Composite AEM rubber plate for solar laminating machine and preparation process of composite AEM rubber plate
By adopting the vulcanization preparation process of composite AEM rubber sheets in a solar laminator, combined with specific components and skeleton grid layers, the problem of high price of AEM rubber sheets has been solved, and wide application in the mid-to-low-end market has been achieved. and performance improvements.
Patent Information
- Application Number
- CN202410807112.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-21
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2044-06-21
AI Technical Summary
Due to the high price, the oil-resistant and high-temperature-resistant rubber sheets for solar laminators prepared from AEM three-component adhesive cannot be widely used and promoted in the mid- to low-end laminator market, resulting in a limited scope of application.
A solar laminator is used to composite AEM rubber sheets, including non-working surface rubber sheets, skeleton grid layers and working surface rubber sheets. Through a vulcanization composite preparation process, EPDM rubber, carbon black, paraffin oil, and inorganic fillers are used. , zinc oxide, antioxidant, tackifying resin, coupling agent and peroxide vulcanizing agent, combined with aramid mesh skeleton material to simplify the process and improve production efficiency.
It achieves good performance under the conditions of 170℃×70h, and at the same time effectively reduces the production cost of AEM rubber sheets, making it widely used and promoted in the mid-to-low-end laminator market and improving production efficiency.
Smart Images

Figure CN118769641A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of rubber sheet preparation, in particular to a solar laminator composite AEM rubber sheet and a preparation process thereof. Background Art
[0002] AEM rubber is called ethylene acrylate rubber (AEM), an ethylene copolymer with 8% to 40% methyl acrylate content, a milky white translucent solid, and a synthetic rubber composed of ethylene and acrylic acid monomers. Ethylene has good low temperature performance, while the acrylic acid part improves oil resistance. The combination of saturated main chain and polar side groups also provides good heat resistance, ozone resistance (weather resistance) and many chemical resistance.
[0003] AEM rubber is widely used in automotive rubber parts, including AEM binary rubber and AEM ternary rubber. Among them, AEM ternary rubber has excellent flex resistance, and the flex life is more than 250,000 times at 100°C. Its dynamic performance is also good, and its shock absorption performance at high temperature is close to that of IIR. AEM rubber has excellent resistance to compression permanent deformation, especially AEM ternary rubber vulcanized with amine vulcanizer, which has a compression permanent deformation of less than 20% under the condition of 170°C×70h, while the resistance to compression permanent deformation of binary rubber vulcanized with peroxide is slightly worse than that of ternary rubber.
[0004] Our company has optimized the selection of the main rubber, plasticizer and vulcanization accelerator of AEM ternary rubber in formula design, improved its two-stage vulcanization process, and developed oil-resistant and high-temperature resistant rubber sheets for solar laminators, which can be used as laminator rubber sheets and have excellent performance even at high temperatures of 170 degrees Celsius and above.
[0005] The oil-resistant and high-temperature resistant rubber sheet for solar laminators prepared with AEM ternary rubber is expensive, which limits its application scope and prevents it from being widely used and promoted in the mid- and low-end laminator market. Therefore, optimizing the oil-resistant and high-temperature resistant rubber sheet through technical means to reduce production costs and increase its application scope is the primary goal at this stage. Summary of the invention
[0006] The invention provides a solar laminator composite AEM rubber sheet and a preparation process thereof, which are used to meet the heat resistance requirements of the rubber sheet and effectively reduce the production cost of the AEM rubber sheet.
[0007] A technical solution adopted by the present invention is: to provide a solar laminator composite AEM rubber sheet, the rubber sheet comprises a non-working surface rubber sheet, a skeleton grid layer and a working surface rubber sheet arranged in sequence from top to bottom, the three being vulcanized and composited;
[0008] The non-working surface rubber sheet mainly comprises the following components by weight:
[0009] 100 parts of EPDM rubber, 50-65 parts of carbon black, 5-8 parts of paraffin oil, 20-30 parts of inorganic filler, 5-10 parts of zinc oxide, 0.5-1.0 parts of stearic acid, 4.5-9 parts of antioxidant, 2-4 parts of tackifying resin, 2-4 parts of coupling agent, 8-10 parts of peroxide vulcanizing agent, 3-5 parts of cross-linking agent;
[0010] The working surface rubber sheet mainly comprises the following components by weight:
[0011] AEM-DP 100 parts, carbon black 50-80 parts, antioxidant 1-2 parts, internal mold release agent 2-5 parts, scorch retarder 0.5-1.5 parts, peroxide vulcanizer 5-7 parts, cross-linking agent 1.5-3 parts.
[0012] Furthermore, the skeleton mesh layer adopts aramid mesh cloth skeleton material.
[0013] Furthermore, the peroxide vulcanizing agent is one of DCP vulcanizing agent, BIPB vulcanizing agent and bis-25 vulcanizing agent.
[0014] Furthermore, the peroxide vulcanizing agent is a bis-25 vulcanizing agent, and the bis-25 vulcanizing agent is a vulcanizing agent with a bis-25 content of 50%.
[0015] Furthermore, the auxiliary crosslinking agent is one of TAC auxiliary crosslinking agent, TAIC auxiliary crosslinking agent, TMPTMA auxiliary crosslinking agent and HVA-2 auxiliary crosslinking agent.
[0016] Furthermore, the auxiliary cross-linking agent is TAIC auxiliary cross-linking agent, which has the best comprehensive performance when combined with di-25 vulcanizing agent.
[0017] Another technical solution adopted by the present invention is to provide a preparation process of a solar laminator composite AEM rubber sheet, comprising the following steps:
[0018] S1, preparing AEM rubber compound and EPDM rubber compound respectively;
[0019] S2, extruding or calendering the AEM rubber compound and the EPDM rubber compound to obtain semi-finished rubber sheets for working surfaces and semi-finished rubber sheets for non-working surfaces;
[0020] S3, tighten the skeleton grid layer and cover it on the semi-finished rubber sheet on the working surface, cover the semi-finished rubber sheet on the non-working surface on the skeleton grid layer, and vulcanize them together to obtain the composite AEM rubber sheet.
[0021] Further, in step S1, preparing the AEM compound rubber comprises the following steps:
[0022] SA1. Mixing masterbatch: AEM-DP, antioxidant, internal release agent, anti-scorch agent and carbon black are put into an internal mixer. The internal mixer is mixed by step-by-step speed reduction, and the AEM masterbatch is obtained by rubber discharge.
[0023] SA2, one-time refining: add AEM masterbatch into the open mixer for refining, and after refining evenly, the sheets are cooled;
[0024] SA3, sulfur addition and mixing: add the AEM masterbatch, vulcanizing agent and cross-linking agent after the first refining into an open mixer or internal mixer for mixing, and discharge the glue to obtain the AEM mixed rubber;
[0025] SA4, Second refining: Add the AEM compound to the open mixer for refining. After refining evenly, the sheet is cooled.
[0026] Furthermore, in the mixing process described in step SA1, the upper push pin pressure is set between 4.5-5.5KGF, the filling factor is between 0.7-0.75, and the step-by-step speed reduction refers to the speed of the internal mixer being increased from the initial 35 to 25 before discharge, and gradually decreased after each lifting of the upper push pin for cleaning, and the discharge temperature is controlled between 135-145°C.
[0027] Furthermore, in the mixing process described in step SA3, the upper push bolt pressure is set between 3.5-4.5KGF, the water temperature of the three zones is controlled within 20°C, the rotation speed is 15-25R / MIN, the filling factor is between 0.5-0.65, the debinding temperature is controlled within 100°C, and the AEM mixed rubber is obtained by debinding.
[0028] The beneficial effects of the solar laminator composite AEM rubber sheet and the preparation process thereof of the present invention are:
[0029] 1. The use of AEM and EPDM composite rubber sheets can not only make the working surface work well under the conditions of 170℃×70h, but also effectively reduce the production cost of AEM rubber sheets, making it more widely used and promoted in the mid- and low-end laminating machine market;
[0030] 2. Since the semi-finished rubber sheet of the working surface has good adhesion with the skeleton material, during the preparation process of the composite AEM rubber sheet, the three-layer structure can be vulcanized and formed at one time, which greatly simplifies the process and improves production efficiency. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 The first embodiment of the present invention is a preparation process of a solar laminator composite AEM rubber sheet;
[0032] Figure 2 It is a comparison table of AEM compound rubber performance test data of various embodiments of the present invention. DETAILED DESCRIPTION
[0033] The preferred embodiments of the present invention are described in detail below in conjunction with the accompanying drawings so that the advantages and features of the present invention can be more easily understood by those skilled in the art, thereby making a clearer and more definite definition of the protection scope of the present invention.
[0034] The first embodiment of the present invention provides a solar laminator composite AEM rubber sheet, wherein the rubber sheet comprises a non-working surface rubber sheet, a skeleton grid layer and a working surface rubber sheet arranged in sequence from top to bottom, and the three are vulcanized and composited;
[0035] The non-working surface rubber sheet mainly includes the following components by weight:
[0036] 100 parts of EPDM rubber, 57 parts of carbon black, 6 parts of paraffin oil, 25 parts of inorganic filler, 7 parts of zinc oxide, 0.7 parts of stearic acid, 6 parts of antioxidant, 3 parts of tackifying resin, 3 parts of coupling agent, 9 parts of peroxide vulcanizing agent, 4 parts of cross-linking agent;
[0037] The carbon black includes 45 parts of N330 and 12 parts of white carbon black 255, the paraffin oil is high flash point paraffin oil P2280, the inorganic filler is calcined kaolin, the antioxidant is RD, MBI and 445 (1:1:1), the tackifying resin is C5, the coupling agent is SI69-50, the peroxide vulcanizer is bis-25 vulcanizer (101-50 powder contains 50% bis-25), and the cross-linking agent is TMPTMA cross-linking agent (350D TMPTMA-50).
[0038] The working surface rubber sheet mainly includes the following components by weight:
[0039] 100 parts of AEM binary rubber, 65 parts of carbon black, 1.5 parts of antioxidant, 3 parts of internal release agent, 1 part of anti-scorch agent, 6 parts of peroxide vulcanizer, 2 parts of cross-linking agent;
[0040] The main rubber is AEM-DP, the carbon black includes 45 parts of N550 and 20 parts of N774, the antioxidant is 445, the internal release agent is a combination of stearic acid, VAM and PE wax (1:3:2), the anti-scorch agent is 18D, the peroxide vulcanizer is a di-25 vulcanizer (101-50 powder contains 50% di-25), and the co-crosslinking agent is TAIC co-crosslinking agent (TAIC-70);
[0041] The skeleton grid layer adopts aramid mesh cloth skeleton material. The aramid mesh cloth skeleton material is treated with glue in advance and can be well bonded with AEM and EPDM mixed rubber, which can improve the flexural fatigue resistance and service life of the rubber plate.
[0042] In the process of studying the compound of AEM and EPDM, based on the characteristics that both AEM binary rubber and EPDM rubber can be vulcanized with peroxide, AEM binary rubber was selected as the main rubber of the working surface rubber plate, so that the working surface rubber plate and the non-working surface rubber plate have a theoretical basis for synchronous vulcanization. On this basis, the specific binary rubber type used by AEM rubber was tested and analyzed:
[0043] Among AEM binary rubbers, the performance of Vamac DP is closer to that of AEM ternary rubber. It also has good oil and high temperature resistance, good compression set resistance and good low temperature elasticity. However, Vamac DHC has insufficient heat resistance (the upper limit of continuous working temperature of ordinary Vamac elastomers is 165°C). Therefore, in order to work well under the conditions of 170°C×70h, AEM-DP is selected as the main rubber for the working surface rubber sheet.
[0044] Peroxide vulcanizers suitable for AEM-DP binary rubber include DCP vulcanizer, BIPB vulcanizer (BIPB is odorless DCP, 1.3 di-tert-butyl peroxy diisopropylbenzene), and bis-25 vulcanizer (bis-25 is DBPMH, 2.5 dimethyl-2.5 di-tert-butyl peroxyhexane):
[0045] The 10-hour half-life temperatures of the three most commonly used peroxides in industry are DCP: 117°C, BIPB: 120°C, and DBPMH: 122°C. This temperature is the safe operating temperature of the rubber material. The higher the temperature, the better the operating safety. In this embodiment, both the working surface rubber sheet and the non-working surface rubber sheet use double 25 as the peroxide vulcanizing agent, which has better operating safety.
[0046] Among them, the bis-25 vulcanizing agent is a vulcanizing agent with a bis-25 content of 50%, which is formed by absorbing liquid bis-25 with inorganic substances.
[0047] Commonly used peroxide crosslinking agents include TAC crosslinking agent (TAC triallyl cyanurate), TAIC crosslinking agent (TAIC triallyl isocyanurate), TMPTMA crosslinking agent (TMPTMA trimethylolpropane trimethacrylate), and HVA-2 crosslinking agent (HVA-2N, N-phenylene bismaleimide):
[0048] Four cross-linking agents were tested in combination with di-25 vulcanizer, and each had advantages in many aspects such as scorch safety, heat resistance, physical and mechanical properties, rebound compression deformation, and flexural fatigue resistance. In this embodiment, TAIC cross-linking agent was selected as the cross-linking agent, and the rubber material prepared in combination with di-25 vulcanizer had the best comprehensive performance.
[0049] See also Figure 1 The first embodiment of the present invention provides a preparation process of a solar laminator composite AEM rubber sheet, comprising the following steps:
[0050] S1, preparing AEM rubber compound and EPDM rubber compound respectively;
[0051] S2, extruding the AEM rubber compound and the EPDM rubber compound respectively to obtain semi-finished rubber plates for working surfaces and semi-finished rubber plates for non-working surfaces;
[0052] S3. Overlap and lay several semi-finished rubber sheets of the working surface on a flat vulcanizer, tighten and cover the skeleton grid layer on it, and then overlap and lay the semi-finished rubber sheets of the non-working surface on the skeleton grid layer, and vulcanize them together to obtain a composite AEM rubber sheet.
[0053] In step S1, preparing the AEM rubber compound comprises the following steps:
[0054] SA1. Mixing masterbatch: AEM-DP, antioxidant 445, internal mold release agent (stearic acid, VAM, PE wax), anti-scorch agent 18D and carbon black (N550, N774) are put into an internal mixer. The upper push pin pressure is set to 5KGF, and the filling factor is 0.7. The internal mixer is mixed in a step-by-step speed reduction manner, from the initial 35 to 25 before discharge. The speed is gradually reduced after each lifting of the upper push pin and cleaning. The discharge temperature is controlled at 140°C, and the AEM masterbatch is obtained by discharge.
[0055] SA2, one-time refining: add AEM masterbatch into the open mixer for refining, and after refining evenly, cool the sheets and leave them for more than 8 hours;
[0056] SA3, sulfur addition and mixing: add the AEM masterbatch, double 25 vulcanizing agent and TAIC cross-linking agent after the first refining into the internal mixer for mixing, set the upper push bolt pressure to 4KGF, control the water temperature of the three zones within 20℃, the speed at 20R / MIN, the filling factor at 0.55, and discharge the glue below 95℃ to obtain the AEM mixed glue;
[0057] SA4. Second refining: Add the AEM compound to the open mixer for refining. After refining evenly, cool the sheet and leave it for more than 24 hours to eliminate the sheet stress of the rubber compound, to achieve sufficient infiltration, dispersion and shrinkage, and to ensure the stability of the size of the semi-finished product.
[0058] AEM compound rubber performance test data in this embodiment:
[0059]
[0060]
[0061] * Refers to the AEM mixed rubber after one stage of vulcanization, and the one-stage vulcanization process is: 180℃×8MIN. The performance test data of the EPDM mixed rubber in this example:
[0062]
[0063] * Refers to the EPDM compound after one-stage vulcanization. One-stage vulcanization process: 180℃×8MIN.
[0064] The composite AEM rubber sheet prepared in this embodiment can have a service life of more than 150,000 times.
[0065] In the second to sixth embodiments of the present invention, the selection of peroxide vulcanizing agent and co-crosslinking agent in the AEM rubber compound is adjusted, and the mass ratio of each embodiment is as shown in the figure below:
[0066]
[0067] Using the same preparation process as the first embodiment, the performance test data of the AEM compound rubber of each embodiment are as follows:
[0068]
[0069]
[0070] Comparison of the various embodiments shows that when the peroxide vulcanizer and the auxiliary cross-linking agent are selected as Bis-25 and TAIC for use in combination, the comprehensive performance is the best.
[0071] The beneficial effects of the solar laminator composite AEM rubber sheet and the preparation process thereof of the present invention are:
[0072] 1. The use of AEM and EPDM composite rubber sheets can not only make the working surface work well under the conditions of 170℃×70h, but also effectively reduce the production cost of AEM rubber sheets, making it more widely used and promoted in the mid- and low-end laminating machine market;
[0073] 2. Since the semi-finished rubber sheet of the working surface has good adhesion with the skeleton material, during the preparation process of the composite AEM rubber sheet, the three-layer structure can be vulcanized and formed at one time, which greatly simplifies the process and improves production efficiency.
[0074] The above descriptions are merely embodiments of the present invention and are not intended to limit the patent scope of the present invention. Any equivalent structure or equivalent process transformation made using the contents of the present invention specification and drawings, or directly or indirectly applied in other related technical fields, are also included in the patent protection scope of the present invention.
Claims
1. A solar laminator composite AEM rubber sheet, the rubber sheet comprising a non-working surface rubber sheet, a skeleton grid layer and a working surface rubber sheet arranged in sequence from top to bottom, the three being vulcanized and composited; The non-working surface rubber sheet mainly comprises the following components by weight: 100 parts of EPDM rubber, 50-65 parts of carbon black, 5-8 parts of paraffin oil, 20-30 parts of inorganic filler, 5-10 parts of zinc oxide, 0.5-1.0 parts of stearic acid, 4.5-9 parts of antioxidant, 2-4 parts of tackifying resin, 2-4 parts of coupling agent, 8-10 parts of peroxide vulcanizing agent, 3-5 parts of cross-linking agent; the working surface rubber plate mainly includes the following components by weight: AEM-DP 100 parts, carbon black 50-80 parts, antioxidant 1-2 parts, internal mold release agent 2-5 parts, scorch retarder 0.5-1.5 parts, peroxide vulcanizer 5-7 parts, cross-linking agent 1.5-3 parts.
2. A solar laminator composite AEM rubber sheet according to claim 1, characterized in that: The skeleton mesh layer adopts aramid mesh cloth skeleton material.
3. A solar laminator composite AEM rubber sheet according to any one of claims 1 or 2, characterized in that: The peroxide vulcanizing agent is one of DCP vulcanizing agent, BIPB vulcanizing agent and bis-25 vulcanizing agent.
4. A solar laminator composite AEM rubber sheet according to claim 3, characterized in that: The peroxide vulcanizing agent is di-25 vulcanizing agent.
5. A solar laminator composite AEM rubber sheet according to claim 4, characterized in that: The auxiliary crosslinking agent is one of TAC auxiliary crosslinking agent, TAIC auxiliary crosslinking agent, TMPTMA auxiliary crosslinking agent and HVA-2 auxiliary crosslinking agent.
6. A solar laminator composite AEM rubber sheet according to claim 5, characterized in that: The auxiliary cross-linking agent is TAIC auxiliary cross-linking agent.
7. A process for preparing a solar laminator composite AEM rubber sheet, comprising the following steps: S1, preparing AEM rubber compound and EPDM rubber compound respectively; S2, extruding or calendering the AEM rubber compound and the EPDM rubber compound to obtain semi-finished rubber sheets for working surfaces and semi-finished rubber sheets for non-working surfaces; S3, tighten the skeleton grid layer and cover it on the semi-finished rubber sheet on the working surface, cover the semi-finished rubber sheet on the non-working surface on the skeleton grid layer, and vulcanize them together to obtain the composite AEM rubber sheet.
8. A solar laminator composite AEM rubber sheet according to claim 7, characterized in that: In step S1, preparing the AEM rubber compound comprises the following steps: SA1. Mixing masterbatch: AEM-DP, antioxidant, internal release agent, anti-scorch agent and carbon black are put into an internal mixer. The internal mixer is mixed by step-by-step speed reduction, and the AEM masterbatch is obtained by rubber discharge. SA2, one-time refining: add AEM masterbatch into the open mixer for refining, and after refining evenly, the sheets are cooled; SA3, sulfur addition and mixing: add the AEM masterbatch, vulcanizing agent and cross-linking agent after the first refining into an open mixer or internal mixer for mixing, and discharge the glue to obtain the AEM mixed rubber; SA4, Second refining: Add the AEM compound to the open mixer for refining. After refining evenly, the sheet is cooled.
9. A solar laminator composite AEM rubber sheet according to claim 8, characterized in that: In the mixing process described in step SA1, the upper push pin pressure is set between 4.5-5.5KGF, the filling factor is between 0.7-0.75, and the step-by-step speed reduction refers to the speed of the internal mixer being increased from the initial 35 to 25 before discharge, and gradually decreased after each lifting of the upper push pin for cleaning, and the discharge temperature is controlled between 135-145°C.
10. A solar laminator composite AEM rubber sheet according to claim 8, characterized in that: In the mixing process described in step SA3, the upper push bolt pressure is set between 3.5-4.5KGF, the water temperature of the three zones is controlled within 20°C, the speed is 15-25R / MIN, the filling factor is between 0.5-0.65, the debonding temperature is controlled within 100°C, and the AEM mixed rubber is obtained by debonding.
Citation Information
Patent Citations
Laminate and application for same
CN108698383A
Tear-resistant ethylene propylene diene monomer molded board and preparation method thereof
CN115368681A
High-temperature-resistant anti-fatigue rubber plate for photovoltaic laminating machine and preparation method of high-temperature-resistant anti-fatigue rubber plate
CN117264327A
Composite high-temperature-resistant rubber plate for photovoltaic laminating machine
CN117264328A