Method for preventing flocculated flow at upper part of submersed nozzle during continuous casting

By designing the bell mouth shape of the upper part of the immersed nozzle and the high-temperature cement seal, combined with the use of induction heating coils, the problem of flocculation in the upper part of the immersed nozzle during continuous casting is solved, the production efficiency and steel quality are improved, and the production cost is reduced.

CN118768557AInactive Publication Date: 2024-10-15ANGANG STEEL CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411274506.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-12
Publication Date
2024-10-15
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

During the continuous casting process, the problem of flocculation in the upper part of the immersed nozzle plagues billet production, especially when refining steel types that cannot be calcium treated, resulting in the risk of casting interruption, increasing production costs and being difficult to effectively solve.

Method used

By designing the shape of the upper bell mouth of the immersed nozzle, smoothing the inner surface, baking and efficient heat preservation, and using high-temperature cement sealing and induction heating coils at the connection between the nozzle and the lower nozzle of the tundish, we ensure that the inner surface of the nozzle is smooth and the temperature is uniform, preventing The occurrence of flocculation.

Benefits of technology

It effectively solves the problem of nozzle flocculation, improves the pourability of molten steel and continuous casting production efficiency, and ensures the stability of the continuous casting process and steel quality. It is suitable for the production of all steel types, is simple to operate and has low cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118768557A_ABST
    Figure CN118768557A_ABST
Patent Text Reader

Abstract

The invention provides a method for preventing flocculation flow on the upper portion of a submersed nozzle during continuous casting, and relates to the technical field of continuous casting production. The method comprises the following steps that the inner side of the upper portion of the submersed nozzle is arranged to be in a horn mouth shape, and the diameter of the inner side of the upper portion is larger than that of a tundish collector nozzle; the joint of the submersed nozzle and the tundish collector nozzle is sealed; the submersed nozzle, the tundish collector nozzle and the inner surface of the joint of the submersed nozzle and the tundish collector nozzle are ground and polished; heat preservation is conducted on the upper portion of the submersed nozzle, the tundish collector nozzle and the joint of the submersed nozzle and the tundish collector nozzle; performing high-temperature baking on the submersed nozzle, the tundish collector nozzle, the joint of the submersed nozzle and the tundish collector nozzle and the tundish; after baking is finished, the heat preservation cover is detached, and induction heating coils are installed on the upper portion of the submersed nozzle, the tundish collector nozzle and the joint of the submersed nozzle and the tundish collector nozzle; and the induction heating coil inductively heats the molten steel in the water gap until the continuous casting process is completed.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of continuous casting production, and in particular to a method for preventing flocculation at the upper part of an immersed nozzle during continuous casting. Background Art

[0002] The problem of continuous casting nozzle flocculation is a common problem in the continuous casting production process, especially in the production of aluminum and titanium-containing steels, which has an adverse effect on the continuity of continuous casting and the cleanliness of the steel.

[0003] The nozzles in the continuous casting process include the sliding nozzles, long nozzles, tundish nozzles and submerged nozzles of the ladle pouring mechanism. These nozzles will form a certain amount of flocculation inside, but the submerged nozzles are more likely to be blocked by flocculation. There are two types of flocculation problems in submerged nozzles: one is flocculation at the lower part of the submerged nozzle, especially at the lower outlet and its vicinity. This type of flocculation usually occurs during the production of slabs, especially when thin slabs are used to produce aluminum and titanium-containing steels such as automobile plates; the other is flocculation at the upper part of the submerged nozzle, especially at the connection between the upper part and the lower nozzle of the tundish. This type of flocculation usually occurs during the production of square billets, and has no obvious relationship with the composition of the steel grade. It is also easy to flocculate during continuous casting of aluminum-free and titanium-free steels. The causes of this type of flocculation are multifaceted and complex, including poor sealing, low nozzle baking temperature, alumina accumulation, etc., which are also difficult to solve during continuous casting. With the continuous development of modern industry and the continuous improvement of steel production technology, users have higher and higher requirements on the performance of steel, the purity of steel, and the content of impurity elements and inclusions in steel. Therefore, it is required to stabilize the production during the steelmaking process to avoid accidents such as continuous casting speed reduction, water inlet change and pouring interruption caused by water inlet flocculants, avoid slag rolls caused by crystallizer liquid level fluctuations caused by water inlet flocculants, and avoid large-sized water inlet flocculants being washed into the molten steel by the molten steel.

[0004] The flocculent flow problem at the top of the submerged nozzle is the key problem that plagues the efficient production of billet continuous casting. It is particularly prominent for steel grades that cannot be treated with calcium in refining. Once severe flocculent flow occurs during continuous casting and there is a risk of interruption in casting, emergency calcium feeding line treatment is usually adopted in the nozzle to maintain continuous casting. However, the billets produced during the calcium feeding period need to be downgraded or scrapped, which increases production costs. Therefore, there is currently no better and economical solution to the flocculent flow problem at the top of the submerged nozzle. Summary of the invention

[0005] According to the above-mentioned technical problem that the flocculation at the upper part of the submerged nozzle affects the continuous casting production, a method for preventing the flocculation at the upper part of the submerged nozzle during continuous casting is provided. The present invention mainly utilizes the special design of the shape of the upper inlet of the submerged nozzle, the smooth treatment of the inner surface of the upper inlet, the design of the baking method, the design of the efficient heat preservation method of the submerged nozzle, and the design of the sealing method of the connection between the submerged nozzle and the lower nozzle of the tundish, so as to achieve the technical effect of suppressing the flocculation at the upper part of the submerged nozzle.

[0006] The technical means adopted by the present invention are as follows: A method for preventing flocculation at the upper part of an immersion nozzle during continuous casting comprises the following steps: Preparation stage: S1, setting the upper inner side of the submerged nozzle into a bell-mouth shape and making the upper inner diameter larger than the inner diameter of the lower nozzle of the tundish; S2. Seal the connection between the submerged nozzle and the lower nozzle of the tundish; S3, grinding and polishing the inner surfaces of the submerged nozzle, the tundish outlet, and the connection between the submerged nozzle and the tundish outlet; S4. Insulating the upper part of the submerged nozzle, the lower nozzle of the tundish, and the connection between the submerged nozzle and the lower nozzle of the tundish; S5, high temperature baking is performed on the submerged nozzle, the tundish outlet, the connection between the submerged nozzle and the tundish outlet, and the tundish; S6. After the baking is completed, the heat preservation cover is removed, and an induction heating coil is installed on the upper part of the immersion nozzle, the lower nozzle of the tundish, and the outer side of the connection between the immersion nozzle and the lower nozzle of the tundish; Use stage: S7, the induction heating coil induction heats the molten steel in the nozzle until the continuous casting process is completed.

[0007] Furthermore, S1 is specifically configured as follows: the inner diameter of the upper portion of the submerged nozzle is greater than the inner diameter of the lower portion thereof, and the inner diameter of the upper portion of the submerged nozzle is greater than the inner diameter of the lower nozzle of the tundish.

[0008] Furthermore, high temperature cement sealing is adopted in S2, and the sealing steps are as follows: S21. Before the submerged nozzle and the tundish are baked at high temperature, apply the cement to the connection between the submerged nozzle and the lower nozzle of the tundish; S22, compact and fix the connection between the submerged nozzle and the lower nozzle of the tundish together with the cement; S23. Based on S22, apply a layer of cement on the outer side of the connection between the submerged nozzle and the lower nozzle of the tundish, with the thickness of the cement being ≥10mm.

[0009] Furthermore, the grinding and polishing in S3 specifically includes: polishing the inner surface with sandpaper of 300 mesh or above, so that the inner surface feels smooth without any raised or recessed defects.

[0010] Furthermore, in S4, the specific insulation treatment method is: wrapping the upper part of the immersion nozzle, the lower nozzle of the tundish and the connection between the immersion nozzle and the lower nozzle of the tundish with a layer of insulation cotton, and the thickness of the insulation cotton is ≥30mm.

[0011] Furthermore, the specific insulation treatment method also includes using an insulation cover to insulate the outer side of the lower water inlet of the tundish and the upper part of the immersion water inlet.

[0012] Furthermore, in S5, the submerged water inlet and the lower water inlet of the tundish are baked by internal combustion, the baking time is ≥2h, and the baking temperature of the tundish is ≥1100°C.

[0013] Further, in S6, the total length of the induction heating coil is consistent with the total length from the lower water inlet of the tundish to the upper part of the immersion water inlet.

[0014] Further, in S7, during continuous casting, the induction heating coil performs induction heating on the molten steel in the nozzle, and the power of the induction coil is ≥300kw.

[0015] Compared with the prior art, the present invention has the following advantages: The method of the present invention can effectively solve the problem of flocculation in the nozzle caused by the ladle lower nozzle and the submerged nozzle being not tightly sealed, the internal baking temperature of the submerged nozzle being low, the inner surface of the nozzle being rough and easy to adhere to deoxidation products, etc. in the continuous casting process of molten steel. The method can be used in the continuous casting production of all types of steel such as aluminum deoxidized steel and non-aluminum deoxidized steel, can fundamentally solve the flocculation problem in the upper part of the continuous casting nozzle, improve the castability of molten steel and the production efficiency of continuous casting, can ensure the stable production of the continuous casting process, improve the internal and external quality of the continuous casting billet and the performance of the steel material, and is very beneficial to the stable production and quality control of pure steel and ultra-pure steel. Moreover, the method is simple to operate and low in cost, so it is conducive to popularization and application. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.

[0017] Figure 1 The figure is a flow chart of the method of the present invention.

[0018] Figure 2 This is a diagram of the sealing of the submerged water inlet, the tundish outlet and their connection in the present invention.

[0019] Figure 3 It is a schematic diagram of the structure of the heat preservation cover in the present invention.

[0020] Figure 4 It is a schematic diagram of the structure of the induction heating coil in the present invention.

[0021] In the figure: 1. Tundish; 2. Tundish outlet; 3. Immersed outlet; 4. High-temperature cement; 5. Insulation cotton; 6. Insulation cover; 7. Induction heating coil. DETAILED DESCRIPTION

[0022] It should be noted that, in the absence of conflict, the embodiments of the present invention and the features in the embodiments can be combined with each other. The present invention will be described in detail below with reference to the accompanying drawings and in combination with the embodiments.

[0023] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. The following description of at least one exemplary embodiment is actually only illustrative and is by no means intended to limit the present invention and its application or use. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0024] It should be noted that the terms used herein are only for describing specific embodiments and are not intended to limit exemplary embodiments according to the present invention. As used herein, unless the context clearly indicates otherwise, the singular form is also intended to include the plural form. In addition, it should be understood that when the terms "comprising" and / or "including" are used in this specification, it indicates the presence of features, steps, operations, devices, components and / or combinations thereof.

[0025] Unless otherwise specifically stated, the relative arrangement, numerical expressions and numerical values ​​of the parts and steps described in these embodiments do not limit the scope of the present invention. At the same time, it should be clear that, for ease of description, the sizes of the various parts shown in the accompanying drawings are not drawn according to the actual proportional relationship. The technology, method and equipment known to those of ordinary skill in the relevant field may not be discussed in detail, but in appropriate cases, the technology, method and equipment should be regarded as a part of the specification. In all examples shown and discussed here, any specific value should be interpreted as being merely exemplary, rather than as a limitation. Therefore, other examples of exemplary embodiments may have different values. It should be noted that similar reference numerals and letters represent similar items in the following drawings, so once a certain item is defined in an accompanying drawing, it does not need to be further discussed in subsequent drawings.

[0026] In the description of the present invention, it is necessary to understand that the directions or positional relationships indicated by directional words such as "front, back, up, down, left, right", "lateral, vertical, perpendicular, horizontal" and "top, bottom" are usually based on the directions or positional relationships shown in the drawings. They are only for the convenience of describing the present invention and simplifying the description. Unless otherwise specified, these directional words do not indicate or imply that the device or element referred to must have a specific direction or be constructed and operated in a specific direction. Therefore, they cannot be understood as limiting the scope of protection of the present invention: the directional words "inside and outside" refer to the inside and outside relative to the contours of each component itself.

[0027] For ease of description, spatially relative terms such as "above", "above", "on the upper surface of", "above", etc. may be used here to describe the spatial positional relationship between a device or feature and other devices or features as shown in the figure. It should be understood that spatially relative terms are intended to include different orientations of the device in use or operation in addition to the orientation described in the figure. For example, if the device in the accompanying drawings is inverted, the device described as "above other devices or structures" or "above other devices or structures" will be positioned as "below other devices or structures" or "below their position devices or structures". Thus, the exemplary term "above" may include both "above" and "below". The device may also be positioned in other different ways (rotated 90 degrees or in other orientations), and the spatially relative descriptions used here are interpreted accordingly.

[0028] In addition, it should be noted that the use of terms such as "first" and "second" to limit components is only for the convenience of distinguishing the corresponding components. If not otherwise stated, the above terms have no special meaning and therefore cannot be understood as limiting the scope of protection of the present invention.

[0029] like Figure 1-4As shown, the present invention provides a method for preventing flocculation at the upper part of an immersion nozzle during continuous casting, which specifically comprises the following steps: S1. The upper inner side of the submerged water nozzle 3 is set to a bell-mouth shape and the upper inner diameter is larger than the inner diameter of the lower water nozzle 2 of the tundish. The upper inner diameter of the submerged water nozzle 3 is larger than the lower inner diameter.

[0030] S2. Seal the connection between the submerged nozzle 3 and the tundish outlet 2 with high-temperature cement 4; before the submerged nozzle 3 and the tundish 1 are baked at high temperature, apply the high-temperature cement 4 to the connection between the submerged nozzle 3 and the tundish outlet 2, compact and fix the connection between the submerged nozzle 3 and the tundish outlet 2 and the high-temperature cement 4 together, and then apply a layer of high-temperature cement 4 on the outer side of the connection between the submerged nozzle 3 and the tundish outlet 2, and the thickness of the high-temperature cement 4 is ≥10mm.

[0031] S3. Grind and polish the inner surfaces of the submerged nozzle 3, the tundish outlet 2 and the connection between the submerged nozzle 3 and the tundish outlet 2. Use sandpaper with a mesh size of 300 or above to polish the inner surfaces so that the inner surfaces feel smooth without any raised or sunken defects.

[0032] S4, heat-insulate the upper part of the immersion nozzle 3, the tundish outlet 2, and the connection between the immersion nozzle 3 and the tundish outlet 2; wrap the upper part of the immersion nozzle 3, the tundish outlet 2, and the connection between the immersion nozzle 3 and the tundish outlet 2 with a layer of insulation cotton 5, and the thickness of the insulation cotton 5 is ≥30mm. Use an insulation cover 6 to heat the outer side of the tundish outlet 2 and the upper part of the immersion nozzle 3.

[0033] S5. The submerged nozzle 3, the tundish outlet 2, the connection between the submerged nozzle 3 and the tundish outlet 2, and the tundish 1 are subjected to high-temperature baking. The submerged nozzle 3 and the tundish outlet 2 are baked by internal combustion, the baking time is ≥2h, and the baking temperature of the tundish 1 is ≥1100℃.

[0034] S6, after the baking is completed, the heat preservation cover 6 is removed, and an induction heating coil is installed on the upper part of the immersion nozzle 3, the tundish outlet 2, and the outer side of the connection between the immersion nozzle 3 and the tundish outlet 2; The total length of the induction heating coil 7 is consistent with the total length from the lower water inlet 2 of the tundish to the upper part of the immersion water inlet 3 .

[0035] S7, the induction heating coil 7 performs induction heating on the molten steel in the nozzle until the continuous casting process is completed. During continuous casting, the induction heating coil 7 performs induction heating on the molten steel in the nozzle, and the induction coil power is ≥300kw.

[0036] Example 1 like Figure 2-4As shown, the present invention provides a method for preventing flocculation at the upper part of the submerged nozzle 3 during continuous casting, which is achieved by the following scheme: 1. The inner side of the upper part of the immersion nozzle 3 is designed to be a bell-mouth shape, specifically: the inner diameter of the upper part of the immersion nozzle 3 is 180mm, the inner diameter of the lower part is 150mm, the inner diameter of the tundish lower nozzle 2 is 150mm, and the inner diameter of the upper part of the immersion nozzle 3 is greater than the inner diameter of the tundish lower nozzle 2; 2. The seal between the submerged nozzle 3 and the tundish outlet 2 is sealed with high-temperature cement 4. The sealing steps are as follows: before the submerged nozzle 3 and the tundish 1 are baked at high temperature, the high-temperature cement 4 is applied between the submerged nozzle 3 and the tundish outlet 2, and then the submerged nozzle 3, the tundish outlet 2 and the high-temperature cement 4 are compacted and fixed together, and then a layer of high-temperature cement 4 is applied on the outer side of the connection between the submerged nozzle 3 and the tundish outlet 2. The thickness of the high-temperature cement 4 is 10 mm; 3. After the immersion nozzle 3 is sealed and connected with the tundish outlet 2, a heat preservation treatment is performed. The treatment method is as follows: a layer of heat preservation cotton 5 with a thickness of 30 mm is wrapped around the upper part of the immersion nozzle 3, the tundish outlet 2 and their connection, and a heat preservation cover 6 is used to keep the outer side of the tundish outlet 2 and the upper part of the immersion nozzle 3 warm; 4. Before high-temperature baking, the inner surfaces of the submerged nozzle 3, the tundish nozzle 2 and their connections are ground and polished. 300-grit sandpaper is used for surface polishing to make the inner surface smooth to the touch without convex and concave defects; 5. After the submerged nozzle 3 and the tundish outlet 2 are connected and sealed, heat-insulated and the inner surface is polished, they are baked together with the tundish 1 at high temperature. The submerged nozzle 3 and the tundish outlet 2 are baked by internal combustion for 2 hours, and the temperature of the tundish is above 1100°C; 6. After the immersion nozzle 3, the tundish outlet 2 and the tundish 1 are baked and ready for continuous casting, remove the heat preservation cover 6, install the induction heating coil 7 on the upper part of the immersion nozzle 3, the tundish outlet 2 and the connection, and the total length of the coil from top to bottom is consistent with the total length from the tundish outlet to the upper part of the immersion nozzle 3. During continuous casting, the induction heating coil 7 induction heats the molten steel in the nozzle, and the induction coil power is 300kw.

[0037] The results are shown in the following table:

[0038] Example 2 like Figure 2-4 As shown, the present invention provides a method for preventing flocculation at the upper part of the submerged nozzle 3 during continuous casting, which is achieved by the following scheme: 1. The inner side of the upper part of the immersion nozzle 3 is designed to be a bell-mouth shape, specifically: the inner diameter of the upper part of the immersion nozzle 3 is 75mm, the inner diameter of the lower part is 55mm, the inner diameter of the tundish lower nozzle 2 is 55mm, and the inner diameter of the upper part of the immersion nozzle 3 is greater than the inner diameter of the tundish lower nozzle 2; 2. The seal between the submerged nozzle 3 and the tundish outlet 2 is sealed with high-temperature cement 4. The sealing steps are as follows: before the submerged nozzle 3 and the tundish 1 are baked at high temperature, the high-temperature cement 4 is applied between the submerged nozzle 3 and the tundish outlet 2, and then the submerged nozzle 3, the tundish outlet 2 and the high-temperature cement 4 are compacted and fixed together, and then a layer of high-temperature cement 4 is applied on the outer side of the connection between the submerged nozzle 3 and the tundish outlet 2. The thickness of the high-temperature cement 4 is 15 mm; 3. After the immersion nozzle 3 is sealed and connected with the tundish outlet 2, insulation treatment is performed. The treatment method is as follows: the upper part of the immersion nozzle 3, the tundish outlet 2 and their connection are wrapped with a layer of insulation cotton 5 with a thickness of 35 mm, and the outer side of the tundish outlet 1 and the upper part of the immersion nozzle 3 are insulated with an insulation cover 6; 4. Before high-temperature baking, the inner surfaces of the submerged nozzle 3, the tundish nozzle 2 and their connections are ground and polished. The surface is polished with 400-grit sandpaper to make the inner surface smooth to the touch without convex and concave defects; 5. After the submerged nozzle 3 and the tundish outlet 2 are connected and sealed, heat-insulated and the inner surface is polished, they are baked together with the tundish 1 at high temperature. The submerged nozzle 3 and the tundish outlet 2 are baked by internal combustion for 2.5 hours, and the temperature of the tundish is above 1150°C; 6. After the immersion nozzle 3, the tundish outlet 2 and the tundish 1 are baked and ready for continuous casting, remove the heat preservation cover 6, install the induction heating coil 7 on the upper part of the immersion nozzle 3, the tundish outlet 2 and the connection, and the total length of the coil from top to bottom is consistent with the total length from the tundish outlet to the upper part of the immersion nozzle 3. During continuous casting, the induction heating coil 7 induction heats the molten steel in the nozzle, and the induction coil power is 350kw.

[0039] The results are shown in the following table:

[0040] Example 3 The present invention provides a method for preventing flocculation at the upper part of the submerged nozzle 3 during continuous casting, which is achieved by the following scheme: 1. The inner side of the upper part of the immersion nozzle 3 is designed to be a bell-mouth shape, specifically: the inner diameter of the upper part of the immersion nozzle 3 is 90mm, the inner diameter of the lower part is 70mm, the inner diameter of the tundish lower nozzle 2 is 70mm, and the inner diameter of the upper part of the immersion nozzle 3 is greater than the inner diameter of the tundish lower nozzle 2; 2. The seal between the submerged nozzle 3 and the tundish outlet 2 is sealed with high-temperature cement 4. The sealing steps are as follows: before the submerged nozzle 3 and the tundish 1 are baked at high temperature, the high-temperature cement 4 is applied between the submerged nozzle 3 and the tundish outlet 2, and then the submerged nozzle 3, the tundish outlet 2 and the high-temperature cement 4 are compacted and fixed together, and then a layer of high-temperature cement 4 is applied on the outer side of the connection between the submerged nozzle 3 and the tundish outlet 2. The thickness of the high-temperature cement 4 is 20 mm; 3. After the immersion nozzle 3 is sealed and connected with the tundish outlet 2, a heat preservation treatment is performed. The treatment method is as follows: a layer of heat preservation cotton 5 with a thickness of 40 mm is wrapped around the upper part of the immersion nozzle 3, the tundish outlet 2 and their connection, and a heat preservation cover 6 is used to keep the outer side of the tundish outlet 2 and the upper part of the immersion nozzle 3 warm; 4. Before high-temperature baking, the inner surfaces of the submerged nozzle 3, the tundish nozzle 2 and their connections are ground and polished. 500-grit sandpaper is used for surface polishing to make the inner surface smooth to the touch without convex and concave defects; 5. After the submerged nozzle 3 and the tundish outlet 2 are connected and sealed, heat-insulated and the inner surface is polished, they are baked together with the tundish 1 at high temperature. The submerged nozzle 3 and the tundish outlet 2 are baked by internal combustion, the baking time is 3.0 hours, and the tundish temperature is above 1200℃; 6. After the immersion nozzle 3, the tundish outlet 2 and the tundish 1 are baked and ready for continuous casting, the heat preservation cover 6 is removed, and the induction heating coil 7 is installed on the upper part of the immersion nozzle 3, the tundish outlet 2 and the connection. The total length of the coil from top to bottom is consistent with the total length from the tundish outlet to the upper part of the immersion nozzle 3. During continuous casting, the induction heating coil 7 induction heats the molten steel in the nozzle, and the induction coil power is 380kw.

[0041] The results are shown in the following table:

[0042] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A method for preventing flocculation at the upper part of an immersion nozzle during continuous casting, characterized in that: The steps include: Preparation stage: S1, setting the upper inner side of the submerged nozzle into a bell-mouth shape and making the upper inner diameter larger than the inner diameter of the lower nozzle of the tundish; S2. Seal the connection between the submerged nozzle and the lower nozzle of the tundish; S3, grinding and polishing the inner surfaces of the submerged nozzle, the tundish outlet, and the connection between the submerged nozzle and the tundish outlet; S4. Insulating the upper part of the submerged nozzle, the lower nozzle of the tundish, and the connection between the submerged nozzle and the lower nozzle of the tundish; S5. High temperature baking is performed on the submerged nozzle, the tundish outlet, the connection between the submerged nozzle and the tundish outlet, and the tundish, and the high temperature range is ≥1100°C; S6. After the baking is completed, the heat preservation cover is removed, and an induction heating coil is installed on the upper part of the immersion nozzle, the lower nozzle of the tundish, and the outer side of the connection between the immersion nozzle and the lower nozzle of the tundish; Use stage: S7, the induction heating coil induction heats the molten steel in the nozzle until the continuous casting process is completed.

2. The method for preventing flocculation at the upper part of an immersion nozzle during continuous casting according to claim 1, characterized in that: The specific configuration in S1 is as follows: the inner diameter of the upper part of the submerged nozzle is larger than the inner diameter of the lower part thereof, and the inner diameter of the upper part of the submerged nozzle is larger than the inner diameter of the lower nozzle of the tundish.

3. The method for preventing flocculation at the upper part of an immersion nozzle during continuous casting according to claim 1, characterized in that: S2 uses high temperature cement sealing, and the sealing steps are as follows: S21. Before the submerged nozzle and the tundish are baked at high temperature, apply the cement to the connection between the submerged nozzle and the lower nozzle of the tundish; S22, compact and fix the connection between the submerged nozzle and the lower nozzle of the tundish together with the cement; S23. Based on S22, apply a layer of cement on the outer side of the connection between the submerged nozzle and the lower nozzle of the tundish, and the thickness of the cement should be ≥10mm.

4. The method for preventing flocculation at the upper part of an immersion nozzle during continuous casting according to claim 1, characterized in that: The grinding and polishing in S3 are specifically as follows: the inner surface is polished with sandpaper of 300 mesh or above, so that the inner surface feels smooth and has no raised or sunken defects.

5. The method for preventing flocculation at the upper part of a submerged nozzle during continuous casting according to claim 1, characterized in that: In S4, the specific insulation treatment method is: wrap the upper part of the immersion nozzle, the lower nozzle of the tundish, and the connection between the immersion nozzle and the lower nozzle of the tundish with a layer of insulation cotton, and the thickness of the insulation cotton is ≥30mm.

6. The method for preventing flocculation at the upper part of a submerged nozzle during continuous casting according to claim 5, characterized in that: The specific insulation treatment method also includes using an insulation cover to insulate the outer side of the lower water outlet of the tundish and the upper part of the immersion water outlet.

7. The method for preventing flocculation at the upper part of a submerged nozzle during continuous casting according to claim 1, characterized in that: In S5, the submerged nozzle and the tundish outlet are baked by internal combustion, the baking time is ≥2h, and the tundish baking temperature is ≥1100℃.

8. The method for preventing flocculation at the upper part of a submerged nozzle during continuous casting according to claim 1, characterized in that: In S6, the total length of the induction heating coil is consistent with the total length from the lower water inlet of the tundish to the upper part of the submerged water inlet.

9. The method for preventing flocculation at the upper part of a submerged nozzle during continuous casting according to claim 1, characterized in that: In S7, during continuous casting, the induction heating coil performs induction heating on the molten steel in the nozzle, and the power of the induction coil is ≥300kw.

Citation Information

Patent Citations

  • Submersed nozzle capable of eliminating flocculation flow and application method

    CN106475552A

  • Method for baking intrusive water gap by means of tundish baking waste heat

    CN107335796A

  • Method for sealing gap between upper nozzle and lower nozzle of continuous casting tundish

    CN116000274A

  • Argon seal protection pouring device for submersed nozzle

    CN210125731U

  • Graphite-based seal for discharge fitting and dip tube, etc,

    DE4420199A1