Photocatalyst magnetized through magnetic concentrate as well as preparation method and application of photocatalyst
By coating SiO2 with γ-Fe2O3 and loading bismuth tungstate or bismuth iodide, a magnetic photocatalyst is prepared, which solves the problem of difficult photocatalyst recovery, achieves efficient degradation and low-cost wastewater treatment, and simplifies the preparation of magnetic carriers. process and has broad application prospects.
Patent Information
- Application Number
- CN202410835827.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-26
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2044-06-26
AI Technical Summary
Existing photocatalysts are difficult to recycle in mineral processing wastewater, causing secondary pollution of the water body and increasing the operating costs of wastewater treatment. Moreover, the synthetic magnetic carrier is lengthy and costly, making it difficult to promote industrialization.
Using magnetic separation concentrate γ-Fe2O3 as a carrier, by coating SiO2 and loading bismuth tungstate or bismuth iodide, a γ-Fe2O3@SiO2/Bi2WO6 or γ-Fe2O3@SiO2/BiOI photocatalyst is prepared, and its magnetic properties are used to facilitate recycling , and synthesized through mechanical stirring method and hydrothermal method to simplify the preparation process.
It achieves efficient degradation of the catalyst and good magnetic recovery, reduces operating costs, simplifies the preparation process of the magnetic carrier, and has broad industrial application prospects.
Smart Images

Figure CN118767937A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of mineral processing wastewater treatment technology, and in particular to a photocatalyst for magnetizing concentrates by magnetic separation, its preparation method and application. Background Technology
[0002] Mineral flotation processes utilize large quantities of collectors, frothers, and depressants, with xanthate being the most commonly used collector. Most xanthate enters the flotation froth product, but some remains in the mineral processing wastewater. Xanthate itself is toxic and has an irritating odor; untreated discharge will pollute water resources. Furthermore, xanthate naturally degrades in wastewater into organic matter such as CS2 (precipitate solids). CS2 is volatile and converts into SO2 in the air, polluting the atmosphere. Therefore, the thorough degradation of xanthate in mineral processing wastewater is of significant environmental importance.
[0003] Currently, the degradation technologies for residual xanthate in mineral processing wastewater can be broadly categorized into six types: coagulation sedimentation, biological methods, hydrogen peroxide methods, Fenton methods, ozone methods, and photocatalytic methods. In recent years, photocatalytic oxidation technology has gained popularity for treating organic waste in wastewater due to its economic efficiency, ease of operation, high mineralization rate, and lack of secondary pollution. It is a highly operable "green" wastewater treatment technology. Catalysts used for photocatalytic xanthate degradation include bismuth tungstate (Bi₂WO₆), bismuth oxyiodide (BiOI), and bismuth ferrite / zinc indium sulfide (Bi₂Fe₄O₉ / ZnIn₂S₄), which have good degradation effects on xanthate. However, since the photocatalyst needs to be dispersed in the wastewater to degrade xanthate, the catalyst needs to be recovered and regenerated before reuse when the xanthate molecules in the wastewater are completely degraded or the catalyst is partially deactivated. Fine-particle photocatalysts are difficult to recover through effective filtration or centrifugation, resulting in a large amount of catalyst residue in the water, causing serious secondary pollution. The loss of catalyst and the subsequent addition of fresh catalyst solution significantly increase the operating costs of wastewater treatment. Therefore, combining the catalyst with magnetic materials can improve its recyclability, thus facilitating the recycling of photocatalysts.
[0004] Currently, most magnetic supports for magnetic photocatalysts are artificially synthesized ferrites. While these materials have high purity, their synthesis process is lengthy and costly, making them unsuitable for industrial application. Therefore, simplifying the preparation steps of magnetic supports has become a pressing technical problem for those skilled in the art. Summary of the Invention
[0005] The purpose of this invention is to provide a photocatalyst that magnetizes magnetically separated concentrate, its preparation method, and its application. Magneticly separated concentrate (γ-Fe₂O₃) is used as a magnetic material and loaded onto bismuth tungstate (Bi₂WO₆) and bismuth oxyiodide (BiOI), thereby imparting magnetism to the photocatalyst for easy recovery. To ensure the degradation efficiency of the photocatalyst, γ-Fe₂O₃ is also coated with SiO₂, i.e., two photocatalysts, γ-Fe₂O₃@SiO₂ / Bi₂WO₆ and γ-Fe₂O₃@SiO₂ / BiOI, are prepared based on the degradation of residual xanthate in mineral processing wastewater using γ-Fe₂O₃@SiO₂ as the magnetic material.
[0006] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0007] This invention provides a method for preparing a photocatalyst by magnetizing magnetic separation concentrate, comprising the following steps:
[0008] 1) After ball milling, the magnetically separated concentrate is dispersed in a mixture of anhydrous ethanol, water and ammonia to obtain suspension 1;
[0009] 2) Add the mixture of tetraethyl orthosilicate and anhydrous ethanol to suspension 1 for coating to obtain γ-Fe2O3@SiO2;
[0010] 3) A magnetic photocatalyst is obtained by mixing the photocatalyst, solvent, and γ-Fe2O3@SiO2;
[0011] The photocatalyst is bismuth tungstate or bismuth oxyiodide;
[0012] When the photocatalyst is bismuth tungstate, the γ-Fe2O3@SiO2 accounts for 3-7% of the amount of bismuth tungstate.
[0013] When the photocatalyst is bismuth iodide, the γ-Fe2O3@SiO2 accounts for 5-20% of the amount of bismuth iodide.
[0014] Optionally, the content of γ-Fe2O3 in the magnetic concentrate is ≥90%;
[0015] The ball milling speed is 500–1000 r / min; the time is 60–120 min;
[0016] The particle size of the magnetically separated concentrate after ball milling is 0.5–1 μm.
[0017] Optionally, the volume ratio of the anhydrous ethanol, water, and ammonia is 50–100:10–30:1;
[0018] The ratio of the magnetic concentrate to the mixture of anhydrous ethanol, water and ammonia is 0.4-0.6g:400-500mL.
[0019] Optionally, the volume ratio of tetraethyl orthosilicate to anhydrous ethanol is 1:20 to 30.
[0020] Optionally, the ratio of the magnetic concentrate to tetraethyl orthosilicate is 0.4–0.6 g: 0.5–1 mL;
[0021] The coating time is 10-15 hours.
[0022] Optionally, the solvent comprises methanol or ethanol;
[0023] The ratio of photocatalyst to solvent is 0.1–0.5 g: 100 mL.
[0024] Optionally, the mixing temperature is 30–40°C and the time is 12–48 h.
[0025] The present invention also provides a photocatalyst for magnetizing magnetic separation concentrate prepared by the above preparation method, wherein the photocatalyst is γ-Fe2O3@SiO2 / Bi2WO6 or γ-Fe2O3@SiO2 / BiOI.
[0026] This invention also provides the application of the above-mentioned magnetically magnetized photocatalyst in the degradation of residual xanthate in mineral processing wastewater.
[0027] Compared with the prior art, the present invention has the following beneficial effects:
[0028] This invention involves coating a layer of silica (SiO2) onto the surface of magnetically separated γ-Fe2O3 concentrate using a simple mechanical stirring method to obtain γ-Fe2O3@SiO2. Bismuth tungstate and bismuth oxyiodide are then synthesized via a hydrothermal method. Finally, γ-Fe2O3@SiO2 is mechanically stirred onto bismuth tungstate or bismuth oxyiodide to obtain composite catalysts γ-Fe2O3@SiO2 / Bi2WO6 or γ-Fe2O3@SiO2 / BiOI. These catalysts exhibit excellent degradation effects on xanthate. Under optimal conditions, both γ-Fe2O3@SiO2 / Bi2WO6 and γ-Fe2O3@SiO2 / BiOI achieve a 100% degradation efficiency for xanthate. Compared to existing photocatalysts, the two magnetic photocatalysts involved in this invention have high degradation efficiency and can be magnetically recovered, significantly reducing operating costs and demonstrating promising application prospects.
[0029] This invention utilizes natural magnetic hematite γ-Fe2O3, avoiding the problems of numerous steps and high costs associated with artificial synthesis, and has broad application prospects in the field of magnetic photocatalysts. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 The image shows the XRD pattern of the magnetic separation concentrate γ-Fe2O3 of this invention.
[0031] Figure 2 The XRD patterns of γ-Fe2O3@SiO2, Bi2WO6, and 5% γ-Fe2O3@SiO2 / Bi2WO6 prepared in Example 1 of this invention are shown.
[0032] Figure 3 The FTIR spectra of γ-Fe2O3@SiO2, Bi2WO6, and 5% γ-Fe2O3@SiO2 / Bi2WO6 prepared in Example 1 of this invention;
[0033] Figure 4 The figure shows the effect of different loading ratios of γ-Fe2O3@SiO2 on the degradation efficiency of Bi2WO6-based catalysts on xanthate.
[0034] Figure 5 Hysteresis loops for γ-Fe2O3@SiO2, Bi2WO6, and 5% γ-Fe2O3@SiO2 / Bi2WO6;
[0035] Figure 6 Circulation diagram of 5% γ-Fe2O3@SiO2 / Bi2WO6;
[0036] Figure 7 XRD patterns of γ-Fe2O3@SiO2, BiOI, and 5% γ-Fe2O3@SiO2 / BiOI;
[0037] Figure 8 FTIR spectra of γ-Fe2O3@SiO2, BiOI, and 5% γ-Fe2O3@SiO2 / BiOI;
[0038] Figure 9 The figure shows the effect of different loading ratios of γ-Fe2O3@SiO2 on the degradation efficiency of BiOI-based catalysts on xanthate.
[0039] Figure 10 Hysteresis loops for γ-Fe2O3@SiO2, BiOI, and 5% γ-Fe2O3@SiO2 / BiOI;
[0040] Figure 11 The diagram shows the cyclic experiment of 5% γ-Fe2O3@SiO2 / BiOI. Detailed Implementation
[0041] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as a limitation of the present invention, but rather as a more detailed description of certain aspects, features, and embodiments of the present invention.
[0042] It should be understood that the terminology used in this invention is merely for describing particular embodiments and is not intended to limit the invention. Furthermore, with respect to numerical ranges in this invention, it should be understood that each intermediate value between the upper and lower limits of the range is also specifically disclosed. Every smaller range between any stated value or intermediate value within a stated range, and any other stated value or intermediate value within said range, is also included in this invention. The upper and lower limits of these smaller ranges may be independently included or excluded from the range.
[0043] Unless otherwise stated, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art. While only preferred methods and materials have been described herein, any methods and materials similar or equivalent to those described herein may be used in the implementation or testing of this invention. All references to this specification are incorporated by way of citation to disclose and describe methods and / or materials associated with those references. In the event of any conflict with any incorporated reference, the content of this specification shall prevail.
[0044] Various modifications and variations can be made to the specific embodiments described in this specification without departing from the scope or spirit of the invention, as will be apparent to those skilled in the art. Other embodiments derived from this specification will also be obvious to those skilled in the art. This application specification and embodiments are merely exemplary.
[0045] The terms “include,” “including,” “have,” “contain,” etc., used in this article are all open-ended terms, meaning that they include but are not limited to.
[0046] Unless otherwise specified, "room temperature" and "normal temperature" in this invention refer to 25±2℃.
[0047] All raw materials used in the following embodiments of the present invention are commercially available.
[0048] This invention provides a method for preparing a photocatalyst by magnetizing magnetic separation concentrate, comprising the following steps:
[0049] 1) After ball milling, the magnetically separated concentrate is dispersed in a mixture of anhydrous ethanol, water and ammonia to obtain suspension 1;
[0050] 2) Add the mixture of tetraethyl orthosilicate and anhydrous ethanol to suspension 1 for coating to obtain γ-Fe2O3@SiO2;
[0051] 3) A magnetic photocatalyst is obtained by mixing the photocatalyst, solvent, and γ-Fe2O3@SiO2.
[0052] In this invention, the photocatalyst is bismuth tungstate or bismuth oxyiodide;
[0053] When the photocatalyst is bismuth tungstate, the γ-Fe2O3@SiO2 accounts for 3-7% of the amount of bismuth tungstate, preferably 4-6%, and most preferably 5%.
[0054] When the photocatalyst is bismuth iodide, the γ-Fe2O3@SiO2 accounts for 5-20% of the amount of bismuth iodide, preferably 10-15%, and most preferably 5%.
[0055] In this invention, γ-Fe2O3 is ineffective in photocatalytic degradation of xanthate. Direct combination of γ-Fe2O3 with Bi2WO6 or BiOI will inhibit the catalytic degradation performance of Bi2WO6 or BiOI on xanthate. To prevent the inhibitory effect of γ-Fe2O3, a SiO2 layer is introduced to encapsulate γ-Fe2O3, separating γ-Fe2O3 from Bi2WO6 or BiOI, and avoiding direct contact between the two to reduce the photocatalytic activity of Bi2WO6 or BiOI.
[0056] In this invention, the preparation method of bismuth tungstate includes the following steps: dispersing bismuth nitrate pentahydrate in nitric acid solution using a magnetic stirrer, denoted as suspension 1; dissolving sodium tungstate dihydrate in ultrapure water and stirring magnetically, denoted as solution 2; slowly adding solution 2 to suspension 1 and adjusting its pH using sodium hydroxide solution and nitric acid solution, denoted as precursor solution 3; pouring precursor solution 3 into a polytetrafluoroethylene-lined reactor for hydrothermal reaction, and after the reaction is completed and naturally cooled to room temperature, washing multiple times with ultrapure water and anhydrous ethanol, and finally drying the product in a constant temperature drying oven, followed by grinding to obtain Bi2WO6 powder.
[0057] In this invention, the method for preparing bismuth oxyiodide includes the following steps: dissolving bismuth nitrate pentahydrate and potassium iodide in ethylene glycol solution respectively, and then mixing the two solutions to obtain a precursor solution; transferring the precursor solution to a polytetrafluoroethylene-lined reactor for hydrothermal reaction, and after the reaction is completed and allowed to cool naturally to room temperature, washing it multiple times with ultrapure water and anhydrous ethanol, and finally placing the product in a constant temperature drying oven for drying, followed by grinding to obtain BiOI powder.
[0058] In this invention, the magnetic separation concentrate is mainly composed of γ-Fe2O3, and the specific oxide composition of the magnetic separation concentrate is: Na2O, MgO, Al2O3, SiO2, P2O5, SO3, Cl, K2O, CaO, TiO2, V2O5, MnO, Fe2O3, CuO, ZnO.
[0059] The content of Na2O is 0.1-0.2%; the content of MgO is 1-2%; the content of Al2O3 is 1-2%; the content of SiO2 is 3-4%; the content of P2O5 is 0.01-0.1%; the content of SO3 is 0.1-1%; the content of Cl is 0.01-0.1%; the content of K2O is 0.1-0.3%; the content of CaO is 0.1-1%; the content of TiO2 is 0.1-0.2%; the content of V2O5 is 0.05-0.1%; the content of MnO is 0.1-0.2%; the content of Fe2O3 is 88-95%; the content of CuO is 0.01-0.06%; and the content of ZnO is 0.01-0.05%.
[0060] The total content of the oxides is 100%.
[0061] In this invention, the content of γ-Fe2O3 in the magnetic separation concentrate is preferably around 91%;
[0062] The ball milling speed is 500-1000 r / min, preferably 600-900 r / min, and more preferably 700-800 r / min; the time is 60-120 min, preferably 70-100 min, and more preferably 80-90 min.
[0063] The particle size of the magnetically separated concentrate after ball milling is 0.5–1 μm, preferably 0.6–0.9 μm, further preferably 0.7–0.8 μm, and most preferably around 0.724 μm.
[0064] In this invention, the volume ratio of anhydrous ethanol, water and ammonia is 50-100:10-30:1, preferably 60-90:15-25:1, and more preferably 70-80:18-20:1;
[0065] The ratio of the magnetic concentrate to the mixture of anhydrous ethanol, water and ammonia is 0.4-0.6g:400-500mL, preferably 0.42-0.58g:450-490mL, and more preferably 0.5g:480mL.
[0066] In this invention, the volume concentration of ammonia water is 20-40%, preferably 25-35%, and more preferably 28-30%.
[0067] In this invention, the magnetically separated concentrate is ball-milled and dispersed in a mixture of anhydrous ethanol, water and ammonia, and sonicated for 10-20 min, preferably 12-18 min, more preferably 14-16 min, and even more preferably 15 min, to obtain suspension 1.
[0068] In this invention, the volume ratio of tetraethyl orthosilicate to anhydrous ethanol is 1:20-30, preferably 1:22-28, more preferably 1:24-27, and even more preferably 1:25-26.
[0069] In this invention, the ratio of magnetic concentrate to tetraethyl orthosilicate is 0.4-0.6g:0.5-1mL, preferably 0.42-0.58g:0.6-0.9mL, and more preferably 0.5g:0.9mL;
[0070] The coating time is 10-15 hours, preferably 11-14 hours, and more preferably 12-13 hours, at room temperature.
[0071] In this invention, step 2) involves adding a mixture of tetraethyl orthosilicate and anhydrous ethanol dropwise to suspension A while mechanically stirring at room temperature. After stirring is complete, the product is collected by centrifugation and washed three times each with ultrapure water and anhydrous ethanol. The product is then dried in a vacuum oven to obtain γ-Fe2O3@SiO2 particles.
[0072] In this invention, the solvent comprises methanol or ethanol, preferably methanol;
[0073] The ratio of photocatalyst to solvent is 0.1-0.5 g:100 mL, preferably 0.2-0.4 g:100 mL, and more preferably 0.3 g:100 mL.
[0074] In this invention, the mixing temperature is 30-40°C, preferably 35°C, and the mixing time is 12-48h, preferably 16-40h, more preferably 20-36h, and even more preferably 24-30h.
[0075] In this invention, the photocatalyst is dispersed in a solvent and subjected to ultrasonic treatment to form a uniform suspension; γ-Fe2O3@SiO2 is added to the suspension and subjected to ultrasonic treatment, followed by mechanical stirring; after stirring, the solid is separated by centrifugation, and the product is placed in a vacuum oven to dry, thereby obtaining the magnetized photocatalyst.
[0076] The present invention also provides a photocatalyst for magnetizing magnetic separation concentrate prepared by the above preparation method, wherein the photocatalyst is γ-Fe2O3@SiO2 / Bi2WO6 or γ-Fe2O3@SiO2 / BiOI.
[0077] This invention also provides the application of the above-mentioned photocatalyst for magnetizing magnetic concentrate in the degradation of residual xanthate in mineral processing wastewater.
[0078] The technical solutions provided by the present invention will be described in detail below with reference to the embodiments, but they should not be construed as limiting the scope of protection of the present invention.
[0079] In the embodiments of the present invention, the oxide composition of the magnetic separation concentrate is: Na2O, MgO, Al2O3, SiO2, P2O5, SO3, Cl, K2O, CaO, TiO2, V2O5, MnO, Fe2O3, CuO, ZnO;
[0080] The composition of the Na₂O is 0.15%; the MgO content is 1.7%; the Al₂O₃ content is 1.32%; the SiO₂ content is 3.47%; the P₂O₅ content is 0.05%; the SO₃ content is 0.57%; the Cl content is 0.05%; the K₂O content is 0.2%; the CaO content is 0.84%; the TiO₂ content is 0.17%; the V₂O₅ content is 0.06%; the MnO content is 0.16%; the Fe₂O₃ content is 91.19%; the CuO content is 0.04%; and the ZnO content is 0.03%.
[0081] Example 1
[0082] The specific steps for preparing γ-Fe2O3@SiO2 / Bi2WO6 are as follows:
[0083] Preparation of bismuth tungstate: 3 mmol of bismuth nitrate pentahydrate was dispersed in 25 mL of 0.3 mol / L HNO3 solution and magnetically stirred for 30 min at room temperature, denoted as suspension A. 1.5 mmol of sodium tungstate dihydrate was dissolved in 55 mL of ultrapure water and magnetically stirred for 30 min, denoted as solution B. Solution B was slowly poured into suspension A and magnetically stirred for 20 min, denoted as suspension C. Subsequently, 4.5 mol / L NaOH solution was added dropwise to suspension C to adjust the pH to 2, denoted as precursor solution D. Precursor solution D was transferred to a 100 mL polytetrafluoroethylene-lined high-pressure reactor, placed in a constant-temperature drying oven, and heated to 180 °C for 24 h. After the reaction, the high-pressure reactor was allowed to cool naturally to room temperature, and the product was collected by high-speed centrifugation and washed three times each with ultrapure water and anhydrous ethanol. The product was dried in a constant-temperature drying oven at 60 °C for 12 h, and then ground to obtain Bi2WO6 powder.
[0084] Preparation of γ-Fe₂O₃@SiO₂: The magnetically separated concentrate was first pretreated by ball milling (90 min, 700 r / min, particle size approximately 0.724 μm). 0.5 g of the pretreated magnetically separated concentrate γ-Fe₂O₃ was uniformly dispersed in a mixture of 375 mL anhydrous ethanol, 100 mL ultrapure water, and 5.0 mL ammonia (28%), and sonicated for 15 min, designated as suspension A. A mixture of 0.9 mL tetraethyl orthosilicate (TEOS) and 25 mL anhydrous ethanol was added dropwise to suspension A, and the mixture was mechanically stirred at room temperature for 12 h. After stirring, the product was collected by centrifugation and washed three times each with ultrapure water and anhydrous ethanol. The product was then dried in a vacuum oven at 80 °C for 3 h to obtain γ-Fe₂O₃@SiO₂ particles.
[0085] Preparation of γ-Fe₂O₃@SiO₂ / Bi₂WO₆: 0.2 g Bi₂WO₆ was dispersed in 100 mL of methanol and sonicated for 15 min, denoted as suspension A. 0.01 g γ-Fe₂O₃@SiO₂ was added to suspension A and sonicated for 15 min, denoted as suspension B. Suspension B was transferred to a constant temperature water bath and mechanically stirred at 35 °C for 24 h. After stirring, the product was collected by centrifugation. The product was dried in a vacuum oven at 60 °C for 12 h, and then ground to obtain 5% γ-Fe₂O₃@SiO₂ / Bi₂WO₆.
[0086] Figure 2 and Figure 3 The images show the XRD and FTIR spectra of Bi2WO6, γ-Fe2O3@SiO2, and 5% γ-Fe2O3@SiO2 / Bi2WO6, respectively. The XRD pattern of 5% γ-Fe2O3@SiO2 / Bi2WO6 clearly shows obvious Bi2WO6 diffraction peaks and some weaker γ-Fe2O3@SiO2 diffraction peaks. The FTIR spectrum of 5% γ-Fe2O3@SiO2 / Bi2WO6 also confirms the presence of γ-Fe2O3 and SiO2, indicating that the composite of 5% γ-Fe2O3@SiO2 / Bi2WO6 was successfully achieved.
[0087] Example 2
[0088] The only difference from Example 1 is that 0.006g of γ-Fe2O3@SiO2 was added to suspension A, which was recorded as 3% γ-Fe2O3@SiO2 / Bi2WO6.
[0089] Example 3
[0090] The only difference from Example 1 is that 0.014g of γ-Fe2O3@SiO2 was added to suspension A, which was recorded as 7% γ-Fe2O3@SiO2 / Bi2WO6.
[0091] Comparative Example 1
[0092] The only difference from Example 1 is that γ-Fe2O3 is not coated; instead, 0.01g of γ-Fe2O3 is directly added to suspension A, which is recorded as 5% γ-Fe2O3 / Bi2WO6.
[0093] Application Example 1
[0094] The specific implementation process of the experiment on the degradation of xanthate by γ-Fe2O3@SiO2 / Bi2WO6 is as follows:
[0095] Purification of xanthate: Weigh a certain amount of xanthate and dissolve it in acetone. After filtration, obtain the supernatant. Add anhydrous diethyl ether to the supernatant until no more precipitate is formed. Then separate the precipitate and dry it in a vacuum oven to obtain the purified xanthate solid.
[0096] Weigh 15 mg of xanthate and prepare 250 mL of a 60 mg / L xanthate solution; weigh 25 mg of γ-Fe₂O₃@SiO₂ / Bi₂WO₆ prepared in different proportions as described in Examples 1-3; weigh Bi₂WO₆ and γ-Fe₂O₃@SiO₂ prepared in Example 1; weigh 5% γ-Fe₂O₃ / Bi₂WO₆ prepared in Comparative Example 1 into quartz test tubes; add 50 mL of xanthate solution to each test tube, sonicate for 2 min to disperse the catalyst evenly, and then place the test tubes in a photoreactometer; allow the catalyst to reach adsorption-desorption equilibrium in the dark for 30 min, then turn on the xenon lamp and allow the photoreacting for 30 min; take samples every 10 min into 10 mL centrifuge tubes, centrifuge and collect the supernatant, and then measure its absorbance at a wavelength of 301 nm using a UV spectrophotometer.
[0097] The degradation efficiency of the catalyst for xanthate within 60 minutes was as follows: Figure 4 As shown, both Bi₂WO₆ and 5% γ-Fe₂O₃@SiO₂ / Bi₂WO₆ exhibited 100% degradation efficiency for xanthate, while γ-Fe₂O₃@SiO₂ showed virtually no degradation effect. When the loading ratio of γ-Fe₂O₃@SiO₂ increased from 3% to 5%, the degradation rate of xanthate accelerated. However, when the loading ratio increased to 7%, the catalyst's effect on xanthate degradation worsened (reaching approximately 85% degradation efficiency within 60 minutes). Therefore, a loading ratio of 5% for γ-Fe₂O₃@SiO₂ is optimal. Figure 4 It can also be seen that the degradation rate of xanthate by Bi2WO6 loaded with γ-Fe2O3@SiO2 is higher than that of directly loaded with γ-Fe2O3. Therefore, covering the surface of γ-Fe2O3 with SiO2 is beneficial to the degradation of xanthate by the catalyst. Although the degradation rate of xanthate by γ-Fe2O3@SiO2 / Bi2WO6 is not as high as that of Bi2WO6, it does not affect its degradation efficiency. At the same time, this catalyst has good magnetic properties (saturation magnetization of 2.48 emu).-1 The coercivity is 371.60 Oe, such as Figure 5 As shown in the image, it has good recyclability. (From...) Figure 6 It can be seen that the catalytic activity of 5% γ-Fe2O3@SiO2 / Bi2WO6 remained at around 100% after five cycles, indicating that the catalyst has excellent chemical stability, can achieve efficient catalyst regeneration, and has broad prospects for industrial application.
[0098] Example 4
[0099] The specific steps for preparing 5% γ-Fe2O3@SiO2 / BiOI are as follows:
[0100] Preparation of BiOI: 4 mmol of bismuth nitrate pentahydrate and 4 mmol of potassium iodide were dissolved in 35 mL of ethylene glycol solution and stirred at room temperature for 30 min, denoted as solution A and solution B. Solution B was slowly added to solution A to form a suspension, and stirred at room temperature for 30 min to form precursor solution C. Solution C was poured into a 100 mL polytetrafluoroethylene-lined stainless steel autoclave and placed in a constant temperature drying oven at 140 °C for 12 h. After the reaction, the autoclave was allowed to cool naturally to room temperature, and the product was collected by high-speed centrifugation and washed three times each with ultrapure water and anhydrous ethanol. The obtained solid was dried in a constant temperature drying oven at 80 °C for 12 h, and then ground to obtain BiOI powder.
[0101] The preparation method of γ-Fe2O3@SiO2 is the same as in Example 1;
[0102] Preparation of 5% γ-Fe₂O₃@SiO₂ / BiOI: 0.2 g BiOI was dispersed in 100 mL of methanol and sonicated for 15 min, denoted as suspension A. 0.01 g γ-Fe₂O₃@SiO₂ was added to suspension A and sonicated for 15 min, denoted as suspension B. Suspension B was transferred to a constant temperature water bath and mechanically stirred at 35 °C for 24 h. After stirring, the product was collected by centrifugation. The product was dried in a vacuum oven at 60 °C for 12 h, and then ground to obtain 5% γ-Fe₂O₃@SiO₂ / BiOI.
[0103] Figure 7 and Figure 8 These are the XRD and FTIR spectra of BiOI, γ-Fe₂O₃@SiO₂, and γ-Fe₂O₃@SiO₂ / BiOI. The XRD pattern of γ-Fe₂O₃@SiO₂ / BiOI shows strong BiOI diffraction peaks as well as some weaker γ-Fe₂O₃ and SiO₂ diffraction peaks. The FTIR pattern of γ-Fe₂O₃@SiO₂ / BiOI also shows the presence of γ-Fe₂O₃ and SiO₂. All of these confirm the successful composite formation of γ-Fe₂O₃@SiO₂ / BiOI.
[0104] Example 5
[0105] The only difference from Example 4 is that 0.02g of γ-Fe2O3@SiO2 was added to suspension A, which was recorded as 10% γ-Fe2O3@SiO2 / BiOI.
[0106] Example 6
[0107] The only difference from Example 4 is that 0.03g of γ-Fe2O3@SiO2 was added to suspension A, which is 15% γ-Fe2O3@SiO2 / BiOI.
[0108] Example 7
[0109] The only difference from Example 4 is that 0.04g of γ-Fe2O3@SiO2 was added to suspension A, which is 20% γ-Fe2O3@SiO2 / BiOI.
[0110] Application Example 2
[0111] The specific implementation process of the experiment on the degradation of xanthate by γ-Fe2O3@SiO2 / BiOI is as follows:
[0112] Weigh 25 mg of xanthate and prepare 250 mL of 100 mg / L xanthate solution; weigh 25 mg of γ-Fe2O3@SiO2 / BiOI prepared in different proportions in Examples 4-7 and BiOI prepared in Example 1 into quartz test tubes respectively; add 50 mL of xanthate solution to each test tube, sonicate for 2 min to disperse the catalyst evenly, and then place the test tube in a photoreactometer; allow the catalyst to reach adsorption-desorption equilibrium in the dark for 30 min, then turn on the xenon lamp and allow the photoreacting for 60 min; take a sample every 10 min into a 10 mL centrifuge tube, centrifuge and collect the supernatant, and then measure its absorbance at a wavelength of 301 nm using an ultraviolet spectrophotometer.
[0113] The degradation efficiency of the catalyst for xanthate within 90 minutes was as follows: Figure 9 As shown, both BiOI and 5% γ-Fe2O3@SiO2 / BiOI achieved 100% degradation efficiency for xanthate. When the loading ratio of γ-Fe2O3@SiO2 increased from 5% to 20%, the degradation rate of xanthate by the catalyst gradually slowed down. Furthermore, when the loading ratio increased to 20%, the catalyst's effect on xanthate degradation deteriorated (the degradation efficiency was approximately 83% within 90 min). Therefore, a loading ratio of 5% for γ-Fe2O3@SiO2 is optimal. Figure 9 It can also be seen that although the degradation rate of xanthate by γ-Fe2O3@SiO2 / BiOI is not as high as that of BiOI, it does not affect the degradation efficiency. At the same time, this catalyst has good magnetic properties (saturation magnetization of 3.35 emu). -1The coercivity is 409.70 Oe, such as Figure 10 As shown in the image, it has good recyclability. (From...) Figure 11 It can be seen that 5% γ-Fe2O3@SiO2 / BiOI can still degrade 92.34% of xanthate after five cycles, indicating that the catalyst has good chemical stability, can be reused, and has broad prospects for industrial application.
[0114] The above description is only a preferred embodiment of the present invention. It should be noted that for those skilled in the art, several improvements and modifications can be made without departing from the principle of the present invention, and these improvements and modifications should also be considered within the scope of protection of the present invention.
Claims
1. A method for preparing a photocatalyst by magnetically imparting magnetism to a magnetically separated ore concentrate. It is characterized in that The following steps are involved: 1) The magnetic concentrate is ball-milled and dispersed into a mixture of anhydrous ethanol, water and aqueous ammonia to obtain a suspension 1; 2) Add a mixture of tetraethyl orthosilicate and anhydrous ethanol to the suspension 1 for coating to obtain γ-Fe 2 O 3 @SiO 2 ; 3) Photocatalyst, solvent, γ-Fe 2 O 3 @SiO 2 After mixing, a magnetic photocatalyst is obtained; The photocatalyst is bismuth tungstate or bismuth iodide oxide; When the photocatalyst is bismuth tungstate, the γ-Fe 2 O 3 @SiO 2 It accounts for 3-7% of the amount of bismuth tungstate used; When the photocatalyst is bismuth iodide, the γ-Fe 2 O 3 @SiO 2 It accounts for 5-20% of the amount of bismuth iodide used.
2. The method for preparing a photocatalyst by magnetically imparting magnetism to a magnetically separated ore concentrate according to claim 1, It is characterized in that The γ-Fe 2 O 3 The content of ≥90%; The ball milling speed is 500-1000 r / min and the time is 60-120 min; The particle size of the magnetic concentrate after ball milling is 0.5-1 μm.
3. The method for preparing a photocatalyst by magnetically imparting magnetism to a magnetically separated concentrate according to claim 2, It is characterized in that The volume ratio of anhydrous ethanol, water and aqueous ammonia is 50-100:10-30:1; The dosage ratio of the magnetic separation concentrate to the mixed solution of anhydrous ethanol, water and ammonia water is 0.4-0.6g:400-500mL.
4. The method for preparing a photocatalyst by magnetically imparting magnetism to a concentrate according to claim 1, It is characterized in that The volume ratio of tetraethyl orthosilicate to anhydrous ethanol is 1:20-30.
5. A method for preparing a photocatalyst by magnetically imparting magnetism to a magnetically separated concentrate according to claim 2 or 4, It is characterized in that The ratio of the magnetic concentrate to tetraethyl orthosilicate is 0.4-0.6 g: 0.5-1 mL; The coating time is 10 to 15 hours.
6. The method for preparing a photocatalyst by magnetically imparting magnetism to a magnetically separated concentrate according to claim 1, It is characterized in that The solvent comprises methanol or ethanol; The dosage ratio of the photocatalyst to the solvent is 0.1-0.5 g:100 mL.
7. The method for preparing a photocatalyst by magnetically imparting magnetism to a magnetically separated concentrate according to claim 1, It is characterized in that The mixing temperature is 30-40° C. and the mixing time is 12-48 hours.
8. The photocatalyst endowed with magnetism by magnetic concentrate prepared by the method for preparing the photocatalyst endowed with magnetism by magnetic concentrate according to any one of claims 1 to 7, It is characterized in that The photocatalyst is γ-Fe 2 O 3 @SiO 2 / Bi 2 WO 6 or γ-Fe 2 O 3 @SiO 2 / BiOI.
9. Use of the photocatalyst imparting magnetism to the magnetic concentrate as claimed in claim 8 in degrading residual xanthate in mineral processing wastewater.
Citation Information
Patent Citations
Conducting polymer modified magnetic photocatalyst and preparation method thereof
CN101856628A
Composite photocatalytic material, and preparation method and application thereof
CN102847536A
Method for preparing Fe3O4 / SiO2 / Bi2WO6 magnetic microsphere photocatalyst
CN103521237A
Recoverable magnetic titanium dioxide photocatalyst capable of rapidly degrading bisphenol A in waste water and preparation method thereof
CN105214665A
Magnetic bismuth tungstate photocatalyst as well as preparation method and application thereof
CN109865517A