Preparation method of carbon fiber composite material artificial jaw bone
Through 3D printing technology and thermosetting molding of carbon fiber composite materials, combined with functional coatings, the problems of high density, stress shielding effect and artifacts of existing artificial jaw materials have been solved, and personalized and precise jaw repair has been achieved, providing It has excellent mechanics and biocompatibility and improves patients' quality of life.
Patent Information
- Application Number
- CN202410933263.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-12
- Publication Date
- 2024-10-15
AI Technical Summary
Existing artificial jaw materials have problems such as high density, stress shielding effect, metal artifacts and insufficient biocompatibility, making it difficult to achieve personalized and precise jaw repair and reconstruction.
3D printing technology is used to assist in the preparation of carbon fiber composite artificial jaws, and the mold is constructed using CT image data. The thermoplastic material printing mold and the thermosetting molding of carbon fiber composite materials are combined to achieve personalized customization, and a functional coating is deposited on the surface to form an excellent Mechanical properties and biocompatibility of prostheses.
It achieves personalized and precise repair of jaw defects, reduces production cycle and cost, avoids demoulding damage, provides mechanical properties and biocompatibility close to human bones, and improves patients' quality of life.
Smart Images

Figure CN118767208A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a method for preparing an artificial jaw, in particular to a method for preparing an artificial jaw made of carbon fiber composite material, and belongs to the technical field of biomedical prostheses. Background Art
[0002] Repairing and reconstructing the jaw is one of the most common surgeries for oral and maxillofacial defects. Jaw defects not only affect human chewing, voice, breathing and normal bone metabolism, but also cause facial anxiety to patients and affect their mental health. Congenital malformations, tumors or later trauma may cause damage to the jaw, and the jaw is closely connected to other facial components such as the eye socket, nose and upper lip. Its repair and reconstruction is particularly important for patients. At present, there are three main options for jaw repair and reconstruction: autologous bone transplantation, allogeneic bone transplantation and artificial bone transplantation. Among them, autologous bone transplantation is the preferred treatment option in clinical practice. Although it can achieve better treatment effects, it has problems such as limited bone sources, high surgical risks, and difficulty in bone plasticity; allogeneic bone transplantation is prone to rejection and disease transmission; therefore, artificial bone transplantation with a wide source of materials, easy processing and good biocompatibility has become the focus of medical research.
[0003] The most common artificial bone repair materials are metals and their alloys, polymers, bioceramics and composite materials. Among them, artificial bones made of titanium alloys have achieved good clinical application results, but due to the high density of metal, when the weight of the bone prosthesis is too large, the prosthesis may fall off after surgery; secondly, the elastic modulus of titanium alloy and bone tissue is quite different, which is prone to stress shielding and poor postoperative effect; when patients undergo MRI examinations, metal implants will have artifacts, affecting postoperative diagnosis. When polymers are used as bone materials, although it is easy to prepare special-shaped structures, they lack biocompatibility and antibacterial properties, and rejection reactions may also occur, increasing the risk of surgical infection. Bioceramic materials are brittle and difficult to process in traditional processing technologies, and cannot form complex structures, but their composition contains elements such as calcium and phosphorus that can be replaced through the normal metabolic pathways of the human body, and have excellent biocompatibility. Therefore, the market needs a product that can overcome the shortcomings of current artificial bone materials. Carbon materials have the advantages of light weight, good chemical stability, small rejection reaction, elastic modulus (1-40GPa) similar to human bone (1-30GPa) and good biocompatibility. They can effectively avoid or reduce the problems and difficulties brought about by the above-mentioned materials. Therefore, the preparation of artificial bones through carbon materials is of great significance in the medical field.
[0004] Chinese patent CN 112190756A first uses a weaving technique to obtain a carbon fiber composite material shaped artificial bone blank, and then uses metal, carbon material and ceramic high temperature resistant molds to assist in curing and molding. However, mold molding has problems such as long design and preparation cycle, high cost and low precision. With the improvement of living standards, personalized customization has gradually become a goal pursued by people, especially when preparing complex artificial bones such as jaws, it is required not only to restore basic functions, but also to ensure a high degree of restoration of the appearance, and mold molding cannot meet the needs of patients in some details. Therefore, personalized and precise repair and reconstruction of jaw defects has become a new goal of clinical treatment. Summary of the invention
[0005] In view of the problems existing in the prior art, the purpose of the present invention is to provide a method for preparing an artificial jaw made of carbon fiber composite materials. The method uses 3D printing technology to assist in molding, which not only can realize the one-piece molding of artificial jaw made of carbon fiber composite materials, but also can be customized according to the needs of patients with high precision, and can meet the patient's precision requirements for jaw defect reconstruction. At the same time, the obtained artificial jaw has the characteristics of light weight, good chemical stability, mechanical properties similar to those of the human body, no artifacts and good biocompatibility, which can achieve the goal of restoring function and appearance and improve the patient's quality of life after surgery. The preparation method has a short cycle, low cost, and can also be mass-produced.
[0006] In order to achieve the above technical objectives, the present invention provides a method for preparing an artificial jaw made of carbon fiber composite material, the method comprising the following steps:
[0007] 1) constructing a jaw 3D model using human CT image data, designing a jaw mold with a cavity using the 3D model, and obtaining a jaw mold blank by 3D printing using a thermoplastic material, and annealing the jaw mold blank to obtain a jaw mold;
[0008] 2) pouring a mixed slurry including chopped carbon fibers, resin, curing agent, diluent and accelerator into a jawbone mold, and then performing thermal curing and high-temperature carbonization to obtain a carbon fiber composite artificial jawbone blank;
[0009] 3) Depositing a functional coating on the surface of the carbon fiber composite material artificial jaw blank to obtain the carbon fiber composite material artificial jaw.
[0010] The preparation method of the carbon fiber composite artificial jaw of the present invention, on the one hand, realizes personalized customization of the mold through CT modeling combined with 3D printing, and the prosthesis prepared by mold-assisted molding is highly consistent with the patient's missing part, and long-term use will not produce greater friction with the autologous bone, reducing the patient's postoperative discomfort, and greatly reducing the production cycle and cost compared with the existing technology; on the other hand, the use of thermoplastic materials to print the mold can not only assist the curing and molding of the carbon fiber composite material, but also can be demolded by itself during the high-temperature curing process, avoiding damage to the blank during the demolding process; thirdly, a special slurry containing carbon fiber and resin is used to prepare the carbon fiber composite material through a casting method. The generated carbon fiber composite material has excellent mechanical, corrosion resistance, high strength and low density properties, can meet the requirements of artificial bone in terms of weight and modulus, and solves the problems of existing artificial bone materials with high density, stress shielding effect and metal artifacts, and the carbon fiber composite material does not react with human tissue, can well support the growth of surrounding tissues, and has excellent biocompatibility.
[0011] As a preferred solution, the thermoplastic material includes PET, PET-CF, PPS, PA or PA-CF. These 3D printed thermoplastic materials are commercial materials. These thermoplastic materials are preferred because they have good heat resistance and can maintain their shape for a long time without collapsing at a curing temperature of 80 to 120°C of epoxy resin. Due to the complex structure of the jawbone, its demolding process is generally difficult. By using thermoplastic materials such as PET-CF as the mold material, after the slurry is poured, heat curing and high-temperature carbonization treatment can be directly carried out. During the heating process, the thermoplastic material softens and melts and flows away, thereby avoiding damage to the blank during the demolding process.
[0012] As a preferred solution, the annealing treatment condition is: annealing at a temperature of 80 to 100°C for 8 to 12 hours. Annealing treatment can further achieve a temperature resistance of more than 150°C and reduce the internal stress of the jawbone mold, improve the mechanical properties and stability of the mold, and prevent the mold from deforming during the pouring of slurry and curing, thereby causing the final artificial jaw to fail to meet the design requirements.
[0013] As a preferred solution, the mixed slurry contains the following components by mass percentage: 48-64% chopped carbon fiber, 12-17% resin, 10-17% curing agent, 12-18% diluent, and 0.5-1.5% accelerator. The content of chopped carbon fiber is very important. If its content ratio is too low, the jaw prosthesis formed will have more macropores and lower fineness; if its content is too high, it will not be easy to cast successfully. The ratio of resin and curing agent needs to be coordinated. If the ratio is not coordinated, it will lead to poor curing effect and the carbon fiber cannot be effectively bonded and formed.
[0014] As a more preferred solution, the chopped carbon fiber is PAN-based carbon fiber with a specification of 1 to 6k;
[0015] As a more preferred solution, the resin includes epoxy resin and / or thermosetting phenolic resin. The epoxy resin or thermosetting phenolic resin is preferably used mainly because of its high high temperature residual carbon content, good rheological properties, viscosity, and good compatibility with carbon fiber. Epoxy resins include E-44, E-51, E-42, E-35, etc. Thermosetting phenolic resins include 616, 2130, 2124, 2127, etc.
[0016] As a more preferred solution, the curing agent is at least one of aliphatic polyamine, aromatic polyamine and low molecular weight polyamide; aliphatic polyamines such as ethylenediamine, triethylenetetramine, etc. Aromatic polyamines such as m-xylylenediamine, etc. Low molecular weight polyamides such as polyamide resin curing agents 650, 651, etc.
[0017] As a more preferred solution, the diluent is alcohol and / or ketone; alcohols are small molecule alcohol solvents such as ethanol, ketones are acetone, etc.
[0018] As a more preferred solution, the accelerator is an amine accelerator, such as triethylamine, hexamethylenetetramine, etc.
[0019] As a preferred solution, the heat curing conditions are: heat curing at 80-120° C. for 1-5 hours.
[0020] As a preferred solution, the high temperature carbonization conditions are: in a N2 protective atmosphere, at a high temperature of 1100 to 1600°C, carbonization for 5 to 20 hours.
[0021] As a preferred solution, the functional coating is at least one of a PyC coating, a ZrO2 coating, a Si coating, a SiC coating, and a DLC coating. These functional coatings can be selected as needed. On the one hand, the PyC coating can fill the small holes on the surface of the carbon fiber composite material to form a dense layer and improve the surface strength of the prosthesis. On the other hand, it can be used as a transition layer to facilitate the deposition of other coatings. The ZrO2 coating and the Si coating can not only improve the strength and fracture toughness of the prosthesis, but also have a light-colored coating color and will not produce a black skin effect, which helps to enhance the patient's self-confidence. The SiC coating and the DLC coating have high hardness and low friction coefficient, which can improve the hardness and wear resistance of the prosthesis surface, and play a role in protecting the ZrO2 coating or other coatings. In addition, the biocompatibility of the prosthesis surface is improved, which is conducive to tissue growth. These coatings can be arbitrarily selected one or several superpositions.
[0022] As a preferred solution, the PyC coating is generated by chemical vapor deposition, and the conditions of chemical vapor deposition are: using a hydrocarbon gas carbon source, at 0.5 to 3 kPa, at a temperature of 900 to 1500° C., and for 10 to 100 hours.
[0023] As a preferred solution, the ZrO2 coating is formed by arc ion plating. The conditions of arc ion plating are: the target material is metal zirconium with a purity of more than 99wt%, and the vacuum degree is 0.5×10 -1 ~3×10 -1 Pa, workpiece negative bias voltage is 100-300V, Ar flow rate is 50-120sccm, O2 flow rate is 200-400sccm, arc voltage is 20-60V, arc current is 40-80A, working temperature is 250-350℃, and time is 10-60min.
[0024] As a preferred solution, the Si coating, SiC coating or DLC coating is formed by magnetron sputtering, and the conditions of magnetron sputtering are: the target material is a silicon target, a silicon carbide target or a graphite target with a purity of more than 99.9wt%, and the vacuum degree is 1×10 -1 ~5×10 -1 Pa, the negative bias voltage of the workpiece is 10-200 V, the Ar flow rate is 50-120 sccm, the ion source power is 0.5-5 kW, the target power is 1-3 kW, the operating temperature is 80-200 ° C, and the time is 10-60 min.
[0025] The present invention provides a method for preparing an artificial jaw made of carbon fiber composite material, comprising the following specific steps:
[0026] 1. Jaw data collection and processing:
[0027] 1.1 Data collection: Use a CT scanner to collect three-dimensional data of the patient's jaw defect;
[0028] 1.2 Data processing: The symmetrical jaw shape is obtained through the mirror inversion technology, and the jaw STL file is obtained by using UG or Solid Works or Creo or CATIA software;
[0029] 2. Preparation of jaw mold:
[0030] 2.1 Model processing: Slice the smoothed jaw STL file through slicing software such as ideaMaker, Cura, Lychee or Reprtier to obtain a hollow jaw mold, create a jaw G-Code file and store it in a USB flash drive;
[0031] 2.2 Printing mold: Insert the USB disk containing the G-Code file into the Forge1 printer and print a hollow jawbone mold made of PET-CF (PET, PPS, PA or PA-CF, etc.) thermoplastic material;
[0032] 2.3 Annealing treatment: The cooled and formed jawbone mold is annealed at 80-100°C for 8-12 hours to reduce the internal stress of the material and improve the mechanical properties and temperature resistance of the material;
[0033] 3. Preparation of carbon fiber composite artificial jaw:
[0034] 3.1 Preparation of slurry: 48-64% chopped carbon fiber, 12-17% resin, 10-17% curing agent, 12-18% diluent, 0.5-1.5% accelerator. Mix evenly according to the mass percentage to obtain a mixed slurry, and then inject the mixed slurry into the above-mentioned hollow jaw mold by vacuum negative pressure, pressure casting or vibration. When pouring, the hollow jaw mold should be preheated at 30-50°C in advance to reduce the occurrence of bubbles and defects;
[0035] 3.2 Curing and molding: After pouring, the jawbone mold containing the mixed slurry is heated and cured at 80-120°C for 1-5 hours under the action of the curing agent and accelerator;
[0036] 3.3 High-temperature carbonization: The cast jaw mold is carbonized in a N2 atmosphere at a high temperature of 1100-1600°C for 5-20h, and the carbon fiber composite artificial jaw blank is obtained after cleaning and polishing; and a PyC coating and / or a ZrO2 coating and / or a Si coating and / or a SiC coating and / or a DLC coating is deposited on its surface. The PyC coating is generated by chemical vapor deposition. The conditions of chemical vapor deposition are: using a hydrocarbon gas carbon source, at 0.5-3kPa, at a temperature of 900-1500°C, and for 10-100h; the ZrO2 coating is generated by arc ion plating. The conditions of arc ion plating are: the target material is metal zirconium with a purity of more than 99wt%, and the vacuum degree is 0.5×10 -1 ~3×10 -1 Pa, the workpiece negative bias voltage is 100-300V, the Ar flow rate is 50-120sccm, the O2 flow rate is 200-400sccm, the arc voltage is 20-60V, the arc current is 40-80A, the working temperature is 250-350℃, and the time is 10-60min; the Si coating, SiC coating or DLC coating is generated by magnetron sputtering, and the conditions of magnetron sputtering are: the target material is a silicon target, a silicon carbide target or a graphite target with a purity of more than 99.9wt%, and the vacuum degree is 1×10 -1 ~5×10 -1Pa, the negative bias voltage of the workpiece is 10-200 V, the Ar flow rate is 50-120 sccm, the ion source power is 0.5-5 kW, the target power is 1-3 kW, the working temperature is 80-200 ° C, and the time is 10-60 min; finally, cleaning, disinfection and sterilization are carried out to obtain a carbon fiber composite artificial jaw.
[0037] The carbon fiber composite material artificial jaw of the present invention has good mechanical properties, such as bending strength ≥118MPa, bending modulus ≥13GPa, which is close to human bones and meets the needs of patients.
[0038] Compared with the prior art, the technical solution of the present invention has the following advantages:
[0039] 1) Compared with the existing CNC subtractive processing and metal casting technologies, the 3D printing mold-assisted molding technology of the present invention has obvious advantages in preparation cycle and process complexity. The mold prepared by the present invention is integrally formed using 3D printing technology, and does not require additional preparation of negative and positive molds. It is simpler and more time-saving, and the printed mold is also more refined. When the mold parameters change and need to be modified and verified again or multiple times, 3D printing is fast and can save materials, reduce the preparation cycle cost, and the molded prosthesis is highly consistent with the patient's missing part. Long-term use will not produce large friction with the autologous bone, reducing the patient's discomfort after surgery.
[0040] 2) For a complex structure like the jawbone, the demoulding process is relatively difficult. The mold material of the present invention is a thermoplastic material such as PET-CF or PPS. After the slurry is poured, a high-temperature carbonization treatment is performed to directly obtain a carbon fiber composite material. Not only does it make full use of the mold and omit the demoulding step, but the carbon fiber composite material has excellent mechanical, corrosion resistance, high strength and low density properties, which can meet the requirements of artificial bones in terms of weight and modulus, and solve the problems of existing artificial bone materials with high density, stress shielding effect and metal artifacts. Secondly, the carbon fiber composite material does not react with human tissue, can well support the growth of surrounding tissues, and has excellent biocompatibility. Therefore, the carbon fiber composite jaw prosthesis of the present invention can provide dual protection of mechanics and biology, which is beneficial to the patient's postoperative recovery.
[0041] 3) A functional coating is deposited on the surface of the mandibular prosthesis to prevent the carbon material from falling off, thus avoiding the problem of the patient's facial appearance being affected by the friction and shedding of the material in the later stage of implantation, and reducing the possibility of the patient needing a secondary repair. The color is bone-like, avoiding the black skin effect after long-term implantation and improving the patient's quality of life after surgery. BRIEF DESCRIPTION OF THE DRAWINGS
[0042] Figure 1The present invention is a flow chart of the preparation process of the carbon fiber composite material artificial jaw.
[0043] Figure 2 Front and back views of the carbon fiber composite artificial jaw designed for Example 1 of the present invention.
[0044] Figure 3 These are the front and back views of the carbon fiber composite material artificial jaw prepared in Example 1 of the present invention.
[0045] Figure 4 The microscopic morphology of the surface of the carbon fiber composite material artificial jaw prepared in Example 1 and Comparative Example 1 of the present invention. DETAILED DESCRIPTION
[0046] The following specific examples are intended to further illustrate the present invention rather than to limit the scope of protection of the claims.
[0047] Example 1
[0048] 1) Use a CT scanner to collect three-dimensional data of the patient's jaw defect, obtain a symmetrical jaw morphology through mirror inversion technology, and use UG software to obtain the jaw STL file.
[0049] 2) The smoothed jaw STL file was sliced using ideaMaker software to obtain a hollow jaw mold, and the jaw G-Code file was created and stored in a USB flash drive. The data was then input into the Forge 1 printer to print a hollow jaw mold made of PET-CF composite material with a thickness of 1.0 mm. The cooled and molded jaw mold was annealed at 100°C for 8 hours to reduce the internal stress of the material and improve the mechanical properties and temperature resistance of the material.
[0050] 3) After epoxy resin E-44 is diluted with anhydrous ethanol solution, short-cut carbon fiber is added and stirred evenly, and then polyamide resin curing agent 651 and a small amount of triethylamine accelerator are added, and the mixed slurry is obtained evenly. The mass percentage of each component is 56% short-cut carbon fiber, 15% epoxy resin, 14% curing agent, 14.5% diluent, and 0.5% accelerator. The hollow jaw mold that has been preheated at 40°C for 3h is placed on a vibration table, and the mixed slurry is poured into the mold, and the vibration table switch is turned on at the same time. The vibration amplitude is 1mm to reduce bubbles and defects. After the pouring is completed, it is cured at 100°C for 2h to obtain a carbon fiber composite resin jaw mold.
[0051] 4) The mandibular mold is placed in a deposition furnace, and carbonized at 1100°C for 15 hours with N2 as protective gas to obtain a carbon fiber composite artificial mandibular blank.
[0052] 5) At 1.5 kPa and 1300 °C, natural gas was used as a carbon source to deposit a PyC coating on the surface of the above-mentioned blank for 10 h. The surface was polished and cleaned, and then a ZrO2 coating was formed by arc ion plating. Specifically, a zirconium target with a purity of 99 wt% was used in a vacuum of 1×10 -1 Pa, workpiece negative bias voltage 150V, Ar flow rate 100sccm, O2 flow rate 300sccm, arc voltage 30V, arc current 40A and working temperature 300℃ surface deposition for 20min. The DLC coating is a graphite target with a purity of 99.9wt% in a vacuum of 4×10 -1 Pa, workpiece negative bias voltage 100V, Ar flow rate 50sccm, ion source power 1kW, graphite target power 1.5kW and temperature 180℃ were used for magnetron sputtering surface deposition for 40min. Finally, cleaning, disinfection and sterilization were performed to obtain a carbon fiber composite artificial jaw.
[0053] 6) The bending strength of the carbon fiber composite artificial jaw is 125MPa, the bending modulus is 15GPa, and there are obvious pores. Figure 4 a. It is beneficial to the growth of tissue cells in the later stage.
[0054] Example 2
[0055] 1) Use a CT scanner to collect three-dimensional data of the patient's jaw defect, obtain a symmetrical jaw morphology through mirror inversion technology, and use UG software to obtain the jaw STL file.
[0056] 2) The smoothed jaw STL file was sliced using ideaMaker software to obtain a hollow jaw mold, a jaw G-Code file was created and stored in a USB flash drive, and then the data was input into the Forge1 printer to print a hollow jaw mold made of PET material with a thickness of 1.0 mm. The cooled and molded jaw mold was annealed at 80°C for 12 hours to reduce the internal stress of the material and improve the mechanical properties and temperature resistance of the material.
[0057] 3) After epoxy resin E-51 is diluted with anhydrous ethanol solution, short-cut carbon fiber is added and stirred evenly, and then polyetheramine resin curing agent D-400 and a small amount of triethylamine accelerator are added, and the mixed slurry is obtained evenly. The mass percentage of each component is 54% short-cut carbon fiber, 17% epoxy resin, 14% curing agent, 14% diluent, and 1% accelerator. The hollow jaw mold that has been preheated at 40°C for 3h is placed on a vibration table, and the mixed slurry is poured into the mold, and the vibration table switch is turned on at the same time. The vibration amplitude is 2mm to reduce bubbles and defects. After the pouring is completed, it is cured at 80°C for 3h to obtain a carbon fiber composite resin jaw mold.
[0058] 4) The mandibular mold is placed in a deposition furnace, and carbonized at 1100°C for 18 hours with N2 as protective gas to obtain a carbon fiber composite artificial mandibular blank.
[0059] 5) At 1.5 kPa and 1200 °C, natural gas was used as a carbon source to deposit a PyC coating on the surface of the above green body for 20 h. The surface was polished and cleaned, and then a ZrO2 coating was formed by arc ion plating. Specifically, a zirconium target with a purity of 99 wt% was used in a vacuum of 1×10 -1 Pa, workpiece negative bias voltage 150V, Ar flow rate 100sccm, O2 flow rate 300sccm, arc voltage 30V, arc current 50A and working temperature 300℃ surface deposition 40min. DLC coating is a graphite target with a purity of 99.9wt% in a vacuum of 4×10 -1 Pa, workpiece negative bias voltage 100V, Ar flow rate 50sccm, ion source power 1kW, graphite target power 2kW and working temperature 180℃ were used for magnetron sputtering surface deposition for 20min. Finally, cleaning, disinfection and sterilization were performed to obtain the carbon fiber composite artificial jaw.
[0060] 6) The flexural strength of the carbon fiber composite artificial jaw is 118MPa, the flexural modulus is 13GPa, and there are obvious pores, which are conducive to the growth of tissue cells in the later stage.
[0061] Example 3
[0062] 1) Use a CT scanner to collect three-dimensional data of the patient's jaw defect, obtain a symmetrical jaw morphology through mirror inversion technology, and use UG software to obtain the jaw STL file.
[0063] 2) The smoothed jaw STL file was sliced using ideaMaker software to obtain a hollow jaw mold, and the jaw G-Code file was created and stored in a USB flash drive. The data was then input into the Forge 1 printer to print a hollow jaw mold made of PA-CF material with a thickness of 1.5 mm. The cooled and molded jaw mold was annealed at 100°C for 10 hours to reduce the internal stress of the material and improve its mechanical properties and temperature resistance.
[0064] 3) Epoxy resin E-44 and phenolic resin 2130 are mixed in a ratio of 7:3, diluted with acetone solution, added with chopped carbon fiber and stirred evenly, and then polyamide resin curing agent 651 and a small amount of triethylamine accelerator are added, and stirred evenly to obtain a mixed slurry, wherein the mass percentage of each component is 56% chopped carbon fiber, 17% resin, 11.5% curing agent, 15% diluent, and 0.5% accelerator. The hollow jaw mold and the mixed slurry that have been preheated at 30°C for 3h are placed in a vacuum casting machine, the vacuum pump is turned on, and the mixed slurry is injected into the mold through a nozzle. After the casting is completed, it is cured at 80°C for 4h to obtain a carbon fiber composite resin jaw mold.
[0065] 4) The jawbone mold is placed in a deposition furnace, and carbonized at 1500°C for 8 hours with N2 as the protective gas to obtain a carbon fiber composite artificial jawbone blank.
[0066] 5) At 1.5 kPa and 1500 °C, natural gas was used as a carbon source to deposit a PyC coating on the surface of the above green body for 10 h. The surface was polished and cleaned, and then a ZrO2 coating was formed by arc ion plating. Specifically, a zirconium target with a purity of 99 wt% was used in a vacuum of 2×10 -1 Pa, workpiece negative bias voltage 100V, Ar flow rate 100sccm, O2 flow rate 300sccm, arc voltage 40V, arc current 40A and working temperature 350℃ surface deposition for 30min. Then DLC coating was further generated. The DLC coating was prepared by graphite target with purity of 99.9wt% under vacuum degree of 3×10 -1 Pa, workpiece negative bias voltage 150V, Ar flow rate 100sccm, ion source power 2kW, graphite target power 2kW and temperature 150℃ were used for magnetron sputtering surface deposition for 30min. Finally, cleaning, disinfection and sterilization were performed to obtain a carbon fiber composite artificial jaw.
[0067] 6) The flexural strength of the carbon fiber composite artificial jaw is 130MPa, the flexural modulus is 18GPa, and there are obvious pores, which are conducive to the growth of tissue cells in the later stage.
[0068] Comparative Example 1
[0069] Steps 1) to 5) are the same as those in Example 1, except that the mass percentages in the mixed slurry are changed to: 40% chopped carbon fiber, 15% epoxy resin, 14% curing agent, 30.5% diluent, and 0.5% accelerator.
[0070] 6) The bending strength of the carbon fiber composite artificial jaw is 89MPa, the bending modulus is 9GPa, the macropores are significantly increased, and the shape refinement of the jaw prosthesis is reduced. Figure 4 b.
[0071] Comparative Example 2
[0072] Steps 1) to 5) are the same as those in Example 1, except that the mass percentages in the mixed slurry are changed to: 30% chopped carbon fiber, 15% epoxy resin, 14% curing agent, 40.5% diluent, and 0.5% accelerator.
[0073] 6) The bending strength of the carbon fiber composite material artificial jaw is 50 MPa, the bending modulus is 7 GPa, the number of macropores is significantly increased, and the shape refinement of the jaw prosthesis is further reduced compared with Comparative Example 1.
Claims
1. A method for preparing an artificial jaw made of carbon fiber composite material, characterized in that: The following steps are involved: 1) constructing a jaw 3D model using human CT image data, designing a jaw mold with a cavity using the 3D model, and obtaining a jaw mold blank by 3D printing using a thermoplastic material, and annealing the jaw mold blank to obtain a jaw mold; 2) pouring a mixed slurry including chopped carbon fibers, resin, curing agent, diluent and accelerator into a jawbone mold, and then performing thermal curing and high-temperature carbonization to obtain a carbon fiber composite artificial jawbone blank; 3) Depositing a functional coating on the surface of the carbon fiber composite material artificial jaw blank to obtain the carbon fiber composite material artificial jaw.
2. The method for preparing an artificial jaw made of carbon fiber composite material according to claim 1, characterized in that: The thermoplastic material is PET, PET-CF, PPS, PA or PA-CF.
3. The method for preparing an artificial jaw made of carbon fiber composite material according to claim 1, characterized in that: The annealing treatment conditions are: annealing at a temperature of 80 to 100° C. for 8 to 12 hours.
4. The method for preparing an artificial jaw made of carbon fiber composite material according to claim 1, characterized in that: The mixed slurry contains the following components in percentage by weight: 48-64% of chopped carbon fibers, 12-17% of resin, 10-17% of curing agent, 12-18% of diluent, and 0.5-1.5% of accelerator.
5. The method for preparing an artificial jaw made of carbon fiber composite material according to claim 1 or 4, characterized in that: The chopped carbon fiber is a PAN-based carbon fiber with a specification of 1 to 6k; The resin includes epoxy resin and / or thermosetting phenolic resin; The curing agent is at least one of aliphatic polyamines, aromatic polyamines, and low molecular weight polyamides; The diluent is alcohol and / or ketone; The accelerator is an amine accelerator.
6. The method for preparing an artificial jaw made of carbon fiber composite material according to claim 1, characterized in that: The heat curing conditions are: heat curing at 80-120° C. for 1-5 hours.
7. The method for preparing an artificial jaw made of carbon fiber composite material according to claim 1, characterized in that: The high temperature carbonization conditions are: carbonization at 1100-1600° C. for 5-20 hours in a N 2 atmosphere.
8. The method for preparing an artificial jaw made of carbon fiber composite material according to claim 1, characterized in that: The functional coating is at least one of a PyC coating, a ZrO2 coating, a Si coating, a SiC coating, and a DLC coating.
9. The method for preparing an artificial jaw made of carbon fiber composite material according to claim 8, characterized in that: The PyC coating is generated by chemical vapor deposition, and the conditions of chemical vapor deposition are: using a hydrocarbon gas carbon source, at 0.5-3 kPa, at a temperature of 900-1500° C., and for 10-100 hours; The ZrO2 coating is formed by arc ion plating. The conditions of arc ion plating are: the target material is metal zirconium with a purity of more than 99wt%, the vacuum degree is 0.5×10 -1 ~3×10 -1 Pa, workpiece negative bias voltage is 100-300V, Ar flow rate is 50-120sccm, O2 flow rate is 200-400sccm, arc voltage is 20-60V, arc current is 40-80A, working temperature is 250-350℃, and time is 10-60min; The Si coating, SiC coating or DLC coating is formed by magnetron sputtering. The conditions of magnetron sputtering are: the target material is a silicon target, a silicon carbide target or a graphite target with a purity of more than 99.9wt%, and the vacuum degree is 1×10 -1 ~5×10 -1 Pa, the negative bias voltage of the workpiece is 10-200 V, the Ar flow rate is 50-120 sccm, the ion source power is 0.5-5 kW, the target power is 1-3 kW, the operating temperature is 80-200 ° C, and the time is 10-60 min.