Preparation method of CdS / Cu / BiVO4 superstructure filler
Through the preparation of CdS/Cu/BiVO4 superstructure filler, combined with photocatalysis and Fenton method, the problem of difficulty in decomposing industrial wastewater in traditional sewage treatment is solved, achieving efficient decomposition of organic pollutants and avoiding the generation of Fe sludge, which has a wide range of applications application potential.
Patent Information
- Application Number
- CN202410777585.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-17
- Publication Date
- 2024-10-15
AI Technical Summary
Traditional sewage treatment methods are difficult to effectively decompose organic pollutants in industrial wastewater, especially because Fe-based Fenton catalysts are sensitive to pH and produce Fe sludge, and a single treatment method cannot meet the needs of large-scale treatment.
Using CdS/Cu/BiVO4 superstructure filler, through the combination of photocatalytic technology and Fenton method, Cu doped catalyst promotes the separation of photogenerated electrons and holes on the CdS/BiVO4 heterojunction, and controls the superstructure by adjusting the number of steps size to avoid the generation of Fe sludge.
It improves the decomposition performance of industrial wastewater, avoids the generation of Fe sludge, has great application potential, and shows excellent catalytic effect in the neutral pH range.
Smart Images

Figure CN118767945A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of water treatment, and in particular relates to a method for preparing a CdS / Cu / BiVO4 superstructure filler for decomposing organic pollutants in blasting waste gas and industrial waste water. Background Art
[0002] In the context of rapid industrial development, the massive consumption of fossil fuels has led to serious energy and environmental crises. Industrial wastewater mixed with heavy metals, toxic chemicals, acids, alkalis, organic matter, oils and other toxic and harmful substances has become the main source of water pollution, and its harm far exceeds the pollution of the environment by domestic sewage, which accounts for more than 70% of the total wastewater. Industrial wastewater has the characteristics of complex composition, many types of organic pollution, high concentration, high and volatile COD, high ammonia nitrogen concentration and deep color, which makes it difficult to decompose. In addition, industrial waste gas contains a large amount of toxic and harmful gases such as CO, H2S, H3P, etc., such as blasting gas in the mining industry, exhaust gas from large diesel engines and gas turbines, etc.
[0003] Traditional sewage treatment methods all have certain shortcomings: the Fenton method has a large amount of H2O2 used and produces secondary pollutants such as Fe sludge, which hinders the application of the Fenton method in environmental governance; the ozone oxidation method is expensive, has high treatment costs, and has selective oxidation. Therefore, a single treatment method is difficult to meet the requirements of large-scale decomposition of industrial wastewater, and the development of efficient wastewater treatment technology has become one of the important links in solving water pollution. Combining traditional Fenton-like oxidation sewage treatment technology with photocatalytic oxidation sewage treatment technology will achieve efficient decomposition of organic pollutants, such as Fenton-like oxidation technology-photocatalytic oxidation technology.
[0004] Semiconductor photocatalytic technology can produce active substances with strong oxidizing ability, such as holes and hydroxyl radicals, and shows great potential in degrading organic matter. Semiconductors such as CdS and BiVO4 have become hot materials for photocatalysts due to their suitable band gap and strong visible light response ability. The construction of CdS / BiVO4 heterojunction is an effective strategy to promote the separation of photogenerated charges and improve photocatalytic performance. Fe-based Fenton catalysts are sensitive to pH values (generally pH < 6), while catalysts with Cu as active sites can adapt to a wider pH range (< 11). Therefore, Cu-doped catalysts are more suitable for treating neutral organic wastewater and have stronger applicability. However, Cu-based catalysts also need to be in a mixed valence state, which is more conducive to the decomposition of H2O2 into free radicals, so they need to be deposited at the hole-rich end of the CdS / BiVO4 heterojunction. Summary of the invention
[0005] The present invention aims to provide a method for preparing a CdS / Cu / BiVO4 superstructure filler.
[0006] To achieve the above object, the present invention adopts the following technical solution:
[0007] A method for preparing a CdS / Cu / BiVO4 superstructure filler comprises the following steps:
[0008] (1) Add Bi(NO3)3·5H2O to ethylene glycol and stir to dissolve to prepare solution A; add ammonium metavanadate NH4VO3 and PVP to hot deionized water and stir to dissolve to prepare solution B; slowly add solution A to solution B under stirring to obtain a suspension containing white particles;
[0009] (2) adding glucose and Cu(CH3COO)2 to the suspension prepared in step (1), heating for a period of time and then centrifuging, washing the filter cake with ethanol and water, and vacuum drying to obtain a Cu / BiVO4 material;
[0010] (3) dispersing the Cu / BiVO4 material into an ethanol aqueous solution containing CdNO3 and ultrasonically treating it; then adding Na2S thereto, reacting and aging under stirring; then centrifuging the prepared suspension, washing with deionized water and anhydrous ethanol, and vacuum drying to obtain CdS / Cu / BiVO4 particles;
[0011] (4) Using the CdS / Cu / BiVO4 particles prepared in step (3) as the nucleation center, repeat steps (1) to (3) 1 to 5 times to obtain the product.
[0012] Preferably, the specific operation of step (1) of the present invention is: adding 5-10 mmol Bi(NO3)3·5H2O to 20-40 ml ethylene glycol, stirring until fully dissolved to obtain solution A; adding 5-10 mmol ammonium metavanadate NH4VO3 and 0.1-0.2 g PVP to 40-60 ml deionized water at a temperature of 50-90°C, stirring until fully dissolved to obtain solution B; slowly adding solution A to solution B under stirring to obtain a suspension containing white particles.
[0013] Preferably, the specific operation of step (2) of the present invention is: add 3-5 g glucose and 3-7 mmol Cu(CH3COO)2 to the suspension prepared in step (1), and heat at 80°C-100°C for 1-5 h; then, centrifuge the suspension, wash with ethanol and water, and vacuum dry at 50°C-80°C to obtain a Cu / BiVO4 sample.
[0014] Preferably, the specific operation of step (3) of the present invention is: dispersing 100 mg to 1000 mg of Cu / BiVO4 sample into 50 to 200 mL of ethanol aqueous solution containing 3 to 8 mmol of CdNO3 and ultrasonically treating it for 0.5 to 2 hours; then adding 3 to 8 mmol of Na2S to the above solution, reacting for 30 to 50 minutes under continuous magnetic stirring, and aging for 1 to 3 hours; subsequently, centrifuging the prepared suspension, washing it with deionized water and anhydrous ethanol for 2 to 3 times, and vacuum drying it at 60 to 80°C for 12-24 hours.
[0015] Preferably, the volume concentration of ethanol in the ethanol aqueous solution in step (3) of the present invention is 30% to 70%.
[0016] Furthermore, the specific operation of step (4) of the present invention is: taking the CdS / Cu / BiVO4 particles prepared in step (3) as the core, repeating steps (1) to (3) 1 to 5 times until the size of the CdS / Cu / BiVO4 superstructure particles is greater than 2um.
[0017] The beneficial technical effects of the present invention are:
[0018] The present invention provides a method for preparing a CdS / Cu / BiVO4 superstructure filler for treating industrial wastewater based on a Fenton method-photocatalytic method. The present invention combines photocatalytic technology with Fenton-like technology. The photocatalyst can continuously provide photogenerated electrons through photoexcitation, and the combination of Cu and electrons can promote the separation of photogenerated electrons and holes. The synergistic effect of photocatalysis and Fenton-like technology improves the performance of CdS / Cu / BiVO4 superstructure filler in decomposing industrial wastewater.
[0019] The present invention can control the size of the superstructure by adjusting the number of steps (1) to (3).
[0020] The present invention dopes Cu to make CdS / Cu / BiVO4 have a Fenton-like effect, thereby avoiding the generation of Fe sludge in the reaction process to cause secondary pollution.
[0021] The present invention can control the doping content of Cu by changing the amount of added Cu(CH3COO)2, and can regulate the size, structure and composition of the CdS / Cu / BiVO4 superstructure, so that the catalyst has a photocatalytic effect and a Fenton effect, and has great application potential. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 This is the SEM of CdS / Cu / BiVO4 prepared by repeating steps (1) to (3) three times in Example 1.
[0023] Figure 2This is the SEM of CdS / Cu / BiVO4 prepared by repeating steps (1) to (3) five times in Example 1.
[0024] Figure 3 This is the Tafel curve of the electron-rich end test of the CdS / BiVO4 heterojunction under light and dark conditions.
[0025] Figure 4 The degradation effect of Rhodamine B on the CdS / BiVO4 superstructure without Cu doping and the CdS / Cu / BiVO4 sample doped with 5% Cu.
[0026] Figure 5 The valence state of Cu in the CdS / Cu / BiVO4 doped with 5% Cu prepared in Example 2 changes after light irradiation.
[0027] Figure 6 This is a diagram showing the degradation effect of Rhodamine B under different pH conditions using CdS / Cu / BiVO4 doped with 5% Cu prepared in Example 2.
[0028] Figure 7 This is a diagram showing the degradation effect of Rhodamine B by BiVO4 / Cu / CdS and CdS / Cu / BiVO4 with a Cu doping content of 5%. DETAILED DESCRIPTION
[0029] The present invention is further described below in conjunction with the accompanying drawings and specific implementation methods. The protection scope of the present invention is not limited to the following description.
[0030] Example 1
[0031] A method for preparing a CdS / Cu / BiVO4 superstructure filler doped with 5% Cu comprises the following steps:
[0032] (1) Add 10 mmol Bi(NO3)3·5H2O to 40 ml ethylene glycol and stir until completely dissolved to prepare solution A. Add 10 mmol ammonium metavanadate (NH4VO3) and 0.2 g PVP to 60 ml deionized water at 70°C and stir until completely dissolved to prepare solution B. Slowly add solution A to solution B under vigorous stirring to obtain a suspension containing white particles.
[0033] (2) Add 5 g of glucose and 5 mmol of Cu(CH3COO)2 to the suspension prepared in step (1), and heat at 80°C for 3 hours. Then, the suspension is centrifuged, washed twice with ethanol and water, and vacuum dried at 80°C for 10 hours to obtain a Cu / BiVO4 sample.
[0034] (3) 500 mg of Cu / BiVO4 sample was dispersed into 100 mL of 50% ethanol aqueous solution containing 5 mmol CdNO3 and ultrasonically treated for 1 hour; then 5 mmol Na2S was slowly added to the above solution, reacted for 30 minutes under continuous magnetic stirring, and aged for 2 hours. Subsequently, the prepared suspension was centrifuged, washed with deionized water and anhydrous ethanol three times, and vacuum dried at 80°C for 24 hours to obtain a CdS / Cu / BiVO4 sample doped with 5% Cu.
[0035] (4) Using the CdS / Cu / BiVO4 particles prepared in step (3) as the core, steps (1) to (3) were repeated three and five times to obtain CdS / Cu / BiVO4 superstructure particles of different sizes with a Cu doping of 5%. The CdS / Cu / BiVO4 superstructure particles prepared by repeating the process three times were used as sample 1. The SEM images of the particles were as follows: Figure 1 Repeat 5 times to prepare the CdS / Cu / BiVO4 superstructure particles as sample 2, the SEM shows Figure 2 .Depend on Figure 1 and Figure 2 It can be seen that the more repeated preparation times, the larger the particle size; the larger the size, the more conducive it is to later filtration.
[0036] Example 2
[0037] A method for preparing a CdS / Cu / BiVO4 superstructure filler with a Cu doping content of 7%, comprising the following steps:
[0038] (1) 8 mmol Bi(NO3)3·5H2O was added to 40 ml ethylene glycol and stirred until completely dissolved to obtain solution A. 8 mmol ammonium metavanadate (NH4VO3) and 0.1 g PVP were added to 50 ml deionized water at 90°C and stirred until completely dissolved to obtain solution B. Solution A was slowly added to solution B under vigorous stirring to obtain a suspension containing white particles.
[0039] (2) Add 4 g of glucose and 7 mmol of Cu(CH3COO)2 to the suspension prepared in step (1), and heat at 80°C for 3 h. Then, the suspension was centrifuged, washed twice with ethanol and water, and vacuum dried at 70°C for 10 h to obtain a Cu / BiVO4 sample.
[0040] (3) 1000 mg of Cu / BiVO4 sample was dispersed into 200 mL of 70% ethanol aqueous solution containing 8 mmol CdNO3 and ultrasonically treated for 2 hours; then 8 mmol Na2S was slowly added to the above solution, reacted for 50 minutes under continuous magnetic stirring, and aged for 3 hours. Subsequently, the prepared suspension was centrifuged, washed with deionized water and anhydrous ethanol three times, and vacuum dried at 60°C for 24 hours to obtain a CdS / Cu / BiVO4 sample doped with 7% Cu.
[0041] (4) Using the CdS / Cu / BiVO4 particles prepared in step (3) as the core, repeat steps (1) to (3) five times to obtain CdS / Cu / BiVO4 superstructure particles of larger size with a Cu doping of 7%.
[0042] Example 3
[0043] A method for preparing a CdS / Cu / BiVO4 superstructure filler doped with 3% Cu comprises the following steps:
[0044] (1) Add 5 mmol Bi(NO3)3·5H2O to 20 ml ethylene glycol and stir until completely dissolved to prepare solution A. Add 5 mmol ammonium metavanadate (NH4VO3) and 0.1 g PVP to 40 ml deionized water at 50°C and stir until completely dissolved to prepare solution B. Slowly add solution A to solution B under vigorous stirring to obtain a suspension containing white particles.
[0045] (2) Add 3 g of glucose and 3 mmol of Cu(CH3COO)2 to the suspension prepared in step (1), and heat at 90°C for 1 h. Then, the suspension is centrifuged, washed twice with ethanol and water, and vacuum dried at 50°C for 12 h to obtain a Cu / BiVO4 sample.
[0046] (3) 100 mg of Cu / BiVO4 sample was dispersed into 50 mL of 40% ethanol aqueous solution containing 3 mmol CdNO3 and ultrasonically treated for 0.5 h; then 3 mmol Na2S was slowly added to the above solution, reacted for 40 min under continuous magnetic stirring, and aged for 1 h. Subsequently, the prepared suspension was centrifuged, washed with deionized water and anhydrous ethanol 3 times, and vacuum dried at 80°C for 12 h to obtain a CdS / Cu / BiVO4 sample doped with 3% Cu.
[0047] (4) Using the CdS / Cu / BiVO4 particles prepared in step (3) as the core, repeat steps (1) to (3) five times to obtain CdS / Cu / BiVO4 superstructure particles of larger size with a Cu doping level of 3%.
[0048] Comparative Example 1
[0049] A method for preparing a Cu-undoped CdS / BiVO4 sample comprises the following steps:
[0050] (1) Add 5 mmol Bi(NO3)3·5H2O to 20 ml ethylene glycol and stir until completely dissolved to prepare solution A. Add 5 mmol ammonium metavanadate (NH4VO3) and 0.1 g PVP to 40 ml deionized water at 50°C and stir until completely dissolved to prepare solution B. Slowly add solution A to solution B under vigorous stirring to obtain a suspension containing white particles.
[0051] (2) Add 3 g of glucose and 3 mmol of CdNO3 in a 40% ethanol aqueous solution to the suspension prepared in step (1) and ultrasonically treat for 0.5 hours; then slowly add 3 mmol of Na2S to the above solution, react for 40 minutes under continuous magnetic stirring, and age for 1 hour. Subsequently, the prepared suspension is centrifuged, washed with deionized water and anhydrous ethanol for 3 times, and vacuum dried at 80°C for 12 hours to obtain a CdS / BiVO4 sample not doped with Cu.
[0052] Comparative Example 2
[0053] A method for preparing a BiVO4 / Cu / CdS superstructure filler with a Cu doping content of 5%, as follows:
[0054] (1) 5 mmol CdNO3 was dissolved in 100 mL of 50% ethanol aqueous solution (volume concentration) and ultrasonically treated for 1 hour, and then 5 mmol Na2S was slowly added dropwise to the above solution and reacted for 30 minutes under continuous magnetic stirring to obtain a suspension.
[0055] (2) Add 3 g of glucose and 5 mmol of Cu(CH3COO)2 to the suspension prepared in step (1), and heat at 80°C for 3 h to obtain a Cu / CdS sample doped with 5% Cu.
[0056] (3) Add 500 mg of Cu / CdS sample and 10 mmol Bi(NO3)3·5H2O to 40 ml of ethylene glycol and stir until completely dissolved to prepare solution A. Add 10 mmol ammonium metavanadate (NH4VO3) and 0.1 g PVP to 60 ml of deionized water at 70°C and stir until completely dissolved to obtain solution B. Solution A was slowly added to solution B under vigorous stirring, white particles appeared, and aged for 3 hours. Subsequently, the prepared suspension was centrifuged, washed with deionized water and anhydrous ethanol 3 times, and vacuum dried at 80°C for 24 hours. A BiVO4 / Cu / CdS superstructure filler with a Cu doping content of 5% was obtained.
[0057] (4) Using the BiVO4 / Cu / CdS particles prepared in step (3) as the core, repeat steps (1) to (3) five times to obtain BiVO4 / Cu / CdS superstructure particles of larger size with a Cu doping of 5%.
[0058] Effect Example 1
[0059] The CdS and BiVO4 samples were subjected to Tafel tests under light and dark conditions, respectively. Figure 3 .Depend on Figure 3 It can be seen that in the absence of light, electrons flow from CdS to BiVO4, and in the presence of light, electrons flow from BiVO4 to CdS; therefore, under light conditions, BiVO4 is the hole-rich end.
[0060] Effect Example 2
[0061] 10 mg of each of the CdS / Cu / BiVO4 sample 2 with 5% Cu doping in Example 1 and the CdS / BiVO4 superstructure filler without Cu doping in Comparative Example 1 were weighed, and then 20 mg / L of rhodamine B solution and 0.2 mL of hydrogen peroxide were added to study the Fenton-like effect of the CdS / Cu / BiVO4 superstructure filler. The results are shown in Figure 4 .from Figure 4 It can be seen that the concentration of Rhodamine B in the water sample treated with CdS / Cu / BiVO4 superstructure filler under lightless conditions also decreased significantly, showing a strong Fenton-like effect; while the concentration of Rhodamine B in the CdS / BiVO4 system without Cu did not change significantly under lightless conditions, indicating that there was no Fenton effect.
[0062] Effect Example 3
[0063] The XPS spectrum of the CdS / Cu / BiVO4 sample 2 with a Cu doping content of 5% prepared in Example 1 was tested, and the results were as follows: Figure 5 shown by Figure 5It can be found that the valence of Cu in the sample just prepared is mainly 0, but after 5 hours of light exposure, a large number of +2 and +1 valences appear in the valence state of Cu, which also verifies Figure 3 As a result, Cu settles at the hole-rich end of the CdS / BiVO4 heterojunction and is oxidized under light to form a mixed valence state.
[0064] Effect Example 4
[0065] The degradation experiment of Rhodamine B was carried out on the CdS / Cu / BiVO4 sample 2 with a Cu doping content of 5% prepared in Example 1 at different pH values. The results are as follows: Figure 6 As shown; it can be seen that within the pH range of 5-7, its catalytic efficiency changes by about 15%, showing better pH adaptability than the Fe-based Fenton catalyst.
[0066] Effect Example 5
[0067] The BiVO4 / Cu / CdS sample 2 with a Cu doping content of 5% prepared in Example 1 and the CdS / Cu / BiVO4 with a Cu doping content of 5% prepared in Comparative Example 2 were subjected to degradation experiments of Rhodamine B. The results are shown in FIG. Figure 7 As shown. Figure 7 It can be seen that the activity of CdS / Cu / BiVO4 is higher than that of BiVO4 / Cu / CdS; Figure 5 and Figure 3 , indicating that Cu ions are deposited at the hole-rich end and form mixed-valence Cu ions under light conditions, which is the fundamental reason for improving catalytic activity. This shows that it is not feasible to simply dope photosensitive heterojunctions with Cu ions, and directional doping should be done to better improve performance.
Claims
1. A method for preparing a CdS / Cu / BiVO4 superstructure filler, characterized in that: The following steps are involved: (1) Add Bi(NO3)3·5H2O to ethylene glycol and stir to dissolve to prepare solution A; add ammonium metavanadate NH4VO3 and PVP to hot deionized water and stir to dissolve to prepare solution B; slowly add solution A to solution B under stirring to obtain a suspension containing white particles; (2) adding glucose and Cu(CH3COO)2 to the suspension prepared in step (1), heating for a period of time and then centrifuging, washing the filter cake with ethanol and water, and vacuum drying to obtain a Cu / BiVO4 material; (3) dispersing the Cu / BiVO4 material into an ethanol aqueous solution containing CdNO3 and ultrasonically treating it; then adding Na2S thereto, reacting and aging under stirring; then centrifuging the prepared suspension, washing with deionized water and anhydrous ethanol, and vacuum drying to obtain CdS / Cu / BiVO4 particles; (4) Using the CdS / Cu / BiVO4 particles prepared in step (3) as the nucleation center, repeat steps (1) to (3) 1 to 5 times to obtain the product.
2. The method for preparing a CdS / Cu / BiVO4 superstructure filler according to claim 1, characterized in that: The specific operation of step (1) is as follows: adding 5-10 mmol Bi(NO3)3·5H2O to 20-40 ml ethylene glycol, stirring until fully dissolved to obtain solution A; adding 5-10 mmol ammonium metavanadate NH4VO3 and 0.1-0.2 g PVP to 40-60 ml deionized water at a temperature of 50-90°C, stirring until fully dissolved to obtain solution B; and slowly adding solution A to solution B under stirring to obtain a suspension containing white particles.
3. The method for preparing a CdS / Cu / BiVO4 superstructure filler according to claim 1, characterized in that: The specific operation of step (2) is as follows: add 3-5 g glucose and 3-7 mmol Cu(CH3COO)2 to the suspension prepared in step (1), and heat at 80°C-100°C for 1-5 hours; then, centrifuge the suspension, wash with ethanol and water, and vacuum dry at 50°C-80°C to obtain a Cu / BiVO4 sample.
4. The method for preparing a CdS / Cu / BiVO4 superstructure filler according to claim 1, characterized in that: The specific operation of step (3) is as follows: 100 mg to 1000 mg of Cu / BiVO4 sample is dispersed in 50 to 200 mL of ethanol aqueous solution containing 3 to 8 mmol CdNO3 and ultrasonically treated for 0.5 to 2 hours; then 3 to 8 mmol Na2S is added to the above solution, reacted for 30 to 50 minutes under continuous magnetic stirring, and aged for 1 to 3 hours; subsequently, the prepared suspension is centrifuged, washed with deionized water and anhydrous ethanol for 2 to 3 times, and vacuum dried at 60 to 80°C for 12 to 24 hours.
5. The method for preparing a CdS / Cu / BiVO4 superstructure filler according to claim 1, characterized in that: The volume concentration of ethanol in the ethanol aqueous solution in step (3) is 30% to 70%.
6. The method for preparing a CdS / Cu / BiVO4 superstructure filler according to claim 1, characterized in that: The specific operation of step (4) is: taking the CdS / Cu / BiVO4 particles prepared in step (3) as the core, repeating steps (1) to (3) 1 to 5 times until the size of the CdS / Cu / BiVO4 superstructure particles is greater than 2um.
Citation Information
Patent Citations
CdS / BiVO4 composite photocatalyst and preparation method thereof
CN105964277A
BiVO4 / CdS compound for comprehensive treatment of water body, preparation method and application thereof
CN108940314A
Reusable large-size hollow adsorbent and preparation method and application thereof
CN110586051A
Z-type photocatalyst as well as preparation method and application thereof
CN115475631A
NiFe / CdS / bismuth vanadate composite photoelectrocatalysis anode material and preparation and application thereof
CN115747828A