, 3-isocyanatopropyltrimethoxysilane, and 3-glycidoxypropyltrimethoxysilane, vinyltrimethoxysilane, allyltrimethoxysilane, 1-hexenyltrimethoxysilane, 1-octenyltrimethoxysilane, N-phenylaminopropyltrimethoxysilane, 3-(4-pyridylethyl)thiopropyltrimethoxysilane, N-(3-trimethoxysilylpropyl)pyrrole, 2-(3-trimethoxysilylpropylthio)thio Phthene, (3-trimethoxysilylpropyl)diethylenetriamine, phenyltrimethoxysilane, ((chloromethyl)phenylethyl)trimethoxysilane, 2-(diphenylphosphino)ethyltriethoxysilane, 4-phenylbutyltrimethoxysilane, 2-phenylethyltrimethoxysilane, 4-biphenyltriethoxysilane, N-[3-(trimethoxysilyl)propyl]allylamine, 3-mercaptopropyltrimethoxysilane, 8-glycidoxyoctyltrimethoxysilane, (3-glycidoxypropyl)trimethoxysilane, ethyl orthosilicate, heptanol, hexanol, octanol, benzyl alcohol, phenol, ethanol, propanol, butanol , oleyl alcohol, dodecanol, octadecanol and triethylene glycol monomethyl ether, (2-{2-[2-methoxy-ethoxy]-ethoxy}-ethyl)phosphonic acid, (6-{2-[2-(2-methoxy-ethoxy)-ethoxy]-ethoxy}-hexyl)phosphonic acid, 11-acryloyloxyundecylphosphonic acid, octanoic acid, acetic acid, propionic acid, 2-[2-(2-methoxyethoxy)ethoxy]acetic acid, oleic acid, benzoic acid, stearic acid, trifluoroacetic acid, biphenyl-4-carboxylic acid, 2-(2-methoxyethoxy)acetic acid, methacrylic acid, mono-2-(methacryloyloxy)ethyl succinate, or any combination thereof.Preferably, the end-capping agent is methyltrimethoxysilane, phenyltrimethoxysilane, m-, p-ethylphenethyltrimethoxysilane, 2-[methoxy(polyethyleneoxy)propyl]-trimethoxysilane, methoxy(trivinyloxy)propyltrimethoxysilane, 3-aminopropyltrimethoxysilane, 3-mercaptopropyltrimethoxysilane, 3-(methacryloyloxy)propyltrimethoxysilane, 3-(acryloyloxy)propyltrimethoxysilane, vinyltrimethoxysilane, allyltrimethoxysilane, (2-{2-[2-methoxy-ethoxy]-ethoxy}-ethyl)phosphonic acid, (6-{2-[2-(2-methoxy-ethoxy)-ethoxy]-ethoxy}-hexyl)phosphonic acid, 11-acryloyloxyundecylphosphonic acid, 2-[2-(2-methoxyethoxy)ethoxy]acetic acid, or any combination thereof.
[0294] 21. The nanocrystal dispersion of embodiment 20, wherein the core-shell nanocrystals are treated with an inorganic passivating agent selected from the group consisting of sodium polyphosphate, lithium nitrate, sodium hypochlorite, sodium hypophosphite, sodium phosphite, lithium chloride, sodium nitrate, sodium chloride, sodium aluminum phosphate, sodium hexametaphosphate, or any combination thereof. Preferably, the inorganic passivating agent comprises NaH2PO2.
[0295] 22. The nanocrystal dispersion of any of embodiments 20-21, wherein the organic content of the at least partially capped nanocrystals, as measured by TGA, is typically 0-25%, such as 0-5%, or 5-10%, or 10-15%, or 15-20%, or 20-25%, or less than 5%, or less than 8% or less than 10%, less than 12%, or less than 14% or less than 16%, less than 18%, or less than 20%, or less than 20%, less than 25%, of the capped nanocrystals.
[0296] 23. The nanocrystal dispersion of any one of embodiments 20-22, wherein the core metal oxide comprises titanium dioxide, zirconium dioxide, and / or barium titanate, and the shell metal oxide comprises silicon dioxide, zirconium dioxide, hafnium dioxide, niobium oxide, aluminum oxide, tantalum oxide, barium titanium oxide, cerium oxide, or any combination thereof. Preferred core-shell nanocrystals comprise a TiO core and a ZrO shell metal oxide.
[0297] 24. The nanocrystal dispersion of any of embodiments 20-23, wherein the at least partially capped core-shell nanocrystals are present in an amount equal to or greater than 50% by weight of the dispersion, and wherein the % organic matter is less than 20% of the at least partially capped core-shell nanocrystals, and the core metal oxide is titanium oxide, the shell metal oxide comprises zirconium oxide, and the average particle size of the at least partially capped core-shell nanocrystals is less than 30 nm as measured by TEM or DLS. The atomic ratio of the shell Zr to the core Ti as measured by SEM EDX is less than 3, such as less than 0.1, less than 0.2, less than 0.3, less than 0.4, less than 0.5, less than 0.6, less than 0.7, less than 0.8 nm, less than 0.9, less than 1, less than 2, or less than 3. Preferably, the atomic ratio of the shell Zr to the core Ti is less than 1.
[0298] 25. The nanocrystal dispersion of any one of embodiments 20-24, wherein the particle size distribution of the at least partially end-capped core-shell nanocrystals is characterized by a D9999 of less than 500 nm when the volume of 5 wt % of the at least partially end-capped core-shell nanocrystals dispersed in a solvent is measured by dynamic light scattering (DLS). Preferably, the D9999 is less than 300 nm.
[0299] 26. The nanocrystal dispersion of any one of embodiments 20-25, wherein the dispersion medium comprises a solvent, a monomer, an oligomer of a polymer, or a combination thereof. Examples of solvents for dispersion include, but are not limited to, THF, acetone, heptane, benzyl alcohol, phenol, oleyl alcohol, butanol, propanol, isopropanol, ethanol, butoxyethanol, butoxypropanol, methanol, tetrahydrofuran, dimethyl ether, ethyl ether, dibutyl ether, propylene glycol monomethyl ether (PGME), diethylene glycol butyl ether, dipropylene glycol methyl ether (DPGME), diethylene glycol monomethyl ether and diethylene glycol monoethyl ether, diethylene glycol, dipropylene glycol, acetone; esters such as propylene glycol methyl ether acetate (PGMEA), ethyl lactate (EL), methyl acetate, ethyl acetate (ETA), butyl acetate, ethylene glycol monobutyl ether acetate, diethylene glycol monobutyl ether acetate, diethylene glycol monoethyl ether acetate, butoxyethyl acetate, ethyl acetate, 2-(2-butoxyethoxy)ethyl acetate, benzene, toluene, and water, and any combination or mixture thereof. Preferred solvents include THF, isopropyl alcohol, ethanol, dipropylene glycol methyl ether (DPGME), propylene glycol monomethyl ether (PGME), propylene glycol methyl ether acetate (PGMEA), ethyl acetate, toluene, and any combination or mixture thereof.Monomers include benzyl (meth)acrylate (BA and BMA), trimethylolpropane tri(meth)acrylate (TMPTA and TMPTMA), trimethylolpropane ethoxylate tri(meth)acrylate (EOTMPTA and EOTMPTMA), 1,6-hexanediol di(meth)acrylate (HDDA and HDDMA), di(ethylene glycol) di(meth)acrylate (DEGDA and DEGDMA), ethylene glycol diacrylate, 1,3-diglyceryl diacrylate, tri(propylene glycol) diacrylate, 1,6-hexanediol ethoxylate diacrylate, ethylene glycol phenyl ether (meth)acrylate (PEA and PEMA), 2-hydroxy-3-phenoxypropyl acrylate (HPPA), 2-hydroxy-3-phenoxypropyl methacrylate (HPPMA), 2-phenoxybenzyl acrylate (PBA), biphenyl methacrylate (BPMA), isobornyl acrylate (IBA), 2-phenylphenol methacrylate (PPMA), isobutyl acrylate (IBA), 2-phenylethyl acrylate (2-PEA), 2-(phenylthio)ethyl acrylate (PTEA), tris(2-phenylethyl) ...PBA), tris(2-phenylethyl)acrylate (PBA), tris(2-phenylethyl)acrylate (PBA), tris(2-phenylethyl)acrylate (PBA), tris(2-phenylethyl)acrylate (P (2-Hydroxyethyl)isocyanurate triacrylate (THEICTA or M370), bisphenol A glycerate dimethacrylate, esters of acrylic acid (OPPEOA), 9,9-bis[4-(2-acryloyloxyethoxy)phenyl]fluorene or bisfluorene diacrylate in OPPEOA (HR6042), bisphenol A ethoxylate diacrylate, bisphenol A propoxylate diacrylate, bisphenol F ethoxylate (2EO / phenol) diacrylate, bisphenol A glycerate diacrylate, bisphenol A ethoxylate dimethacrylate, ethoxy (4) bis Phenol A diacrylate (SR-601), bisphenol A ethoxylate diacrylate (SR-349), tris(2-acryloyloxy)ethyl}isocyanurate, tricyclodecane dimethanol diacrylate, cresol novolac epoxy acrylate (CN112C60), tri(ethylene glycol) diacrylate, ethylene glycol diacrylate, poly(ethylene glycol) diacrylate, 1,3-diglyceryl ester diacrylate and N-vinyl pyrrolidone (NVP), phenyl norbornene, styrene (STY), 4-methylstyrene, 4-vinylanisole, divinylbenzene and combinations thereof. In some preferred embodiments, the monomers, oligomers and / or polymers may be selected from 2-phenylethyl acrylate (2-PEA), biphenyl methacrylate (BPMA), 2-phenoxybenzyl acrylate (PBA), trimethylolpropane tri(meth)acrylate (TMPTA and TMPTMA), tris(2-hydroxyethyl)isocyanurate triacrylate (THEICTA), 9,9-bis[4-(2-acryloyloxyethoxy)phenyl]fluorene or bisfluorene diacrylate in OPPEOA (HR6042), and combinations thereof.The dispersions described herein may also have a viscosity in the range of about 1 cp to about 1000 cp, such as about 1 cP-2 cP, about 2 cP-5 cP, about 5 cP-10 cP, about 10 cP-15 cP, about 15 cP-20 cP, about 20 cP-25 cP, about 25 cP-30 cP, about 30 cP-40 cP, about 40 cP-50 cP, about 50 cP-60 cP, about 60 cP-75 cP, about 75 cP-100 cP, about 100 cP-200 cP, about 200 cP- The viscosity can be adjusted in the range of 0.5-1.0 cP to 0.5-0.5 cP, or about 500-1000 cp, or about 1000-2000 cp, about 2000-3000 cp, or about 3000-4000 cp, or about 4000-5000 cp, or about 5000-6000 cp, or about 6000-7000 cp, or about 7000-8000 cp, or about 8000-9000 cp, or about 9000-10000 cp, or >10000 cp.
[0300] 27. A nanocomposite formulation comprising 1) at least partially end-capped core-shell TiO2 nanocrystals having an outer shell, the outer shell of the TiO2 nanocrystals comprising a shell metal oxide; 2) a monomer, oligomer and / or polymer; 3) an optional solvent; and 4) a curing agent, wherein the at least partially end-capped core-shell TiO2 nanocrystals are present in an amount greater than 20 weight percent relative to the monomer, oligomer and / or polymer, wherein the core of the at least partially end-capped core-shell TiO2 nanocrystals comprises crystalline titanium dioxide and is treated with at least one inorganic passivating agent; and wherein the at least partially end-capped core-shell TiO2 nanocrystals have an average particle size in the range of 3-50 nm when measured by DLS at 5% of the nanocrystals dispersed in PGMEA, and a shell thickness measured by TEM of between 0.1 nm and 3 nm. The at least partially capped core-shell TiO nanocrystals are capped with at least one capping agent selected from the group consisting of methyltrimethoxysilane, phenyltrimethoxysilane, m-, p-ethylphenethyltrimethoxysilane, 2-[methoxy(polyethyleneoxy)propyl]-trimethoxysilane, methoxy(trivinyloxy)propyltrimethoxysilane, 3-aminopropyltrimethoxysilane, 3-mercaptopropyltrimethoxysilane, 3-(methacryloyloxy)propyltrimethoxysilane, )propyltrimethoxysilane, 3-(acryloyloxy)propyltrimethoxysilane, vinyltrimethoxysilane, allyltrimethoxysilane, (2-{2-[2-methoxy-ethoxy]-ethoxy}-ethyl)phosphonic acid, (6-{2-[2-(2-methoxy-ethoxy)-ethoxy]-ethoxy}-hexyl)phosphonic acid, 11-acryloyloxyundecylphosphonic acid, 2-[2-(2-methoxyethoxy)ethoxy]acetic acid, or any combination thereof.
[0301] 28. The nanocomposite formulation of embodiment 27, wherein the shell metal oxide comprises silica, zirconium dioxide, hafnium dioxide, niobium oxide, aluminum oxide, tantalum oxide, barium titanium oxide, cerium oxide, or any combination thereof. Preferably, the shell metal oxide comprises silica, cerium oxide, and / or zirconium oxide.
[0302] 29. The nanocomposite formulation of any one of embodiments 27-28, wherein the at least partially capped core-shell nanocrystals are present in an amount equal to or greater than 35% by weight relative to the monomer, oligomer, and / or polymer, and the viscosity of the formulation is in the range of 1-10,000 cP. Preferably, the viscosity of the formulation is in the range of 1-3,000 cP.
[0303] 30. The nanocomposite formulation of any one of embodiments 27-29, wherein the at least partially capped core-shell TiO nanocrystals have low photocatalytic activity as measured by a haze meter at 4 mW / cm2 for a 1-10 μm thick film made from the formulation comprising the core-shell nanocrystals. 2 Exposure to 320nm-390nm UV for 66h, or at 16mW / cm 2 Exposure to UV at 450nm or above for 1000h, or at 25mW / cm 2 Exposure to UV light at 405 nm or above for 148 h, or at 0.89 mW / cm 2 The change in b* before and after exposure to 340 nm UV at an intensity of 100 nm is measured by a change in b* of less than 50%, such as less than 1%, or less than 5%, or less than 10%, or less than 15%, or less than 20%, or less than 25%, less than 30%, less than 40%, or less than 50%. The nanocomposite formulation according to any one of embodiments 27-29, wherein the at least partially capped core-shell structured TiO2 nanocrystals have low photocatalytic activity, the photocatalytic activity being measured by a 1-10 μm thick film made of the formulation comprising core-shell nanocrystals at 4 mW / cm when measured using a haze meter. 2 Exposure to 320nm-390nm UV for 66h, or at 16mW / cm 2 Exposure to UV at 450nm or above for 1000h, or at 25mW / cm 2 Exposure to UV light at 405 nm or above for 148 h, or at 0.89 mW / cm 2 The change in E* is measured by the change in E* before and after exposure to 340 nm UV at a concentration of 100 nm and a relative intensity of 0.1 nm, and the change in E* is less than 50%, such as less than 1%, or less than 5%, or less than 10%, or less than 15%, or less than 20%, or less than 25%, less than 30%, less than 40%, or less than 50%.
[0304] 31. The nanocomposite formulation of any one of embodiments 27-30, wherein the at least partially capped core-shell TiO nanocrystals have low photocatalytic activity as measured by a prism coupler or ellipsometer at 4 mW / cm2 for a film comprising the core-shell nanocrystals. 2 Exposure to 320nm-390nm UV for 66h, or at 16mW / cm 2 Exposure to UV at 450nm or above for 1000h, or at 25mW / cm 2Exposure to UV light at 405 nm or above for 148 h, or at 0.89 mW / cm 2 The change in refractive index before and after exposure to 340 nm UV at a relative intensity of less than 0.08 is less than 0.01, less than 0.02, less than 0.03, less than 0.04, less than 0.05, less than 0.06, less than 0.07, less than 0.08, less than 0.09, less than 0.1.
[0305] 32. A nanocomposite material comprising a cured film, the cured film comprising at least partially end-capped core-shell TiO nanocrystals with an outer shell comprising a shell metal oxide and at least one monomer, oligomer and / or polymer, wherein the at least partially end-capped core-shell TiO nanocrystals are present in an amount greater than 35% by weight of the nanocomposite material, wherein the film having a thickness of 1 micron has a transmittance greater than 80% at wavelengths greater than 400 nm, and the film has a refractive index of about 1.55 to about 2.20 as measured using a prism coupler or an ellipsometer.
[0306] 33. The nanocomposite film of embodiment 32, wherein the at least partially end-capped core-shell TiO nanocrystals have an average particle size greater than 3 nm but less than 50 nm as measured by TEM and a shell thickness of 0.1 nm to 3 nm as measured by TEM. The atomic ratio of the shell metal oxide to Ti as measured by SEM EDX is less than 0.1, less than 0.2, less than 0.3, less than 0.4, less than 0.5, less than 0.6, less than 0.7, less than 0.8, less than 0.9, or less than 1. The at least partially end-capped core-shell TiO nanocrystals are end-capped with at least one end-capping agent selected from methyltrimethoxysilane, phenyltrimethoxysilane, m-,p-ethylphenethyltrimethoxysilane, 2-[methoxy(polyethyleneoxy)propyl]-trimethoxysilane, methoxy(trivinyloxy)propyltrimethoxysilane, 3-aminopropyltrimethoxysilane, 3-mercaptopropyltrimethoxysilane, 3-(methacryloyloxy)propyltrimethoxysilane, The shell metal oxide comprises silicon dioxide, zirconium dioxide, hafnium dioxide, niobium oxide, aluminum oxide, tantalum oxide, cerium oxide, barium titanium oxide, or any combination thereof.
[0307] 34. The nanocomposite material of any one of embodiments 32-33, comprising monomers selected from the group consisting of benzyl (meth)acrylate (BA and BMA), trimethylolpropane tri(meth)acrylate (TMPTA and TMPTMA), trimethylolpropane ethoxylate tri(meth)acrylate (EOTMPTA and EOTMPTMA), 1,6-hexanediol di(meth)acrylate (HDDA and HDDMA), di(ethylene glycol) di(meth)acrylate (DEGDA and DEGDMA), ethylene glycol diacrylate, 1,3-diglycerol dipropylene glycol. Ester, tripropylene glycol diacrylate, 1,6-hexanediol ethoxylate diacrylate, ethylene glycol phenyl ether (meth)acrylate (PEA and PEMA), 2-hydroxy-3-phenoxypropyl acrylate (HPPA), 2-hydroxy-3-phenoxypropyl methacrylate (HPPMA), 2-phenoxybenzyl methacrylate (PBA), biphenyl methacrylate (BPMA), isobornyl acrylate (IBA), 2-phenylphenol methacrylate (PPMA), isobutyl acrylate (IBA), 2-phenylethyl acrylate (2-PEA), 2-(phenyl)benzene thio)ethyl acrylate (PTEA), tris(2-hydroxyethyl)isocyanurate triacrylate (THEICTA or M370), bisphenol A glycerate dimethacrylate, esters of acrylic acid (OPPEOA), 9,9-bis[4-(2-acryloyloxyethoxy)phenyl]fluorene or bisfluorene diacrylate in OPPEOA (HR6042), bisphenol A ethoxylate diacrylate, bisphenol A propoxylate diacrylate, bisphenol F ethoxylate (2EO / phenol) diacrylate, bisphenol A glycerate diacrylate, bisphenol A ethoxylate dimethacrylate Ester, ethoxy (4) bisphenol A diacrylate (SR-601), bisphenol A ethoxylate diacrylate (SR-349), tris(2-acryloyloxy)ethyl} isocyanurate, tricyclodecane dimethanol diacrylate, cresol novolac epoxy acrylate (CN112C60), tri(ethylene glycol) diacrylate, ethylene glycol diacrylate, poly(ethylene glycol) diacrylate, 1,3-diglyceryl ester diacrylate and N-vinyl pyrrolidone (NVP), phenyl norbornene, styrene (STY), 4-methylstyrene, 4-vinylanisole, divinylbenzene and combinations thereof.In some preferred embodiments, the monomers, oligomers and / or polymers may be selected from 2-phenylethyl acrylate (2-PEA), biphenyl methacrylate (BPMA), 2-phenoxybenzyl acrylate (PBA), trimethylolpropane tri(meth)acrylate (TMPTA and TMPTMA), tris(2-hydroxyethyl)isocyanurate triacrylate (THEICTA), 9,9-bis[4-(2-acryloyloxyethoxy)phenyl]fluorene or bisfluorene diacrylate in OPPEOA (HR6042), and combinations thereof.
[0308] 35. An exemplary formulation comprising at least one acrylic monomer selected from HR6042 and BPMA, at least partially end-capped titanium oxide nanocrystals (e.g., any of those described herein, such as any of those preferred or exemplified herein), or at least partially end-capped core-shell nanocrystals comprising TiO2 as a core and ZrO2 as a shell metal oxide (e.g., any of those described herein, such as any of those preferred or exemplified herein), wherein the weight ratio of the nanocrystals to the combined weight of the monomers is from 0.5:1 to 3:1. The formulation may further comprise a photoinitiator, TPO, and at least one solvent (e.g., any of those described herein, such as any of those preferred or exemplified herein). The formulation may be applied to a surface by spin coating and is nanoimprintable. The nanocomposite film formed by applying the formulation to a surface preferably has a transmittance greater than 80%, or greater than 90%, or greater than 93% at a film thickness of 40 nm to 30 μm. The nanocomposite has an RI at 520 nm in the range of 1.6 to 2.2, such as in the range of 1.6-1.7, or 1.7-1.8, or 1.8-1.9 or 1.9-2.0. Preferably, the RI is in the range of 1.8-2.0. The nanocomposite also has a low haze of less than 1% and a b* of less than 1.
[0309] 36. Another exemplary formulation comprises acrylic monomers including PBA and / or THEICTA, and at least partially end-capped titanium oxide nanocrystals (e.g., any of those described herein, such as any of those preferred or exemplified herein) or at least partially end-capped core-shell nanocrystals comprising TiO2 as a core and ZrO2 as a shell metal oxide (e.g., any of those described herein, such as any of those preferred or exemplified herein), wherein the at least partially end-capped nanocrystals are present in a range of 20 wt% to 60 wt% relative to the total formulation and the monomers are present in a range of 3 wt% to 25 wt% relative to the total formulation, such that the ratio of nanocrystals to monomers is 3:7 to 8:2. The formulation may also include a photoinitiator (e.g., any of those described herein, such as any of those preferred or exemplified herein) present in the range of 0.5-2.5 wt % relative to the total formulation and a solvent (e.g., any of those described herein, such as any of those preferred or exemplified herein) present in the range of 20-40 wt % relative to the total formulation. The formulation can be applied to a surface by spin coating and is nanoimprintable. The nanocomposite film formed by applying the formulation to a surface preferably has a transmittance greater than 80%, or greater than 90%, or greater than 93% when the film thickness is 40nm to 30um. The nanocomposite has an RI at 520nm in the range of 1.6 to 2.2, such as in the range of 1.6-1.7, or 1.7-1.8, or 1.8-1.9 or 1.9-2.0. Preferably, the RI is in the range of 1.7-1.9. The nanocomposite also has a low haze of less than 1% and a b* of less than 1.
[0310] 37. Another exemplary formulation comprises at least partially capped nanocrystals, core-shell nanocrystals, or inorganically treated core-shell nanocrystals (e.g., any of those described herein, such as any of those preferred or exemplified herein) and at least one monomer, wherein the core-shell nanocrystals comprise a TiO2 core and a ZrO2 shell. The nanocrystals are present in a range of 35-80 wt %, preferably 65-75 wt %, relative to the total formulation. The monomer preferably comprises at least one of 2-PEA, PTEA, PEA, PBA, and / or IBA, present in a range of 3-18 wt %, relative to the total formulation, and TEICHTA is present in a range of 1-10 wt %, relative to the total formulation. The formulation optionally contains an additive such as Tinivin 405, Irganox 1010, present in a range of 0.5-2.5 wt %, relative to the total formulation, and / or a photoinitiator (e.g., any of those described herein, such as any of those preferred or exemplified herein) in a range of 0.5-2.5 wt %, relative to the total formulation. Said preparation contains less than 6.5% solvent usually. Having nanocrystal loading is that the preparation of 65-75% demonstrates the low viscosity of 500-5000cP, preferably 1000-3000cP. By applying said preparation to the nanocomposite film formed on the surface, there is greater than 80% or greater than 90% or greater than 93% transmittance when film thickness is 40nm to 30um. At 520nm, the RI of nanocomposite is in the scope of 1.6 to 2.2, such as in the scope of 1.6-1.7 or 1.7-1.8 or 1.8-1.9 or 1.9-2.0. Preferably, said RI is in the scope of 1.75-1.9. Nanocomposite also has a low haze less than 5% and a b* less than 2 under the thickness of about 10um.
[0311] 38. Another exemplary formulation comprises at least partially capped nanocrystals, core-shell nanocrystals, or inorganically treated core-shell nanocrystals (e.g., those described herein, such as any of those preferred or exemplified herein) and at least one monomer, wherein the core-shell nanocrystals comprise a TiO2 core and a ZrO2 shell. The nanocrystals are present in a range of 20-60% by weight relative to the total formulation, a monomer blend comprising at least one of BA, BPMA, and / or DVE is present in a range of 40-80% by weight relative to the total formulation; the formulation optionally contains a diluent such as STY or ethyl acetate present in a range of 0.5-5% by weight relative to the total formulation, and at least one photoinitiator and photosensitizer selected from Irgacure 819, ITX, and Esacure 1001M present in a range of 0.5-2.5% by weight relative to the total formulation. The solvent content of the formulation is less than 6.5% by weight relative to the total formulation. The formulation can be prepared as described in method 2 of the present disclosure. The nanocomposite material of the present invention is characterized in that the nanocomposite material has a nanocrystal loading of 20-50% and exhibits a low viscosity of 10-100 cP, preferably 10-40 cP. The nanocomposite material is inkjet printable. The transmittance of the nanocomposite material film formed by applying the nanocomposite material to the surface when the film thickness is 40 nm to 30 μm is greater than 80%, or greater than 90%, or greater than 93%. At 589 nm, the RI of the nanocomposite material is within the range of 1.6 to 1.9, for example, within the range of 1.6-1.7, 1.7-1.8, or 1.8-1.9. Preferably, the RI is within the range of 1.6-1.8. The nanocomposite material also has a low haze of less than 2% and a b* of less than 3 at a thickness of about 10 μm.
[0312] 39. The nanocomposite material of any one of embodiments 32-38, wherein the film having a thickness of <5 μm is thermally stable when subjected to a temperature greater than 200° C. for 5 min, wherein the change in b* relative to the initial b* as measured by a haze meter is less than 1%, or less than 5%, or less than 10%, or less than 15%, or less than 20%, or less than 25%, and the change in % haze is less than 1%, or less than 5%, or less than 10%, or less than 15%, or less than 20%, or less than 25%.
[0313] 40. The nanocomposite film of any one of embodiments 32-39, wherein the at least partially capped core-shell TiO nanocrystals have low photocatalytic activity as measured by a haze meter at 4 mW / cm2 for a 1 μm thick film comprising the core-shell structure. 2 Exposure to 320nm-390nm UV for 66h, or at 16mW / cm 2Exposure to UV at 450nm or above for 1000h, or at 25mW / cm 2 Exposure to UV light at 405 nm or above for 148 h, or at 0.89 mW / cm 2 The change in b* before and after exposure to 340 nm UV at an intensity of 100 nm for 72 hours is measured as a change in b* of less than 50%, such as less than 1%, or less than 5%, or less than 10%, or less than 15%, or less than 20%, or less than 25%, less than 30%, less than 40%, or less than 50%. The nanocomposite film of any one of embodiments 32-39, wherein the at least partially capped core-shell TiO2 nanocrystals have low photocatalytic activity, as measured by a haze meter at 4 mW / cm2 for a 1-10 μm thick film made from the formulation comprising the core-shell nanocrystals. 2 Exposure to 320nm-390nm UV for 66h, or at 16mW / cm 2 Exposure to UV at 450nm or above for 1000h, or at 25mW / cm 2 Exposure to UV light at 405 nm or above for 148 h, or at 0.89 mW / cm 2 The change in E* before and after exposure to 340 nm UV at a constant intensity for 72 hours is measured as a change in E* of less than 50%, such as less than 1%, or less than 5%, or less than 10%, or less than 15%, or less than 20%, or less than 25%, less than 30%, less than 40%, or less than 50%. In addition, the change in % haze is less than 1%, or less than 5%, or less than 10%, or less than 15%, or less than 20%, or less than 25%, less than 30%, less than 40%, or less than 50% of the initial haze.
[0314] 41. The nanocomposite film of any one of embodiments 32-40, wherein the at least partially capped core-shell TiO nanocrystals have low photocatalytic activity as measured by a prism coupler or ellipsometer at 4 mW / cm2 for a film comprising the core-shell nanocrystals. 2 Exposure to 320nm-390nm UV for 66h, or at 16mW / cm 2 Exposure to UV at 450nm or above for 1000h, or at 25mW / cm 2 Exposure to UV light at 405 nm or above for 148 h, or at 0.89 mW / cm 2The film may have a refractive index that is less than 0.08, such as less than 0.01, less than 0.02, less than 0.03, less than 0.04, less than 0.05, less than 0.06, or less than 0.07, as measured by the change in refractive index before and after exposure to 340 nm UV at a relative intensity of 100 nm for 72 hours. In addition, the film may have a percent change in film thickness of less than 0.1, or less than 0.2, or less than 0.3, or less than 0.4, or less than 0.5, or less than 0.6, or less than 0.7, or less than 0.8, or less than 0.9, or less than 1.0, or less than 1.5, or less than 2.0, or less than 2.5, or less than 3.0, or less than 3.5, or less than 4.0, or less than 4.5, or less than 5, or less than 10, or less than 15, or less than 20, or less than 25, or less than 50%.
[0315] 42. A device comprising the nanocomposite film of any one of embodiments 32-41.
[0316] Example
[0317] Example 1: Synthesis of Titanium Oxide (TiO2) Nanocrystals:
[0318] Titanium oxide nanocrystals with a size in the range of 1-30 nm are prepared from precursors such as titanium (IV) methoxide, titanium (IV) ethoxide, titanium (IV) propoxide, titanium (IV) isopropoxide, titanium (IV) butoxide or titanium (IV) oxyacetylacetonate. Depending on the desired end product, titanium n-butoxide, chlorotriisopropoxytitanium (IV), titanium n-propoxide, titanium (IV) chloride, titanium tri-n-butoxide chloride, or titanium dichloride dipropoxide will advantageously be used as a precursor.
[0319] In an exemplary method, a titanium alkoxide precursor, such as but not limited to titanium n-butoxide, titanium n-propoxide, titanium isopropoxide or titanium ethoxide, is mixed with water and a solvent or solvent mixture (including benzyl alcohol, phenol, oleyl alcohol, butanol, propanol, isopropanol, tetrahydrofuran, ethanol, methanol, acetonitrile, toluene, PGMEA, propylene glycol propyl ether (PGPE), PGME, 2-methyl-1-propanol or triethylene glycol monomethyl ether) as a reagent and sealed in an autoclave. The reaction mixture is heated to a temperature of 140-300° C., preferably to a temperature of 180-250° C. Once the reaction mixture reaches the set temperature, the temperature is maintained for a period of 20 min to 24 h, preferably 30 min to 2 h, depending in part on the solvent or solvent mixture and / or the reaction temperature. Titanium oxide nanocrystals are obtained as a white milky suspension. TiO2 is separated from the suspension by centrifugation. The milky suspension is transferred to a centrifuge bottle and centrifuged at 4500 rpm for 10 min. The centrifugation step causes the TiO2 to collect at the bottom of the bottle, with a clear supernatant on top. The clear supernatant is decanted and discarded, leaving a white solid at the bottom of the bottle. This solid is called a "wet cake" because it has most of the solvent removed but is still in a wet form.
[0320] In a preferred method, 879 g of 100% (w / w) titanium (IV) n-butoxide is mixed with 3550 g of benzyl alcohol and 116.3 g of water in an inertized 2-gallon Parr reactor. The apparatus is sealed under inert conditions, such as a nitrogen atmosphere, to prevent oxygen contamination. The Parr reactor is then heated to 200° C. while stirring at 600 rpm and maintained at this temperature for 1 hour. After the reaction, the reactor is cooled to room temperature and the white milky solution of the synthesized titanium oxide nanocrystals is collected. The milky suspension is transferred to a centrifuge bottle and centrifuged at 4500 rpm for 10 minutes to collect the wet cake.
[0321] Example 2: Synthesis of Zirconium Oxide (ZrO2) Nanocrystals:
[0322] An exemplary synthesis method using zirconium n-butoxide as a precursor is as follows: 21.58 g of 80% (w / w) zirconium (IV) n-butoxide in 1-butanol solution (containing 17.26 g or 45 mmol of zirconium n-butoxide) is mixed with 300 ml of benzyl alcohol and then transferred to an autoclave. Optionally, water is added as a reactant in an amount of 0.1 to 2 mol% of the zirconium precursor. The apparatus is sealed under an inert atmosphere to prevent contamination by oxygen and moisture. The autoclave is then heated to 325°C. This temperature is maintained for 1 hour and then cooled to room temperature. The synthesized white milky solution of zirconium oxide nanocrystals is collected.
[0323] Zirconium n-butoxide is received as a solution in 1-butanol (80% w / w). 1-Butanol can be removed from the precursor prior to synthesis under vacuum and / or heat (30-50°C), during synthesis by releasing the pressure of the autoclave when the temperature reaches approximately 100°C, or after the reaction is complete. The nanocrystals are spherical with a diameter of approximately 5 nm.
[0324] Example 3: High-temperature ZrO2 shell formation on TiO2 and subsequent surface modification
[0325] The TiO2 wet cake from Example 1 (450 g) was mixed with benzyl alcohol (1240 g). The resulting milky white suspension was centrifuged at 4500 rpm for 10 minutes. The supernatant was decanted, and the nanocrystals settled as a wet cake at the bottom of the centrifuge bottle. The wet cake was then redispersed in benzyl alcohol (3400 g), and the slurry was transferred to a 2-gallon reactor. The reactor was closed and sealed. 340 g of zirconium butoxide (80% in n-butanol) was then charged to the reactor, followed by 200 g of benzyl alcohol. The reactor was inerted with nitrogen and stirred for 20 minutes. The reactor was then heated to 205°C and maintained at this temperature for 4 hours. After cooling to room temperature, the material was discharged.
[0326] The treated TiO2 obtained was separated from the reaction mixture by centrifugation at 4500 rpm for 10 min. The solid material was then dispersed into vigorously shaken PGMEA and then collected by centrifugation at 45000 rpm for 10 min, wherein the PGMEA was decanted. The material (46 g) was then transferred to a flask and dispersed into PGMEA (85 g). Methoxy(triethoxy)propyltrimethoxysilane (6.9 g) was then added and the reaction mixture was heated at 70°C for 40 min. 3-(methacryloyloxy)propyltrimethoxysilane (13.8 g) was then added and heated at 70°C for another 30 min. Water (2.3 g) was then added to the reaction mixture and the reaction mixture was heated at 70°C for another 30 min to form capped nanocrystals.
[0327] By using heptane (700ml) to precipitate nanocrystals, end-capped nanocrystals are separated from the reaction mixture. By centrifugal collection solid and decant liquid. Then the solid material is dispersed in the dimethylbenzene of 100ml and continues 2min, then adds the THF of 200ml, then adds the heptane of 700ml. By centrifugal collection solid and decant liquid. Then this solid is dispersed among the 300ml THF, and uses heptane (700ml) to precipitate. By centrifugal collection solid, and decant liquid. Then solid is dried in a vacuum drying oven overnight. Then the dry material is dispersed among the PGMEA with 50 % by weight loading, then filters.
[0328] Example 4: Formation of a ZrO2 shell on TiO2 to produce TiO2-ZrO2 nanocrystals
[0329] The TiO2 from Example 1, collected as a wet cake, was dispersed in acetone and homogenized using zirconium oxide beads. The homogenized TiO2 was separated from the reaction mixture by centrifugation at 4500 rpm for 10 minutes. The supernatant was decanted, and the nanocrystals settled as a wet cake at the bottom of the centrifuge bottle. This process was repeated. The resulting wet cake (wet solid) was then dispersed in water using zirconium oxide beads until a homogeneous mixture was obtained. The TiO2 was again collected by centrifugation at 4500 rpm for 10 minutes. The supernatant was decanted, and the nanocrystals settled as a wet cake at the bottom of the centrifuge bottle. This process was repeated once more. The purified TiO2 wet cake was then transferred to a three-necked flask, and water was added to the wet cake (water to TiO2 wet cake weight ratio of 10:1). The mixture was stirred until homogenized. ZrOCl2.8H2O (30% by weight relative to the TiO2 wet cake) was then added to the reaction mixture. The reaction mixture was then heated at 90°C for 24 hours. After cooling to room temperature, the reaction mixture obtained after the ZrO2 shell formation process was a transparent dispersion in water.
[0330] Example 5: End-capping of TiO2-ZrO2 core-shell nanocrystals
[0331] The TiO2-ZrO2 core-shell nanocrystals from Example 4 were purified by precipitation using THF at a reaction mixture to THF weight ratio of 1:4. The resulting milky white suspension was centrifuged at 4500 rpm for 10 minutes. The supernatant was decanted, and the nanocrystals settled as a wet cake at the bottom of a centrifuge bottle. The wet cake was redispersed in water at a wet cake to water weight ratio of 1:1 and precipitated with THF at a nanocrystal dispersion to THF weight ratio of 1:4. The resulting milky white suspension was centrifuged at 4500 rpm for 10 minutes, and the supernatant was decanted. The collected wet cake was redispersed in water, reprecipitated in THF, and centrifuged to collect the purified wet cake. The wet cake was dispersed in ethanol at a wet cake to water weight ratio of 1:1 and precipitated with acetone at a nanocrystal dispersion to acetone weight ratio of 1:4. The nanocrystal dispersion was centrifuged at 4500 rpm for 10 minutes. The supernatant was decanted and the wet cake was collected at the bottom of the bottle. This dispersion, precipitation and centrifugation process was repeated two more times.
[0332] After the final centrifugation and decantation steps, the resulting wet cake was transferred to a 1.0 L round-bottom flask with the aid of PGMEA to prepare a final suspension of 25 wt % wet cake in PGMEA. The mixture was stirred at room temperature for 15 min to obtain a homogeneous suspension. Methoxy(trivinyloxy)propyltrimethoxysilane was then added to the reaction flask at 17 wt % of silane relative to the wet cake. The mixture was then stirred at room temperature for 15 min. A solution of ammonium hydroxide in water (28-30%) was carefully added to the reaction mixture in the flask at 15 wt % of alkali relative to the wet cake. The mixture was heated to 120° C. for 100 min. When the reaction was complete, the mixture had a translucent appearance.
[0333] The reaction mixture is then cooled to room temperature and washed to remove excess end-capping agent and impurities. The reaction mixture is precipitated in an antisolvent such as heptane at a weight ratio of heptane to the reaction mixture of 4:1. The suspension is centrifuged at 4500 rpm for 10 min. The resulting supernatant is decanted and discarded. The resulting solid is then dispersed in THF at a weight ratio of THF to the wet cake of 2:1. The dispersed solid is again precipitated in an antisolvent such as heptane at a weight ratio of heptane to the reaction mixture of 4:1. The suspension is centrifuged at 4500 rpm for 10 min. The resulting supernatant is decanted and discarded. The resulting solid is again dispersed in THF at a weight ratio of THF to the wet cake of 2:1. The dispersed solid is again precipitated in an antisolvent such as heptane at a weight ratio of heptane to the reaction mixture of 4:1. The precipitate is centrifuged at 4500 rpm for 10 min. The resulting supernatant is decanted and discarded. The solid is then placed in a vacuum oven to dry overnight.
[0334] The dried solids were redispersed in PGMEA at a solids to solvent weight ratio of 1 : 1 to produce a 50 wt% loaded dispersion.The resulting dispersion was filtered through a 0.45 micron absolute filter and then through a 0.2 micron absolute filter.
[0335] DLS of 5 wt % capped titanium oxide nanocrystals with ZrO 2 shells dispersed in PGMEA showed average particle sizes of 34.30 nm (by intensity) and 25.67 nm (by volume) with a narrow size distribution showing a D9999 of 84.3.
[0336] Example 6: TiO 2- ZrO2 core-shell nanocrystals were capped and then treated with an inorganic passivating agent
[0337] The TiO2-ZrO2 core-shell nanocrystals from Example 4 were purified by precipitation using THF at a reaction mixture to THF weight ratio of 1:4. The resulting milky white suspension was centrifuged at 4500 rpm for 10 minutes. The supernatant was decanted, and the nanocrystals settled as a wet cake at the bottom of a centrifuge bottle. The wet cake was redispersed in water at a wet cake to water weight ratio of 1:1 and precipitated using THF at a nanocrystal dispersion to THF weight ratio of 1:4. The resulting milky white suspension was centrifuged at 4500 rpm for 10 minutes, and the supernatant was decanted. The collected wet cake was redispersed in water, reprecipitated in THF, and centrifuged to collect the purified wet cake. The wet cake was dispersed in ethanol at a wet cake to water weight ratio of 1:1 and precipitated using acetone at a nanocrystal dispersion to acetone weight ratio of 1:4. The nanocrystal dispersion was centrifuged at 4500 rpm for 10 minutes. The supernatant was decanted and the wet cake was collected at the bottom of the bottle. This dispersion, precipitation and centrifugation process was repeated two more times.
[0338] After the final centrifugation and decantation steps, the resulting wet cake was transferred to a 1.0 L round-bottom flask with the aid of ethanol to prepare a final suspension of 25% by weight of wet cake in ethanol. The mixture was stirred at room temperature for 15 minutes to obtain a homogeneous suspension. Methoxy(trivinyloxy)propyltrimethoxysilane was then added to the reaction flask at a silane content of 30% by weight relative to the wet cake. The mixture was then stirred at room temperature for 15 minutes. A solution of ammonium hydroxide in water (28-30%) was carefully added to the reaction mixture in the flask at a base content of 30% by weight relative to the wet cake. The mixture was heated to 70° C. for 30 minutes. After a 30-minute hold time, 3% by weight of sodium hypophosphite monohydrate powder relative to the weight of the wet cake was weighed and slowly added to the reaction mixture. The mixture was heated at 70° C. for another 30 minutes. When the reaction was complete, the mixture had a translucent appearance.
[0339] The reaction mixture is then cooled to room temperature and washed to remove excess end-capping agent and impurities. The reaction mixture is diluted in THF at a ratio of 1:2 between the reaction mixture and THF, and precipitated in an antisolvent such as heptane at a weight ratio of heptane to the reaction mixture and THF of 4:1. The suspension is centrifuged at 4500 rpm for 10 min. The resulting supernatant is decanted and discarded. The resulting solid is then dispersed in THF at a weight ratio of 2:1 between ethanol and the wet cake. The dispersed solid is again precipitated in an antisolvent such as heptane at a weight ratio of 4:1 between heptane and the reaction mixture. The suspension is centrifuged at 4500 rpm for 10 min. The resulting supernatant is decanted and discarded. The resulting solid is again dispersed in ethanol at a weight ratio of 2:1 between ethanol and the wet cake. The dispersed solid is again precipitated in an antisolvent such as heptane at a weight ratio of 4:1 between heptane and the reaction mixture. The precipitate is centrifuged at 4500 rpm for 10 min. The resulting supernatant is decanted and discarded. The solid was then placed in a vacuum oven to dry overnight.
[0340] The dried solids were redispersed in PGMEA at a solids to solvent weight ratio of 1 : 1 to produce a 50 wt% loaded dispersion.The resulting dispersion was filtered through a 0.45 micron absolute filter and then through a 0.2 micron absolute filter.
[0341] exist Figure 1 A DLS profile of capped titanium oxide nanocrystals with a ZrO2 shell dispersed at 5 wt% in PGMEA is shown in FIG. The figure shows a DLS profile of intensity versus particle size as a measure, showing an average particle size of 37.15 nm with a narrow size distribution.
[0342] exist Figure 2 Figure 2 shows a DLS profile of capped titanium oxide nanocrystals with a ZrO2 shell dispersed at 5 wt% in PGMEA. This figure, which shows the volume versus particle size as a measure of the DLS profile, shows an average particle size of 25.46 nm with a narrow size distribution. The D9999 of this dispersion is 91.1.
[0343] High-resolution TEM images of Ti and Zr with elemental mapping are shown in Figure 3 The figure shows two images of the same particle.
[0344] Example 7: Inorganic surface passivation of TiO2-ZrO2 core-shell nanocrystals before capping
[0345] The TiO2-ZrO2 core-shell nanocrystals from Example 4 were purified by precipitation using THF at a reaction mixture to THF weight ratio of 1:4. The resulting milky white suspension was centrifuged at 4500 rpm for 10 minutes. The supernatant was decanted, and the nanocrystals settled as a wet cake at the bottom of a centrifuge bottle. The wet cake was redispersed in water at a wet cake to water weight ratio of 1:1 and precipitated with THF at a nanocrystal dispersion to THF weight ratio of 1:4. The resulting milky white suspension was centrifuged at 4500 rpm for 10 minutes, and the supernatant was decanted. The collected wet cake was redispersed in water, reprecipitated in THF, and centrifuged to collect the purified white wet cake. The wet cake was redispersed in ethanol at a wet cake to water weight ratio of 1:1 and precipitated with acetone at a nanocrystal dispersion to acetone weight ratio of 1:4. The nanocrystal dispersion was centrifuged at 4500 rpm for 10 minutes. The supernatant was decanted and the wet cake was collected at the bottom of the bottle. The process of dispersion, sedimentation and centrifugation was repeated two more times.
[0346] After the final centrifugation and decantation steps, the resulting wet cake was redispersed in 50% by weight ethanol and stirred at room temperature for 15 minutes to homogenize the solids in the solvent. Sodium hypophosphite monohydrate powder was carefully added to the nanocrystal suspension at 3% by weight relative to the weight of the wet cake. The mixture was stirred at room temperature for 12 hours. After the desired duration, the solid portion was separated from the liquid by centrifugation at 4500 rpm for 10 minutes. The resulting supernatant was decanted, leaving a white, wet, solid cake at the bottom of the centrifuge bottle. The wet cake was then rinsed with ethanol at a solvent to wet cake weight ratio of 2.75:1 and then vigorously stirred. The suspension was then centrifuged again at 4500 rpm for 10 minutes, and the resulting supernatant was decanted from the top. This rinsing step was repeated twice. At the end of the rinsing step, a white, wet, solid cake was obtained.
[0347] The wet cake was then transferred to a 1.0 L round-bottom flask with the aid of ethanol to prepare a final suspension of 25% by weight of the wet cake in ethanol. The mixture was stirred at room temperature for 15 minutes to obtain a homogeneous suspension. Methoxy(trivinyloxy)propyltrimethoxysilane was then added to the reaction flask at a silane content of 30% by weight relative to the wet cake. The mixture was then stirred at room temperature for 15 minutes. A solution of ammonium hydroxide in water (28-30%) was carefully added to the reaction mixture in the flask at a base content of 30% by weight relative to the wet cake. The mixture was heated to 70° C. for 45 minutes. When the reaction was complete, the mixture had a translucent appearance.
[0348] The reaction mixture is then cooled to room temperature and washed to remove excess end-capping agent and impurities. The reaction mixture is diluted in THF at a ratio of 1:2 between the reaction mixture and THF, and precipitated in an antisolvent such as heptane at a weight ratio of heptane to the reaction mixture and THF of 4:1. The suspension is centrifuged at 4500 rpm for 10 min. The resulting supernatant is decanted and discarded. The resulting solid is then dispersed in THF at a weight ratio of 2:1 between ethanol and the wet cake. The dispersed solid is again precipitated in an antisolvent such as heptane at a weight ratio of 4:1 between heptane and the reaction mixture. The suspension is centrifuged at 4500 rpm for 10 min. The resulting supernatant is decanted and discarded. The resulting solid is again dispersed in ethanol at a weight ratio of 2:1 between ethanol and the wet cake. The dispersed solid is again precipitated in an antisolvent such as heptane at a weight ratio of 4:1 between heptane and the reaction mixture. The precipitate is centrifuged at 4500 rpm for 10 min. The resulting supernatant is decanted and discarded. The solid was then placed in a vacuum oven to dry overnight.
[0349] The dried solids were redispersed in PGMEA at a solids to solvent weight ratio of 1 : 1 to produce a 50 wt% loaded dispersion.The resulting dispersion was filtered through a 0.45 micron absolute filter and then through a 0.2 micron absolute filter.
[0350] DLS of 5 wt% dispersed titanium oxide nanocrystals with ZrO2 shells in PGMEA showed an average particle size of 41.37 nm relative to particle size by intensity and 26.47 nm relative to particle size by volume, respectively, with a narrow size distribution. The D9999 of this dispersion was 102.
[0351] Example 8: Capping TiO2-ZrO2 core-shell nanocrystals that were first inorganically surface passivated and then additionally treated with an inorganic agent;
[0352] The TiO2-ZrO2 core-shell nanocrystals from Example 4 were purified by precipitation using THF at a reaction mixture to THF weight ratio of 1:4. The resulting milky white suspension was centrifuged at 4500 rpm for 10 minutes. The supernatant was decanted, and the nanocrystals settled as a wet cake at the bottom of a centrifuge bottle. The wet cake was redispersed in water at a wet cake to water weight ratio of 1:1 and precipitated with THF at a nanocrystal dispersion to THF weight ratio of 1:4. The resulting milky white suspension was centrifuged at 4500 rpm for 10 minutes, and the supernatant was decanted. The collected wet cake was redispersed in water, reprecipitated in THF, and centrifuged to collect the purified white wet cake. The wet cake was redispersed in ethanol at a wet cake to water weight ratio of 1:1 and precipitated with acetone at a nanocrystal dispersion to acetone weight ratio of 1:4. The nanocrystal dispersion was centrifuged at 4500 rpm for 10 minutes. The supernatant was decanted and the wet cake was collected at the bottom of the bottle. The process of dispersion, sedimentation and centrifugation was repeated two more times.
[0353] After the final centrifugation and decantation steps, the resulting wet cake was redispersed in 50% by weight ethanol and stirred at room temperature for 15 minutes to homogenize the solids in the solvent. Sodium hypophosphite monohydrate powder was carefully added to the nanocrystal suspension at 3% by weight relative to the weight of the wet cake. The mixture was stirred at room temperature for 12 hours. After the desired duration, the solid portion was separated from the liquid by centrifugation at 4500 rpm for 10 minutes. The resulting supernatant was decanted, leaving a white, wet, solid cake at the bottom of the centrifuge bottle. The wet cake was then rinsed with ethanol at a solvent to wet cake weight ratio of 2.75:1 and then vigorously stirred. The suspension was then centrifuged again at 4500 rpm for 10 minutes, and the resulting supernatant was decanted from the top. This rinsing step was repeated twice. At the end of the rinsing step, a white, wet, solid cake was obtained.
[0354] The wet cake was then transferred to a 1.0 L round-bottom flask with the aid of ethanol to prepare a final suspension of 25% wet cake in ethanol. The mixture was stirred at room temperature for 15 minutes to obtain a homogeneous suspension. Methoxy(trivinyloxy)propyltrimethoxysilane was then added to the reaction flask at a ratio of 30% by weight of silane relative to the wet cake. The mixture was then stirred at room temperature for 15 minutes. A solution of ammonium hydroxide in water (28-30%) was carefully added to the reaction mixture in the flask at a ratio of 30% by weight of base relative to the wet cake. The mixture was heated to 70°C for 45 minutes. At the end of the 30-minute hold time, sodium hypophosphite monohydrate powder was carefully added to the nanocrystal suspension at a ratio of 3% by weight relative to the weight of the wet cake. The reaction mixture was held at 70°C for an additional 30 minutes. When the reaction was complete, the mixture had a translucent appearance.
[0355] The reaction mixture is then cooled to room temperature and washed to remove excess end-capping agent and impurities. The reaction mixture is diluted in THF at a ratio of 1:2 between the reaction mixture and THF, and precipitated in an antisolvent such as heptane at a weight ratio of heptane to the reaction mixture and THF of 4:1. The suspension is centrifuged at 4500 rpm for 10 min. The resulting supernatant is decanted and discarded. The resulting solid is then dispersed in THF at a weight ratio of 2:1 between ethanol and the wet cake. The dispersed solid is again precipitated in an antisolvent such as heptane at a weight ratio of 4:1 between heptane and the reaction mixture. The suspension is centrifuged at 4500 rpm for 10 min. The resulting supernatant is decanted and discarded. The resulting solid is again dispersed in ethanol at a weight ratio of 2:1 between ethanol and the wet cake. The dispersed solid is again precipitated in an antisolvent such as heptane at a weight ratio of 4:1 between heptane and the reaction mixture. The precipitate is centrifuged at 4500 rpm for 10 min. The resulting supernatant is decanted and discarded. The solid was then placed in a vacuum oven to dry overnight.
[0356] The dried solids were redispersed in PGMEA at a solids to solvent weight ratio of 1 : 1 to produce a 50 wt% loaded dispersion.The resulting dispersion was filtered through a 0.45 micron absolute filter and then through a 0.2 micron absolute filter.
[0357] Example 9: Inorganic treatment of TiO2 prior to ZrO2 shell coating followed by end-capping
[0358] The TiO nanocrystals from Example 1 were redispersed in 50% by weight ethanol and stirred at room temperature for 15 minutes to homogenize the solids in the solvent. Sodium hypophosphite monohydrate powder was carefully added to the nanocrystal suspension at 3% by weight relative to the weight of the wet cake. The mixture was stirred at room temperature for 12 hours. After the desired duration, the solid portion was separated from the liquid by centrifugation at 4500 rpm for 10 minutes. The resulting supernatant was decanted, leaving a white, wet, solid cake at the bottom of the centrifuge bottle. The wet cake was then rinsed with ethanol at a weight ratio of 2.75:1 to the wet cake, and then stirred vigorously. The suspension was then centrifuged again at 4500 rpm for 10 minutes, and the resulting supernatant was decanted from the top. This rinsing step was repeated twice. At the end of the rinsing step, a white, wet, solid cake was obtained.
[0359] The wet cake was then dispersed in water at a weight ratio of 10:1 water to TiO wet cake. The mixture was stirred until homogeneous. ZrOCl2.8H2O was added to the reaction mixture (30% by weight relative to the TiO wet cake). The reaction mixture was then heated at 90°C for 24 hours. After cooling to room temperature, the resulting reaction mixture, following the ZrO2 shell formation process, was a transparent dispersion in water.
[0360] The TiO2-ZrO2 nanocrystals from the example were purified by precipitation using THF in a reaction mixture at a weight ratio of 1:4 relative to THF. The resulting milky white suspension was centrifuged at 4500 rpm for 10 minutes. The supernatant was decanted, and the nanocrystals settled as a wet cake at the bottom of a centrifuge bottle. The wet cake was redispersed in water at a weight ratio of 1:1 between the wet cake and water, and precipitated with THF at a weight ratio of 1:4 between the nanocrystal dispersion and THF. The resulting milky white suspension was centrifuged at 4500 rpm for 10 minutes, and the supernatant was decanted. The collected wet cake was redispersed in water, reprecipitated in THF, and centrifuged to collect the purified wet cake. The wet cake was dispersed in ethanol at a weight ratio of 1:1 between the wet cake and water, and precipitated with acetone at a weight ratio of 1:4 between the nanocrystal dispersion and acetone. The nanocrystal dispersion was centrifuged at 4500 rpm for 10 minutes. The supernatant was decanted, and the wet cake was collected at the bottom of the bottle. This dispersion, precipitation and centrifugation process was repeated two more times.
[0361] After the final centrifugation and decantation steps, the resulting wet cake was transferred to a 1.0 L round-bottom flask with the aid of ethanol to prepare a final suspension of 25% by weight of wet cake in ethanol. The mixture was stirred at room temperature for 15 minutes to obtain a homogeneous suspension. Methoxy(trivinyloxy)propyltrimethoxysilane was then added to the reaction flask at a silane content of 30% by weight relative to the wet cake. The mixture was then stirred at room temperature for 15 minutes. A solution of ammonium hydroxide in water (28-30%) was carefully added to the reaction mixture in the flask at a base content of 30% by weight relative to the wet cake. The mixture was heated to 70° C. for 30 minutes. When the reaction was complete, the mixture had a translucent appearance.
[0362] The reaction mixture is then cooled to room temperature and washed to remove excess end-capping agent and impurities. The reaction mixture is diluted in THF at a ratio of 1:2 between the reaction mixture and THF, and precipitated in an antisolvent such as heptane at a weight ratio of heptane to the reaction mixture and THF of 4:1. The suspension is centrifuged at 4500 rpm for 10 min. The resulting supernatant is decanted and discarded. The resulting solid is then dispersed in THF at a weight ratio of 2:1 between ethanol and the wet cake. The dispersed solid is again precipitated in an antisolvent such as heptane at a weight ratio of 4:1 between heptane and the reaction mixture. The suspension is centrifuged at 4500 rpm for 10 min. The resulting supernatant is decanted and discarded. The resulting solid is again dispersed in ethanol at a weight ratio of 2:1 between ethanol and the wet cake. The dispersed solid is again precipitated in an antisolvent such as heptane at a weight ratio of 4:1 between heptane and the reaction mixture. The precipitate is centrifuged at 4500 rpm for 10 min. The resulting supernatant is decanted and discarded. The solid was then placed in a vacuum oven to dry overnight.
[0363] The dried solids were redispersed in PGMEA at a solids to solvent weight ratio of 1 : 1 to produce a 50 wt% loaded dispersion.The resulting dispersion was filtered through a 0.45 micron absolute filter and then through a 0.2 micron absolute filter.
[0364] Example 10: Inorganic treatment of TiO2 nanocrystals without metal oxide shells followed by end-capping
[0365] The TiO nanocrystals synthesized from Example 1 were redispersed in ethanol at 50% by weight and stirred at room temperature for 15 minutes to homogeneously distribute the solids in the solvent. Sodium hypophosphite monohydrate powder was carefully added to the nanocrystal suspension at 3% by weight relative to the weight of the wet cake. The mixture was stirred at room temperature for 12 hours. After the desired duration, the solid portion was separated from the liquid by centrifugation at 4500 rpm for 10 minutes. The resulting supernatant was decanted, leaving a white wet solid cake at the bottom of the centrifuge bottle. The wet cake was then rinsed with ethanol at a weight ratio of 2.75:1 to the wet cake, and then stirred vigorously. The suspension was then centrifuged at 4500 rpm for 10 minutes, and the resulting supernatant was decanted from the top. This rinsing step was repeated twice. At the end of the rinsing step, a white wet solid cake was obtained.
[0366] The wet cake was transferred to a 1.0 L round-bottom flask with the aid of ethanol to prepare a final suspension of 30% by weight of the wet cake in ethanol. The mixture was stirred at room temperature for 15 minutes to obtain a homogeneous suspension. Methoxy(trivinyloxy)propyltrimethoxysilane was then added to the reaction flask at a silane content of 30% by weight relative to the wet cake. The mixture was then stirred at room temperature for 15 minutes. A solution of ammonium hydroxide in water (28-30%) was carefully added to the reaction mixture in the flask at a base content of 30% by weight relative to the wet cake. The mixture was heated to 70° C. for 45 minutes. When the reaction was complete, the mixture had a translucent appearance.
[0367] The reaction mixture is then cooled to room temperature and washed to remove excess end-capping agent and impurities. The reaction mixture is diluted in THF at a ratio of 1:2 between the reaction mixture and THF, and precipitated in an antisolvent such as heptane at a weight ratio of heptane to the reaction mixture and THF of 4:1. The suspension is centrifuged at 4500 rpm for 10 minutes. The resulting supernatant is discarded. The resulting solid is then dispersed in THF at a weight ratio of 2:1 between ethanol and the wet cake. The dispersed solid is again precipitated in an antisolvent such as heptane at a weight ratio of 4:1 between heptane and the reaction mixture. The suspension is centrifuged at 4500 rpm for 10 minutes. The resulting supernatant is decanted and discarded. The resulting solid is again dispersed in ethanol at a weight ratio of 2:1 between ethanol and the wet cake. The dispersed solid is again precipitated in an antisolvent such as heptane at a weight ratio of 4:1 between heptane and the reaction mixture. The precipitate is centrifuged at 4500 rpm for 10 minutes. The resulting supernatant is decanted and discarded. The solid was then placed in a vacuum oven to dry overnight.
[0368] The dried solids were redispersed in PGME at a solids to solvent weight ratio of 1 : 1 to produce a 50 wt% loaded dispersion.The resulting dispersion was filtered through a 0.45 micron absolute filter and then through a 0.2 micron absolute filter.
[0369] Example 11: Capping of TiO2 Nanocrystals with ZrO2 Shells and Inorganic Surface Passivation
[0370] The TiO2 from Example 1, collected as a wet cake, was dispersed in acetone and homogenized with zirconium oxide beads. The homogenized TiO2 was separated from the reaction mixture by centrifugation at 4500 rpm for 10 minutes. The supernatant was decanted, and the nanocrystals settled as a wet cake at the bottom of the centrifuge bottle. The purified TiO2 wet cake was then transferred to a three-necked flask, and water was added to the wet cake (the weight ratio of TiO2 wet cake to water was 1:4). The mixture was stirred until it became homogenous. ZrOCl2.8H2O (30% by weight relative to the TiO2 wet cake) was then added to the reaction mixture. The reaction mixture was then heated at 90°C for 8 hours. After cooling to room temperature, the resulting reaction mixture, following the ZrO2 shell formation process, was a transparent dispersion in water.
[0371] Example 11A:
[0372] The resulting TiO2-ZrO2 core-shell nanocrystals were purified by precipitating the NCs from the mother liquor with acetone at a reaction mixture to acetone weight ratio of 1:4. The resulting milky white suspension was centrifuged at 4500 rpm for 10 minutes. The supernatant was decanted, and the nanocrystals settled as a wet cake at the bottom of the centrifuge bottle. The wet cake was redispersed in ethanol at a wet cake to ethanol weight ratio of 1:1 and precipitated with acetone at a nanocrystal dispersion to acetone weight ratio of 1:4. The resulting milky white suspension was centrifuged at 4500 rpm for 10 minutes, the supernatant was decanted, and the wet cake was collected.
[0373] The resulting wet cake was then transferred to a 1.0L round-bottom flask with the aid of ethanol to prepare a final suspension of 25% by weight of the wet cake in ethanol. The suspension was stirred at room temperature for 15 minutes to obtain a homogeneous distribution of the solid in the solvent. After the desired duration, methoxy(trivinyloxy)propyltrimethoxysilane was added to the reaction flask at a silane content of 30% by weight relative to the wet cake. The mixture was then stirred at room temperature for 30 minutes. A solution of ammonium hydroxide in water (28-30%) was carefully added to the reaction mixture in the flask at a base content of 30% by weight relative to the wet cake. The mixture was heated to 70°C for 45 minutes. At the end of the 45-minute hold time, sodium hypophosphite monohydrate powder was carefully added to the reaction mixture at a 3% by weight content relative to the weight of the wet cake and continued to be held at 70°C for another 30 minutes. When the reaction was complete, the mixture had a light-colored, milky appearance. The mixture was stirred at room temperature for 1 hour.
[0374] The reaction mixture is then cooled to room temperature and washed to remove excess end-capping agent and impurities. The reaction mixture is diluted in THF at a ratio of 1:2 between the reaction mixture and THF, and precipitated in an antisolvent such as heptane at a weight ratio of heptane to the reaction mixture and THF of 4:1. The suspension is centrifuged at 4500 rpm for 10 min. The resulting supernatant is decanted and discarded. The resulting solid is then dispersed in THF at a weight ratio of 2:1 between ethanol and the wet cake. The dispersed solid is again precipitated in an antisolvent such as heptane at a weight ratio of 4:1 between heptane and the reaction mixture. The suspension is centrifuged at 4500 rpm for 10 min. The resulting supernatant is decanted and discarded. The resulting solid is again dispersed in ethanol at a weight ratio of 2:1 between ethanol and the wet cake. The dispersed solid is again precipitated in an antisolvent such as heptane at a weight ratio of 4:1 between heptane and the reaction mixture. The precipitate is centrifuged at 4500 rpm for 10 min. The resulting supernatant is decanted and discarded. The solid was then placed in a vacuum oven to dry overnight.
[0375] The dried solid was redispersed in ETA (ethyl acetate) at a solid to solvent weight ratio of 1: 1 to produce a 50 wt% loaded dispersion. The resulting dispersion was filtered through a 0.45 micron absolute filter and then through a 0.2 micron absolute filter.
[0376] Capped titanium oxide nanocrystals with ZrO2 shells dispersed in ETA at 50 wt% had a % organic of 11.32.
[0377] Example 11B:
[0378] The resulting TiO2-ZrO2 core-shell nanocrystals were purified by precipitating the NCs from the mother liquor with acetone at a reaction mixture to acetone weight ratio of 1:4. The resulting milky white suspension was centrifuged at 4500 rpm for 10 minutes. The supernatant was decanted, and the nanocrystals settled as a wet cake at the bottom of the centrifuge bottle. The wet cake was redispersed in ethanol at a wet cake to ethanol weight ratio of 1:1 and precipitated with acetone at a nanocrystal dispersion to acetone weight ratio of 1:4. The resulting milky white suspension was centrifuged at 4500 rpm for 10 minutes, the supernatant was decanted, and the wet cake was collected.
[0379] After the final centrifugation and decantation steps, the resulting wet cake was then transferred to a 1.0 L round-bottom flask with the aid of ethanol to prepare a final suspension of 25 wt% wet cake in ethanol. This was stirred at room temperature for 15 minutes to achieve a homogeneous distribution of the solids in the solvent. Sodium hypophosphite monohydrate powder was carefully added to the nanocrystal suspension at 3 wt% relative to the weight of the wet cake. The mixture was stirred at room temperature for 1 hour. After the desired holding time, methoxy(trivinyloxy)propyltrimethoxysilane was added to the reaction flask at 30 wt% silane relative to the wet cake. The mixture was then stirred at room temperature for 30 minutes. A solution of ammonium hydroxide in water (28-30%) was carefully added to the reaction mixture in the flask at 15 wt% base relative to the wet cake. The mixture was heated to 70°C for 45 minutes. At the end of the 45-minute hold time, 3-(methacryloyloxy)propyltrimethoxysilane was carefully added to the nanocrystal suspension at 10 wt% relative to the weight of the wet cake. The reaction mixture was maintained at 70° C. for an additional 30 min. When the reaction was complete, the mixture had a light milky appearance.
[0380] The reaction mixture is then cooled to room temperature and washed to remove excess end-capping agent and impurities. The reaction mixture is diluted in THF at a ratio of 1:2 between the reaction mixture and THF, and precipitated in an antisolvent such as heptane at a weight ratio of heptane to the reaction mixture and THF of 4:1. The suspension is centrifuged at 4500 rpm for 10 min. The resulting supernatant is decanted and discarded. The resulting solid is then dispersed in ethanol at a weight ratio of 2:1 between ethanol and the wet cake. The dispersed solid is again precipitated in an antisolvent such as heptane at a weight ratio of 4:1 between heptane and the reaction mixture. The suspension is centrifuged at 4500 rpm for 10 min. The resulting supernatant is decanted and discarded. The resulting solid is again dispersed in ethanol at a weight ratio of 2:1 between ethanol and the wet cake. The dispersed solid is again precipitated in an antisolvent such as heptane at a weight ratio of 4:1 between heptane and the reaction mixture. The precipitate is centrifuged at 4500 rpm for 10 min. The resulting supernatant is decanted and discarded. The solid was then placed in a vacuum oven to dry overnight.
[0381] The dried solids were redispersed in PGMEA or ETA (ethyl acetate) at a solid to solvent weight ratio of 1: 1 to produce a 50 wt% loaded dispersion. The resulting dispersion was filtered through a 0.45 micron absolute filter and then through a 0.2 micron absolute filter.
[0382] The capped titanium oxide nanocrystals with ZrO2 shells dispersed in ETA at 50 wt% had % organics of 9.93 and 9.55, respectively.
[0383] DLS of 5 wt% dispersed titanium oxide nanocrystals capped with a ZrO2 shell in ETA showed an average particle size of 33.850 nm relative to particle intensity and 24.42 nm relative to particle size by volume, with a narrow size distribution. The D9999 of this dispersion was 85.5.
[0384] Example 11C:
[0385] The resulting TiO2-ZrO2 core-shell nanocrystals were purified by precipitating the NCs from the mother liquor with acetone at a reaction mixture to acetone weight ratio of 1:4. The resulting milky white suspension was centrifuged at 4500 rpm for 10 minutes. The supernatant was decanted, and the nanocrystals settled as a wet cake at the bottom of the centrifuge bottle. The wet cake was redispersed in ethanol at a wet cake to ethanol weight ratio of 1:1 and precipitated with acetone at a nanocrystal dispersion to acetone weight ratio of 1:4. The resulting milky white suspension was centrifuged at 4500 rpm for 10 minutes, the supernatant was decanted, and the wet cake was collected.
[0386] The obtained wet cake was redispersed in PGMEA at a weight ratio of 1:4 between the wet cake and PGMEA. The obtained milky white suspension was centrifuged at 4500 rpm for 10 min, and the supernatant was decanted. The obtained wet cake was then transferred to a 1.0 L round-bottom flask with the aid of PGMEA to prepare a final suspension having a wet cake content of 25% by weight in PGMEA. It was stirred at room temperature for 15 min to obtain a homogeneous distribution of the solid in the solvent. After the desired duration, methoxy(triethyleneoxy)propyltrimethoxysilane was added to the reaction flask at a silane content of 17% by weight relative to the wet cake. The mixture was then stirred at room temperature for 30 min. A solution of ammonium hydroxide in water (28-30%) was carefully added to the reaction mixture in the flask at a base content of 15% by weight relative to the wet cake. The mixture was heated to 100° C. for 45 min. At the end of the 45-minute hold time, 3-(methacryloyloxy)propyltrimethoxysilane was carefully added to the nanocrystal suspension at 30% by weight relative to the weight of the wet cake. The reaction mixture was held at 100° C. for an additional 30 minutes. Thereafter, sodium hypophosphite monohydrate powder was carefully added to the reaction mixture at 1% by weight relative to the weight of the wet cake, and the temperature was maintained at 70° C. for an additional 30 minutes. When the reaction was complete, the mixture had a light, milky appearance.
[0387] The reaction mixture is then cooled to room temperature and washed to remove excess end-capping agent and impurities. The reaction mixture is diluted in THF at a ratio of 1:2 between the reaction mixture and THF, and precipitated in an antisolvent such as heptane at a weight ratio of heptane to the reaction mixture and THF of 4:1. The suspension is centrifuged at 4500 rpm for 10 min. The resulting supernatant is decanted and discarded. The resulting solid is then dispersed in ethanol at a weight ratio of 2:1 between ethanol and the wet cake. The dispersed solid is again precipitated in an antisolvent such as heptane at a weight ratio of 4:1 between heptane and the reaction mixture. The suspension is centrifuged at 4500 rpm for 10 min. The resulting supernatant is decanted and discarded. The resulting solid is again dispersed in ethanol at a weight ratio of 2:1 between ethanol and the wet cake. The dispersed solid is again precipitated in an antisolvent such as heptane at a weight ratio of 4:1 between heptane and the reaction mixture. The precipitate is centrifuged at 4500 rpm for 10 min. The resulting supernatant is decanted and discarded. The solid was then placed in a vacuum oven to dry overnight.
[0388] The dried solids were redispersed in PGMEA or ETA (ethyl acetate) at a solid to solvent weight ratio of 1: 1 to produce a 50 wt% loaded dispersion. The resulting dispersion was filtered through a 0.45 micron absolute filter and then through a 0.2 micron absolute filter.
[0389] Capped titanium oxide nanocrystals with ZrO2 shells dispersed in ETA at 50 wt% had a % organic of 13.99.
[0390] DLS of 5 wt% dispersed titanium oxide nanocrystals capped with a ZrO2 shell in ETA showed an average particle size of 29.81 nm relative to particle size by intensity and 15.11 nm relative to particle size by volume, with a narrow size distribution. The D9999 of this dispersion was 88.5.
[0391] Example 11D:
[0392] The resulting TiO2-ZrO2 core-shell nanocrystals were purified by precipitating the NCs from the mother liquor with acetone at a reaction mixture to acetone weight ratio of 1:4. The resulting milky white suspension was centrifuged at 4500 rpm for 10 minutes. The supernatant was decanted, and the nanocrystals settled as a wet cake at the bottom of the centrifuge bottle. The wet cake was redispersed in water at a wet cake to water weight ratio of 1:1 and precipitated with acetone at a nanocrystal dispersion to acetone weight ratio of 1:4. The resulting milky white suspension was centrifuged at 4500 rpm for 10 minutes, the supernatant was decanted, and the wet cake was collected.
[0393] After the final centrifugation and decantation steps, the resulting wet cake was then transferred to a 1.0 L round-bottom flask with the aid of water to prepare a final suspension of 15 wt% wet cake in water. This was stirred at room temperature for 15 minutes to achieve a homogeneous distribution of the solids in the solvent. Sodium hypophosphite monohydrate powder was carefully added to the nanocrystal suspension at 3 wt% relative to the weight of the wet cake. The mixture was stirred at room temperature for 1 hour. After the desired holding time, methoxy(trivinyloxy)propyltrimethoxysilane was added to the reaction flask at 30 wt% silane relative to the wet cake. The mixture was then stirred at room temperature for 30 minutes. A solution of ammonium hydroxide in water (28-30%) was carefully added to the reaction mixture in the flask at 15 wt% base relative to the wet cake. The mixture was heated to 95°C for 45 minutes. At the end of the 45-minute hold time, 3-(methacryloyloxy)propyltrimethoxysilane was carefully added to the nanocrystal suspension at 10 wt% relative to the weight of the wet cake. The reaction mixture was maintained at 95° C. for an additional 30 min. When the reaction was complete, the mixture had a light milky appearance.
[0394] The reaction mixture is then cooled to room temperature to obtain a slurry of white precipitate suspended in the reaction solvent. The solid white precipitate is collected by centrifugation at 3000 rpm for 10 min. The obtained solid is then dispersed in THF with a weight ratio of THF to wet cake of 2:1. The dispersed solid is again precipitated in an anti-solvent such as heptane at a weight ratio of heptane to reaction mixture of 4:1. The suspension is centrifuged at 4500 rpm for 10 min. The obtained supernatant is decanted and discarded. The obtained solid is again dispersed in ethanol with a weight ratio of ethanol to wet cake of 2:1. The dispersed solid is again precipitated in an anti-solvent such as heptane at a weight ratio of heptane to reaction mixture of 4:1. The precipitate is centrifuged at 4500 rpm for 10 min. The obtained supernatant is decanted and discarded. The solid is then placed in a vacuum oven to dry overnight.
[0395] The dried solids were redispersed in PGMEA or ETA (ethyl acetate) at a solid to solvent weight ratio of 1: 1 to produce a 50 wt% loaded dispersion. The resulting dispersion was filtered through a 0.45 micron absolute filter and then through a 0.2 micron absolute filter.
[0396] Capped titanium oxide nanocrystals with ZrO2 shells dispersed in ETA at 50 wt% had a % organic of 11.42%.
[0397] The DLS of the capped titanium oxide nanocrystals with ZrO2 shells dispersed in ETA at 5 wt% showed an average particle size of 43.23 nm relative to the particle size by intensity and 29.21 nm relative to the particle size by volume, with a narrow size distribution.
[0398] Example 12:
[0399] The TiO2 from Example 1, collected as a wet cake, was dispersed in acetone and homogenized with zirconium oxide beads. The homogenized TiO2 was separated from the reaction mixture by centrifugation at 4500 rpm for 10 minutes. The supernatant was decanted, and the nanocrystals settled as a wet cake at the bottom of the centrifuge bottle. The purified TiO2 wet cake was then transferred to a three-necked flask, and water was added to the wet cake (the weight ratio of TiO2 wet cake to water was 1:4). The mixture was stirred until homogenized. ZrOCl2.8H2O was then added to the reaction mixture (17% by weight relative to the TiO2 wet cake), followed by CeCl3.7H2O (cerium(III) chloride heptahydrate) or Ce2CO3)3.xH2O (cerium(III) carbonate hydrate) at 3% by weight relative to the TiO2 wet cake. The reaction mixture was then heated at 90°C for 24 hours. After cooling to room temperature, the reaction mixture obtained after the ZrO2 shell formation process was a transparent dispersion in water.
[0400] The pH of the resulting dispersion was 1 and was neutralized to pH 4 using aqueous ammonium hydroxide solution (5N). The ammonium hydroxide solution was slowly added to the reaction mixture while stirring. The pH change of the mixture was monitored using a pH meter. Once the pH reached 4, the NC was collected from the reaction mixture using a centrifuge. The NC from the mother liquor was treated with acetone at a weight ratio of 1:4 between the reaction mixture and acetone. The resulting milky white suspension was centrifuged at 4500 rpm for 10 min. The supernatant was decanted and the nanocrystals settled as a wet cake at the bottom of the centrifuge bottle. The wet cake was redispersed in ethanol at a weight ratio of 1:1 between the wet cake and ethanol and precipitated with acetone at a weight ratio of 1:4 between the nanocrystal dispersion and acetone. The resulting milky white suspension was centrifuged at 4500 rpm for 10 min and the supernatant was decanted.
[0401] After the final centrifugation and decantation steps, the resulting wet cake was redispersed in ethanol at 15% by weight and stirred at room temperature for 15 minutes to obtain a homogeneous distribution of the solids in the solvent. Sodium hypophosphite monohydrate powder was carefully added to the nanocrystal suspension at 3% by weight relative to the weight of the wet cake. The mixture was stirred at room temperature for 12 hours. After the desired duration, the solid portion was separated from the liquid by centrifugation at 4500 rpm for 10 minutes. The resulting supernatant was decanted, leaving a white, wet, solid cake at the bottom of the centrifuge bottle. The wet cake was then rinsed with ethanol at a solvent to wet cake weight ratio of 2.75:1 and then vigorously stirred. The suspension was then centrifuged again at 4500 rpm for 10 minutes, and the resulting supernatant was decanted from the top. The resulting wet cake was capped according to the procedures described in Examples 12A and 12B.
[0402] Example 12A:
[0403] The wet cake from Example 12 was then transferred to a 1.0 L round-bottom flask with the aid of ethanol to prepare a final suspension of 25% by weight of the wet cake in ethanol. The mixture was stirred at room temperature for 15 minutes to obtain a homogeneous suspension. Methoxy(trivinyloxy)propyltrimethoxysilane was then added to the reaction flask at a silane content of 30% by weight relative to the wet cake. The mixture was then stirred at room temperature for 15 minutes. Aqueous ammonium hydroxide solution (28-30%) was carefully added to the reaction mixture in the flask at a base content of 30% by weight relative to the wet cake. The mixture was heated to 70° C. for 45 minutes. When the reaction was complete, the mixture had a translucent appearance.
[0404] The reaction mixture is then cooled to room temperature and washed to remove excess end-capping agent and impurities. The reaction mixture is diluted in THF at a ratio of 1:2 between the reaction mixture and THF, and precipitated in an antisolvent such as heptane at a weight ratio of heptane to the reaction mixture and THF of 4:1. The suspension is centrifuged at 4500 rpm for 10 min. The resulting supernatant is decanted and discarded. The resulting solid is then dispersed in THF at a weight ratio of 2:1 between ethanol and the wet cake. The dispersed solid is again precipitated in an antisolvent such as heptane at a weight ratio of 4:1 between heptane and the reaction mixture and THF. The suspension is centrifuged at 4500 rpm for 10 min. The resulting supernatant is decanted and discarded. The resulting solid is again dispersed in ethanol at a weight ratio of 2:1 between ethanol and the wet cake. The dispersed solid is again precipitated in an antisolvent such as heptane at a weight ratio of 4:1 between heptane and the reaction mixture and THF. The precipitate is centrifuged at 4500 rpm for 10 min. The resulting supernatant is decanted and discarded. The solid was then placed in a vacuum oven to dry overnight.
[0405] The dried solids were redispersed in PGMEA at a solids to solvent weight ratio of 1 : 1 to produce a 50 wt% loaded dispersion.The resulting dispersion was filtered through a 0.45 micron absolute filter and then through a 0.2 micron absolute filter.
[0406] Capped titanium oxide nanocrystals with ZrO2 shells dispersed in PGMEA at 50 wt% had a % organic of 8.97.
[0407] The DLS pattern of the capped titanium oxide nanocrystals with ZrO2 shells dispersed in PGMEA at 5 wt% showed an average particle size of 53.85 nm and 36.15 nm relative to the particle size by intensity, with a narrow size distribution. The D9999 of this dispersion was 141.0.
[0408] Example 12B:
[0409] The wet cake from Example 12 was then transferred to a 1.0 L round-bottom flask with the aid of ethanol to prepare a final suspension of 25% wet cake by weight in ethanol. The mixture was stirred at room temperature for 15 minutes to obtain a homogeneous suspension. After the desired holding time, methoxy(trivinyloxy)propyltrimethoxysilane was then added to the reaction flask at a ratio of 30% by weight of silane relative to the wet cake. The mixture was then stirred at room temperature for 30 minutes. A solution of ammonium hydroxide in water (28-30%) was carefully added to the reaction mixture in the flask at a ratio of 15% by weight of base relative to the wet cake. The mixture was heated to 70°C for 45 minutes. At the end of the 30-minute hold time, 3-(methacryloyloxy)propyltrimethoxysilane was carefully added to the nanocrystal suspension at a ratio of 5% by weight relative to the weight of the wet cake. The reaction mixture was held at 70°C for an additional 30 minutes. When the reaction was complete, the mixture had a light, milky appearance.
[0410] The reaction mixture is then cooled to room temperature and washed to remove excess end-capping agent and impurities. The reaction mixture is diluted in THF at a ratio of 1:2 between the reaction mixture and THF, and precipitated in an antisolvent such as heptane at a weight ratio of heptane to the reaction mixture and THF of 4:1. The suspension is centrifuged at 4500 rpm for 10 min. The resulting supernatant is decanted and discarded. The resulting solid is then dispersed in THF at a weight ratio of 2:1 between ethanol and the wet cake. The dispersed solid is again precipitated in an antisolvent such as heptane at a weight ratio of 4:1 between heptane and the reaction mixture. The suspension is centrifuged at 4500 rpm for 10 min. The resulting supernatant is decanted and discarded. The resulting solid is again dispersed in ethanol at a weight ratio of 2:1 between ethanol and the wet cake. The dispersed solid is again precipitated in an antisolvent such as heptane at a weight ratio of 4:1 between heptane and the reaction mixture. The precipitate is centrifuged at 4500 rpm for 10 min. The resulting supernatant is decanted and discarded. The solid was then placed in a vacuum oven to dry overnight.
[0411] The dried solids were redispersed in PGMEA at a solid to solvent weight ratio of 1:1 to produce a 50 wt% loaded dispersion. The resulting dispersion was filtered through a 0.45 micron absolute filter and then through a 0.2 micron absolute filter. The capped titanium oxide nanocrystals with ZrO2 shells dispersed in PGMEA at 50 wt% had a % organic matter of 10.03.
[0412] Example 13: Formation of SiO2 Shell on Capped TiO2
[0413] Use acoustic mixer to disperse previously blocked TiO powder (51g) in ethanol (1400g). After it is allowed to stand overnight, blocked TiO is resuspended and transferred to a 2-gallon reactor. Then close and seal the reactor. The stirring in the reactor is set to 150-200RPM. Pressure check is performed on the reactor, where it is maintained at 10PSIG for 10min and then vented to 2PSIG. Ammonia (224g) is added to 1900g water and then transferred to the reactor. The pipeline is then rinsed with 470g water. 69g of ethyl orthosilicate is added to the reactor, followed by the addition of 100g of ethanol. The reactor is inertized (repeated 10 times) by pressurizing with N and then venting to 2Psig. Then the stir speed is increased to 600rpm, and the temperature is raised to 200°C. After keeping at 200°C for 3h, the reactor is cooled to room temperature. The reactor is then vented and the material is discharged into a container. A white slurry is obtained.
[0414] Example 14: Formation of SiO2 Shell on TiO2
[0415] The TiO2 wet cake from Example 1 was rinsed with ethanol by mixing ethanol with the wet cake in a 1:1 ratio. The resulting milky white suspension was centrifuged at 4500 rpm for 10 min. The supernatant was decanted and the nanocrystals settled as a wet cake at the bottom of a centrifuge bottle. This purification step was repeated. The rinsed TiO2 wet cake (97 g) was then dispersed into ethanol (1400 g) using an acoustic mixer. After allowing it to sit overnight, the TiO2 was resuspended and transferred to a 2-gallon reactor. The reactor was then closed and sealed. The agitation in the reactor was set to 150-200 RPM. A pressure check was performed on the reactor, where the pressure was maintained at 10 PSIG for 10 min and then vented to 2 PSIG. Ammonia (224 g) was added to 1900 g of water, which was then transferred to the reactor. The lines were then rinsed with 470 g of water. 69 g of ethyl orthosilicate was added to the reactor, followed by 100 g of ethanol. The reactor was inerted by pressurizing with N2 and then venting to 2 psig (this was repeated 10 times). The stirring rate was then increased to 600 rpm and the temperature was raised to 200°C. After holding at 200°C for 3 hours, the reactor was cooled to room temperature. The reactor was then vented and the contents discharged into a container. A white slurry was obtained.
[0416] Example 15: Formation of HfO2 Shell on TiO2
[0417] The TiO2 from Example 1, collected as a wet cake, was dispersed in acetone and homogenized using zirconium oxide beads. The homogenized TiO2 was separated from the reaction mixture by centrifugation at 4500 rpm for 10 minutes. The supernatant was decanted, and the nanocrystals settled as a wet cake at the bottom of the centrifuge bottle. This process was repeated. The resulting wet cake (wet solid) was then dispersed in water using zirconium oxide beads until a homogeneous mixture was obtained. The TiO2 was collected again by centrifugation at 4500 rpm for 10 minutes. The supernatant was decanted, and the nanocrystals settled as a wet cake at the bottom of the centrifuge bottle. This process was repeated once more. The purified TiO2 wet cake was then transferred to a three-necked flask, and water was added to the wet cake (at a weight ratio of 10:1 to the TiO2 wet cake). HfOCl2.8H2O (38% by weight relative to the TiO2 wet cake) was then added to the reaction mixture. The mixture was stirred until homogenized. The reaction mixture was then heated at 90°C for 24 hours. After cooling to room temperature, the reaction mixture obtained after the ZrO2 shell formation process was a transparent dispersion in water.
[0418] The nanocrystals were capped as described in Example 7.
[0419] Example 16: Formation of Al2O3 Shell on TiO2
[0420] The TiO2 from Example 1, collected as a wet cake, was dispersed in acetone and homogenized with zirconium oxide beads. The homogenized TiO2 was separated from the reaction mixture by centrifugation at 4500 rpm for 10 minutes. The supernatant was decanted, and the nanocrystals settled as a wet cake at the bottom of the centrifuge bottle. This process was repeated. The obtained wet cake (wet solid) was then dispersed in water using zirconium oxide beads until a uniform mixture was obtained. The TiO2 was collected again by centrifugation at 4500 rpm for 10 minutes. The supernatant was decanted, and the nanocrystals settled as a wet cake at the bottom of the centrifuge bottle. This process was repeated. The purified TiO2 wet cake was then transferred to a three-necked flask, and water was added to the wet cake (in a weight ratio of 10:1 to the TiO2 wet cake). The pH of the reaction mixture was adjusted to pH 10 using 2M NaOH solution. The mixture was then heated to 60°C and a 2M NaAlO solution in water was added to the reaction mixture (the total amount of NaAlO added was 35% of the weight of the TiO nanocrystals). The pH of the reaction mixture was then adjusted to pH 8 using a 2M HCl solution. The reaction mixture temperature was raised to 90°C for 12 hours. After cooling to room temperature, the product was centrifuged and washed twice with water and then twice with ethanol.
[0421] Example 17: Test to Determine UV Stability of Uncapped Nanocrystals
[0422] A domestic color test was used to test the stability of the titanium oxide and titanium oxide with metal oxide shell of the present invention to various film treatment conditions. A polystyrene-PGMEA dispersion was prepared by dissolving polystyrene in PGMEA at 50 wt % of polystyrene in PGMEA. The dried nanocrystal powder was vigorously mixed in the polystyrene-PGMEA dispersion at a weight ratio of nanocrystals to polystyrene / PGMEA dispersion of 1:2 for 10 minutes to obtain a white opaque viscous paste. The viscous paste or drop-cast was dropped onto a glass surface using a pipette and processed. The drop-cast was baked on a hot plate at 110°C for 5 minutes in air and then subjected to 120 seconds (5 J / cm 2 ) or 60s (7.5J / cm 2 ). The drop cast was then baked in air on a hot plate at 135°C for 5 minutes, followed by an additional baking process at 200°C in an oven for 5 minutes. The degree of color change of the drop cast during each treatment step was recorded as any discoloration. Any type of discoloration was measured as stability to the process. UV stability. The results for TiO2 nanocrystals without a shell and with a ZrO2 shell for various film treatment conditions are shown in Tables 1 and 2.
[0423] Table 1: Results of drop casts containing TiO2 nanocrystals without any shell and TiO2 nanocrystals with ZrO2 shells as present in the present disclosure, and polystyrene mixed with polystyrene after each treatment step. The TiO2 nanocrystals were not capped and were not subjected to any inorganic treatment. The color change after UV irradiation was rated on a scale of 0 to 6; "0" indicates no change after treatment and "6" indicates the greatest degree of yellowing after treatment. The TiO2 without any ZrO2 shells in particular showed the greatest degree of yellowing after UV irradiation, while those with ZrO2 shells showed less color change during treatment.
[0424]
[0425] Table 1: Results of drop casts containing TiO2 nanocrystals without any shell and TiO2 nanocrystals with ZrO2 shells as present in the present disclosure, and polystyrene mixed with polystyrene after each treatment step. The nanocrystals were not capped nor subjected to any inorganic treatment. The paste changed color when exposed to different conditions. The color change was rated on a scale of 0 to 6; "0" means no change after treatment and "6" means maximum yellowing after treatment. TiO2 without any ZrO2 shells showed the greatest yellowing, in particular, after UV irradiation, while TiO2 with ZrO2 shells showed less color change during treatment.
[0426] Table 2 shows the formulation of a paste prepared by mixing at least partially capped TiO nanocrystals (treated with an inorganic passivating agent during capping) with polystyrene on a glass substrate and at various stages of film processing conditions. TiO nanocrystals without any inorganic treatment turned yellow upon heating, while inorganically treated TiO nanocrystals showed less discoloration. Furthermore, Table 3 shows the thermal stability of at least partially capped titanium oxide nanocrystals with ZrO shell powder at elevated temperatures of 100°C to 200°C.
[0427] Table 2: Results of pastes containing TiO2 without any metal oxide shell and subjected to different inorganic treatments when exposed to various film treatment conditions. The pastes changed color upon exposure to the different conditions. The color change was rated on a scale of 0 to 6; "0" indicates no change after treatment, and "6" indicates maximum yellowing after treatment. TiO2 without any ZrO2 shell specifically exhibited the greatest yellowing after UV irradiation, while TiO2 with a ZrO2 shell exhibited less discoloration during treatment.
[0428]
[0429] Example 18: Thermal Stability of Capped TiO2-ZrO2 Core-Shell Nanocrystals
[0430] The thermal stability of at least part of end-blocked titanium oxide and core-shell nanocrystals of the present disclosure is tested by: making the dry powder of the end-blocked nanocrystal continue different times at different temperatures in air before being dispersed in any solvent. The dry end-blocked nanocrystal powder of about 10 g is put into an aluminum pan and placed in a baking oven. The powder is baked for the time period of setting at the desired temperature. The color change degree of the powder is recorded and measured as thermal stability. The result of one such experiment is shown in Table 3.
[0431] Compared to TiO2 without any oxide shell (oxide coating), TiO2 nanocrystals without ZrO2 shells but only inorganically treated (Example 10) did not show any discoloration up to 150°C, and showed a small amount of discoloration when heated at 200°C / 10 min (Table 3). TiO2 nanocrystals with ZrO2 shells but no inorganic treatment (Example 5) showed a lower degree of discoloration at lower temperatures, but began to discolor at higher temperatures. However, TiO2 nanocrystals with ZrO2 shells and inorganic treatment showed better thermal stability. This shows that inorganic treatment is necessary to make the nanocrystals more thermally stable.
[0432] Table 3: Results of dried powders before and after exposure to elevated temperatures. Discoloration was rated on a scale of 0 to 6; "0" indicating no change after treatment and "6" indicating maximum yellowing after treatment.
[0433]
[0434]
[0435] Example 19: Formulation and Nanocomposite Process Using TiO2 Nanocrystals Including Metal Oxide Shells
[0436] An exemplary formulation comprises PGMEA (as a solvent), an acrylic monomer combination of HR6042 and BPMA (with a weight ratio of HR6042 to BPMA of 1:1), at least partially end-capped titanium oxide nanocrystals of the present disclosure (with a weight ratio of nanocrystals to the combined weight of monomers of 1.6:1), and 4 wt % of a photoinitiator, TPO, relative to the weight of the combined monomers.
[0437] The monomers HR6042 and BPMA were mixed in a 1:1 weight ratio. 50 wt% of capped titanium oxide nanocrystals with a ZrO2 shell in propylene glycol monomethyl ether acetate (PGMEA) was mixed with the monomers at a weight ratio of 1.6:1 nanocrystals to combined monomers. The mixture was blended by stirring on a stir plate using a magnetic stirrer or vortexing at 25-30°C for 1-2 hours to obtain a homogeneous mixture. The photoinitiator TPO was added to the formulation at 4 wt% relative to the monomers and mixed again at room temperature for 5-30 minutes using a magnetic stirrer on a stir plate at 20-30°C. The resulting formulation was filtered through a membrane filter to produce a clear, transparent liquid. The viscosity of the formulation was between 5-6 cP as measured by a Brookfield RVDV-II+PCP cone and plate viscometer.
[0438] The nanocomposite coating or film with this formulation was applied to a 2.5×2.5 inch (0.7 mm thick) soda lime glass wafer. The glass wafer was cleaned according to an internal cleaning procedure before applying the film to remove contaminants and dust. The 1-2 micron thick films were each spin coated on the glass wafer at 2000-4000 rpm for 1 min. Since this is a solvent-containing formulation, the applied film was treated by an initial baking process on a hot plate at 110° C. for 2 min to remove some of the solvent prior to UV exposure. The film was then heated to 40° C. using a Phoseon FireJet LED lamp (365 nm) at 125 mW / cm 2 (11.25J / cm 2 ) The film was exposed to a 365 nm LED for 90 seconds under nitrogen. The film was then post-baked on a hot plate at 135° C. for 2 minutes to remove residual solvent. The film thickness was measured using a Metricon 2010 / M prism coupler.
[0439] Table 4 shows the film properties of some exemplary 1 micron thick nanocomposites containing at least partially capped titanium oxide or core-shell nanocrystals of the present disclosure prepared according to Example 19. Refractive index and film thickness were measured using a Metricon 2010 / M prism coupler, and b* and % haze were measured using a HunterLab Vista haze meter. Low % haze indicates high clarity of the film.
[0440] Table 4: Optical properties of nanocomposites prepared using the formulation described in Example 19
[0441]
[0442] Nanocomposites prepared using the formulations exhibit high light transmittance. FIG4 shows the light transmittance of films prepared (solid lines) using (a) the nanocrystals of Example 5, (b) the nanocrystals of Example 6, and (c) the nanocrystals of Example 7, as measured using a PerkinElmer Lambda 850 spectrophotometer with blank soda-lime glass as a reference or background. The thickness of the films was approximately 1 micron. The films exhibited >90% light transmittance at wavelengths of 375-800 nm. The ripples in the spectrum are the result of interference between the incident and reflected light, which is generally a sign of high film quality, i.e., high smoothness, high uniformity, and high transparency.
[0443] Example 20: UV stability test of the nanocomposite prepared in Example 19
[0444] The photocatalytic stability of the nanocomposites made from the nanocrystals proposed in the present disclosure, prepared as described in Example 19, was evaluated by exposing the nanocomposites to various UV wavelength ranges for a set duration. The exposure wavelengths used were 320-390 nm (4 mW / cm 2 strength) for 66h (dosage 950.4J / cm 2 ) or 72h (dosage 1036.8J / cm 2 )、450nm(16mW / cm 2 Strength) for 1000h (dosage 57600J / cm 2 ) and 405nm(25mW / cm 2 Strength) for 148h (dosage 13600J / cm 2 ). General film properties of the nanocomposite materials, such as b*, % haze, RI and film thickness, were measured at different intervals during the test. At the end of the test, the changes in b*, % haze, RI and film thickness of the films from the beginning of the test to the end were evaluated to determine the light stability of the nanocrystals to UV irradiation. The nanocomposite materials that showed minimal film property changes were considered to be the most light stable. Refractive index and film thickness were measured using a 2010 / M prism coupler from Metricon, and b* and % haze were measured using a Vista haze meter from HunterLab.
[0445] Example 20A: Photostability test at 320-390 nm
[0446] Test by having ZrO2 shell TiO2 nanocrystal (such as embodiment 5,6,7 and 8 described in those) nanocomposite material that makes and embodiment 10 does not have ZrO2 outer shell (TiO2 without shell) and the nanocomposite material of those nanocrystals through inorganic treatment to the light stability of 320-390nm UV irradiation.Table 5 has shown the film property of these nanocomposites before any exposure and the change of film property (b*, % haze, RI and film thickness) after exposure.Compared with TiO2 nanocrystal and embodiment 10 without shell, embodiment 5,6,7 and 8 show minimum b* change and % haze change.The lower b* change of the nanocomposite material of embodiment 5,6,7 and 8 shows that TiO2 with ZrO2 shell does not turn yellow to the extent that nanocrystal does not have shell.The lower % haze change also shows that this nanocomposite material degrades less when being exposed to light.A typical sign of TiO2 photocatalytic activity is that chalkiness and haze increase in coating.
[0447] Table 5: Continuous exposure to 320-390 nm wavelength for 66 h (950.4 J / cm 2 ) after the b*, % haze, RI at 520nm and film thickness changes
[0448]
[0449] Example 20B: Photostability test at 405 nm
[0450] The nanocrystals described in test example 7, 11B, 11C, 12A, 12B and those nanocrystals that do not have ZrO shell (TiO that does not have shell ) the nanocomposite material of preparation is irradiated 148h photostability to 405nm UV.Table 6 has shown the film properties of these nanocomposites before any exposure and the variation (b*, % haze, RI and film thickness) of film properties after exposure.Among the samples in the list, the TiO that does not have ZrO shell nanocrystal demonstrates the highest initial b* and the highest b* variation.
[0451] Table 6: Continuous exposure to 405 nm wavelength for 148 h (13600 J / cm 2 ), changes in b*, haze %, RI at 520 nm and film thickness after filtration.
[0452]
[0453] Example 20C: Photostability test at 450 nm
[0454] Nanocomposites prepared from the nanocrystals described in Examples 5, 6, and 7 and those without a ZrO shell (TiO without a shell) were tested for photostability to 1000 h of 450 nm UV irradiation. Table 7 shows the film properties of these nanocomposites before any exposure and the change in film properties (b*, % haze, RI, and film thickness) after exposure. Of the samples listed, the TiO nanocrystals without a ZrO shell showed the highest initial b* and the highest b* change.
[0455] Table 7: Continuous exposure to 450 nm wavelength for 1000 h (57600 J / cm 2 ), changes in b*, haze %, RI at 520 nm (measured using a prism coupler) and film thickness after filtration.
[0456]
[0457] Example 21: Solvent-free Formulation (Solvent-free)
[0458] Another exemplary formulation comprises at least partially end-capped nanocrystals proposed in the present disclosure and at least one monomer. The nanocrystals are present in a range of 65-75 weight % relative to the total formulation. The monomers include at least one of 2-PEA, PTEA, PEA, PBA and / or IBA, which are present in a range of 3-18 weight % relative to the total formulation, and THEICTA (M370) is present in a range of 1-10 weight % relative to the total formulation. The formulation optionally contains additives such as T405 (Tinivin 405), I1010 (Irganox 1010) (which are present in a range of 0.5-2.5 weight % relative to the total formulation), a photoinitiator TPO (which are present in a range of 0.5-2.5 weight % relative to the total formulation), and a balance of solvent (which are present in a range of 4.0-6.5 weight % relative to the total formulation). The formulation is prepared as described in method 2 of the present disclosure. The at least partially end-capped nanocrystals dispersed in the low-boiling point solvent ETA are mixed with the monomers, additives, and photoinitiator. After mixing, the formulation was subjected to rotary evaporation to remove the solvent and produce a homogenous solvent-free mixture. Various variations of the formulation were prepared using the different nanocrystals present in the present disclosure. Table 8a includes the composition and viscosity of such formulations.
[0459] The formulation was spin-coated on a glass substrate and coated with a 365 nm UV lamp at 3 J / cm 2 The film was also coated on a PET substrate with a glass backing and PET was used as the upper cover. The film was then cured with a broadband UV lamp at 1 J / cm 2The films were cured in air using the amounts of The initial optical properties of the cured films and the changes in properties after exposure to light of different wavelengths and condensation conditions are shown in Tables 8b, 8c and 8d.
[0460] Example 21A
[0461] The exemplary formulation comprises 73.0 wt % of at least partially capped TiO nanocrystals without a ZrO shell, 14.6 wt % 2-PEA and 7.5 wt % THEICTA, 1.0 % TPO, and 4.5 % residual solvent after rotary evaporation. The viscosity of the formulation at 25° C. was 1030 cP as measured by a Brookfield RVDV-II+PCP cone and plate viscometer. 10 micron thick films prepared with this formulation on glass or PET substrates exhibited an RI of 1.86 at 589 nm. The films on glass substrates were prepared by spin coating the formulation and then evaporating the film under N2 with a 365 nm UV lamp at 3 J / cm 2 The film on PET had a glass backing and used PET as the upper cover and was then UV cured with a broadband UV lamp at 1 J / cm 2 Curing in air.
[0462] Example 21B
[0463] An exemplary formulation comprises 70.0 wt% of at least partially capped TiO nanocrystals without a ZrO shell, 15.9 wt% 2-PEA and 8.6 wt% THEICTA, 1.0% TPO, and 4.5% residual solvent after rotary evaporation. The viscosity of the formulation at 25°C was 660 cP as measured by a Brookfield RVDV-II+PCP cone and plate viscometer. 10 micron thick films prepared with this formulation on glass or PET substrates exhibited an RI of 1.85 at 589 nm. The films on glass substrates were prepared by spin coating the formulation and then evaporating the film under N2 with a 365 nm UV lamp at 3 J / cm 2 The film on PET had a glass backing and used PET as the upper cover and was then UV cured with a broadband UV lamp at 1 J / cm 2 Curing in air.
[0464] Example 21C
[0465] An exemplary formulation comprises 71.0 wt% of at least partially capped TiO nanocrystals having a ZrO shell of Example 11A, 14.6 wt% 2-PEA and 7.9 wt% THEICTA, 2.0% TPO, and 4.5% residual solvent after rotary evaporation. The viscosity of the formulation at 25°C was 700 cP as measured by a Brookfield RVDV-II+PCP cone and plate viscometer. 10 micron thick films prepared with this formulation on glass or PET substrates exhibited an RI of 1.84 at 589 nm. The films on glass substrates were prepared by spin coating the formulation and then evaporating the film under N2 with a 365 nm UV lamp at 3 J / cm 2 The film on PET had a glass backing and used PET as the upper cover and was then UV cured with a broadband UV lamp at 1 J / cm 2 Curing in air.
[0466] Example 21D
[0467] An exemplary formulation comprises 71.0 wt% of at least partially capped TiO nanocrystals having a ZrO shell of Example 11A, 17.2 wt% PEA and 5.3 wt% THEICTA, 2.0% TPO, and 4.5% residual solvent after rotary evaporation. The viscosity of the formulation at 25° C. was 950 cP as measured by a Brookfield RVDV-II+PCP cone and plate viscometer. 10 μm thick films prepared with this formulation on glass or PET substrates exhibited an RI of 1.81 at 589 nm. The films on glass substrates were prepared by spin coating the formulation and then evaporating the film under N2 with a 365 nm UV lamp at 3 J / cm 2 The film on PET had a glass backing and used PET as the upper cover and was then UV cured with a broadband UV lamp at 1 J / cm 2 Curing in air.
[0468] Example 21E
[0469] An exemplary formulation comprises 71.6 wt% of at least partially capped TiO nanocrystals having a ZrO shell of Example 11B, 13.7 wt% 2-PEA and 7.4 wt% THEICTA, 1.0% TPO, and 6.4% residual solvent after rotary evaporation. The viscosity of the formulation at 25°C was 1700 cP as measured by a Brookfield RVDV-II+PCP cone and plate viscometer. 10 micron thick films prepared with this formulation on glass or PET substrates exhibited an RI of 1.82 at 589 nm. The films on glass substrates were prepared by spin coating the formulation and then evaporating the film under N2 with a 365 nm UV lamp at 3 J / cm 2The film on PET had a glass backing and used PET as the upper cover and was then UV cured with a broadband UV lamp at 1 J / cm 2 Curing in air.
[0470] Example 21F
[0471] An exemplary formulation comprises 72.8 wt% of at least partially capped TiO nanocrystals having a ZrO shell of Example 11B, 10.2 wt% 2-PEA, 5.1% PBA and 3.7% THEICTA, 1.9% TPO and 6.3% residual solvent after rotary evaporation. The viscosity of the formulation at 25°C was 2200 cP as measured by a Brookfield RVDV-II+PCP cone and plate viscometer. 10 micron thick films prepared with this formulation on glass or PET substrates exhibited an RI of 1.8 at 589 nm. The films on glass substrates were prepared by spin coating the formulation and then evaporating the film under N2 with a 365 nm UV lamp at 3 J / cm 2 The film on PET had a glass backing and used PET as the upper cover and was then UV cured with a broadband UV lamp at 1 J / cm 2 Curing in air.
[0472] Example 21G
[0473] An exemplary formulation comprises 71.6 wt% of at least partially capped TiO nanocrystals having a ZrO shell of Example 11B, 13.7 wt% 2-PEA and 4.4 wt% THEICTA, additives 1.0% T405, 2.0% I1010, 1.0% TPO, and 6.4% residual solvent after rotary evaporation. The viscosity of the formulation at 25°C was 2700 cP as measured by a Brookfield RVDV-II+PCP cone and plate viscometer. 10 micron thick films prepared with this formulation on glass or PET substrates exhibited an RI of 1.81 at 589 nm. The films on glass substrates were prepared by spin coating the formulation and then evaporating the film under N2 with a 365 nm UV lamp at 3 J / cm 2 The film on PET had a glass backing and used PET as the upper cover and was then UV cured with a broadband UV lamp at 1 J / cm 2 Curing in air.
[0474] Example 21H
[0475] An exemplary formulation comprises 73.0 wt% of at least partially capped TiO nanocrystals having a ZrO shell of Example 6, 14.0 wt% 2-PEA and 7.5 wt% THEICTA, 1.0% TPO, and 4.5% residual solvent after rotary evaporation. The viscosity of the formulation at 25°C was 4180 cP as measured by a Brookfield RVDV-II+PCP cone and plate viscometer. 10 micron thick films prepared with this formulation on glass or PET substrates exhibited an RI of 1.83 at 589 nm. The films on glass substrates were prepared by spin coating the formulation and then evaporating the film under N2 with a 365 nm UV lamp at 3 J / cm 2 The film on PET had a glass backing and used PET as the upper cover and was then UV cured with a broadband UV lamp at 1 J / cm 2 Curing in air.
[0476] Example 21I
[0477] An exemplary formulation comprises 71.0 wt% of at least partially capped TiO nanocrystals having a ZrO shell of Example 11A, 14.6 wt% IBA and 7.9 wt% THEICTA, 2.0% TPO, and 4.5% residual solvent after rotary evaporation. The viscosity of the formulation at 25°C was 1510 cP as measured by a Brookfield RVDV-II+PCP cone and plate viscometer. 10 micron thick films prepared with this formulation on glass or PET substrates exhibited an RI of 1.78 at 589 nm. The films on glass substrates were prepared by spin coating the formulation and then evaporating the film under N2 with a 365 nm UV lamp at 3 J / cm 2 The film on PET had a glass backing and used PET as the upper cover and was then UV cured with a broadband UV lamp at 1 J / cm 2 Curing in air.
[0478] Example 21J
[0479] An exemplary formulation comprises 71.6 wt% of at least partially capped TiO nanocrystals having a ZrO shell of Example 11D, 13.7 wt% 2-PEA and 4.4 wt% THEICTA, additives 1.0% T405, 2.0% I1010, 1.0% TPO, and 6.4% residual solvent after rotary evaporation. The viscosity of the formulation at 25°C was 2700 cP as measured by a Brookfield RVDV-II+PCP cone and plate viscometer. 10 micron thick films prepared with this formulation on glass or PET substrates exhibited an RI of 1.81 at 589 nm. The films on glass substrates were prepared by spin coating the formulation and then evaporating the film under N2 with a 365 nm UV lamp at 3 J / cm 2 The film on PET had a glass backing and used PET as the upper cover and was then UV cured with a broadband UV lamp at 1 J / cm 2 Curing in air.
[0480] Table 8a: Summary of formulation composition and properties of the formulation described in Example 21. Included are samples having titania nanocrystals and titania-zirconia core-shell nanocrystals.
[0481]
[0482] Table 8b: The nanocomposite material described in Example 21 was shown to be effective when exposed to 405 UV light for 148 h (25 mW / cm 2 ) when. The initial optical properties and the change in optical properties of the films on the PET substrate were measured. The b* change of the 21A nanocomposite was significantly higher than that of nanocomposite 21E, 21F and 21I, where the films were prepared on the same substrate with similar thicknesses. The film thickness and RI change of all nanocomposites were comparable; however, for the nanocomposites made with nanocrystals having a ZrO2 shell, the initial RI values were lower.
[0483]
[0484] Table 8c: The nanocomposite material described in Example 21 was exposed to UVA light at 320-390 nm for 72 h (dosage 1036.8 J / cm 2 ; Average intensity 4mW / cm 2 The initial optical properties and changes in optical properties of the films on the glass substrate were measured. Nanocomposites 21A and 21B were made by mixing the same titanium dioxide nanocrystals with different monomers.
[0485]
[0486] Table 8d: The nanocomposite material described in Example 21 was exposed to QUV accelerated weathering test at 340 nm for 72 h (0.89 mW / cm 2 ) at . Initial optical measurements and changes in optical measurements were performed on PET samples. ΔE* is a calculated value that includes ΔL*, Δa*, and Δb*.
[0487]
[0488] Example 22: Nanocomposite formulation (containing solvent)
[0489] Exemplary formulations include at least partially capped nanocrystals present in the present disclosure (present in the range of 20-60 wt % relative to the total formulation), a monomer blend comprising PBA and / or THEICTA (present in the range of 3-25 wt % relative to the total formulation, such that the ratio of nanocrystals to monomers is in the range of 3:7 to 8:2), a photoinitiator TPO (present in the range of 0.5-2.5 wt % relative to the total formulation), and a solvent such as PGMEA (PGA) present in the range of 20-40 wt % relative to the total formulation. The formulations are prepared as described in Method 2 of the present disclosure. Preferred ratios of PBA to THEICTA (or M370) are in the range of 1:1 to 4:1. Table 9a shows the composition and viscosity of the exemplary formulations.
[0490] 2-3 μm thick nanocomposite films of the formulations were prepared on glass substrates by spin coating the formulations, prebaking on a hot plate at 50°C for 5 min, and then irradiating with a 365 nm UV lamp at 3 J / cm 2 The nanocomposites or films were UV cured at 405 nm for 148 h (dosage 13600 J / cm 2 ) before and after optical properties.
[0491] Example 22A
[0492] The exemplary formulation comprises 45.3 wt% of at least partially capped TiO nanocrystals without a shell in an acrylate blend consisting of 18.3 wt% PBA, 5.6 wt% T HEICTA, 0.8 wt% TPO, and 30.0 wt% PGMEA. The formulation had a viscosity of 18 cP at 25°C as measured by a Brookfield RVDV-II+PCP cone and plate viscometer. The nanocomposite was deposited as a 2-3 micron film, and the cured film on a glass substrate had an RI of 1.82 at 589 nm.
[0493] Example 22B
[0494] An exemplary formulation comprises 45.3 wt% of the at least partially capped core-shell nanocrystals of Example 11B in an acrylate blend consisting of 13.1 wt% PBA, 4.0 wt% THEICTA, 0.7 wt% TPO, and 30.5 wt% PGMEA. The formulation had a viscosity of 18.4 cP at 25°C, as measured by a Brookfield RVDV-II+PCP cone and plate viscometer. The nanocomposite was deposited as a 2-3 micron film, and the cured film on a glass substrate had an RI of 1.84 at 589 nm. As shown by an approximately 10-fold reduction in Δb*, nanocomposite 22B exhibited significantly less yellowing than 22A.
[0495] Table 9a: Summary of the formulation composition and viscosity described in Example 22
[0496]
[0497] Table 9b: Optical properties of the nanocomposite material on a glass substrate described in Example 22 upon exposure to 405 nm light for 148 h (13600 J / cm2)
[0498]
[0499] Example 23: Nanocomposite formulation (without solvent)
[0500] Exemplary formulations include at least partially end-capped nanocrystals present in the present disclosure (present in the range of 20-60 wt % relative to the total formulation), a monomer blend comprising at least one of BA, BPMA, and / or DVE (present in the range of 40-80 wt % relative to the total formulation), optionally containing a diluent (such as STY and ethyl acetate, present in the range of 0.5-5 wt % relative to the total formulation), at least one of a photoinitiator and a photosensitizer (selected from Irgacure 819, ITX, and Esacure 1001M, present in the range of 0.5-5 wt % relative to the total formulation), and residual solvent (present in the range of 1.0-6.5 wt % relative to the total formulation). The formulations are prepared as described in Method 2 of the present disclosure. The at least partially end-capped nanocrystals dispersed in the low boiling point solvent ETA are mixed with the monomers, additives, and photoinitiator. After mixing, the formulation is subjected to rotary evaporation to remove the solvent and produce a homogeneous solvent-free mixture. Various variations of the formulations are prepared using different nanocrystals present in the present disclosure. Table 10a includes the composition, viscosity, and optical properties of the cured films.
[0501] The formulation was spin-coated on a glass substrate and coated with a 385 nm UV lamp at 1 J / cm 2 Tables 10b and 10c include the changes in properties after exposure to 340 nm QUV and condensation.
[0502] Example 23A
[0503] An exemplary formulation comprises 40.0 wt% of at least partially capped nanocrystals of TiO2 without a shell in an acrylate blend consisting of 17.0 wt% BA, 33.0 wt% BPMA, 5.0% DVE, 2.0% Irgacure 819, 1.0% ITX, 1.0% Esacure 1001M, 2.0% STY, and 0.1% BYK 333. The viscosity of the formulation was 25 cp at 25°C as measured by a Brookfield RVDV-II+PCP cone and plate viscometer. The nanocomposite was deposited as an 11.0 micron film on a glass substrate and heated in air at 385 nm UV at 1 J / cm 2 The film was cured and had a refractive index of 1.717 at 589 nm.
[0504] Example 23B
[0505] An exemplary formulation comprises 45.0 wt% of at least partially capped core-shell nanocrystals of Example 11B in an acrylate blend consisting of 33.0 wt% BA, 17.0 wt% BPMA, 2.0% Irgacure 819, 2.0% ITX, and 1.0% BYK 333. The viscosity of the formulation at 25° C. was 19 cP as measured by a Brookfield RVDV-II+PCP cone and plate viscometer. The...
Claims
1. A nanocrystal having a core-shell structure, comprising a core and a shell, wherein the core is at least partially encapsulated by the shell, wherein the core comprises a core metal oxide, and the shell comprises a shell metal oxide, wherein: The core metal oxide is characterized by having an average particle size greater than 3 nm but less than 50 nm as measured by TEM; and The outer shell is characterized by having a thickness of 0.1 nm to 5 nm as measured by TEM, wherein the core metal oxide and the shell metal oxide are the same or different.
2. The nanocrystal of claim 1 , wherein the atomic ratio of the shell metal oxide to the core metal oxide as measured by SEM EDX is less than 3, such as less than 0.1, less than 0.2, less than 0.3, less than 0.4, less than 0.5, less than 0.6, less than 0.7, less than 0.8 nm, less than 0.9, less than 1, less than 2, less than 3.
3. The nanocrystal according to any one of claims 1 and 2, wherein the core metal oxide has a narrow particle size distribution, characterized by: 1) the ratio of D90:D10 is less than 5, preferably less than 3, or less than 2, such as about 1.1 to about 2, about 1.5 to about 2, about 1.2 to about 1.8, about 1.2 to about 3, or about 1.5 to about 3; 2) the ratio of D90:D50 is less than 3, preferably less than 2, or less than 1.5, such as about 1.1 to about 2, about 1.5 to about 2, about 1.2 to about 1.5; and / or 3) the ratio of D50:D10 is less than 3, preferably less than 2, or less than 1.5, such as about 1.1 to about 2, about 1.5 to about 2, about 1.2 to about 1.
5.
4. The nanocrystal according to any one of claims 1 and 2, characterized in that Having a narrow particle size distribution, characterized by: 1) a D90:D10 ratio of less than 5, preferably less than 3, or less than 2, such as from about 1.1 to about 2, from about 1.5 to about 2, from about 1.2 to about 1.8, from about 1.2 to about 3, or from about 1.5 to about 3; 2) a D90:D50 ratio of less than 3, preferably less than 2, or less than 1.5, such as from about 1.1 to about 2, from about 1.5 to about 2, from about 1.2 to about 1.5; and / or 3) a D50:D10 ratio of less than 3, preferably less than 2, or less than 1.5, such as from about 1.1 to about 2, from about 1.5 to about 2, from about 1.2 to about 1.
5.
5. The nanocrystal according to any one of claims 1-4, comprising a core and / or core-shell treated with an inorganic passivating agent, wherein the inorganic passivating agent comprises NaH2PO2, Na2HPO3, NaCl, NaNO3 and / or LiNO3.
6. The nanocrystal according to any one of claims 1 to 5, comprising at least partially end-capped nanocrystals, wherein the at least partially end-capped nanocrystals are end-capped with at least one end-capping agent selected from the group consisting of methyltrimethoxysilane, ethyltrimethoxysilane, n-propyltrimethoxysilane, n-propyltriethoxysilane, n-octyltrimethoxysilane, n-octyltriethoxysilane, phenyltrimethoxysilane, dodecyltrimethoxysilane, m-, p-ethylphenethyltrimethoxysilane, 2-[methoxy(polyethyleneoxy)propyl]-trimethoxysilane, methoxy(trivinyloxy)propyltrimethoxysilane, 3- aminopropyltrimethoxysilane, 3-mercaptopropyltrimethoxysilane, 3-(methacryloyloxy)propyltrimethoxysilane, 3-(acryloyloxy)propyltrimethoxysilane, 3-isocyanatopropyltriethoxysilane, 3-isocyanatopropyltrimethoxysilane, and 3-glycidoxypropyltrimethoxysilane, vinyltrimethoxysilane, allyltrimethoxysilane, 1-hexenyltrimethoxysilane, 1-octenyltrimethoxysilane, N-phenylaminopropyltrimethoxysilane, 3-(4-pyridylethyl)thiopropyltrimethoxysilane, N-(3-trimethoxysilylpropyl)pyrrole, 2-( 3-Trimethoxysilylpropylthio)thiophene, (3-trimethoxysilylpropyl)diethylenetriamine, phenyltrimethoxysilane, ((chloromethyl)phenylethyl)trimethoxysilane, 2-(diphenylphosphino)ethyltriethoxysilane, 4-phenylbutyltrimethoxysilane, 2-phenylethyltrimethoxysilane, 4-biphenyltriethoxysilane, N-[3-(trimethoxysilyl)propyl]allylamine, 3-mercaptopropyltrimethoxysilane, 8-glycidoxyoctyltrimethoxysilane, (3-glycidoxypropyl)trimethoxysilane, ethyl orthosilicate, heptanol, hexanol, octanol, benzyl alcohol, phenol, Ethanol, propanol, butanol, oleyl alcohol, dodecanol, octadecyl alcohol and triethylene glycol monomethyl ether, (2-{2-[2-methoxy-ethoxy]-ethoxy}-ethyl)phosphonic acid, (6-{2-[2-(2-methoxy-ethoxy)-ethoxy]-ethoxy}-hexyl)phosphonic acid, 11-acryloyloxyundecylphosphonic acid, octanoic acid, acetic acid, propionic acid, 2-[2-(2-methoxyethoxy)ethoxy]acetic acid, oleic acid, benzoic acid, stearic acid, trifluoroacetic acid, biphenyl-4-carboxylic acid, 2-(2-methoxyethoxy)acetic acid, methacrylic acid, mono-2-(methacryloyloxy)ethyl succinate, or any combination thereof.
7. Nanocrystals according to claim 6, wherein the organic content of the at least partially capped nanocrystals is less than 25%, such as less than 5%, or between 5% and 8%, or between 8% and 10%, or between 10% and 12%, or between 12% and 14%, or between 14% and 16%, or between 16% and 18%, or between 18% and 20%.
8. The nanocrystal of any one of claims 1-7, wherein the core metal oxide comprises titanium dioxide, zirconium dioxide and / or barium titanate.
9. The nanocrystal of any one of claims 1-7, wherein the shell metal oxide comprises silicon dioxide, zirconium dioxide, hafnium dioxide, niobium oxide, aluminum oxide, tantalum oxide, barium titanium oxide, or any combination thereof.
10. The nanocrystal of any one of claims 1-7, wherein the core metal oxide comprises TiO2, and the shell metal oxide comprises silicon dioxide, zirconium dioxide, hafnium dioxide, niobium oxide, aluminum oxide, tantalum oxide, barium titanium oxide, or any combination thereof.
11. The nanocrystal according to any one of claims 1 to 10, wherein the nanocrystal exhibits low photocatalytic activity, the photocatalytic activity being measured at 4 mW / cm2 for a 1 um thick film comprising the core-shell structure using a haze meter. 2 The change in b* before and after exposure to UV light intensity at 320nm-390nm for 66h is measured by the change in b*, and the change in b* is less than 50%, such as less than 1%, or less than 5%, or less than 10%, or less than 15%, or less than 20%, or less than 25%, less than 30%, less than 40%, or less than 50%.
12. The nanocrystal according to any one of claims 1 to 10, wherein the nanocrystal exhibits low photocatalytic activity, the photocatalytic activity being measured at 16 mW / cm2 for a 1 um thick film comprising the core-shell structure using a haze meter. 2 b* before and after exposure to UV at 450 nm or above for 1000 h at a light intensity of 25 mW / cm 2 The change in b* is measured by the change in b* before and after exposure to UV at or above 405 nm for 148 h at a light intensity of 405 nm, and the change in b* is less than 50%, such as less than 1%, or less than 5%, or less than 10%, or less than 15%, or less than 20%, or less than 25%, less than 30%, less than 40%, or less than 50%.
13. The nanocrystal according to any one of claims 1-10, wherein the nanocrystal exhibits low photocatalytic activity, the photocatalytic activity being measured by the change in refractive index of a film comprising the core-shell nanocrystals before and after exposure to UV at or above 405 nm for 148 h at a light intensity of 25 mW / cm2 using a prism coupler or an ellipsometer, the change in refractive index being less than 0.08, e.g., less than 0.01, less than 0.02, less than 0.03, less than 0.04, less than 0.05, less than 0.06, less than 0.
07.
14. The nanocrystal according to any one of claims 1 to 10, wherein the nanocrystal exhibits low photocatalytic activity as measured by a prism coupler or ellipsometer at 16 mW / cm2 for a film comprising the core-shell nanocrystal. 2 The change in refractive index is measured by the change in refractive index before and after exposure to UV at 450 nm or above for 1000 h, and the change in refractive index is less than 0.08, for example, less than 0.01, less than 0.02, less than 0.03, less than 0.04, less than 0.05, less than 0.06, or less than 0.
07.
15. The nanocrystal of any one of claims 11-14, wherein the core metal oxide is titanium oxide, the shell metal oxide comprises zirconium oxide, and the nanocrystal has an average particle size of less than 30 nm as measured by TEM.
16. The nanocrystal of claim 15, wherein the atomic ratio of the shell Zr to the core Ti measured by SEM EDX is less than 3, such as less than 0.1, less than 0.2, less than 0.3, less than 0.4, less than 0.5, less than 0.6, less than 0.7, less than 0.8 nm, less than 0.9, less than 1, less than 2, less than 3.
17. The nanocrystal of any one of claims 1-16, wherein the nanocrystal has a particle size distribution characterized by a D9999 of less than 500 nm when the volume of 5 wt% of the nanocrystals dispersed in a solvent is measured by dynamic light scattering (DLS).
18. A method for preparing core-shell structured TiO2 nanocrystals, the core-shell TiO2 nanocrystals comprising a core comprising TiO2 nanocrystals and a shell comprising a shell metal oxide, the method comprising converting a precursor of the shell metal oxide into the shell metal oxide that at least partially encapsulates the core comprising the TiO2 nanocrystals in a solvent, wherein the conversion comprises 1) mixing the precursor of the shell metal oxide in a reaction mixture of the solvent and the core comprising the TiO2 nanocrystals, and 2) heating the reaction mixture at a reaction temperature, such as about 90°C, for a period of time to provide the shell metal oxide that at least partially encapsulates the core comprising the TiO2 nanocrystals.
19. The method of claim 18, wherein the converting comprises 1) mixing the precursor of the shell metal oxide directly or in water into a reaction mixture of the solvent and the core containing TiO2 nanocrystals, and 2) heating the reaction mixture at a reaction temperature of about 50°C to about 90°C for about 10 minutes to about 7 days to form the shell metal oxide that at least partially encapsulates the core containing TiO2 nanocrystals.
20. The method of any one of claims 18-19, wherein the shell metal oxide comprises zirconium oxide.
21. The method of claim 20, wherein the precursor of zirconium dioxide is a zirconium alkoxide, such as a zirconium alkoxide having the formula Zr(OR)4, a zirconium alkoxide having the formula Zr(OR) x G y or a combination thereof, or a zirconium oxyhalide or a zirconium halide, wherein each R group can independently be an alkyl group (e.g., a C1-C6 alkyl group) or a substituted alkyl group, and each occurrence of the G group is independently a halogen (e.g., Cl), wherein x is an integer from 0 to 4, and y is an integer from 0 to 4, provided that x+y is 4.
22. The method according to any one of claims 18 to 21, wherein the solvent comprises one or more solvents selected from the group consisting of benzyl alcohol, phenol, oleyl alcohol, butanol, propanol, isopropanol, ethanol, butoxyethanol, butoxypropanol, methanol, 2-(isopentyloxy)ethanol, 2-propoxy-propanol (PnP), 2-(hexyloxy)ethanol, tetrahydrofuran, dimethyl ether, ethyl ether, dibutyl ether, propylene glycol monomethyl ether (PGME), diethylene glycol butyl ether, dipropylene glycol methyl ether (DPGME), diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol, dipropylene glycol, acetone, propylene glycol methyl ether acetate (PGMEA), ethyl lactate (EL), methyl acetate, ethyl acetate, butyl acetate, ethylene glycol monobutyl ether acetate, diethylene glycol monoethyl ether acetate, butoxyethyl acetate, ethyl acetate, 2-(2-butoxyethoxy)ethyl acetate, benzene, toluene and water.
23. The method of any one of claims 18-22, wherein the core-shell structured TiO2 nanocrystals have an average particle size of about 3 nm to about 50 nm as measured by TEM.
24. The method of any one of claims 18-23, wherein the core comprising TiO2 nanocrystals has an average particle size of 3 nm to 50 nm, and the shell comprising the shell metal oxide has a shell thickness of 0.1 nm to 5 nm, as measured by TEM.
25. The method of any one of claims 20-24, wherein the shell metal oxide comprises ZrO2, and the atomic ratio of Zr / Ti of the core TiO2 nanocrystals to the shell ZrO2 as measured by SEM EDX is less than 3, such as less than 0.1, less than 0.2, less than 0.3, less than 0.4, less than 0.5, less than 0.6, less than 0.7, less than 0.8 nm, less than 0.9, less than 1, less than 2, less than 3.
26. The method of any one of claims 18-25, wherein the shell of at least one metal oxide material on the TiO2 nanocrystals fully or partially encapsulates the TiO2 nanocrystals.
27. The method of any one of claims 18-26, wherein the shell comprises the shell metal oxide in crystalline and / or amorphous form.
28. The method according to any one of claims 18 to 27, wherein the core-shell structured TiO2 nanocrystals prepared according to the method have a narrow particle size distribution, characterized by: 1) the ratio of D90:D10 is less than 5, preferably less than 3, or less than 2, such as about 1.1 to about 2, about 1.5 to about 2, about 1.2 to about 1.8, about 1.2 to about 3, or about 1.5 to about 3; 2) the ratio of D90:D50 is less than 3, preferably less than 2, or less than 1.5, such as about 1.1 to about 2, about 1.5 to about 2, about 1.2 to about 1.5; and / or 3) the ratio of D50:D10 is less than 3, preferably less than 2, or less than 1.5, such as about 1.1 to about 2, about 1.5 to about 2, about 1.2 to about 1.
5.
29. A method for capping a core-shell structured TiO2 nanocrystal having a core comprising a TiO2 nanocrystal with a shell comprising ZrO2, comprising reacting the nanocrystal of any one of claims 1 to 5 with a first capping agent in a first capping solvent to produce a first at least partially capped core-shell structured TiO2 nanocrystal.
30. The method according to claim 29, wherein the end-capping agent is methyltrimethoxysilane, ethyltrimethoxysilane, n-propyltrimethoxysilane, n-propyltriethoxysilane, n-octyltrimethoxysilane, n-octyltriethoxysilane, phenyltrimethoxysilane, dodecyltrimethoxysilane, m-, p-ethylphenethyltrimethoxysilane, 2-[methoxy(polyethyleneoxy)propyl]-trimethoxysilane, methoxy(trivinyloxy)propyltrimethoxysilane, 3-aminopropyltrimethoxysilane, 3-mercaptopropyltrimethoxysilane, 3-(methacryloyloxy)propyltrimethoxysilane, methoxysilane, 3-(acryloyloxy)propyltrimethoxysilane, 3-isocyanatopropyltriethoxysilane, 3-isocyanatopropyltrimethoxysilane, and 3-glycidoxypropyltrimethoxysilane, vinyltrimethoxysilane, allyltrimethoxysilane, 1-hexenyltrimethoxysilane, 1-octenyltrimethoxysilane, N-phenylaminopropyltrimethoxysilane, 3-(4-pyridylethyl)thiopropyltrimethoxysilane, N-(3-trimethoxysilylpropyl)pyrrole, 2-(3-trimethoxysilylpropylthio)thiophene, (3-trimethoxysilane trimethoxysilane, ethyl orthosilicate, heptanol, hexanol, octanol, benzyl alcohol, phenol, ethanol, propanol, butanol, oleyl alcohol, dodecanol, octadecyl alcohol, 1,2-dimethylformamide, 1,2-dimethylformamide, 1,2-dimethylformamide, 1,2-dimethylformamide, 1,2-dimethylformamide, 1,2-dimethylformamide, 1,2-dimethylformamide, 1,2-dimethylformamide, 1,2-dimethylformamide, 1,2-dimethylformamide, 1,2-dimethylformamide, 1,2-dimethylformamide, 1,2-dimethylformamide, 1,2-dimethylformamide, 1,2-dimethylformamide, 1,2-dimethylformamide, 1,2-dimethylformamide, 1,2-dimethylformamide, 1,2-dimethylformamide, 1,2-dimethylformamide, 1,2-dimethylformamide, 1,2-dimethylformamide, 1,2-dimethylformamide, 1,2-dimethylformamide, 1,2-dimethylformamide alcohol and triethylene glycol monomethyl ether, (2-{2-[2-methoxy-ethoxy]-ethoxy}-ethyl)phosphonic acid, (6-{2-[2-(2-methoxy-ethoxy)-ethoxy]-ethoxy}-hexyl)phosphonic acid, 11-acryloyloxyundecylphosphonic acid, octanoic acid, acetic acid, propionic acid, 2-[2-(2-methoxyethoxy)ethoxy]acetic acid, oleic acid, benzoic acid, stearic acid, trifluoroacetic acid, biphenyl-4-carboxylic acid, 2-(2-methoxyethoxy)acetic acid, methacrylic acid, mono-2-(methacryloyloxy)ethyl succinate, or any combination thereof.
31. A nanocrystal dispersion comprising at least partially capped core-shell nanocrystals comprising a core metal oxide with an outer shell comprising a shell metal oxide, at least one capping agent, and a dispersion medium, wherein: The core metal oxide is characterized by having an average particle size greater than 3 nm but less than 50 nm as measured by TEM or DLS, and the shell is characterized by having a thickness of 0.2 nm to 5 nm as measured by TEM or DLS; and The at least partially capped core-shell structured nanocrystals are present in an amount greater than 10% by weight of the dispersion.
32. The nanocrystal dispersion of claim 31 , wherein the at least partially end-capped core-shell structured nanocrystals are end-capped with at least one end-capping agent selected from the group consisting of methyltrimethoxysilane, ethyltrimethoxysilane, n-propyltrimethoxysilane, n-propyltriethoxysilane, n-octyltrimethoxysilane, n-octyltriethoxysilane, phenyltrimethoxysilane, dodecyltrimethoxysilane, m-, p-ethylphenethyltrimethoxysilane, 2-[methoxy(polyethyleneoxy)propyl]-trimethoxysilane, methoxy(trivinyloxy)propyltrimethoxysilane, 3-aminopropyltrimethoxysilane, trimethoxysilane, 3-mercaptopropyltrimethoxysilane, 3-(methacryloyloxy)propyltrimethoxysilane, 3-(acryloyloxy)propyltrimethoxysilane, 3-isocyanatopropyltriethoxysilane, 3-isocyanatopropyltrimethoxysilane, and 3-glycidoxypropyltrimethoxysilane, vinyltrimethoxysilane, allyltrimethoxysilane, 1-hexenyltrimethoxysilane, 1-octenyltrimethoxysilane, N-phenylaminopropyltrimethoxysilane, 3-(4-pyridylethyl)thiopropyltrimethoxysilane, N-(3-trimethoxysilylpropyl)pyrrole, 2-(3-trimethoxy trimethoxysilane, ethyl orthosilicate, heptyl alcohol, hexyl alcohol, octanol, benzyl alcohol, phenol, ethanol, Propanol, butanol, oleyl alcohol, dodecanol, octadecyl alcohol and triethylene glycol monomethyl ether, (2-{2-[2-methoxy-ethoxy]-ethoxy}-ethyl)phosphonic acid, (6-{2-[2-(2-methoxy-ethoxy)-ethoxy]-ethoxy}-hexyl)phosphonic acid, 11-acryloyloxyundecylphosphonic acid, octanoic acid, acetic acid, propionic acid, 2-[2-(2-methoxyethoxy)ethoxy]acetic acid, oleic acid, benzoic acid, stearic acid, trifluoroacetic acid, biphenyl-4-carboxylic acid, 2-(2-methoxyethoxy)acetic acid, methacrylic acid, mono-2-(methacryloyloxy)ethyl succinate, or any combination thereof.
33. A nanocrystal dispersion according to any one of claims 31-32, wherein the core-shell structured nanocrystals are treated with an inorganic passivating agent comprising NaH2PO2, Na2HPO3, NaCl, NaNO3 and / or LiNO3.
34. A nanocrystal dispersion according to any one of claims 31-33, wherein the organic content of the at least partially capped nanocrystals is less than 25%, such as less than 5%, or less than 8%, or less than 10%, less than 12%, or less than 14%, or less than 16%, or less than 18%, or less than 20%.
35. The nanocrystalline dispersion of any one of claims 31-34, wherein the core metal oxide comprises titanium dioxide, zirconium dioxide and / or barium titanate.
36. The nanocrystalline dispersion of any one of claims 31-35, wherein the shell metal oxide comprises silicon dioxide, zirconium dioxide, hafnium dioxide, niobium oxide, aluminum oxide, tantalum oxide, barium titanium oxide, or any combination thereof.
37. A nanocrystal dispersion according to any one of claims 31-36, wherein the at least partially terminated core-shell structured nanocrystals are present in an amount equal to or greater than 50% by weight of the dispersion, and wherein the % organic matter is less than 20% of the at least partially terminated core-shell structured nanocrystals.
38. A nanocrystal dispersion according to any one of claims 31-37, wherein the core metal oxide is titanium oxide, the shell metal oxide comprises zirconium oxide, and the average particle size of the at least partially terminated core-shell structured nanocrystals is less than 30 nm as measured by TEM or DLS.
39. according to the nanocrystalline dispersion described in any one of claims 31-38, wherein the atomic ratio of described shell ZrO2 and described core TiO2 measured by SEM EDX is less than 3, such as less than 0.1, less than 0.2, less than 0.3, less than 0.4, less than 0.5, less than 0.6, less than 0.7, less than 0.8nm, less than 0.9, less than 1, less than 2, less than 3.
40. A nanocrystal dispersion according to any one of claims 31-39, wherein the particle size distribution of the at least partially blocked core-shell structured nanocrystals is characterized by a D9999 of less than 500 nm when the volume of 5 wt % of the at least partially blocked core-shell structured nanocrystals dispersed in a solvent is measured by dynamic light scattering (DLS).
41. A nanocrystal dispersion according to any one of claims 31-39, wherein the particle size distribution of the at least partially blocked core-shell structured nanocrystals is characterized by a D9999 of less than 300 nm when the volume of 5 wt % of the at least partially blocked core-shell structured nanocrystals dispersed in a solvent is measured by dynamic light scattering (DLS).
42. The nanocrystal dispersion of any one of claims 31-41, wherein the dispersion medium comprises a solvent, a monomer, an oligomer of a polymer, or a combination thereof.
43. A nanocomposite formulation comprising 1) at least partially capped core-shell TiO2 nanocrystals having an outer shell, the outer shell of the TiO2 nanocrystals comprising a shell metal oxide; 2) a monomer, oligomer and / or polymer; 3) an optional solvent; and 4) a curing agent, wherein the at least partially capped core-shell TiO2 nanocrystals are present in an amount greater than 20 wt % relative to the monomer, oligomer and / or polymer, wherein the core of the at least partially capped core-shell TiO2 nanocrystals comprises crystalline titanium dioxide and is treated with at least one inorganic passivating agent; and wherein the average particle size of the at least partially capped core-shell TiO2 nanocrystals is in the range of 3-50 nm when measured by DLS at 5% nanocrystals dispersed in PGMEA.
44. The nanocomposite formulation of claim 43, wherein the at least partially capped core-shell structured TiO2 nanocrystals have an average particle size greater than 3 nm but less than 50 nm and a shell thickness of 0.1 nm to 3 nm as measured by TEM.
45. The nanocomposite formulation of any one of claims 43-44, wherein the at least partially capped core-shell structured TiO2 nanocrystals are capped with at least one capping agent selected from methyltrimethoxysilane, ethyltrimethoxysilane, n-propyltrimethoxysilane, n-propyltriethoxysilane, n-octyltrimethoxysilane, n-octyltriethoxysilane, phenyltrimethoxysilane, dodecyltrimethoxysilane, m-, p-ethylphenethyltrimethoxysilane, 2-[methoxy(polyethyleneoxy)propyl]-trimethoxysilane, methoxy(trivinyloxy)propyltrimethoxysilane, 3-aminopropyltrimethoxysilane, 3-mercaptopropyltrimethoxysilane, 3-(methacryloyloxy)propyltrimethoxysilane, 3-(acryloyloxy)propyltrimethoxysilane, 3-isocyanatopropyltriethoxysilane, 3-isocyanatopropyltrimethoxysilane, and 3-glycidoxypropyltrimethoxysilane, vinyltrimethoxysilane, allyltrimethoxysilane, 1-hexenyltrimethoxysilane, 1-octenyltrimethoxysilane, N-phenylaminopropyltrimethoxysilane, 3-(4-pyridylethyl)thiopropyltrimethoxysilane, N-(3-trimethoxysilylpropyl)pyrrole, 2- (3-Trimethoxysilylpropylthio)thiophene, (3-trimethoxysilylpropyl)diethylenetriamine, phenyltrimethoxysilane, ((chloromethyl)phenylethyl)trimethoxysilane, 2-(diphenylphosphino)ethyltriethoxysilane, 4-phenylbutyltrimethoxysilane, 2-phenylethyltrimethoxysilane, 4-biphenyltriethoxysilane, N-[3-(trimethoxysilyl)propyl]allylamine, 3-mercaptopropyltrimethoxysilane, 8-glycidyltrimethoxysilane, (3-glycidyl)trimethoxysilane, ethyl orthosilicate, heptanol, hexanol, octanol, benzyl alcohol, phenol, Ethanol, propanol, butanol, oleyl alcohol, dodecanol, octadecyl alcohol and triethylene glycol monomethyl ether, (2-{2-[2-methoxy-ethoxy]-ethoxy}-ethyl)phosphonic acid, (6-{2-[2-(2-methoxy-ethoxy)-ethoxy]-ethoxy}-hexyl)phosphonic acid, 11-acryloyloxyundecylphosphonic acid, octanoic acid, acetic acid, propionic acid, 2-[2-(2-methoxyethoxy)ethoxy]acetic acid, oleic acid, benzoic acid, stearic acid, trifluoroacetic acid, biphenyl-4-carboxylic acid, 2-(2-methoxyethoxy)acetic acid, methacrylic acid, mono-2-(methacryloyloxy)ethyl succinate, or any combination thereof.
46. The nanocomposite formulation of any one of claims 43-45, wherein the shell metal oxide comprises silicon dioxide, zirconium dioxide, hafnium dioxide, niobium oxide, aluminum oxide, tantalum oxide, barium titanium oxide, or any combination thereof.
47. The nanocomposite formulation of any one of claims 43-46, wherein the at least partially terminated core-shell structured nanocrystals are present in an amount equal to or greater than 50% relative to the monomers, oligomers and / or polymers.
48. The nanocomposite formulation of any one of claims 43-47, wherein the viscosity of the formulation is in the range of 1-1000 cP.
49. A nanocomposite formulation according to any one of claims 43-48, wherein the at least partially capped core-shell structured TiO2 nanocrystals have low photocatalytic activity, the photocatalytic activity being measured by the change in b* when a 1 um thick film comprising the core-shell structure is measured using a haze meter before and after exposure to UV at 320nm-390nm for 100h, the change in b* being less than 50%, such as less than 1%, or less than 5%, or less than 10%, or less than 15%, or less than 20%, or less than 25%, less than 30%, less than 40%, or less than 50%.
50. According to any one of claims 43-48, the at least partially capped core-shell structured TiO2 nanocrystals have low photocatalytic activity, the photocatalytic activity is measured by the change in b* when a 1 um thick film comprising the core-shell structure is measured using a haze meter before and after exposure to UV at 450 nm or above for 1000 h, the change in b* is less than 50%, such as less than 1%, or less than 5%, or less than 10%, or less than 15%, or less than 20%, or less than 25%, less than 30%, less than 40%, less than 50%.
51. A nanocomposite formulation according to any one of claims 43-48, wherein the at least partially capped core-shell structured TiO2 nanocrystals have low photocatalytic activity, the photocatalytic activity being measured by the change in refractive index when a film comprising the core-shell nanocrystals is measured before and after exposure to UV at or above 320-390 nm for 100 h using a prism coupler or ellipsometer, the change in refractive index being less than 0.08, such as less than 0.01, less than 0.02, less than 0.03, less than 0.04, less than 0.05, less than 0.06, less than 0.
07.
52. A nanocomposite formulation according to any one of claims 43-48, wherein the at least partially capped core-shell structured TiO2 nanocrystals have low photocatalytic activity, the photocatalytic activity being measured by the change in refractive index when a film comprising the core-shell nanocrystals is measured before and after exposure to UV at or above 450 nm for 1000 h using a prism coupler or ellipsometer, the change in refractive index being less than 0.08, such as less than 0.01, less than 0.02, less than 0.03, less than 0.04, less than 0.05, less than 0.06, less than 0.
07.
53. A nanocomposite material comprising a cured film, the cured film comprising at least partially terminated core-shell TiO nanocrystals with an outer shell comprising a shell metal oxide and at least one monomer, oligomer and / or polymer, wherein the at least partially terminated core-shell TiO nanocrystals are present in an amount greater than 50% by weight of the nanocomposite material, wherein the film having a thickness of 1 micron has a transmittance of greater than 80% at a wavelength of 400 nm or above, and the film has a refractive index of about 1.60 to about 2.20 measured using a prism coupler or an ellipsometer.
54. according to the nanocomposite material described in claim 53, wherein the described film with<5 μ m thickness is heat-stable when being subjected to the temperature higher than 200 ℃ and continues 5min, wherein the variation of b* measured by haze meter is less than 1%, or less than 5%, or less than 10%, or less than 15%, or less than 20%, or less than 25%, and the variation of haze percentage is less than 1%, or less than 5%, or less than 10%, or less than 15%, or less than 20%, or less than 25%.
55. according to the nanocomposite film described in any one of claim 53 and 54, wherein said at least partially terminated core-shell structured TiO2 nanocrystals have an average particle size greater than 3nm but less than 50nm measured by TEM and a shell thickness of 0.2nm to 3nm measured by TEM.
56. The nanocomposite film of any one of claims 53-55, wherein the at least partially end-capped core-shell structured TiO2 nanocrystals are end-capped with at least one end-capping agent selected from the group consisting of methyltrimethoxysilane, ethyltrimethoxysilane, n-propyltrimethoxysilane, n-propyltriethoxysilane, n-octyltrimethoxysilane, n-octyltriethoxysilane, phenyltrimethoxysilane, dodecyltrimethoxysilane, m-, p-ethylphenethyltrimethoxysilane, 2-[methoxy(polyethyleneoxy)propyl]-trimethoxysilane, methoxy(trivinyloxy)propyltrimethoxysilane, 3-aminopropyltrimethoxysilane, 3-mercaptopropyltrimethoxysilane, 3-(methacryloyloxy)propyltrimethoxysilane, 3-(acryloyloxy)propyltrimethoxysilane, 3-isocyanatopropyltriethoxysilane, 3-isocyanatopropyltrimethoxysilane, and 3-glycidoxypropyltrimethoxysilane, vinyltrimethoxysilane, allyltrimethoxysilane, 1-hexenyltrimethoxysilane, 1-octenyltrimethoxysilane, N-phenylaminopropyltrimethoxysilane, 3-(4-pyridylethyl)thiopropyltrimethoxysilane, N-(3-trimethoxysilylpropyl)pyrrole, 2- (3-Trimethoxysilylpropylthio)thiophene, (3-trimethoxysilylpropyl)diethylenetriamine, phenyltrimethoxysilane, ((chloromethyl)phenylethyl)trimethoxysilane, 2-(diphenylphosphino)ethyltriethoxysilane, 4-phenylbutyltrimethoxysilane, 2-phenylethyltrimethoxysilane, 4-biphenyltriethoxysilane, N-[3-(trimethoxysilyl)propyl]allylamine, 3-mercaptopropyltrimethoxysilane, 8-glycidyltrimethoxysilane, (3-glycidyl)trimethoxysilane, ethyl orthosilicate, heptanol, hexanol, octanol, benzyl alcohol, phenol, Ethanol, propanol, butanol, oleyl alcohol, dodecanol, octadecyl alcohol and triethylene glycol monomethyl ether, (2-{2-[2-methoxy-ethoxy]-ethoxy}-ethyl)phosphonic acid, (6-{2-[2-(2-methoxy-ethoxy)-ethoxy]-ethoxy}-hexyl)phosphonic acid, 11-acryloyloxyundecylphosphonic acid, octanoic acid, acetic acid, propionic acid, 2-[2-(2-methoxyethoxy)ethoxy]acetic acid, oleic acid, benzoic acid, stearic acid, trifluoroacetic acid, biphenyl-4-carboxylic acid, 2-(2-methoxyethoxy)acetic acid, methacrylic acid, mono-2-(methacryloyloxy)ethyl succinate, or any combination thereof.
57. The nanocomposite film of any one of claims 53-56, wherein the shell metal oxide comprises silicon dioxide, zirconium dioxide, hafnium dioxide, niobium oxide, aluminum oxide, tantalum oxide, barium titanium oxide, or any combination thereof.
58. According to the nanocomposite film described in any one of claims 53-57, the at least partially capped core-shell structured TiO2 nanocrystals have low photocatalytic activity, and the photocatalytic activity is measured by the change in b* when a 1 um thick film including the core-shell structure is measured using a haze meter before and after exposure to UV at 320nm-390nm for 100h, and the change in b* is less than 50%, such as less than 1%, or less than 5%, or less than 10%, or less than 15%, or less than 20%, or less than 25%, less than 30%, less than 40%, or less than 50%.
59. A nanocomposite film according to any one of claims 53-57, wherein the at least partially capped core-shell structured TiO2 nanocrystals have low photocatalytic activity, the photocatalytic activity being measured by the change in b* when a 1 um thick film comprising the core-shell structure is measured using a haze meter before and after exposure to UV at or above 450 nm for 1000 h, the change in b* being less than 50%, such as less than 1%, or less than 5%, or less than 10%, or less than 15%, or less than 20%, or less than 25%, less than 30%, less than 40%, or less than 50%.
60. A nanocomposite film according to any one of claims 53-57, wherein the at least partially capped core-shell structured TiO2 nanocrystals have low photocatalytic activity, the photocatalytic activity being measured by the change in refractive index when a film comprising the core-shell nanocrystals is measured before and after exposure to UV at or above 320-390 nm for 100 h using a prism coupler or ellipsometer, the change in refractive index being less than 0.08, such as less than 0.01, less than 0.02, less than 0.03, less than 0.04, less than 0.05, less than 0.06, less than 0.
07.
61. A nanocomposite film according to any one of claims 53-57, wherein the at least partially capped core-shell structured TiO2 nanocrystals have low photocatalytic activity, the photocatalytic activity being measured by the change in refractive index when a film comprising the core-shell nanocrystals is measured before and after exposure to UV at or above 450 nm for 1000 h using a prism coupler or ellipsometer, the change in refractive index being less than 0.08, such as less than 0.01, less than 0.02, less than 0.03, less than 0.04, less than 0.05, less than 0.06, less than 0.
07.
62. A device comprising a nanocomposite film according to any one of claims 53-61.