Preparation method of hydrodemetallization catalyst

By modifying aluminum oxide compounds and rolling ball forming technology, a catalyst with a gradient pore structure is prepared, which solves the problems of reduced activity and insufficient matching of existing catalysts, and achieves efficient hydrogenation and activity of high-impurity heavy residual oil. Improved stability.

CN118767936AActive Publication Date: 2024-10-15CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202310357034.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-04-06
Publication Date
2024-10-15
Estimated Expiration
2043-04-06

AI Technical Summary

Technical Problem

During the heavy oil hydrogenation process, existing hydrogenation catalysts suffer from a decrease in apparent activity and poisoning of active centers due to the deposition of heavy and residual oil molecules. In addition, the matching between active metals and catalyst pores is insufficient, making it difficult to effectively treat heavy residual oil with high impurity content.

Method used

After roasting aluminum nitrate, it is treated with an impregnation solution containing W and Co, and hydrothermal treatment is carried out in a propylene oxide solution to form modified flaky pseudo-boehmite. Combined with rolling ball forming technology, an oxidized composite with a gradient pore structure is prepared. An aluminum carrier is used to load Mo and Ni active metals on it to improve the matching between the pore volume of the catalyst and the active metals.

Benefits of technology

It significantly improves the activity and stability of the catalyst, reduces metal and carbon deposition, is suitable for the hydrotreating of heavy residual oil with high impurity content, and extends the operating cycle of the catalyst.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118767936A_ABST
    Figure CN118767936A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a hydrodemetallization catalyst, which comprises the following steps: roasting aluminum nitrate, carrying out impregnation treatment by using an impregnation liquid containing W and Co, drying, and roasting to obtain a modified aluminum oxide compound; (2) putting the modified aluminum oxide into an epoxy propane solution, and carrying out sealed hydrothermal treatment to obtain modified flaky pseudo-boehmite HP; (3) mixing pseudo-boehmite P2 with HP to obtain a mixed material H1, and carrying out rolling ball molding on H1 to obtain a spherical precursor S1; (4) mixing pseudo-boehmite P2 with HP to obtain a mixed material H2, then mixing the spherical precursor S1 with H2, and continuing rolling ball forming to obtain a spherical precursor S2; and (5) mixing HP and S2, carrying out rolling ball molding, drying, roasting, and loading Mo and Ni to obtain the hydrodemetallization catalyst. The heavy residual oil hydrotreating agent prepared by the method is especially suitable for hydrotreating processes of heavy residual oil with relatively high content of impurities such as colloid and asphaltene.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of catalyst preparation, and specifically relates to a method for preparing a hydrogenation demetallization catalyst. Background Art

[0002] With the heavy and inferior quality of crude oil and the increasing market demand for high-quality light fuel oil, inferior heavy oil processing technology has become a key research direction for major oil companies and petroleum research institutions. Among them, hydroprocessing technology is one of the most effective technical solutions to improve the quality of inferior heavy oil and provide high-quality raw oil for downstream devices, and it is currently receiving widespread attention. Heavy and residual oil molecules have complex three-dimensional structures. During the catalytic hydrogenation process, heavy oil macromolecules are adsorbed and deposited on the surface or pores of the catalyst, which increases the diffusion resistance in the reaction and causes the apparent activity of the catalyst to decrease. At the same time, heavy and residual oils contain more coke precursors, which will generate coke and deposit in the pores under certain conditions, causing the active center of the catalyst to be poisoned. Therefore, catalysts with larger pore volume and larger pore diameter have strong metal and carbon storage capacity, which can slow down the deactivation of the catalyst and extend the operation cycle of the catalyst.

[0003] CN201510191156.7 discloses a heavy oil hydrogenation catalyst and a preparation method thereof. The catalyst comprises an alumina carrier composed of flaky polycrystalline γ-alumina and a hydrogenation active metal. The preparation method of the catalyst is as follows: adding a binder and an extrusion aid to the flaky γ-polycrystalline alumina raw powder, kneading, molding, drying and calcining to obtain an alumina carrier, and loading the active metal on the obtained alumina carrier by a conventional method. The preparation method of the flaky γ-polycrystalline alumina comprises the following steps: (1) mixing an inorganic aluminum salt, a low-carbon alcohol and / or water, and a low-carbon alkylene oxide uniformly to form a gel, and then aging the gel; (2) soaking the gel obtained in step (1) with a low-carbon alcohol, and then drying and calcining; (3) immersing the material obtained in step (2) in ammonia water for closed hydrothermal treatment, solid-liquid separation, and drying to obtain a flaky γ-polycrystalline alumina raw powder. This invention adjusts the pore structure of the carrier by adding flaky polycrystalline γ-alumina into the alumina carrier. However, the preparation process of flaky polycrystalline γ-alumina is relatively complicated. On the other hand, the matching degree between the active metal component and the catalyst pore needs to be further improved.

[0004] CN104646008A discloses a catalyst for demetallization of inferior heavy oil by hydrodesulfurization and a preparation method thereof. The catalyst uses alumina as a carrier, and group VIII and VIB elements, especially Ni-Mo, as active components. The catalyst has a pore volume of 0.61-0.70 mL / g and a specific surface area of ​​155-200 m 2 / g, and the average pore diameter is 13.0-18.0nm. The preparation method of the catalyst is to treat the carrier particles after forming and calcining with an acid solution with continuously increasing concentration. Although this method can make the average pore diameter of the final catalyst gradually increase along the radial direction of the catalyst particles from the center to the outer surface, this treatment method is difficult to form larger pores on the carrier surface. Summary of the invention

[0005] In view of the shortcomings of the prior art, the present invention provides a method for preparing a hydrodemetallization catalyst. The hydrodemetallization catalyst prepared by the method has wide pores on the surface, and the high-activity hydrodemetallization active sites have a high degree of matching with the catalyst pores. The hydrodemetallization catalyst is particularly suitable for use in the hydroprocessing process of heavy residue oil with a high content of impurities such as colloids and asphaltene.

[0006] The preparation method of the hydrodemetallization catalyst of the present invention comprises the following contents: (1) Calcine aluminum nitrate, impregnate the calcined material with an impregnation solution containing W and Co, dry it, The modified aluminum oxide compound is obtained by calcination; (2) crushing and sieving the modified aluminum oxide compound, placing the sieving material in a sealed propylene oxide solution for hydrothermal treatment, and drying the treated material to obtain modified flaky pseudo-boehmite HP; (3) Pseudo-boehmite P2 and modified flaky pseudo-boehmite HP are mixed to obtain a mixed material H1. The mixed material H1 is formed by rolling balls to obtain a spherical precursor S1; (4) Mixing pseudo-boehmite P2 with modified flaky pseudo-boehmite HP A mixed material H2 is obtained, and then the spherical precursor S1 is mixed with the mixed material H2 and continuously subjected to ball forming to obtain a spherical precursor S2; (5) The modified flaky pseudo-boehmite HP is mixed with the spherical precursor S2, and then rolled into a ball, and then dried and calcined to obtain a modified alumina carrier; (6) The modified alumina carrier is impregnated with an impregnation solution containing Mo and Ni. The impregnated material is dried and calcined to obtain a hydrogenation demetallization catalyst.

[0007] In the method of the present invention, the calcination temperature of the aluminum nitrate in step (1) is 450-650° C., and the calcination time is 4-8 hours.

[0008] In the method of the present invention, in the impregnation solution containing W and Co in step (1), W is in the form of WO 3The concentration is 1g / 100mL-3.5g / 100mL, the concentration of Co as CoO is 0.3g / 100mL-1.0g / 100mL, the impregnation is carried out by over volume impregnation, the impregnation time is 0.5-2 hours, the drying conditions of the impregnated material are 80-140℃ for 4-8 hours, and the roasting conditions are 400-550℃ for 4-8 hours.

[0009] In the method of the present invention, the pulverization in step (2) is performed to a particle size greater than 100 mesh.

[0010] In the method of the present invention, the concentration of the propylene oxide solution in step (2) is 2.5wt%-12wt%, preferably 4wt%-8wt%, and the mass ratio of the propylene oxide solution to the modified aluminum oxide compound is 3:1-10:1, preferably 4:1-8:1.

[0011] In the method of the present invention, the sealed hydrothermal treatment in step (2) is carried out in a sealed container, which is preferably an autoclave. The hydrothermal treatment temperature is 110-180°C, preferably 120-160°C, and the treatment time is 4-8 hours. The pressure in the sealed container during the hydrothermal treatment is autogenous pressure.

[0012] In the method of the present invention, the drying temperature in step (2) is generally 80-160° C., and the drying time is 4-8 hours.

[0013] In the method of the present invention, the pseudo-boehmite P2 particles described in step (3) are generally in granular form and may be a commercially available product or pseudo-boehmite prepared by methods such as acid precipitation, alkali precipitation, alcohol aluminum hydrolysis, etc., preferably pseudo-boehmite having a pore size greater than 10 nm.

[0014] In the method of the present invention, the mass ratio of the modified flaky pseudo-boehmite HP to the pseudo-boehmite P2 in the H1 mixed material in step (3) is 1:9-1:3.

[0015] In the method of the present invention, the ball forming in step (3) is carried out in a turntable forming machine, and the rotation operating conditions of the turntable forming machine are: the inclination angle of the turntable is 40-70°, the rotation speed of the turntable is 10-30rpm; the forming time of the material in the turntable is 10-120min. The radius of the spherical precursor S1 is 0.2r-0.5r, wherein r is the radius of the final modified alumina carrier, that is, the straight-line distance from the center of the sphere to the outer surface. During the ball forming process, an aqueous solution containing a gelling agent is sprayed into the material; the aqueous solution containing a gelling agent is one or a mixture of aqueous solutions of nitric acid, phosphoric acid, oxalic acid, and acetic acid, and the mass concentration of the solution is 1%-3%, preferably an aqueous solution of acetic acid.

[0016] In the method of the present invention, the mass ratio of the modified flaky pseudo-boehmite HP to the pseudo-boehmite P2 in step (4) is 3:7-1:1.

[0017] In the method of the present invention, the ball forming in step (4) is carried out in a turntable forming machine, and the rotation operating conditions of the turntable forming machine are: the inclination angle of the turntable is 40-70°, the rotation speed of the turntable is 10-30 rpm; the forming time of the material in the turntable is 10-120 min. The radius of the spherical precursor S2 is 0.5r-0.9r, wherein r is the radius of the final modified alumina carrier, that is, the straight-line distance from the center of the sphere to the outer surface. During the ball forming process, an aqueous solution containing a gelling agent is sprayed into the material; the aqueous solution containing a gelling agent is one or a mixture of aqueous solutions of nitric acid, phosphoric acid, oxalic acid, and acetic acid, and the mass concentration of the solution is 1%-3%, preferably an aqueous solution of acetic acid.

[0018] In the method of the present invention, the ball forming in step (5) is carried out in a turntable forming machine, and the rotating operating conditions of the turntable forming machine are: the inclination angle of the turntable is 40-70°, the rotation speed of the turntable is 10-30rpm; the forming time of the material in the turntable is 10-60min, and the final sphere diameter is 5-10mm. During the ball forming process, an aqueous solution containing a peptizing agent is sprayed into the material; the aqueous solution containing a peptizing agent is one or a mixture of aqueous solutions of nitric acid, phosphoric acid, oxalic acid, and acetic acid, and the mass concentration of the solution is 1%-3%, preferably an aqueous solution of acetic acid.

[0019] In the method of the present invention, the drying time in step (5) is 1-8 hours, preferably 2-6 hours, and the drying temperature is 60°C-180°C, preferably 80°C-150°C; the roasting temperature is 350-800°C, preferably 500-750°C, and the roasting time is 2-6 hours, preferably 2-4 hours.

[0020] In the method of the present invention, in the impregnation solution containing Mo and Ni in step (6), Mo is in the form of MoO 3 The concentration is 5.5g / 100mL-12.5g / 100mL, the concentration of Ni as NiO is 1.4g / 100mL-3.2g / 100mL, and equal volume impregnation is adopted during impregnation. The drying conditions of the impregnated material are 80-120℃ for 4-8 hours, and the roasting conditions are 400-550℃ for 4-8 hours.

[0021] Compared with the prior art, the present invention has the following advantages: (1) The present invention firstly calcines aluminum nitrate, and then pre-impregnates the material with active metal after calcination to obtain W and Co modified aluminum oxide compounds. When the W and Co modified aluminum oxide compounds are hydrothermally treated in a propylene oxide solution, the aluminum oxide compounds grow directionally into W and Co modified flaky pseudo-boehmite. During the hydrothermal treatment, the active metal component grows secondary with the aluminum compound. The treatment process can improve the interaction between the active metal and the flaky pseudo-boehmite. The flaky pseudo-boehmite grains are interwoven and stacked to form a large number of 50-150nm macropore channels. The content of active metal components in the macropores is relatively high, and the macropores have strong macropore volume metal and anti-carbon deposition ability. The active sites of hydrogenation reaction are well matched with the macropores, ensuring the high activity of the catalyst and making the catalyst have high activity stability. At the same time, the flaky grains support each other, which can ensure that the channels formed by the stacking are not easily destroyed when the carrier is formed. When the flaky pseudo-boehmite is used as a raw material to prepare an alumina carrier, the macropore content of the carrier can be effectively increased.

[0022] (2) The present invention selects raw materials with different morphologies and structures for step-by-step sintering during the carrier sintering process, and adjusts the pore distribution of the carrier by adjusting the content of the active metal-modified flaky pseudo-boehmite material. The macropore content and pore size distribution of the carrier obtained are gradiently distributed, that is, the surface layer has a high macropore content, a large pore size, and a wide pore, the middle layer is second, and the core layer is third. This pore structure is conducive to the diffusion of heavy residue oil reactant molecules into the interior of the catalyst, and can effectively reduce metal deposition and carbon deposition on the catalyst surface. It is particularly suitable for heavy residue oil hydroprocessing processes with high impurity contents such as metals (Ni, V), colloids, and asphaltene. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 This is a SEM image of the active metal-modified flaky pseudo-boehmite HP1 prepared in Example 1.

[0024] Figure 2 This is the SEM image of material HP5 prepared in Comparative Example 3.

[0025] Figure 3 This is the SEM image of material HP7 prepared in Comparative Example 4. Implementation

[0026] The technical scheme and technical effect of the present invention are further described below in conjunction with the embodiments, but are not limited to the following embodiments. In the present invention, wt% represents mass fraction.

[0027] BET method: Application of N 2 Physical adsorption-desorption characterization of the carrier pore structure of the embodiment and the comparative example, the specific operation is as follows: ASAP-2420 type N 2Physical adsorption-desorption instrument is used to characterize the pore structure of the sample. A small amount of sample is vacuum treated at 300℃ for 3-4 hours, and finally the product is placed in liquid nitrogen low temperature (-200℃) for nitrogen adsorption-desorption test. The specific surface area is obtained according to the BET equation, and the pore volume and the distribution rate of pore diameters below 30nm are obtained according to the BJH model.

[0028] Scanning electron microscopy was used to characterize the microstructure of the alumina carrier. The specific operation was as follows: a JSM-7500F scanning electron microscope was used to characterize the microstructure of the carrier, with an accelerating voltage of 5 KV, an accelerating current of 20 µA, and a working distance of 8 mm.

[0029] Mercury intrusion method: A mercury intrusion instrument was used to characterize the pore diameter distribution of the carriers of the embodiment and the comparative example. The specific operation is as follows: The pore distribution of the sample was characterized using the American Micromeritics AutoPore 9500 fully automatic mercury intrusion instrument. After the sample was dried, it was weighed and loaded into the dilatometer, and degassed for 30 minutes under the vacuum conditions given by the instrument, and then loaded with mercury. The dilatometer was then placed in an autoclave and vented. Then, a pressure increase and pressure reduction test was performed. The mercury contact angle was 130°, and the mercury interfacial tension was 0.485N.cm -1 The distribution rate of pores with a diameter of more than 100 nm is measured by mercury intrusion porosimetry.

[0030] The most probable pore size determination: Take the material pore size as the horizontal coordinate and the rate of change of pore volume with pore size as the vertical coordinate to obtain the pore size differential distribution curve. The peak value in the curve is the most probable pore size.

[0031] The GB / T 34099-2017 standard method was used to determine the Ni and V contents in oil products.

[0032] V+Ni removal rate % = (metal V+Ni content of crude oil - metal V+Ni content of product) / metal V+Ni content of crude oil × 100%.

[0033] Relative demetallization rate: Determine the demetallization rate of a certain catalyst, define its relative demetallization rate as 100%, and the impurity removal rate of other catalysts / defined catalyst impurity removal rate × 100% is the relative deimpurity removal rate.

[0034] Preparation of active metal modified flake pseudo-boehmite material HP: Example 1 (1) Weigh an appropriate amount of aluminum nitrate and place it in a crucible and calcine it at 550℃ for 5.5 hours. 3 The active component impregnation solution with a concentration of 2.1 g / 100 mL and a CoO concentration of 0.5 g / 100 mL was impregnated for 1 hour, and the impregnated material was calcined at 500° C. for 5 hours to obtain an active metal-modified aluminum oxide compound; (2) The active metal modified aluminum oxide compound obtained in step (1) is crushed to a size of 100 mesh or more and weighed 100 g of the sieved material was added with 650 g of propylene oxide aqueous solution with a mass concentration of 5.5%, and magnetic stirring was performed for 30 minutes. Then, the mixture was transferred into an autoclave, sealed, and heated at 130° C. for 6.5 hours. After cooling, the solid material was filtered, washed, and dried at 120° C. for 4 hours to obtain active metal-modified flaky pseudo-boehmite HP1. The microstructure of the sample was observed by scanning electron microscopy to be flaky grain accumulation, with a flaky grain size of 125-680 nm and a thickness of 30-65 nm. The scanning electron microscopy image is shown in FIG. Figure 1 .

[0035] Example 2 Same as Example 1, except that the calcination temperature of aluminum nitrate in step (1) is 500°C, the calcination time is 6.5 hours, and the active component impregnation solution contains WO 3 The concentration is 2.7 g / 100 mL, and the CoO concentration is 0.6 g / 100 mL. In step (2), the concentration of propylene oxide is 6.6%, the amount of solution is 570 g, the hydrothermal treatment temperature is 140°C, and the treatment time is 5.5 hours. Active metal-modified flaky pseudo-boehmite HP2 is obtained. Scanning electron microscopy shows that the microstructure of the sample is flaky grain accumulation, the flaky grain size is 110-650 nm, and the thickness is 25-60 nm.

[0036] Example 3 Same as Example 1, except that the calcination temperature of aluminum nitrate in step (1) is 600°C, the calcination time is 4.5 hours, and the active component impregnation solution contains WO 3 The concentration is 1.3 g / 100 mL, and the concentration of CoO is 0.3 g / 100 mL. In step (2), the concentration of propylene oxide is 4.4%, the amount of solution is 740 g, the hydrothermal treatment temperature is 100 ° C, and the treatment time is 7.5 hours. Active metal modified flaky pseudo-boehmite HP3 is obtained. The microstructure of the sample is flaky grain accumulation, the flaky grain size is 130-700 nm, and the thickness is 30-65 nm.

[0037] Example 4 Same as Example 1, except that the calcination temperature of aluminum nitrate in step (1) is 450°C, the calcination time is 7.5 hours, and the active component impregnation solution contains WO 3 The concentration is 3.2 g / 100 mL, and the CoO concentration is 0.8 g / 100 mL. In step (2), the concentration of propylene oxide is 7.8%, the amount of solution is 430 g, the hydrothermal treatment temperature is 155° C., and the treatment time is 4.5 hours. Active metal-modified flaky pseudo-boehmite HP4 is obtained. Scanning electron microscopy shows that the microstructure of the sample is flaky grain accumulation, the flaky grain size is 120-600 nm, and the thickness is 25-60 nm.

[0038] Comparative Example 1 The same as Example 1, except that the propylene oxide in step (2) was replaced by the same amount of ethylene oxide, no lamellar grains were observed in the microstructure of the material HP5 after the hydrothermal treatment.

[0039] Comparative Example 2 The same as Example 1, except that the aluminum nitrate in step (1) is replaced by aluminum sulfate, and the solid material particles are dissolved after hydrothermal treatment, and the product is not separated.

[0040] Comparative Example 3 The same as Example 1, except that the aluminum nitrate in step (1) was replaced by aluminum chloride. No lamellar grains were observed in the microstructure of the material HP6 after hydrothermal treatment. The scanning electron microscope image shows Figure 2 .

[0041] Comparative Example 4 The same as Example 1, except that the W and Co modification treatment was not performed, that is, step (1) did not use the impregnation solution containing Wo and Co active components for impregnation treatment. The scanning electron microscope image of the material after hydrothermal treatment is shown in FIG. Figure 3 .

[0042] Preparation of heavy residue hydrodemetallization catalyst: Example 5 Weigh 50 g of the active metal-modified pseudo-boehmite HP1 prepared in Example 1 and 283 g of pseudo-boehmite P2 (prepared by aluminum sulfate-sodium aluminate method, with a most probable pore size of 13.5 nm) was mixed evenly, and the mixed material was placed in a turntable molding machine for full mixing, and the inclination angle of the turntable was adjusted to 43°, and the speed of the turntable was adjusted to 15 rpm; an acetic acid aqueous solution with a mass concentration of 1% was sprayed onto the material in the turntable through a sprayer. After mixing and contacting, the material was molded in the turntable for 30 minutes, and a spherical precursor S with a diameter of 2.0-3.0 mm was obtained. 1 ; (2) Weigh 100 g of the active metal-modified flaky pseudo-boehmite HP1 prepared in Example 1 and 122 g of the pseudo-boehmite P2, mix the above materials evenly, and then add the mixed materials and the spherical precursor S prepared in step (1) to the mixture. 1 Place the mixture in a rotating disk molding machine for thorough mixing. Adjust the inclination angle of the rotating disk to 40° and the rotating speed of the rotating disk to 13 rpm. Spray an acetic acid aqueous solution with a mass concentration of 1.2% onto the material in the rotating disk through a sprayer. After mixing and contacting, the material is molded in the rotating disk for 25 minutes to obtain a spherical precursor S with a diameter of 4-5 mm. 2 ; (3) The active metal-modified flaky pseudo-boehmite HP1 prepared in Example 1 and the spherical precursor S prepared in step (2) are mixed. 2The mixture was placed in a turntable forming machine for thorough mixing, the inclination of the turntable was adjusted to 35°, the rotation speed of the turntable was 12 rpm, and an acetic acid aqueous solution with a mass concentration of 1.3% was sprayed onto the material in the turntable through a sprayer. After mixed contact, the material was formed in the turntable for 15 minutes to obtain a spherical material with a diameter of 6-8 mm. The obtained spherical material was dried at 120°C for 4 hours and calcined at 550°C for 4 hours to obtain a spherical alumina carrier.

[0043] (4) Weigh 50 g of the alumina carrier prepared in step (3), and impregnate the carrier with a Mo-Ni-P impregnation solution having a molybdenum oxide concentration of 7.6 g / 100 mL and a nickel oxide concentration of 2.1 g / 100 mL by an equal volume impregnation method. The impregnated material is dried at 120° C. for 6 h and calcined at 500° C. for 4 h to obtain the hydrodemetallation catalyst Cat-1 of the present invention. The catalyst properties are shown in Table 1.

[0044] Example 6 The same as implementation 5, except that the active metal modified flaky pseudo-boehmite HP1 in step (1), step (2) and step (3) is replaced by active metal modified flaky pseudo-boehmite HP2, the amount of pseudo-boehmite P2 added in step (1) is 200 g, and the amount of pseudo-boehmite P2 added in step (2) is 150 g, to obtain the hydrodemetallization catalyst Cat-2 of the present invention. The catalyst properties are shown in Table 1.

[0045] Example 7 The same as implementation 5, except that the active metal modified flaky pseudo-boehmite HP1 in step (1), step (2) and step (3) is replaced by active metal modified flaky pseudo-boehmite HP3, the amount of pseudo-boehmite P2 added in step (1) is 367 g, and the amount of pseudo-boehmite P2 added in step (2) is 108 g, to obtain the hydrodemetallization catalyst Cat-3 of the present invention. The catalyst properties are shown in Table 1.

[0046] Example 8 The same as implementation 5, except that the active metal modified flaky pseudo-boehmite HP1 in step (1), step (2) and step (3) is replaced by active metal modified flaky pseudo-boehmite HP4, the amount of pseudo-boehmite P2 added in step (1) is 177 g, and the amount of pseudo-boehmite P2 added in step (2) is 186 g, to obtain the hydrodemetallization catalyst Cat-4 of the present invention. The catalyst properties are shown in Table 1.

[0047] Comparative Example 4 The same as in Example 5, except that the active metal-modified flaky pseudo-boehmite HP1 in step (1), step (2) and step (3) is replaced by the material HP5 prepared in Comparative Example 1, to prepare a comparative hydrodemetallization catalyst Cat-5. The catalyst properties are shown in Table 1.

[0048] Comparative Example 5 The same as in Example 5, except that the active metal-modified flaky pseudo-boehmite HP1 in step (1), step (2) and step (3) is replaced by the material HP6 prepared in comparative example 3, to prepare comparative hydrodemetallization catalyst Cat-6. The catalyst properties are shown in Table 1.

[0049] Comparative Example 6 The same method as in Example 5 was used, except that the active metal-modified flaky pseudo-boehmite HP1 in step (1), step (2) and step (3) was replaced with the material prepared in Comparative Example 4, and the same amount of active components was loaded onto the alumina carrier by a single impregnation method to prepare a comparative hydrodemetallization catalyst Cat-7. The catalyst properties are shown in Table 1. Table 1 Catalyst properties Example 5 Example 6 Example 7 Example 8 Comparative Example 4 Comparative Example 5 Comparative Example 6 catalyst Cat-1 Cat-2 Cat-3 Cat-4 Cat-5 Cat-6 Cat-7 <![CDATA[Specific surface area, m 2 / g]]> 179 163 188 196 173 174 191 Pore ​​volume, mL / g 0.89 0.88 0.91 0.93 0.77 0.83 0.91 <![CDATA[MoO 3 Content, wt%]]> 7.8 7.6 7.6 7.5 7.7 7.9 7.8 NiO content, wt% 2.3 2.2 2.3 2.1 2.4 2.2 2.3 <![CDATA[WO 3 Content, wt%]]> 0.8 1.3 0.4 0.6 0.7 0.8 0.8 CoO content, wt% 0.2 0.4 0.1 0.2 0.3 0.2 0.3 10-20nm pore content, v% 52.1 49.3 54.4 56.8 62.4 64.3 51.7 50-100nm pore content, v% 16.4 18.1 14.3 11.9 7.3 5.8 15.9 Pore ​​content greater than 100nm, v% 15.1 17.3 13.9 12.4 2.7 2.6 14.3

[0050] The catalytic performance of the hydrodemetallization catalysts (Cat-1-Cat-6) prepared in the above examples and comparative examples was evaluated by the following method: Using a certain residual oil as raw material, the metal (Ni+V) content in the raw oil is 183μg / g, the colloid content is 57.2%, and the asphaltene content is 1.9%. The catalytic performance of the hydrodemetallization catalyst Cat-1-Cat-6 was evaluated on a 200mL small evaluation device. The reaction conditions are as follows: reaction temperature is 375℃, pressure is 14.5MPa, liquid hourly volume space velocity is 0.55h -1 The volume ratio of hydrogen to oil was 750. The contents of various impurities in the generated oil were determined after 500 hours and 3000 hours of reaction, and the impurity removal rate was calculated. The evaluation results are shown in Table 2.

[0051] Table 2 Comparison of catalyst hydrogenation performance Catalyst No. Cat-1 Cat-2 Cat-3 Cat-4 Cat-5 Cat-6 Cat-7 500 hours relative demetallization (V+Ni) rate, % 127 131 135 126 100 97 125 3000 hours relative demetallization (V+Ni) rate, % 134 139 136 130 100 88 119 It can be seen from the data in Table 2 that when the reaction time is 500 hours, the catalyst prepared by the method of the present invention has a higher hydrodemetallization activity than the comparative catalyst. When the reaction time is 3000 hours, the catalyst prepared by the method of the present invention still has a higher hydrodemetallization activity than the comparative catalyst, indicating that the hydrodemetallization catalyst has a strong ability to resist metal deposition and carbon deposition, and is particularly suitable for use in the hydroprocessing process of heavy residue oil with high impurity content such as metal (Ni, V), colloid, and asphaltene.

Claims

1. A method for preparing a hydrodemetallization catalyst, characterized in that The method comprises the following steps: (1) calcining aluminum nitrate, impregnating the calcined material with an impregnation solution containing W and Co, drying and calcining the material to obtain a modified aluminum oxide compound; (2) crushing and screening the modified aluminum oxide compound, placing the sieved material in a sealed hydrothermal treatment in a propylene oxide solution, and drying the treated material to obtain a modified flaky pseudo-boehmite HP; (3) mixing the pseudo-boehmite P2 with the modified flaky pseudo-boehmite HP to obtain a mixed material H1, and rolling the mixed material H1 into a spherical precursor S 1; (4) Pseudo-boehmite P2 is mixed with modified flaky pseudo-boehmite HP to obtain a mixed material H2, and then the spherical precursor S1 is mixed with the mixed material H2 and continuously rolled into a ball to obtain a spherical precursor S2; (5) The modified flaky pseudo-boehmite HP is mixed with the spherical precursor S2, and the mixed material H2 is rolled into a ball, and then dried and calcined to obtain a modified alumina carrier; (6) The modified alumina carrier is impregnated with an impregnation solution containing Mo and Ni, and the impregnated material is dried and calcined to obtain a hydrogenation demetallization catalyst.

2. The method according to claim 1, characterized in that: The aluminum nitrate calcination temperature in step (1) is 450-650° C., and the calcination time is 4-8 hours.

3. The method according to claim 1, characterized in that: In the impregnation solution containing W and Co in step (1), the concentration of W as WO3 is 1g / 100mL-3.5g / 100mL, and the concentration of Co as CoO is 0.3g / 100mL-1.0g / 100mL; the impregnation is carried out by over volume impregnation, and the impregnation time is 0.5-2 hours; the drying condition of the material after impregnation is 80-140°C for 4-8 hours, and the roasting condition is 400-550°C for 4-8 hours.

4. The method according to claim 1, characterized in that: The step (2) is crushing to a particle size greater than 100 mesh.

5. The method according to claim 1, characterized in that: The concentration of the propylene oxide solution in step (2) is 2.5wt%-12wt%, preferably 4wt%-8wt%.

6. The method according to claim 1, characterized in that: The mass ratio of the propylene oxide solution to the modified aluminum oxide compound is 3:1-10:1, preferably 4:1-8:

1.

7. The method according to claim 1, characterized in that: The sealed hydrothermal treatment in step (2) is carried out in a sealed container at a temperature of 110-180°C, preferably 120-160°C, for 4-8 hours. The pressure in the sealed container during the hydrothermal treatment is autogenous pressure.

8. The method according to claim 1, characterized in that: The pseudo-boehmite P2 in step (3) is in granular form, and the pseudo-boehmite has a pore size greater than 10 nm.

9. The method according to claim 1, characterized in that: In step (3), the mass ratio of the modified flaky pseudo-boehmite HP to the pseudo-boehmite P2 in the H1 mixed material is 1:9-1:

3.

10. The method according to claim 1, characterized in that: The ball forming in step (3) is carried out in a turntable forming machine, and the rotation operating conditions of the turntable forming machine are: the inclination angle of the turntable is 40-70°, the rotation speed of the turntable is 10-30 rpm; the forming time of the material in the turntable is 10-120 min; the radius of the spherical precursor S1 is 0.2r-0.5r, where r is the radius of the final modified alumina carrier, that is, the straight-line distance from the center of the sphere to the outer surface.

11. The method according to claim 1, characterized in that: The mass ratio of the modified flaky pseudo-boehmite HP to the pseudo-boehmite P2 in step (4) is 3:7-1:

1.

12. The method according to claim 1, characterized in that: The ball forming in step (4) is carried out in a rotating disk forming machine, and the rotating operation conditions of the rotating disk forming machine are: the inclination angle of the rotating disk is 40-70°, the rotating disk speed is 10-30 rpm; the forming time of the material in the rotating disk is 10-120 min. The radius of the spherical precursor S2 is 0.5r-0.9r, where r is the radius of the final modified alumina carrier, that is, the straight-line distance from the center of the sphere to the outer surface.

13. The method according to claim 1, characterized in that: The ball forming in step (5) is carried out in a turntable forming machine, and the rotation operating conditions of the turntable forming machine are: the inclination angle of the turntable is 40-70°, the rotation speed of the turntable is 10-30 rpm; the forming time of the material in the turntable is 10-60 minutes, and the final sphere diameter is 5-10 mm.

14. The method according to claim 1, characterized in that: The drying time in step (5) is 1-8 hours, preferably 2-6 hours, and the drying temperature is 60°C-180°C, preferably 80°C-150°C; the roasting temperature is 350-800°C, preferably 500-750°C, and the roasting time is 2-6 hours, preferably 2-4 hours.

15. The method according to claim 1, characterized in that: In the impregnation solution containing Mo and Ni in step (6), the concentration of Mo in terms of MoO3 is 5.5 g / 100 mL-12.5 g / 100 mL, and the concentration of Ni in terms of NiO is 1.4 g / 100 mL-3.2 g / 100 mL. During impregnation, equal volume impregnation is adopted. After impregnation, the material is dried at 80-120° C. for 4-8 hours, and calcined at 400-550° C. for 4-8 hours.

Citation Information

Patent Citations

  • Hydrodemetalization catalyst and preparation method thereof

    CN103785405A

  • Hydrogenation catalyst as well as preparation method and application thereof

    CN104549430A

  • Heavy oil hydrogenation catalyst and preparation method thereof

    CN106140180A

  • Catalyst having hydrogenation catalysis effect, preparation method and application thereof, and heavy oil hydrogenating and deasphaltenizing method

    CN108014808A

  • Preparation method of high-activity hydrodemetallization catalyst

    CN111821992A