Energy-saving reflective polyolefin composite modified asphalt waterproof coiled material as well as preparation method and application thereof
By using a combination of a reflective polyolefin elastomer layer and a high-performance modified asphalt layer in the waterproofing membrane, the problems of poor adhesion and aging resistance during exposed use are solved, and the solar reflectivity and hemispheric emissivity are improved. , achieving the energy-saving and thermal insulation effect of the building roof.
Patent Information
- Application Number
- CN202410683335.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-30
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2044-05-30
AI Technical Summary
Existing modified asphalt waterproofing membranes on the surface of mineral granules have problems such as poor adhesion, poor aging resistance, and low solar reflectivity when used in exposed locations.
A polyolefin composite modified asphalt waterproofing membrane composed of a reflective polyolefin elastomer layer, a barrier adhesive layer and a high-performance modified asphalt layer is used, using thermoplastic polyolefin elastomer, polymer compatibilizer, visible light reflective filler and Near-infrared light reflective filler, combined with ethylene-acrylate copolymer modified asphalt rubber, improves adhesion and reflective heat insulation properties.
It improves the adhesion and heat resistance of the waterproof membrane, enhances the solar reflectivity and hemispheric emissivity, extends the service life, and improves the energy-saving and thermal insulation effect of the building roof.
Smart Images

Figure BDA0004866421890000021 
Figure BDA0004866421890000071 
Figure BDA0004866421890000072
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of building waterproof materials, and specifically relates to an energy-saving reflective polyolefin composite modified asphalt waterproof coiled material and a preparation method thereof. Background Art
[0002] Modified asphalt waterproofing membranes are widely used in waterproofing projects of various buildings or structures such as roofs, basements, side walls, subways, tunnels, bridges, etc. due to their low manufacturing cost and high waterproof reliability, and currently occupy the main market of domestic waterproofing materials. However, since asphalt materials are not resistant to aging, modified asphalt waterproofing membranes are mainly used in various non-exposed scenes, and when used for roof waterproofing, they often require an additional cement mortar protective layer.
[0003] At present, only modified asphalt waterproofing membranes with mineral granules on the surface can be used for exposed waterproofing. However, the modified asphalt waterproofing membranes also have the following disadvantages: (1) The mineral granules have poor adhesion and are easy to fall off during transportation and use; (2) The modified asphalt waterproofing membranes have poor aging resistance. Although there is a certain degree of mineral granule protection on the surface, part of the asphalt is still in direct contact with the external environment. Under the influence of external water, oxygen and sunlight, it will gradually age, powder and harden, crack, and eventually lose its waterproof performance. The peeling of mineral granules will also accelerate this process. In addition, since mineral granules are often dark in color and have a low reflectivity of sunlight, heat is absorbed by the asphalt layer, which also continuously aggravates the aging of the modified asphalt waterproofing membrane and is not conducive to the thermal insulation of the roof. Summary of the invention
[0004] The technical problem actually solved by the present invention is to provide an energy-saving reflective polyolefin composite modified asphalt waterproofing membrane for exposed use, in view of the problems of poor adhesion, poor aging resistance and low sunlight reflectivity of the existing modified asphalt waterproofing membrane on the surface of mineral granular particles when exposed for use.
[0005] In order to achieve the above object, the technical solution adopted by the present invention is:
[0006] A polyolefin composite modified asphalt waterproofing coiled material comprises a reflective polyolefin elastomer layer, a barrier adhesive layer, a modified asphalt layer and an anti-sticking layer which are sequentially arranged from top to bottom, wherein the raw materials of the reflective polyolefin elastomer layer comprise a thermoplastic polyolefin elastomer, a polymer compatibilizer, a reflective filler and a thermal radiation filler, wherein the mass ratio of the thermoplastic polyolefin elastomer, the polymer compatibilizer, the reflective filler and the thermal radiation filler is 1:0.01-0.5:0.05-1:0.01-0.5, the reflective filler comprises a visible light reflective filler and a near infrared light reflective filler, and the mass ratio of the visible light reflective filler to the near infrared light reflective filler is 1:0.2-5.
[0007] The thermoplastic polyolefin elastomer is a polyolefin elastomer prepared by a reactor synthesis method.
[0008] According to some embodiments of the present invention, the median particle size D of the visible light reflecting filler is 50 The medium particle size D of the near-infrared light reflecting filler is 200-350nm. 50 It is 500-1100nm.
[0009] In some specific embodiments, the visible light reflecting filler is rutile nano-titanium dioxide; the near-infrared light reflecting filler is rutile nano-titanium dioxide.
[0010] In some specific embodiments, the polymer compatibilizer is one or a combination of maleic anhydride grafted polypropylene and methyl methacrylate grafted polypropylene.
[0011] In some specific embodiments, the particle size of the thermal radiation filler is 5 to 40 μm.
[0012] In some specific embodiments, the thermal radiation filler is ZrO 2 , Fe 2 O 3 Cr 2 O、SiO 2 、MnO 2 、NiO、Co 2 O 3 and CuO.
[0013] In some specific embodiments, the raw material formula of the reflective polyolefin elastomer layer includes, by weight:
[0014]
[0015] In some specific embodiments, the thermoplastic resin is polypropylene.
[0016] In some specific embodiments, the raw material of the reflective polyolefin elastomer layer further includes an auxiliary agent, and the auxiliary agent includes one or a combination of several of a light stabilizer and an antioxidant, and the amount of the auxiliary agent is 0.3 to 2 parts.
[0017] In some specific embodiments, the reflective polyolefin elastomer layer has a thickness of 0.05 to 0.4 mm.
[0018] In some specific embodiments, the barrier adhesive layer is a polyamide layer with a thickness of 0.02 to 0.12 mm.
[0019] According to some embodiments of the present invention, a high-strength and high-viscosity modifier is added to the modified asphalt layer, and the high-strength and high-viscosity modifier is an ethylene-acrylate copolymer. Further, the ethylene-acrylate copolymer is at least one of ethylene-methyl acrylate copolymer, ethylene-ethyl acrylate copolymer, and ethylene-butyl acrylate copolymer.
[0020] Adding high-strength and high-viscosity modifiers to the modified asphalt layer can help improve the cohesive strength of the modified asphalt layer, improve its heat resistance, and at the same time improve its excellent bonding performance with the base layer or roll material.
[0021] According to some embodiments of the present invention, the raw material of the modified asphalt layer contains asphalt, and the mass ratio of the asphalt to the high-strength and high-viscosity modifier is 1:0.03-0.2.
[0022] According to some embodiments of the present invention, the modified asphalt layer includes a first modified asphalt rubber layer, a polyester tire base layer and a second modified asphalt rubber layer stacked in sequence, and the high-strength and high-viscosity modifier is added to the first modified asphalt rubber layer and the second modified asphalt rubber layer, respectively, wherein the first modified asphalt rubber layer is arranged between the barrier bonding layer and the polyester tire base layer, and the anti-sticking layer is arranged on the second modified asphalt rubber layer.
[0023] In some specific embodiments, the raw materials of the first modified asphalt rubber layer and the second modified asphalt rubber layer independently include, by weight: 30-50 parts of petroleum asphalt, 8-15 parts of plasticizer, 5-15 parts of rubber modifier, 2-5 parts of high-strength and high-viscosity modifier, 2-5 parts of tackifying resin, 5-10 parts of tire rubber powder and 15-40 parts of filler.
[0024] In some specific embodiments, the petroleum asphalt is at least one of 70# and 90# petroleum asphalt.
[0025] In some specific embodiments, the plasticizer is at least one of paraffin oil or naphthenic oil.
[0026] In some specific embodiments, in the first modified asphalt rubber layer and the second modified asphalt rubber layer, the rubber modifier is at least one of SBS, SEBS, and SBR, and the filler is at least one of talc, heavy calcium carbonate, light calcium carbonate, montmorillonite, and kaolin.
[0027] In some specific embodiments, the tackifying resin is C 5 Petroleum resin, C 9 Petroleum resin, C 5 / C 9 At least one of copolymerized petroleum resin, rosin resin and hydrogenated rosin resin.
[0028] In some specific embodiments, the thickness of the first modified asphalt rubber layer and the second modified asphalt rubber layer are 1.0-1.5 mm respectively.
[0029] In some specific embodiments, the anti-sticking layer is a PE film or a release film.
[0030] In some specific embodiments, the thickness of the polyolefin composite modified asphalt waterproof membrane is 3.0 to 4.5 mm.
[0031] The second technical solution adopted by the present invention is: a method for preparing the above-mentioned polyolefin composite modified asphalt waterproof membrane, the preparation method comprising the following steps:
[0032] (1) Preparation of reflective polyolefin elastomer layer
[0033] Adding resin material into an extruder, mixing, extruding, and granulating to obtain a resin mixture, wherein the resin material includes a thermoplastic polyolefin elastomer and a polymer compatibilizer;
[0034] Mixing powders to obtain a powder mixture, wherein the powders include reflective fillers and thermal radiation fillers;
[0035] The resin mixture and the powder mixture are added into an extruder for extrusion, calendering and cooling to form a polyolefin elastomer sheet;
[0036] (2) Preparation of waterproof membrane
[0037] On the modified asphalt coiled material production line, the modified asphalt rubber is coated on the upper and lower surfaces of the base, and then the polyolefin elastomer sheet is compounded on the upper surface and the anti-sticking layer is compounded on the lower surface to obtain the polyolefin composite modified asphalt waterproof coiled material.
[0038] The third technical solution adopted by the present invention: application of the above-mentioned polyolefin composite modified asphalt waterproofing membrane in the field of building or structure waterproofing, wherein the polyolefin composite modified asphalt waterproofing membrane is used for exposed waterproofing.
[0039] Due to the application of the above technical solution, the present invention has the following advantages compared with the prior art:
[0040] The waterproofing roll of the present invention adopts a specific reflective polyolefin elastomer layer as a mask-modified asphalt waterproofing roll, which not only has good adhesion to the asphalt rubber layer, but also has a large solar reflectivity and a high hemispherical emissivity, which is beneficial to energy saving and heat preservation of building roofs. DETAILED DESCRIPTION
[0041] The existing exposed modified asphalt waterproofing membrane has the problems of poor adhesion, poor aging resistance and low solar reflectivity. The present invention prepares a polyolefin composite modified asphalt waterproofing membrane by combining a specific reflective polyolefin elastomer layer with a barrier adhesive layer and a high-performance modified asphalt layer. On the one hand, an energy-saving reflective polyolefin elastomer layer is used as a mask of the waterproofing membrane, which has good adhesion to the asphalt rubber layer and high solar reflectivity, and can overcome the problems of poor adhesion and low solar reflectivity of conventional mineral particle surface modified asphalt waterproofing membranes, which is beneficial to energy saving and heat preservation of building roofs; on the other hand, a visible light reflecting filler, a near-infrared light reflecting filler and a thermal radiation filler are compounded and prepared. The reflective polyolefin elastomer layer, the combination of visible light reflective filler and near-infrared light reflective filler can ensure that the reflective polyolefin elastomer layer reflects most of the visible light and near-infrared light in the sunlight. At the same time, the thermal radiation filler can radiate the remaining absorbed part of the sunlight heat, thereby further improving the thermal insulation effect of the reflective polyolefin elastomer layer; thirdly, a polymer compatibilizer is used to improve the compatibility of the resin and filler in the reflective polyolefin elastomer layer, and to enhance the bonding force between the two, thereby effectively increasing not only the amount of filler added, but also the density of the reflective polyolefin elastomer layer, thereby further improving the energy-saving reflective effect of the reflective polyolefin elastomer layer.
[0042] A further concept of the present invention is to optimize the formula of the modified asphalt rubber compound and adopt ethylene-acrylate copolymers such as ethylene-methyl acrylate copolymer, ethylene-ethyl acrylate copolymer, and ethylene-butyl acrylate copolymer to modify the asphalt. On the first hand, since the ethylene-acrylate copolymers contain both non-polar and polar segments, the bonding force between the modified asphalt and the filler in the modified asphalt rubber compound can be effectively improved, thereby improving the density, cohesive strength and heat resistance of the modified asphalt rubber compound; on the second hand, since the polar segments in the ethylene-acrylate copolymers have good adhesion to the base layers such as metal and concrete, the coiled material can not only be constructed by self-adhesion or wet laying, but also has excellent adhesion to the base layer.
[0043] The technical solution of the present invention is described in detail below in conjunction with specific embodiments so that those skilled in the art can better understand and implement the technical solution of the present invention, but the present invention is not limited to the scope of the examples.
[0044] Example 1
[0045] The energy-saving reflective polyolefin composite modified asphalt waterproof membrane provided in this embodiment has a thickness of 4 mm and includes a reflective polyolefin elastomer layer, a barrier adhesive layer, a first modified asphalt rubber layer, a polyester tire base layer, a second modified asphalt rubber layer and an anti-sticking layer stacked in sequence from top to bottom, wherein the raw material formula of the reflective polyolefin elastomer layer is as shown in Table 1.
[0046] The thickness of the reflective polyolefin elastomer layer is 0.2 mm, wherein the polyolefin elastomer is a reactor-polymerized thermoplastic polyolefin Hifax CA10A purchased from Basel Company;
[0047] The thermoplastic resin is polypropylene;
[0048] The polymer compatibilizer is maleic anhydride grafted polypropylene;
[0049] The visible light reflecting filler is rutile titanium dioxide with a medium particle size of 260nm;
[0050] The near-infrared light reflecting filler is rutile titanium dioxide with a medium particle size of 700nm;
[0051] The thermal radiation filler is SiO 2 .
[0052] The light stabilizer is selected from hindered amine light stabilizers;
[0053] The antioxidant is 2,6-bis(1,1-dimethylethyl)-4-methylphenol.
[0054] The barrier adhesive layer is a polyamide layer with a thickness of 0.06 mm.
[0055] The thickness of the first high-performance modified asphalt rubber layer and the second high-performance modified asphalt rubber layer are 1.4 mm respectively, and the raw material formulas are as follows:
[0056] Petroleum asphalt (70#) 40 parts, plasticizer (paraffin oil) 10 parts, thermoplastic elastomer (SBS411) 4 parts, styrene-butadiene rubber SBR 3 parts, high strength and high viscosity modifier (ethylene-ethyl acrylate copolymer) 3 parts, tackifying resin (C 5 Petroleum resin) 3 parts, 60 mesh tire rubber powder 10 parts and filler (talc) 27 parts.
[0057] The preparation method of the energy-saving reflective polyolefin composite modified asphalt waterproof membrane of this embodiment is as follows:
[0058] (1) Preparation of reflective polyolefin elastomer layer
[0059] Adding polyolefin elastomer, thermoplastic resin and polymer compatibilizer into a high-speed mixer and mixing them evenly at room temperature, and then adding them into the main feeding port of a twin-screw extruder for blending and granulation to obtain a resin mixture;
[0060] Add visible light reflective filler, near infrared light reflective filler, thermal radiation filler, light stabilizer and antioxidant into a high-speed mixer and mix them evenly at room temperature to obtain a powder mixture. The processing temperature of the extruder is 180-190°C, the screw speed is 80rpm, the traction speed is 12m / min, and the particle size of the granulated material is controlled at about 6mm;
[0061] The resin mixture is added to the main feeding port of the twin-screw extruder, and the powder is added to the side feeding port. The sheet is melted and extruded through the extruder, and then calendered and cooled and formed by a three-roll system, and then cooled and rolled into a sheet. The processing temperature of the extruder is 180℃~190℃, the screw speed is 15rpm, the traction speed is 0.9m / min, and the tension is controlled at 10N±5N.
[0062] (2) Preparation of high-performance modified asphalt
[0063] Add petroleum asphalt and plasticizer into the reactor, stir and dehydrate at 135-140°C for 30 minutes, then add thermoplastic elastomer, styrene-butadiene rubber, high-strength and high-viscosity modifier and tire rubber powder, heat to 185°C, shear mix for 3 hours, then add petroleum resin, shear mix for 0.5 hours, finally add filler, stir and mix for 1 hour to obtain high-performance modified asphalt rubber.
[0064] (3) Preparation of waterproof membrane
[0065] On the modified asphalt roll production line, the high-performance modified asphalt rubber prepared in step (2) is added to the dipping tank, the temperature is controlled at 170-180°C, and then the upper and lower surfaces of the polyester base are coated with the material to form the sheet prepared in step (1) on the upper surface and the PE isolation film on the lower surface to obtain an energy-saving reflective polyolefin composite modified asphalt waterproof roll.
[0066] Example 2
[0067] The energy-saving reflective polyolefin composite modified asphalt waterproofing membrane provided in this embodiment is basically the same as that in embodiment 1, except that: the raw material formula of the polyolefin elastomer layer is shown in Table 1, and the polyolefin elastomer is a reactor-polymerized thermoplastic polyolefin Hifax CA60A purchased from Basel Company;
[0068] Example 3
[0069] The energy-saving reflective polyolefin composite modified asphalt waterproof membrane provided in this embodiment is basically the same as that in Embodiment 1, except that: the raw material formula of the polyolefin elastomer layer is shown in Table 1, and the polyolefin elastomer is POE6202 purchased from Exxon Chemical.
[0070] Example 4
[0071] The energy-saving reflective polyolefin composite modified asphalt waterproofing membrane provided in this embodiment is basically the same as that in embodiment 1, except that the raw material formula of the polyolefin elastomer layer is shown in Table 1. 50 The near-infrared light reflective filler is rutile titanium dioxide with a medium particle size of 1000nm, and the thermal radiation filler is ZrO 2 .
[0072] Example 5
[0073] The energy-saving reflective polyolefin composite modified asphalt waterproof membrane provided in this embodiment is basically the same as that in Embodiment 1, except that:
[0074] The raw material formula of high-performance modified asphalt layer is: 50 parts of petroleum asphalt (90#), 14 parts of plasticizer (paraffin oil), 4 parts of thermoplastic elastomer (SBS411), 3 parts of styrene-butadiene rubber SBR, 4 parts of high-strength and high-viscosity modifier (ethylene-butyl acrylate copolymer), 4 parts of tackifying resin (C 9 Petroleum resin) 5 parts, 60 mesh tire rubber powder 5 parts and filler (talc) 10 parts.
[0075] Example 6
[0076] The energy-saving reflective polyolefin composite modified asphalt waterproof membrane provided in this embodiment is basically the same as that in Embodiment 1, except that no thermoplastic resin is added, that is, the amount of polypropylene used is 0.
[0077] Comparative Example 1
[0078] The energy-saving reflective polyolefin composite modified asphalt waterproofing membrane provided in this comparative example is basically the same as Example 1, except that: the raw material formula of the polyolefin elastomer layer is shown in Table 1. Among them, the addition amount of the visible light reflective filler is 10 parts, and the addition amount of the near infrared light reflective filler is 0.
[0079] Comparative Example 2
[0080] The energy-saving reflective polyolefin composite modified asphalt waterproofing membrane provided in this comparative example is basically the same as Example 1, except that the raw material formula of the polyolefin elastomer layer is shown in Table 1. Among them, the addition amount of the visible light reflective filler is 0 parts, and the addition amount of the near infrared light reflective filler is 10 parts.
[0081] Comparative Example 3
[0082] The energy-saving reflective polyolefin composite modified asphalt waterproofing membrane provided in this comparative example is basically the same as Example 1, except that the raw material formula of the polyolefin elastomer layer is shown in Table 1. Among them, the addition amount of the visible light reflective filler and the near infrared light reflective filler is 7.5 parts respectively, and the addition amount of the heat radiation filler is 0.
[0083] Comparative Example 4
[0084] The energy-saving reflective polyolefin composite modified asphalt waterproof membrane provided in this comparative example is basically the same as Example 1, except that:
[0085] The raw material formula of high-performance modified asphalt layer is: 40 parts of petroleum asphalt, 10 parts of plasticizer (paraffin oil), 4 parts of thermoplastic elastomer (SBS411), 3 parts of styrene-butadiene rubber SBR, 3 parts of tackifying resin (C 5 Petroleum resin) 3 parts, 60 mesh tire rubber powder 10 parts and filler (talc) 30 parts.
[0086] Comparative Example 5
[0087] The energy-saving reflective polyolefin composite modified asphalt waterproofing membrane provided in this comparative example is basically the same as that in Example 1, except that: the raw material formula of the polyolefin elastomer layer is shown in Table 1, and no polymer compatibilizer is added.
[0088] Table 1 Raw material formula of polyolefin elastomer layer of Examples 1 to 6 and Comparative Examples 1 to 5 (in parts by weight)
[0089]
[0090] For the waterproof membranes of Examples 1 to 6 and Comparative Examples 1 to 5, the solar reflectivity and hemispherical emissivity were tested according to Appendix B and C of JG / T 235-2014 "Architectural Reflective Insulation Coatings", the heat resistance was tested according to GB 18242-2008 "Elastomer SBS Modified Asphalt Waterproof Membrane", and the peel strength between the membranes and the peel strength between the membranes and the aluminum plate were tested according to GB T 23260-2009 "Waterproof Membrane with Self-Adhesive Layer". The results are shown in Table 2.
[0091] Table 2 Performance test results of waterproof membranes of Examples 1 to 6 and Comparative Examples 1 to 5
[0092]
[0093]
[0094] The results show that in the preparation of the polyolefin elastomer layer in Examples 1-6, maleic anhydride grafted polypropylene is used as a polymer compatibilizer, rutile titanium dioxide with a medium particle size of 260 nm is used as a visible light reflective filler, rutile titanium dioxide with a medium particle size of 700 nm is used as a near-infrared light reflective filler, and SiO 2 As heat radiation fillers, the solar reflectivity of the roll is above 74%, and the hemispherical emissivity is above 85%, indicating that the energy-saving reflective polyolefin composite modified asphalt waterproof roll prepared by the present invention has good reflective heat insulation performance.
[0095] Compared with Example 1, in Comparative Examples 1 and 2, only near-infrared light reflecting filler or visible light reflecting filler was added separately when preparing the polyolefin elastomer layer. Since nano-titanium dioxide of different particle sizes has inconsistent reflection efficiency for sunlight of different wavelengths, the sunlight reflectivity drops to below 70%, and the hemispherical emissivity also drops to 78% and 80%, respectively.
[0096] Compared with Example 1, in Comparative Example 3, when preparing the polyolefin elastomer layer, the contents of near-infrared light reflecting filler and visible light reflecting filler were respectively increased, and no thermal radiation filler was added. Due to the increase in the content of light reflecting filler, the solar reflectivity was further increased to 82%. However, since no thermal radiation filler was added to the formula, the heat absorbed in the system could not be effectively dissipated in the form of thermal radiation, and the hemispherical emissivity was reduced to 72%, affecting the reflective heat insulation effect of the coil.
[0097] Compared with Example 1, in Comparative Example 5, no polymer compatibilizer is added when preparing the polyolefin elastomer layer. Since the amount of light-emitting filler and thermal radiation filler added is large, on the one hand, the filler cannot be effectively and evenly dispersed in the resin system, and on the other hand, it affects the density of the polyolefin elastomer layer, resulting in a decrease in solar reflectivity and hemispherical emissivity.
[0098] In the preparation of high-performance modified asphalt materials in Examples 1 to 6 and Comparative Examples 1 to 3, ethylene-acrylate copolymers were added as high-strength and high-viscosity modifiers. The coils have good cohesive strength and heat resistance. The peel strength between the coils is above 2.40 N / mm, and the heat resistance can pass 105°C. At the same time, since the ethylene-acrylate copolymer resin contains polar segments, the bonding performance between the coils and the base layer can also be effectively improved.
[0099] Compared with Example 1, in Comparative Example 4, when preparing the modified asphalt layer, no ethylene-acrylate copolymer was added as a high-strength and high-viscosity modifier, and the peel strength between the coils decreased to 1.75 N / mm, and the heat resistance could not pass the 105-degree test, indicating that the cohesive strength of the modified asphalt was significantly reduced. In addition, the peel strength between the coil and the aluminum plate also decreased to 1.96 N / mm, indicating that the bonding performance of the modified asphalt and the base layer was also significantly reduced.
[0100] The above embodiments are only for illustrating the technical concept and features of the present invention, and their purpose is to enable people familiar with the technology to understand the content of the present invention and implement it accordingly, and they cannot be used to limit the protection scope of the present invention. Any equivalent changes or modifications made according to the spirit of the present invention should be included in the protection scope of the present invention.
[0101] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
Claims
1. A polyolefin composite modified asphalt waterproofing membrane, characterized in that: The invention comprises a reflective polyolefin elastomer layer, a barrier adhesive layer, a modified asphalt layer and an anti-sticking layer which are arranged in sequence from top to bottom. The raw materials of the reflective polyolefin elastomer layer comprise a thermoplastic polyolefin elastomer, a polymer compatibilizer, a reflective filler and a thermal radiation filler, wherein the mass ratio of the thermoplastic polyolefin elastomer, the polymer compatibilizer, the reflective filler and the thermal radiation filler is 1:0.01-0.5:0.05-1:0.01-0.5, the reflective filler comprises a visible light reflective filler and a near infrared light reflective filler, and the mass ratio of the visible light reflective filler to the near infrared light reflective filler is 1:0.2-5.
2. The polyolefin composite modified asphalt waterproofing membrane according to claim 1, characterized in that: The median particle size D of the visible light reflecting filler 50 The near-infrared light reflecting filler has a medium particle size D 50 It is 500-1100nm.
3. The polyolefin composite modified asphalt waterproofing membrane according to claim 2, characterized in that: The visible light reflecting filler is rutile nano-titanium dioxide; and / or the near-infrared light reflecting filler is rutile nano-titanium dioxide.
4. The polyolefin composite modified asphalt waterproofing membrane according to claim 1, characterized in that: The particle size of the thermal radiation filler is 5 to 40 um, and the thermal radiation filler is at least one of ZrO2, Fe2O3, Cr2O, SiO2, MnO2, NiO, Co2O3 and CuO.
5. The polyolefin composite modified asphalt waterproofing membrane according to claim 1, characterized in that: The polymer compatibilizer is one or a combination of maleic anhydride grafted polypropylene and methyl methacrylate grafted polypropylene; and / or, The raw material formula of the reflective polyolefin elastomer layer includes, by weight:
6. The polyolefin composite modified asphalt waterproofing membrane according to claim 5, characterized in that: The thermoplastic resin is polypropylene.
7. The polyolefin composite modified asphalt waterproofing membrane according to claim 6, characterized in that: The raw material formula of the reflective polyolefin elastomer layer also includes an auxiliary agent, and the auxiliary agent includes one or a combination of several of a light stabilizer and an antioxidant, and the dosage of the auxiliary agent is 0.3 to 2 parts.
8. The polyolefin composite modified asphalt waterproofing membrane according to any one of claims 1 to 7, characterized in that: A high-strength and high-viscosity modifier is added to the modified asphalt layer.
9. The polyolefin composite modified asphalt waterproofing membrane according to claim 8, characterized in that: The high-strength and high-viscosity modifier is an ethylene-acrylate copolymer; and / or the raw material of the modified asphalt layer contains asphalt, and the mass ratio of the asphalt to the high-strength and high-viscosity modifier is 1:0.03-0.
2.
10. The polyolefin composite modified asphalt waterproofing membrane according to claim 9, characterized in that: The ethylene-acrylic acid ester copolymer is at least one of ethylene-methacrylate copolymer, ethylene-ethylacrylate copolymer and ethylene-butylacrylate copolymer.
11. The polyolefin composite modified asphalt waterproofing membrane according to claim 10, characterized in that: The modified asphalt layer includes a first modified asphalt rubber layer, a polyester tread base layer and a second modified asphalt rubber layer which are stacked in sequence, the high-strength and high-viscosity modifier being added to the first modified asphalt rubber layer and the second modified asphalt rubber layer respectively, wherein the first modified asphalt rubber layer is arranged between the barrier adhesive layer and the polyester tread base layer, and the anti-sticking layer is arranged on the second modified asphalt rubber layer.
12. The polyolefin composite modified asphalt waterproofing membrane according to claim 11, characterized in that: In parts by weight, the raw materials of the first modified asphalt rubber layer and the second modified asphalt rubber layer independently include: 30-50 parts of petroleum asphalt, 8-15 parts of plasticizer, 5-15 parts of rubber modifier, 2-5 parts of high-strength and high-viscosity modifier, 2-5 parts of tackifying resin, 5-10 parts of tire rubber powder and 15-40 parts of filler.
13. The polyolefin composite modified asphalt waterproofing membrane according to claim 12, characterized in that: The petroleum asphalt is at least one of 70# and 90# petroleum asphalt; and / or, The plasticizer is at least one of paraffin oil or naphthenic oil; and / or, In the first modified asphalt rubber layer and the second modified asphalt rubber layer, the rubber modifier is at least one of SBS, SEBS and SBR; and / or, The tackifying resin is at least one of C5 petroleum resin, C9 petroleum resin, C5 / C9 copolymerized petroleum resin, rosin resin, and hydrogenated rosin resin; and / or, In the first modified asphalt rubber layer and the second modified asphalt rubber layer, the filler is at least one of talc, heavy calcium carbonate, light calcium carbonate, montmorillonite and kaolin; and / or, The thickness of the first modified asphalt rubber layer and the second modified asphalt rubber layer are 1.0-1.5 mm respectively.
14. The polyolefin composite modified asphalt waterproofing membrane according to claim 1, characterized in that: The thickness of the reflective polyolefin elastomer layer is 0.05 to 0.4 mm; and / or, The barrier adhesive layer is a polyamide layer; and / or, The thickness of the barrier adhesive layer is 0.02 to 0.12 mm; and / or, The anti-adhesive layer is a PE film or a release film; and / or, The thickness of the polyolefin composite modified asphalt waterproofing membrane is 3.0-4.5 mm.
15. A method for preparing the polyolefin composite modified asphalt waterproofing membrane according to any one of claims 1 to 14, characterized in that: The preparation method comprises the following steps: (1) Preparation of reflective polyolefin elastomer layer Adding a resin material into an extruder, mixing, extruding, and granulating to obtain a resin mixture, wherein the resin material comprises a thermoplastic polyolefin elastomer and a polymer compatibilizer; Mixing powders to obtain a powder mixture, wherein the powders include reflective fillers and thermal radiation fillers; The resin mixture and the powder mixture are added into an extruder for extrusion, calendering and cooling to form a polyolefin elastomer sheet; (2) Preparation of waterproof membrane On the modified asphalt coiled material production line, the modified asphalt rubber is coated on the upper and lower surfaces of the base, and then the polyolefin elastomer sheet is compounded on the upper surface and the anti-sticking layer is compounded on the lower surface to obtain the polyolefin composite modified asphalt waterproof coiled material.
16. Use of the polyolefin composite modified asphalt waterproofing membrane according to any one of claims 1 to 15 in the field of building or structure waterproofing, wherein the polyolefin composite modified asphalt waterproofing membrane is used for exposed waterproofing.
Citation Information
Patent Citations
Infrared reflective coating composition
CN102464943A
Environment-friendly flame-resistant high polymer SBS modified asphalt water-emulsion-type waterproof coating
CN106519979A
Self-adhered asphalt and preparation method thereof and self-adhered asphalt waterproof roll
CN107118576A
NIR-reflective multi-layer material sheet
CN112385050A
Polymer composite coiled material with heat management function and preparation method thereof
CN115522689A
Cited By
Waterproofing structure using polyester fiber, its composition, and waterproofing method for coating
KR103028903B1