Preparation process of wormwood antibacterial insole upper pulling cloth
Through the preparation process of mugwort antibacterial midsole cuffs, the toxicity and environmental protection problems of glue adhesives in traditional shoe production are solved. Materials such as mugwort and modified nano-TiO2 are used to form environmentally friendly and antibacterial midsole cuffs. , achieving the dual benefits of environmental protection and human health.
Patent Information
- Application Number
- CN202410973097.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-10-15
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The glue and adhesive used in the traditional shoe manufacturing process are toxic and evaporate to produce toxic gases, posing a threat to human health and the environment. The process is complex and not environmentally friendly.
Using the preparation process of mugwort antibacterial midsole fabric, the carded polypropylene fiber and mugwort Chinese herbal medicine are fully mixed, and then processed through laying, acupuncture, sizing, PU impregnation, alkali reduction fiber opening, dyeing and hot pressing. Molding and other steps form an environmentally friendly midsole base layer, which is combined with mugwort powder material and formed into an integrated midsole cuff through hot pressing.
Achieving environmentally friendly and pollution-free shoe production. Mugwort has natural antibacterial, moisture-proof, cold-proof and other effects. Modified nano-TiO2 and guanidine antibacterial agents improve the antibacterial durability and stability of the material, ensuring human health and environmental safety. .
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The invention relates to the field of preparation technology of midsole pull-up cloth for shoes, and in particular to a preparation technology of wormwood antibacterial midsole pull-up cloth. Background Art
[0002] The shoes currently on the market are generally composed of three parts: outsole, midsole, and upper. The manufacturing process is generally to make the outsole, midsole, and upper separately first, and then use glue adhesive to glue the outsole, midsole, and upper together to form a finished shoe. The midsole and upper can also be connected by sewing. The traditional shoemaking process is relatively complicated and requires the use of glue adhesive. The glue adhesive is generally toxic and produces toxic gases through volatilization, which threatens human health and easily pollutes the environment, which is not environmentally friendly. Summary of the invention
[0003] The purpose of the present invention is to provide a preparation process of an antibacterial midsole zip-up cloth made of mugwort to solve the problems raised in the above-mentioned background technology. The midsole zip-up cloth has the advantages of enhancing medicinal properties, relaxing muscles and tendons, eliminating fatigue, removing odor and moisture from mugwort, and preventing cold and resisting foot diseases.
[0004] To achieve the above object, the present invention provides the following technical solution: a preparation process of an antibacterial midsole pull-up cloth made of wormwood, comprising the following steps: S1. Preparation of midsole antibacterial base layer: S11, web laying: After the combed polypropylene fibers and the Chinese herbal medicine of mugwort are fully mixed, the combed polypropylene fibers are clamped by the upper and lower carbon curtains of the web laying machine, and the web is cross-laid to achieve an ideal laying effect; S12, needle punching: the polypropylene fibers output from the web are conveyed by the web forming machine into the needle punching machine for processing, and the composite base fabric is obtained by entanglement of the non-woven needle punched fibers; S13, sizing: performing basic impregnation antibacterial treatment on the composite base fabric in an aqueous solution of PVA; S14, PU impregnation: the composite base fabric is subjected to PU impregnation treatment in a mixture of PU resin and DMF, the composite base fabric is impregnated at a speed of 5-15 m / min, the pressure between the rolling tubes through which the impregnated fabric passes is 0.001-1 MPa, the impregnated fabric is coagulated in a DMF aqueous solution through a coagulation bath, and then washed and dried, the formula ratio of each component per hundred parts by weight of the mixture of PU resin and DMF is: 3-20 parts of PU resin, 80-97 parts of DMF; the weight ratio of each component per hundred parts by weight of the DMF aqueous solution is: 10-20 parts of DMF, 80-90 parts of water, 6-9 parts of antibacterial agent, 4-6 parts of NaHCO3, and 10-20 parts of guanidine antibacterial agent are added to the obtained mixture of PU resin and DMF, The antibacterial agent is prepared by the following method: 1-3g chitosan is dispersed in 100-300ml isopropanol and subjected to ultrasonic treatment, the ultrasonic power is 50-70W, and the ultrasonic time is 20-50min; 5-9g cross-linking agent is added, stirred evenly, and reacted at 50-80℃ for 2-5h; after the reaction is completed, the mixture is washed and dried to obtain chitosan quaternary ammonium salt; Dissolve 0.8-1.5g of the chitosan quaternary ammonium salt, 3-5g of the grafting monomer, 0.005-0.02g of the inhibitor, 0.25-0.7g of the initiator and 0.01-0.03g of nano-TiO2 in 10-30ml of deionized water, stir evenly, and heat at 110-150°C for 5-20min; after the reaction is completed, wash and dry; The nano-TiO2 is a modified nano-TiO2, which is prepared by the following method: 0.3-0.5g of nano-TiO2 and 0.01-0.03g of hexadecyl glycidyl dimethyl ammonium chloride are placed in 80-100ml of deionized water for ultrasonic dispersion, with an ultrasonic power of 50-70W and an ultrasonic time of 10-30min, and then centrifuged and dried to obtain the modified nano-TiO2; The grafting monomer is a mixture of citric acid and N-hydroxyethyl acrylamide in a mass ratio of (1-3): (1-3); The cross-linking agent is one or two of hexadecyl epoxypropyl dimethyl ammonium chloride and 2,3-epoxypropyl trimethyl ammonium chloride; S15, alkali reduction fiber opening, the fiber opening temperature is 100±5℃, and the temperature is kept for 30-45 minutes; the composite matrix obtained in step S14 is soaked in a sodium hydroxide solution, the sodium hydroxide concentration is maintained at 6-8g / L, the soaking time is 1 hour, and the temperature is 90-105℃; S16, dyeing: the seam ends of the grey cloth are pre-treated, dyed, reduced and cleaned, washed with hot water, washed with water, dehydrated and shaped. During the initial dyeing, the initial dyeing temperature of the disperse dye is controlled at 50-60°C, and gradually heated to 130°C after 1 hour, kept warm for 1-2 hours, and then fully washed with water. When dyeing dark colors, reduction cleaning is performed; S17, shaping and drying: after reduction cleaning, adding polypropylene fiber to perform drying and shaping again, during shaping, the base fabric temperature is controlled to be 100-170°C, and the speed is adjusted to 5-30 m / min to form a midsole base layer; S2. Mugwort treatment: S21, selecting and washing: removing weeds from the purchased wormwood and then washing it to remove dirt and dust from the grass; S22, powdering: the washed wormwood is withered, sterilized, sun-dried, combed, hammered, and then ground into wormwood powder particles; S23, grinding: using plant grinding equipment, the dry mugwort leaves are made into 150 mesh mugwort powder, and the dust and black matter in the mugwort powder are filtered out by negative pressure suction equipment to obtain light yellow pure mugwort powder; S24, stirring: using a dry-wet separation dual mixing mixer to stir, prepare 5-20 parts of raw materials of wormwood powder, 30-60 parts of waterborne polyurethane, 5-10 parts of filler, and 2-7 parts of defoamer, place the above raw materials in the upper dry material stirring system for initial stirring, put them into the lower stirring system after the initial stirring, add 20-40 parts of solvent and 2-6 parts of film-forming aid for wet stirring, so that the coating is fully integrated, the filler is titanium dioxide or talcum powder; the solvent is deionized water; S25, pressing and drying: squeezing water out of the stirred wormwood powder particles, and then placing them in the sun to allow the wormwood powder to fully absorb sunlight, thereby obtaining the wormwood Chinese herbal medicine; S26, proportioning and foaming: using the Osole material as a carrier, adding mugwort Chinese herbal medicine, and preparing a plant foaming sponge material; S3, hot pressing: stirring the plant material obtained in step S26, and then hot pressing it with the midsole base layer through a hot press to form an integrated midsole zipper cloth; S4. Packaging: After hot pressing, the midsole pull cloth is rolled, needle tested, packaged, cut and packaged.
[0005] Preferably, the raw material of the polypropylene fiber is recycled polypropylene plastic that is processed by physical crushing.
[0006] Preferably, in the step S12, the needle punching pressure parameter of the nonwoven is 100-200 bar, the speed of the web forming machine is controlled at 60-90 m / min, the needle punching frequency is 500-700 punctures / min, and the needle density of the needle board is 5500-6500 needles / m.
[0007] Preferably, in step S13, the temperature of the PVA aqueous solution is controlled to be 60-90°C, the composite base fabric impregnation speed is 10-20 m / min, the pressure between the rolling tubes through which the impregnated fabric passes is 0.001-1 MPa, and the drying temperature is controlled at 100-190°C.
[0008] Preferably, in step S22, 80% of the moisture is removed during sun drying, hammering is artificially beating into fibers, and grinding is screened through a 20-40 mesh molecular sieve.
[0009] Preferably, the hot pressing temperature of the hot press in step S3 is 125-145°C.
[0010] Compared with the prior art, the present invention has the following beneficial effects: 1. The raw materials of wormwood are all from wild wormwood leaves, which are natural and healthy. Wormwood has the functions of sterilization, warming the meridians, removing dampness, dispelling cold, stopping bleeding, anti-inflammatory, relieving asthma, relieving cough, stabilizing pregnancy, and anti-allergy. It is a natural plant pigment, environmentally friendly and pollution-free, and has health benefits for the human body. 2. Modified nano-TiO2 is introduced into reactive chitosan quaternary ammonium salt, which effectively improves the antibacterial and wear resistance and imparts anti-ultraviolet properties. Hexadecyl glycidyl dimethyl ammonium chloride is used to modify nano-TiO2. On the one hand, it improves the dispersibility of nano-TiO2 that is easy to agglomerate, while modifying nano-TiO2 to impart the antibacterial properties of quaternary ammonium salt and obtain antibacterial durability; on the other hand, it can improve the stability of the reaction system for preparing reactive chitosan quaternary ammonium salt / nano-TiO2 composite materials; 3. The activity of the guanidine group in guanidine antimicrobial agents makes polymers containing multiple (—NH) amine groups positively charged, so they are easily adsorbed by various bacteria, viruses and other microorganisms that are usually negatively charged. The structure containing amine groups also improves the effective activity of guanidine groups. The interaction between guanidine groups and amine groups in guanidine antimicrobial agents greatly improves their bactericidal and antifungal capabilities. DETAILED DESCRIPTION
[0011] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0012] In the embodiment of the present invention, Example
[0013] A preparation process of an antibacterial midsole pull-up cloth made of wormwood comprises the following steps: S1. Preparation of midsole antibacterial base layer: S11, web laying: After the combed polypropylene fibers and the Chinese herbal medicine of mugwort are fully mixed, the combed polypropylene fibers are clamped by the upper and lower carbon curtains of the web laying machine, and the web is cross-laid by synchronous movement to achieve an ideal laying effect; S12, needle punching: the polypropylene fibers output from the web are conveyed by the web forming machine into the needle punching machine for processing, and the composite base fabric is obtained by entanglement of the non-woven needle punched fibers; S13, sizing: performing basic impregnation treatment on the composite base fabric in an aqueous solution of PVA; S14, PU impregnation: the composite base fabric is subjected to PU impregnation treatment in a mixture of PU resin and DMF, the composite base fabric impregnation vehicle speed is controlled to be 5-15 m / min, the pressure between the rolling tubes through which the impregnated fabric passes is 0.001-1 MPa, the impregnated fabric is coagulated in a DMF aqueous solution through a coagulation bath, and then washed and dried, the formula ratio of each component per hundred parts by weight of the mixture of PU resin and DMF is: 3 parts of PU resin, 80 parts of DMF; the weight ratio of each component per hundred parts by weight of the DMF aqueous solution is: 10 parts of DMF, 80 parts of water, 6 parts of antibacterial agent, 4 parts of NaHCO3, and 10 parts of guanidine antibacterial agent are added to the obtained mixture of PU resin and DMF, The antibacterial agent is prepared by the following method: 1-3g chitosan is dispersed in 100-300ml isopropanol and subjected to ultrasonic treatment, the ultrasonic power is 50-70W, and the ultrasonic time is 20-50min; 5-9g cross-linking agent is added, stirred evenly, and reacted at 50-80℃ for 2-5h; after the reaction is completed, the mixture is washed and dried to obtain chitosan quaternary ammonium salt; Dissolve 0.8g of the chitosan quaternary ammonium salt, 3g of grafting monomer, 0.005g of inhibitor, 0.25g of initiator and 0.01g of nano-TiO2 in 10-30ml of deionized water, stir evenly, and heat at 110-150°C for 5-20min; after the reaction, wash and dry; The nano-TiO2 is a modified nano-TiO2, which is prepared by the following method: 0.3g of nano-TiO2 and 0.01g of hexadecyl glycidyl dimethyl ammonium chloride are placed in 80-100ml of deionized water for ultrasonic dispersion, with an ultrasonic power of 50-70W and an ultrasonic time of 10-30min, and then centrifuged and dried to obtain the modified nano-TiO2; The grafting monomer is a mixture of citric acid and N-hydroxyethyl acrylamide in a mass ratio of (1-3): (1-3); The cross-linking agent is one or two of hexadecyl epoxypropyl dimethyl ammonium chloride and 2,3-epoxypropyl trimethyl ammonium chloride; S15, alkali reduction fiber opening, the fiber opening temperature is 100±5℃, and the temperature is kept for 30-45 minutes; the composite matrix obtained in step S14 is soaked in a sodium hydroxide solution, the sodium hydroxide concentration is maintained at 6-8g / L, the soaking time is 1 hour, and the temperature is 90-105℃; S16, dyeing: the seam ends of the grey cloth are pre-treated, dyed, reduced and cleaned, washed with hot water, washed with water, dehydrated and shaped. During the initial dyeing, the initial dyeing temperature of the disperse dye is controlled at 50-60°C, and gradually heated to 130°C after 1 hour, kept warm for 1-2 hours, and then fully washed with water. When dyeing dark colors, reduction cleaning is performed; S17, shaping and drying: after reduction cleaning, adding polypropylene fiber to perform drying and shaping again, during shaping, the base fabric temperature is controlled to be 100-170°C, and the speed is adjusted to 5-30 m / min to form a midsole base layer; S2. Mugwort treatment: S21, selecting and washing: removing weeds from the purchased wormwood and then washing it to remove dirt and dust from the grass; S22, powdering: the washed wormwood is withered, sterilized, sun-dried, combed, hammered, and then ground into wormwood powder particles; S23, grinding: using plant grinding equipment, the dry mugwort leaves are made into 150 mesh mugwort powder, and the dust and black matter in the mugwort powder are filtered out by negative pressure suction equipment to obtain light yellow pure mugwort powder; S24, stirring: using a dry-wet separation dual mixing mixer to stir, prepare 5 parts of raw materials of wormwood powder, 30 parts of waterborne polyurethane, 5 parts of filler, and 2 parts of defoamer, place the above raw materials in the upper dry material stirring system for initial stirring, put them into the lower stirring system after the initial stirring, add 20 parts of solvent and 2 parts of film-forming aid for wet stirring, so that the coating is fully integrated, the filler is titanium dioxide or talcum powder; the solvent is deionized water; S25, pressing and drying: squeezing water out of the stirred wormwood powder particles, and then placing them in the sun to allow the wormwood powder to fully absorb sunlight, thereby obtaining the wormwood Chinese herbal medicine; S26, proportioning and foaming: using the Osole material as a carrier, adding mugwort Chinese herbal medicine, and preparing a plant foaming sponge material; S3, hot pressing: stirring the plant material obtained in step S26, and then hot pressing it with the midsole base layer through a hot press to form an integrated midsole zipper cloth; S4. Packaging: After hot pressing, the midsole pull cloth is rolled, needle tested, packaged, cut and packaged.
[0014] The raw material of the polypropylene fiber is recycled polypropylene plastic and is processed by physical crushing.
[0015] In the step S12, the needle punching pressure parameter of the nonwoven is 100-200 bar, the speed of the web forming machine is controlled at 60-90 m / min, the needle punching frequency is 500-700 punctures / min, and the needle density of the needle board is 5500-6500 needles / m.
[0016] In step S13, the temperature of the PVA aqueous solution is controlled to be 60-90°C, the speed of the composite base fabric impregnation vehicle is 10-20 m / min, the pressure between the rolling tubes through which the impregnated fabric passes is 0.001-1 MPa, and the drying temperature is controlled to be 100-190°C.
[0017] In the step S22, 80% of the moisture is removed during sun drying, hammering is artificially beating into fibers, and grinding is screened through a 20-40 mesh molecular sieve.
[0018] The hot pressing temperature of the hot pressing machine in step S3 is 125-145°C.
[0019] Mugwort is produced in Enshi, the selenium capital of Hubei Province, with an average altitude of 1,000 meters and an average annual temperature of around 23 degrees Celsius. Example
[0020] A preparation process of an antibacterial midsole pull-up cloth made of wormwood comprises the following steps: S1. Preparation of midsole antibacterial base layer: S11, web laying: After the combed polypropylene fibers and the Chinese herbal medicine of mugwort are fully mixed, the combed polypropylene fibers are clamped by the upper and lower carbon curtains of the web laying machine, and the web is cross-laid by synchronous movement to achieve an ideal laying effect; S12, needle punching: the polypropylene fibers output from the web are conveyed by the web forming machine into the needle punching machine for processing, and the composite base fabric is obtained by entanglement of the non-woven needle punched fibers; S13, sizing: performing basic impregnation treatment on the composite base fabric in an aqueous solution of PVA; S14, PU impregnation: the composite base fabric is subjected to PU impregnation treatment in a mixture of PU resin and DMF, the composite base fabric is impregnated at a speed of 5-15 m / min, the pressure between the rolling tubes through which the impregnated fabric passes is 0.001-1 MPa, the impregnated fabric is coagulated in a DMF aqueous solution through a coagulation bath, and then washed and dried, the formula ratio of each component per hundred parts by weight of the mixture of PU resin and DMF is: 10 parts of PU resin, 90 parts of DMF; the weight ratio of each component per hundred parts by weight of the DMF aqueous solution is: 15 parts of DMF, 85 parts of water, 8 parts of antibacterial agent, 5 parts of NaHCO3, and 15 parts of guanidine antibacterial agent are added to the obtained mixture of PU resin and DMF, The antibacterial agent is prepared by the following method: 1.5g chitosan is dispersed in 100-300ml isopropanol and subjected to ultrasonic treatment, the ultrasonic power is 50-70W, and the ultrasonic time is 20-50min; 7g cross-linking agent is added, stirred evenly, and reacted at 50-80℃ for 2-5h; after the reaction is completed, the mixture is washed and dried to obtain chitosan quaternary ammonium salt; Dissolve 1g of the chitosan quaternary ammonium salt, 4g of the grafting monomer, 0.01g of the polymerization inhibitor, 0.5g of the initiator and 0.02 nano-TiO2 in 10-30ml of deionized water, stir evenly, and heat at 110-150°C for 5-20min; after the reaction is completed, wash and dry; The nano-TiO2 is a modified nano-TiO2, which is prepared by the following method: 0.4g of nano-TiO2 and 0.02g of hexadecyl glycidyl dimethyl ammonium chloride are placed in 80-100ml of deionized water for ultrasonic dispersion, with an ultrasonic power of 50-70W and an ultrasonic time of 10-30min, and then centrifuged and dried to obtain the modified nano-TiO2; The grafting monomer is a mixture of citric acid and N-hydroxyethyl acrylamide in a mass ratio of (1-3): (1-3); The cross-linking agent is one or two of hexadecyl epoxypropyl dimethyl ammonium chloride and 2,3-epoxypropyl trimethyl ammonium chloride; S15, alkali reduction fiber opening, the fiber opening temperature is 100±5℃, and the temperature is kept for 30-45 minutes; the composite matrix obtained in step S14 is soaked in a sodium hydroxide solution, the sodium hydroxide concentration is maintained at 6-8g / L, the soaking time is 1 hour, and the temperature is 90-105℃; S16, dyeing: the seam ends of the grey cloth are pre-treated, dyed, reduced and cleaned, washed with hot water, washed with water, dehydrated and shaped. During the initial dyeing, the initial dyeing temperature of the disperse dye is controlled at 50-60°C, and gradually heated to 130°C after 1 hour, kept warm for 1-2 hours, and then fully washed with water. When dyeing dark colors, reduction cleaning is performed; S17, shaping and drying: after reduction cleaning, adding polypropylene fiber to perform drying and shaping again, during shaping, the base fabric temperature is controlled to be 100-170°C, and the speed is adjusted to 5-30 m / min to form a midsole base layer; S2. Mugwort treatment: S21, selecting and washing: removing weeds from the purchased wormwood and then washing it to remove dirt and dust from the grass; S22, powdering: the washed wormwood is withered, sterilized, sun-dried, combed, hammered, and then ground into wormwood powder particles; S23, grinding: using plant grinding equipment, the dry mugwort leaves are made into 150 mesh mugwort powder, and the dust and black matter in the mugwort powder are filtered out by negative pressure suction equipment to obtain light yellow pure mugwort powder; S24, stirring: using a dry-wet separation dual mixing mixer to stir, prepare 15 parts of raw materials of wormwood powder, 45 parts of waterborne polyurethane, 7 parts of filler, and 4.5 parts of defoamer, place the above raw materials in the upper dry material stirring system for initial stirring, put them into the lower stirring system after the initial stirring, add 30 parts of solvent and 4 parts of film-forming aid for wet stirring, so that the coating is fully integrated, the filler is titanium dioxide or talcum powder; the solvent is deionized water; S25, pressing and drying: squeezing water out of the stirred wormwood powder particles, and then placing them in the sun to allow the wormwood powder to fully absorb sunlight, thereby obtaining the wormwood Chinese herbal medicine; S26, proportioning and foaming: using the Osole material as a carrier, adding mugwort Chinese herbal medicine, and preparing a plant foaming sponge material; S3, hot pressing: stirring the plant material obtained in step S26, and then hot pressing it with the midsole base layer through a hot press to form an integrated midsole zipper cloth; S4. Packaging: After hot pressing, the midsole pull cloth is rolled, needle tested, packaged, cut and packaged.
[0021] The raw material of the polypropylene fiber is recycled polypropylene plastic and is processed by physical crushing.
[0022] In the step S12, the needle punching pressure parameter of the nonwoven is 100-200 bar, the speed of the web forming machine is controlled at 60-90 m / min, the needle punching frequency is 500-700 punctures / min, and the needle density of the needle board is 5500-6500 needles / m.
[0023] In step S13, the temperature of the PVA aqueous solution is controlled to be 60-90°C, the speed of the composite base fabric impregnation vehicle is 10-20 m / min, the pressure between the rolling tubes through which the impregnated fabric passes is 0.001-1 MPa, and the drying temperature is controlled to be 100-190°C.
[0024] In the step S22, 80% of the moisture is removed during sun drying, hammering is artificially beating into fibers, and grinding is screened through a 20-40 mesh molecular sieve.
[0025] The hot pressing temperature of the hot pressing machine in step S3 is 125-145°C.
[0026] Mugwort is produced in Enshi, the selenium capital of Hubei Province, with an average altitude of 1,000 meters and an average annual temperature of around 23 degrees Celsius. Example
[0027] A preparation process of an antibacterial midsole pull-up cloth made of wormwood comprises the following steps: S1. Preparation of midsole antibacterial base layer: S11, web laying: After the combed polypropylene fibers and the Chinese herbal medicine of mugwort are fully mixed, the combed polypropylene fibers are clamped by the upper and lower carbon curtains of the web laying machine, and the web is cross-laid by synchronous movement to achieve an ideal laying effect; S12, needle punching: the polypropylene fibers output from the web are conveyed by the web forming machine into the needle punching machine for processing, and the composite base fabric is obtained by entanglement of the non-woven needle punched fibers; S13, sizing: performing basic impregnation treatment on the composite base fabric in an aqueous solution of PVA; S14, PU impregnation: the composite base fabric is subjected to PU impregnation treatment in a mixture of PU resin and DMF, the composite base fabric impregnation vehicle speed is controlled to be 5-15 m / min, the pressure between the rolling tubes through which the impregnated fabric passes is 0.001-1 MPa, the impregnated fabric is coagulated in a DMF aqueous solution through a coagulation bath, and then washed and dried, the formula ratio of each component per hundred parts by weight of the mixture of PU resin and DMF is: 20 parts of PU resin, 97 parts of DMF; the weight ratio of each component per hundred parts by weight of the DMF aqueous solution is: 20 parts of DMF, 90 parts of water, 9 parts of antibacterial agent, 6 parts of NaHCO3, and 20 parts of guanidine antibacterial agent are added to the obtained mixture of PU resin and DMF, The antibacterial agent is prepared by the following method: 1-3g chitosan is dispersed in 100-300ml isopropanol and subjected to ultrasonic treatment, the ultrasonic power is 50-70W, and the ultrasonic time is 20-50min; 9g cross-linking agent is added, stirred evenly, and reacted at 50-80℃ for 2-5h; after the reaction is completed, the mixture is washed and dried to obtain chitosan quaternary ammonium salt; Dissolve 1.5g of the above chitosan quaternary ammonium salt, 5g of grafting monomer, 0.02g of inhibitor, 0.7g of initiator and 0.03g of nano-TiO2 in 10-30ml of deionized water, stir evenly, and heat at 110-150℃ for 5-20min; after the reaction, wash and dry; The nano-TiO2 is a modified nano-TiO2, which is prepared by the following method: 0.5g of nano-TiO2 and 0.03g of hexadecyl glycidyl dimethyl ammonium chloride are placed in 80-100ml of deionized water for ultrasonic dispersion, with an ultrasonic power of 50-70W and an ultrasonic time of 10-30min, and then centrifuged and dried to obtain the modified nano-TiO2; The grafting monomer is a mixture of citric acid and N-hydroxyethyl acrylamide in a mass ratio of (1-3): (1-3); The cross-linking agent is one or two of hexadecyl epoxypropyl dimethyl ammonium chloride and 2,3-epoxypropyl trimethyl ammonium chloride; S15, alkali reduction fiber opening, the fiber opening temperature is 100±5℃, and the temperature is kept for 30-45 minutes; the composite matrix obtained in step S14 is soaked in a sodium hydroxide solution, the sodium hydroxide concentration is maintained at 6-8g / L, the soaking time is 1 hour, and the temperature is 90-105℃; S16, dyeing: the seam ends of the grey cloth are pre-treated, dyed, reduced and cleaned, washed with hot water, washed with water, dehydrated and shaped. During the initial dyeing, the initial dyeing temperature of the disperse dye is controlled at 50-60°C, and gradually heated to 130°C after 1 hour, kept warm for 1-2 hours, and then fully washed with water. When dyeing dark colors, reduction cleaning is performed; S17, shaping and drying: after reduction cleaning, adding polypropylene fiber to perform drying and shaping again, during shaping, the base fabric temperature is controlled to be 100-170°C, and the speed is adjusted to 5-30 m / min to form a midsole base layer; S2. Mugwort treatment: S21, selecting and washing: removing weeds from the purchased wormwood and then washing it to remove dirt and dust from the grass; S22, powdering: the washed wormwood is withered, sterilized, sun-dried, combed, hammered, and then ground into wormwood powder particles; S23, grinding: using plant grinding equipment, the dry mugwort leaves are made into 150 mesh mugwort powder, and the dust and black matter in the mugwort powder are filtered out by negative pressure suction equipment to obtain light yellow pure mugwort powder; S24, stirring: using a dry-wet separation dual mixing mixer to stir, prepare 20 parts of raw materials of wormwood powder, 60 parts of waterborne polyurethane, 10 parts of filler, and 7 parts of defoamer, place the above raw materials in the upper dry material stirring system for initial stirring, put them into the lower stirring system after the initial stirring, add 40 parts of solvent and 6 parts of film-forming aid for wet stirring, so that the coating is fully integrated, the filler is titanium dioxide or talcum powder; the solvent is deionized water; S25, pressing and drying: squeezing water out of the stirred wormwood powder particles, and then placing them in the sun to allow the wormwood powder to fully absorb sunlight, thereby obtaining the wormwood Chinese herbal medicine; S26, proportioning and foaming: using the Osole material as a carrier, adding mugwort Chinese herbal medicine, and preparing a plant foaming sponge material; S3, hot pressing: stirring the plant material obtained in step S26, and then hot pressing it with the midsole base layer through a hot press to form an integrated midsole zipper cloth; S4. Packaging: After hot pressing, the midsole pull cloth is rolled, needle tested, packaged, cut and packaged.
[0028] The raw material of the polypropylene fiber is recycled polypropylene plastic and is processed by physical crushing.
[0029] In the step S12, the needle punching pressure parameter of the nonwoven is 100-200 bar, the speed of the web forming machine is controlled at 60-90 m / min, the needle punching frequency is 500-700 punctures / min, and the needle density of the needle board is 5500-6500 needles / m.
[0030] In step S13, the temperature of the PVA aqueous solution is controlled to be 60-90°C, the speed of the composite base fabric impregnation vehicle is 10-20 m / min, the pressure between the rolling tubes through which the impregnated fabric passes is 0.001-1 MPa, and the drying temperature is controlled to be 100-190°C.
[0031] In the step S22, 80% of the moisture is removed during sun drying, hammering is artificially beating into fibers, and grinding is screened through a 20-40 mesh molecular sieve.
[0032] The hot pressing temperature of the hot pressing machine in step S3 is 125-145°C.
[0033] Mugwort is produced in Enshi, the selenium capital of Hubei Province, with an average altitude of 1,000 meters and an average annual temperature of around 23 degrees Celsius.
[0034] Test experiment: The test was carried out in accordance with GB / T 20944.3-2008 Evaluation of antibacterial properties of textiles Part 3: Oscillation method. The test results are as follows:
[0035] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
Claims
1. A preparation process of an antibacterial midsole pull-up cloth made of wormwood, characterized in that: The following steps are involved: S1. Preparation of midsole antibacterial base layer: S11, web laying: After the combed polypropylene fibers and the Chinese herbal medicine of mugwort are fully mixed, the combed polypropylene fibers are clamped by the upper and lower carbon curtains of the web laying machine, and the web is cross-laid by synchronous movement to achieve an ideal laying effect; S12, needle punching: the polypropylene fibers output from the web are conveyed by the web forming machine into the needle punching machine for processing, and the composite base fabric is obtained by entanglement of the non-woven needle punched fibers; S13, sizing: performing basic antibacterial impregnation treatment on the composite base fabric in an aqueous solution of PVA; S14, PU impregnation: the composite base fabric is subjected to PU impregnation treatment in a mixture of PU resin and DMF, the composite base fabric is impregnated at a speed of 5-15 m / min, the pressure between the rolling tubes through which the impregnated fabric passes is 0.001-1 MPa, the impregnated fabric is coagulated in a DMF aqueous solution through a coagulation bath, and then washed and dried, the formula ratio of each component per hundred parts by weight of the mixture of PU resin and DMF is: 3-20 parts of PU resin, 80-97 parts of DMF; the weight ratio of each component per hundred parts by weight of the DMF aqueous solution is: 10-20 parts of DMF, 80-90 parts of water, 6-9 parts of antibacterial agent, 4-6 parts of NaHCO3, and 10-20 parts of guanidine antibacterial agent are added to the obtained mixture of PU resin and DMF, The antibacterial agent is prepared by the following method: 1-3g chitosan is dispersed in 100-300ml isopropanol and subjected to ultrasonic treatment, the ultrasonic power is 50-70W, and the ultrasonic time is 20-50min; 5-9g cross-linking agent is added, stirred evenly, and reacted at 50-80℃ for 2-5h; after the reaction is completed, the mixture is washed and dried to obtain chitosan quaternary ammonium salt; Dissolve 0.8-1.5g of the chitosan quaternary ammonium salt, 3-5g of the grafting monomer, 0.005-0.02g of the inhibitor, 0.25-0.7g of the initiator and 0.01-0.03g of nano-TiO2 in 10-30ml of deionized water, stir evenly, and heat at 110-150°C for 5-20min; after the reaction is completed, wash and dry; The nano-TiO2 is a modified nano-TiO2, which is prepared by the following method: 0.3-0.5g of nano-TiO2 and 0.01-0.03g of hexadecyl glycidyl dimethyl ammonium chloride are placed in 80-100ml of deionized water for ultrasonic dispersion, with an ultrasonic power of 50-70W and an ultrasonic time of 10-30min, and then centrifuged and dried to obtain the modified nano-TiO2; The grafting monomer is a mixture of citric acid and N-hydroxyethyl acrylamide in a mass ratio of (1-3): (1-3); The cross-linking agent is one or two of hexadecyl epoxypropyl dimethyl ammonium chloride and 2,3-epoxypropyl trimethyl ammonium chloride; S15, alkali reduction fiber opening, the fiber opening temperature is 100±5℃, and the temperature is kept for 30-45 minutes; the composite matrix obtained in step S14 is soaked in a sodium hydroxide solution, the sodium hydroxide concentration is maintained at 6-8g / L, the soaking time is 1 hour, and the temperature is 90-105℃; S16, dyeing: the seam ends of the grey cloth are pre-treated, dyed, reduced and cleaned, washed with hot water, washed with water, dehydrated and shaped. During the initial dyeing, the initial dyeing temperature of the disperse dye is controlled at 50-60°C, and gradually heated to 130°C after 1 hour, kept warm for 1-2 hours, and then fully washed with water. When dyeing dark colors, reduction cleaning is performed; S17, shaping and drying: after reduction cleaning, adding polypropylene fiber to perform drying and shaping again, during shaping, the base fabric temperature is controlled to be 100-170°C, and the speed is adjusted to 5-30 m / min to form a midsole base layer; S2. Mugwort treatment: S21, selecting and washing: removing weeds from the purchased wormwood and then washing it to remove dirt and dust from the grass; S22, powdering: the washed wormwood is withered, sterilized, sun-dried, combed, hammered, and then ground into wormwood powder particles; S23, grinding: using plant grinding equipment, the dry mugwort leaves are made into 150 mesh mugwort powder, and the dust and black matter in the mugwort powder are filtered out by negative pressure suction equipment to obtain light yellow pure mugwort powder; S24, stirring: using a dry-wet separation dual mixing mixer to stir, prepare 5-20 parts of raw materials of wormwood powder, 30-60 parts of waterborne polyurethane, 5-10 parts of filler, and 2-7 parts of defoamer, place the above raw materials in the upper dry material stirring system for initial stirring, put them into the lower stirring system after the initial stirring, add 20-40 parts of solvent and 2-6 parts of film-forming aid for wet stirring, so that the coating is fully integrated, the filler is titanium dioxide or talcum powder; the solvent is deionized water; S25, pressing and drying: squeezing water out of the stirred wormwood powder particles, and then placing them in the sun to allow the wormwood powder to fully absorb sunlight, thereby obtaining the wormwood Chinese herbal medicine; S26, proportioning and foaming: using the Osole material as a carrier, adding mugwort Chinese herbal medicine, and preparing a plant foaming sponge material; S3, hot pressing: the plant material obtained in step S26 is stirred, and then hot pressed with the midsole base layer through a hot press to form an integrated midsole pull-up cloth; S4. Packaging: After hot pressing, the midsole pull cloth is rolled, needle tested, packaged, cut and packaged.
2. The preparation process of the wormwood antibacterial midsole zip-up cloth according to claim 1, characterized in that: The raw material of the polypropylene fiber is recycled polypropylene plastic and is processed by physical crushing.
3. The preparation process of the wormwood antibacterial midsole zip-up cloth according to claim 1, characterized in that: In the step S12, the needle punching pressure parameter of the nonwoven is 100-200 bar, the speed of the web forming machine is controlled at 60-90 m / min, the needle punching frequency is 500-700 punctures / min, and the needle density of the needle board is 5500-6500 needles / m.
4. The preparation process of the wormwood antibacterial midsole zip-up cloth according to claim 1, characterized in that: In step S13, the temperature of the PVA aqueous solution is controlled to be 60-90°C, the speed of the composite base fabric impregnation vehicle is 10-20 m / min, the pressure between the rolling tubes through which the impregnated fabric passes is 0.001-1 MPa, and the drying temperature is controlled to be 100-190°C.
5. The preparation process of the wormwood antibacterial midsole zip-up cloth according to claim 1, characterized in that: In the step S22, 80% of the moisture is removed during sun drying, hammering is artificially beating into fibers, and grinding is screened through a 20-40 mesh molecular sieve.
6. The preparation process of the wormwood antibacterial midsole zip-up cloth according to claim 1, characterized in that: The hot pressing temperature of the hot pressing machine in step S3 is 125-145°C.
Citation Information
Patent Citations
Preparation method of wormwood paint
CN105153908A
Multifunctional mildewproof antibacterial agent
CN105211089A
Antibacterial fabric
CN112144278A
Preparation method of regenerated fiber carex meyeriana insole upper pulling cloth
CN112841815A