High-thermal-conductivity MIM copper optical module processing technology

Through process steps such as sintering forming, mold shaping and CNC processing, the problem of imprecise dimensional tolerance and easy deformation after the MIM copper optical module is formed is solved, and high-precision and stable high thermal conductivity optical module processing is achieved, which is suitable for mass production.

CN118768876AInactive Publication Date: 2024-10-15DONGGUAN XINGHE PRECISION DIECASTING MOLD CO LTD
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411121976.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-15
Publication Date
2024-10-15
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Traditional die-cast optical modules have difficulty dissipating heat in high-speed transmission environments. MIM copper optical modules have poor dimensional tolerances and are easily deformed after forming, making it difficult to meet high-precision and mass production requirements.

Method used

Process steps such as sintering forming, mold shaping, CNC processing, sand blasting, electroplating and drilling are used, combined with pallet anti-collision and full inspection processing to ensure product flatness, dimensions and structural accuracy, and reduce the risk of deformation.

Benefits of technology

It effectively solves the problem of imprecise dimensional tolerance and easy deformation of MIM copper optical modules after forming, improves the accuracy and stability of the product, and is suitable for mass production.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention provides a high-thermal-conductivity MIM copper optical module machining process which comprises the following process steps that firstly, MIM copper is sintered to form a blank material, and a water gap is flushed away; secondly, a mold is used for shaping, and the flatness of the product is adjusted to be within 0.075; thirdly, CNC machining is adopted, and the boundary dimension of the product is guaranteed; fourthly, sand blasting equipment is adopted for conducting sand blasting treatment on the product; 5, electroplating treatment is conducted on the product; sixthly, drilling and tapping are conducted on the product through a machine tool; and 7, detecting electroplating flaws and the appearance structure of the product by adopting detection equipment to obtain a qualified product. Aiming at several defects of the MIM copper optical module, the problems that the product is easy to deform and the dimensional tolerance is not in place after the MIM copper is subjected to injection molding and sintering are solved, and the problem that the MIM copper optical module is easy to damage and deform due to collision is solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of optical module processing, and in particular to a high thermal conductivity MIM copper optical module processing technology. Background Art

[0002] In 2024, the capital expenditure of global telecom operators in the optical communication industry will be approximately US$334 billion. The global optical communication industry will enter a new investment cycle. According to the forecast of market research organization Lightcounting, the global optical communication industry will maintain an annual growth rate of 15% in the next five years. Due to the active promotion of domestic national policies, it is expected that domestic optical communications will continue to show a rapid growth momentum at an average annual rate of at least 20% in the next five years, becoming the world's largest optical communication market. Affected by this environment, the domestic optical module market will usher in a booming development opportunity.

[0003] Although the requirements for the photoelectric transmission speed of optical modules are getting faster and faster, 400G and 800G have become the mainstream, and 1.2T and 1.5T have become the development direction. The rapid development of transmission speed has brought high requirements for the process of traditional die-cast optical modules, because the faster the transmission speed, the more serious the heat of the optical module products. If the heat is quickly dissipated, it is a difficult problem that needs to be solved in the optical module processing industry. As we all know, the thermal conductivity of pure copper (red copper) is much higher than that of zinc alloy (the thermal conductivity of zinc alloy is 113W / Mk, and the thermal conductivity of pure copper is about 300W / Mk), but pure copper is not easy to die-cast. Therefore, MIM copper has become the first choice for the forming process of pure copper optical modules. However, MIM copper is easy to deform, and the larger the product features, the larger the forming tolerance. How to ensure that the MIM copper optical module is formed and processed into a qualified optical module product is a difficult problem facing all optical module processing industries.

[0004] If pure copper optical modules are 100% machined, the cost will be very high and not suitable for mass production. The die-casting process of pure copper is very easy to stick to the mold because of the high melting point of copper (close to the melting point of the mold core). In addition, the fluidity of pure copper during die-casting is poor, making it extremely difficult to form. At present, attempts to use pure copper die-casting in the industry have not been successful; and forging pure copper is difficult to achieve because some small features of the optical module cannot guarantee the accuracy. Therefore, the use of MIM copper first uses powder metallurgy to make a blank, and then uses shaping machining to achieve the dimensional accuracy required by the optical module. This is a more ideal process. MIM copper (i.e. pure copper powder metallurgy) has three key disadvantages. First, due to the characteristics of the powder metallurgy process, the tolerance fluctuation will be larger when the product specifications are larger, that is, the tolerance accuracy will be difficult to ensure that the dimensional tolerance is within the qualified range due to the large specifications; second, because pure copper is relatively soft, it is easy to deform after powder metallurgy sintering and needs to be reshaped; third, because pure copper is relatively soft and has a relatively high density, some edges of the optical module are relatively thin, and it may be deformed by a slight collision with external force. Summary of the invention

[0005] The present invention provides a high thermal conductivity MIM copper optical module processing technology. Aiming at several shortcomings of the MIM copper optical module, we adopt targeted improvements in the process to solve the three shortcomings of the MIM copper optical module.

[0006] To achieve the above object, the present invention adopts the following technical solution:

[0007] A high thermal conductivity MIM copper optical module processing technology includes the following process steps:

[0008] Step 1: Sinter the MIM copper into a blank and flush the nozzle;

[0009] Step 2: Use mold shaping to adjust the flatness of the product to within 0.075;

[0010] Step 3: Use CNC processing to ensure the product's dimensions;

[0011] Step 4: Use sandblasting equipment to sandblast the product;

[0012] Step 5: Electroplating the product;

[0013] Step 6: Use machine tools to drill and tap the product;

[0014] Step 7: Use testing equipment to detect electroplating defects and product appearance structure to obtain qualified products.

[0015] Preferably, in step 2, rough shaping is first performed to adjust the flatness to within 0.15, and then fine shaping is performed to adjust the flatness to within 0.075.

[0016] Preferably, after the processing in step three is completed, the product is deburred.

[0017] Preferably, in step 4, the sandblasting equipment uses 100# steel sand and the air pressure is 2.0KG.

[0018] Preferably, after completing step 4, the product needs to be fully inspected to detect defects. Qualified products proceed to the next step, otherwise they need to be sandblasted and fully inspected again.

[0019] Preferably, in the electroplating treatment in step five, Ni: 2-7um; Cu: 10-25um.

[0020] Preferably, from the beginning of step one to the end of step seven, pallets are used throughout the entire process to prevent collisions.

[0021] Compared with the prior art, the beneficial effects of the present invention are that it addresses several shortcomings of MIM copper optical modules, solves the problems of easy deformation and inadequate dimensional tolerance of MIM copper products after injection molding and sintering, and solves the problem of easy scratches and deformation of MIM copper optical modules. DETAILED DESCRIPTION

[0022] The technical solutions in the embodiments of the present invention will be described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments.

[0023] It should be noted that when a component / part is referred to as being "set on" another component / part, it may be directly set on the other component / part or there may also be an intermediate component / part. When a component / part is referred to as being "connected / coupled" to another component / part, it may be directly connected / coupled to the other component / part or there may be an intermediate component / part at the same time. The term "connection / coupling" as used herein may include electrical and / or mechanical physical connections / couplings. The term "includes / comprising" as used herein refers to the presence of a feature, step or component / part, but does not exclude the presence or addition of one or more other features, steps or components / parts. The term "and / or" as used herein includes any and all combinations of one or more relevant listed items.

[0024] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which this application belongs. The terms used herein are only for the purpose of describing specific embodiments and are not intended to limit this application.

[0025] In view of several shortcomings of MIM copper optical modules, we have adopted targeted improvements in the process. First, we conduct a full-size review according to the customer's 2D drawing dimension specifications. What powder metallurgy can meet is guaranteed by the powder metallurgy process. What powder metallurgy cannot meet is to increase the machining allowance and ensure it by post-processing. The specific process flow is as follows:

[0026] A high thermal conductivity MIM copper optical module processing technology includes the following process steps:

[0027] Step 1: Sinter the MIM copper into a blank and flush out the blank nozzle to keep the blank clean;

[0028] Step 2: Use mold shaping to adjust the flatness of the product to within 0.075; in this step, it is necessary to first perform rough shaping to adjust the flatness to within 0.15, and then perform fine shaping to adjust the flatness to within 0.075;

[0029] Step 3: Use CNC processing to ensure the product's external dimensions; the product shape and size can be processed according to the drawing. After processing, the product needs to be deburred, which can be removed manually;

[0030] Step 4: Use sandblasting equipment to sandblast the product; the sandblasting equipment uses 100# steel sand and the air pressure is 2.0KG; after completing this step, the product needs to be fully inspected to detect the defects of the product. Large defects can be checked manually, and small defects can be checked by testing equipment. Qualified products proceed to the next step, otherwise they need to be sandblasted and fully inspected again.

[0031] Step 5: Electroplating the product; using ordinary electroplating process, Ni: 2-7um; Cu: 10-25um.

[0032] Step 6: Use machine tools to drill and tap the product; the position and size of the drilling and tapping can be carried out according to the processing drawings;

[0033] Step 7: Use testing equipment to detect electroplating defects and product appearance structure to obtain qualified products. From step 1 to step 7, pallets are used throughout the entire process to prevent collisions.

[0034] The present invention aims at several shortcomings of MIM copper optical modules, solves the problems that MIM copper products are easy to deform and dimensional tolerances cannot be achieved after injection molding and sintering, and solves the problem that MIM copper optical modules are easy to be scratched and deformed.

[0035] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A high thermal conductivity MIM copper optical module processing technology, characterized in that: The process steps include: Step 1: Sinter the MIM copper into a blank and flush the nozzle; Step 2: Use mold shaping to adjust the flatness of the product to within 0.075; Step 3: Use CNC processing to ensure the product's dimensions; Step 4: Use sandblasting equipment to sandblast the product; Step 5: Electroplating the product; Step 6: Use machine tools to drill and tap the product; Step 7: Use testing equipment to detect electroplating defects and product appearance structure to obtain qualified products.

2. The high thermal conductivity MIM copper optical module processing technology according to claim 1 is characterized in that: In the step 2, rough shaping is first performed to adjust the flatness to within 0.15, and then fine shaping is performed to adjust the flatness to within 0.

075.

3. The high thermal conductivity MIM copper optical module processing technology according to claim 1 is characterized in that: After the processing in step three is completed, the product needs to be deburred.

4. The high thermal conductivity MIM copper optical module processing technology according to claim 1 is characterized in that: In step 4, the sandblasting equipment uses 100# steel sand and the air pressure is 2.0KG.

5. The high thermal conductivity MIM copper optical module processing technology according to claim 4 is characterized in that: After completing step 4, the product needs to be fully inspected to detect defects. Qualified products will proceed to the next step, otherwise they need to be sandblasted and fully inspected again.

6. The high thermal conductivity MIM copper optical module processing technology according to claim 1 is characterized in that: In the electroplating process of step five, Ni: 2-7um; Cu: 10-25um.

7. The high thermal conductivity MIM copper optical module processing technology according to claim 1 is characterized in that: From the beginning of step one to the end of step seven, pallets are used throughout the entire process to prevent collisions.

Citation Information

Cited By

  • Manufacturing process of high-reliability copper optical module

    CN120190583A

  • A manufacturing process for a high-reliability copper optical module

    CN120190583B