Battery bag film with enhanced formability and preparation method thereof

By using an outer layer composed of polyamide and polyethylene terephthalate and a barrier layer composed of aluminum in the battery bag film, combined with specific surface treatment and drying processes, cracks in the battery bag film during the high molding process are solved Problem, the formation of thick edges and the improvement of battery molding depth are achieved, which is suitable for large and medium-sized battery applications.

CN118769652APending Publication Date: 2024-10-15YOUL CHON CHEMICAL CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202410403390.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-04-06
Filing Date
2024-04-03
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Existing battery bag films are prone to cracks during the high molding process, resulting in insufficient thickness at the edges, affecting the molding depth and safety of the battery.

Method used

It adopts a battery bag film structure composed of an outer layer, a barrier layer, and a sealing layer laminated in sequence. The outer layer is composed of polyamide and polyethylene terephthalate. The surface roughness on the barrier layer side is controlled below 1.5 μm. Specific surface treatment and drying processes ensure that the residual thickness and molding depth of the edge metal layer reaches more than 34 μm, and the drying process is performed above 160°C.

Benefits of technology

It effectively suppresses the occurrence of edge cracks during high molding and forms thick edges, which improves the molding characteristics and energy density of the battery. It is suitable for large and medium-sized batteries, such as electric vehicles and energy storage devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118769652A_ABST
    Figure CN118769652A_ABST
Patent Text Reader

Abstract

The invention discloses a battery pouch film with enhanced moldability, a preparation method thereof, and a secondary battery using the battery pouch film. According to the present invention, the corresponding battery pouch film can suppress the occurrence of edge cracks occurring during high molding, and thus can form a thick edge, thereby having excellent high molding characteristics. The battery bag film can improve the energy density of a secondary battery, and can be effectively used for large and medium-sized battery bags of electric automobiles or energy storage devices and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present specification relates to a battery bag film with enhanced formability and a method for preparing the same, a battery bag using the same, a secondary battery and a method for preparing the same, and more specifically, to a battery bag film and a method for preparing the same, a battery bag using the same, a secondary battery and a method for preparing the same, that is, a battery bag film that can prevent cracks from being generated during the high forming process of the secondary battery bag film to form a thick edge portion, thereby being effectively used in large and medium-sized batteries based on excellent high forming properties.

[0002] [Korean R&D project supporting this invention]

[0003]

Project unique number

[0004]

Project number

[0005]

Department name

[0006] [Name of project management (specialized) organization] Korea Industrial Technology Evaluation and Management Institute

[0007]

Research Project Name

[0008] [Research Topic Name] Development of a next-generation secondary battery bag that can achieve more than twice the bonding strength (60°C)

[0009]

Contribution rate

[0010]

Project execution organization name

[0011] [Study period] January 1, 2023 to December 31, 2023 Background Art

[0012] Lithium secondary batteries (LiB) are used in many applications due to their various advantages such as high energy density and excellent output.

[0013] Battery pouch film is a multi-layer packaging laminate film that surrounds the electrode group and electrolyte of secondary batteries and other batteries. It is a core component that determines the stability, service life characteristics and operating sustainability of the battery. Therefore, it requires mechanical flexibility and strength, high oxygen / water vapor barrier properties, high heat sealing strength, chemical resistance to electrolytes, electrical insulation, high temperature stability, etc.

[0014] As the application fields of lithium secondary batteries gradually expand from small fields to large and medium-sized fields such as automobiles and energy storage devices (ESS), battery pouch films also need to have properties suitable for large and medium-sized fields, especially high safety and solid properties.

[0015] In this regard, the battery size and battery bag molding depth of automotive lithium secondary batteries (LiB) are factors that greatly affect the capacity of secondary batteries. In the case of battery size, the size needs to be larger than that of ordinary small batteries and higher moldability is required. Since the battery capacity depends on the battery molding depth, the molding depth can be regarded as a basic condition for achieving the capacity of 700Wh / L required for the next generation of secondary batteries.

[0016] On the other hand, in general, the first step of surface treatment of one side of the metal layer of the battery bag, the second step of surface treatment of the other side of the metal layer, the third step of bonding the outer layer to one side, and the fourth step of bonding the sealing layer to the other side can be performed repeatedly in the order of coating, drying and winding. However, in this case, when the fabric is transferred, the probability of operation loss and process defects increases, so it needs to be improved.

[0017] Prior art literature

[0018] Patent Literature

[0019] Patent Document 1: Korean Patent Publication No. 10-2016-0070468

[0020] Patent Document 2: Korean Patent Publication No. 10-2022-0031820 Summary of the invention

[0021] Technical issues

[0022] On the one hand, an exemplary implementation example of the present invention provides a battery pouch film having a thick edge portion and a secondary battery having the battery pouch film externally provided, which can suppress the occurrence of edge cracks during high molding.

[0023] On the other hand, an exemplary implementation example of the present invention provides a battery pouch film having excellent high molding properties and a secondary battery having the battery pouch film externally mounted thereon.

[0024] Technical Solution

[0025] An exemplary implementation example of the present invention provides a battery pouch film (the battery pouch film of technical solution 1), which is composed of at least an outer layer, a barrier layer, and a sealing layer stacked in sequence. After peeling off the outer layer and the barrier layer of the battery pouch film, the surface roughness Ra of the peeling surface on the barrier layer side is less than 1.5μm.

[0026] An exemplary implementation example of the present invention provides a battery pouch film (the battery pouch film of technical solution 2), which is composed of at least an outer layer, a barrier layer, and a sealing layer stacked in sequence, and the outer layer is formed by bonding polyamide and polyethylene terephthalate (PET). The longitudinal (MD direction) elastic modulus of the outer layer is less than 2450, and the transverse (TD direction) elastic modulus is less than 2400.

[0027] In an exemplary implementation example, the battery pouch film of Technical Solution 1 and / or the battery pouch film of Technical Solution 2 may be a battery pouch film (battery pouch film of Technical Solution 3) in which the thickness of the barrier layer before molding is 60 μm and the residual thickness of the metal layer at the edge of the battery pouch film measured according to the following method is 34 μm or more.

[0028] [Measurement of the residual thickness of the metal layer at the edge]

[0029] A battery pouch film of 240 mm (MD) × 266 mm (TD) was formed by a forming machine. After 12 mm of forming, the edge was cut by a cross-section cutting machine and the maximum thickness of the metal layer cross section in the battery pouch film was measured by a scanning electron microscope (SEM).

[0030] In an exemplary implementation example, the above-mentioned battery pouch film (the battery pouch film of any one of Technical Solutions 1 to 3) may be a battery pouch film (the battery pouch film of Technical Solution 4) having a maximum molding depth of 16 mm or more measured according to the following method.

[0031] [Moldability measurement]

[0032] The battery bag film was prepared into a test piece of 240 mm (MD) × 266 mm (TD), and the moldability was evaluated by a molding machine. The molding results were measured 10 times, and the molding without cracks in all 10 times was evaluated as the maximum molding depth of the bag.

[0033] The preparation method of the battery pouch film provided in the exemplary implementation example of the present invention (the preparation method of the battery pouch film of technical solution 5) is used to prepare the above-mentioned battery pouch film (the battery pouch film of any one of technical solutions 1 to 4), including: a two-side surface treatment step, surface treating the two sides of the metal fabric contained in the barrier layer; a drying step, drying the above-mentioned metal fabric that has been surface-treated on both sides; an outer surface adhesive layer coating step, applying an adhesive to one side of the above-mentioned metal fabric that has been surface-treated to form an outer surface adhesive layer; and an outer layer bonding step, bonding the outer layer fabric to the upper part of the above-mentioned outer surface adhesive layer. After the above-mentioned two-side surface treatment, the drying temperature of the metal fabric is above 160°C.

[0034] In an exemplary implementation example, the above method (battery pouch film preparation method of technical solution 5) may be a method (battery pouch film preparation method of technical solution 6) comprising the following steps: after the first bonding of polyamide and polyethylene terephthalate (PET) film, the above-mentioned bonded polyamide and polyethylene terephthalate (PET) film are bonded to aluminum serving as a barrier layer.

[0035] In an exemplary implementation example, the above method (battery pouch film preparation method of technical solution 5 or 6) may be a method (battery pouch film preparation method of technical solution 7) comprising the following steps: after surface-treating one side of the metal fabric in the above-mentioned two-sided surface treatment step, surface-treating the other side of the above-mentioned metal fabric in turn without performing a drying step.

[0036] In an exemplary implementation example, the above method (the preparation method of the battery pouch film of any one of Technical Solutions 5 to 7) can be a method for drying the metal fabric whose two sides have been surface-treated by floating in the above-mentioned drying step (the preparation method of the battery pouch film of Technical Solution 8).

[0037] In an exemplary implementation example, the above method (the battery pouch film preparation method of any one of Technical Solutions 5 to 8) may be the above-mentioned two-sided surface treatment steps, including applying a water-based coating liquid and a solvent-based coating liquid to one side of the metal fabric by a combination of direct coating (Direct coating) and reverse contact coating (RKC, Reverse Kiss Coating) to perform a first coating, and applying a coating liquid to the other side of the metal fabric by RKC and film up / down coating to perform a second coating (the battery pouch film preparation method of Technical Solution 9).

[0038] In an exemplary implementation example, the above method (the battery pouch film preparation method of any one of Technical Solutions 5 to 9) may include: a step of performing a first winding after the above-mentioned outer layer laminating step; a step of forming an inner surface adhesive layer on the other side of the surface-treated metal fabric that is not laminating to the outer layer after the above-mentioned first winding; a step of laminating a sealing layer fabric to the lower part of the above-mentioned inner surface adhesive layer; and a method of performing a second winding after laminating the above-mentioned sealing layer fabric (the battery pouch film preparation method of Technical Solution 10).

[0039] An exemplary implementation example of the present invention provides a battery bag made of the above-mentioned battery bag film (the battery bag film of any one of Technical Solutions 1 to 4) or a secondary battery (the secondary battery of Technical Solution 11) externally thereto.

[0040] Furthermore, the secondary battery preparation method provided by the exemplary implementation example of the present invention (the secondary battery preparation method of technical solution 12) includes the step of placing the above-mentioned battery pouch film (the battery pouch film of any one of technical solutions 1 to 4) on the outside of the secondary battery.

[0041] Effects of the Invention

[0042] The exemplary implementation of the present invention can suppress the occurrence of cracks at the edge of the secondary battery bag film during high molding, thereby forming a thick edge, thereby having excellent high molding properties. This battery bag film can increase the energy density of the secondary battery and can be effectively used in large and medium-sized battery bags for electric vehicles or energy storage devices. BRIEF DESCRIPTION OF THE DRAWINGS

[0043] Figure 1 FIG. 1 is a diagram briefly showing a cross section of a battery pouch film according to an exemplary implementation of the present invention.

[0044] Figure 2 It is a schematic diagram of a device for preparing a battery pouch film according to an exemplary implementation example of the present invention. DETAILED DESCRIPTION

[0045] Definition of terms

[0046] In this specification, unless the context clearly indicates different meanings, singular expressions may include plural expressions. In this application, the terms "including" or "having" are used to specify the existence of features, numbers, steps, operations, structural elements, components or their combinations recorded in the specification, and do not exclude the existence or additional possibility of one or more other features, numbers, steps, operations, structural elements, components or their combinations.

[0047] In the present specification, unless otherwise defined, expressions such as “first” and “second” are used to distinguish structures but do not indicate a specific order.

[0048] In the present specification, “formed on” a specific layer not only means being directly formed on the corresponding layer but also may include being formed with other layers additionally interposed therebetween.

[0049] In this specification, the term "battery (cell)" refers to a battery in its broadest sense, including various batteries such as secondary batteries such as lithium ion batteries and lithium polymer batteries, and portable storage batteries.

[0050] In this specification, the term "cell pouch" or "cell pouch film" is used to refer to a component that immerses and houses battery structural elements such as an anode, cathode, and separator in an electrolyte, and includes the broadest meaning of a film with a laminated structure processed into a bag shape or a box shape, etc., in order to house the above-mentioned battery structural elements, taking into account gas barrier properties, flexibility, electrolyte resistance, and thermal adhesion.

[0051] In this specification, the final structure refers to the final layer structure of the battery pouch film. This final structure may be slightly different depending on various types of manufacturing processes.

[0052] For example, the final structure may consist of an outer covering substrate (or outer layer), a first adhesive layer, an outer surface surface treatment layer, a reference substrate (or barrier layer), an inner surface surface treatment layer, a second adhesive layer, and an inner covering substrate (or sealing layer). Alternatively, the final structure may consist of an outer covering substrate (or outer layer), a first adhesive layer, an outer surface surface treatment layer, a reference substrate (or barrier layer), an inner surface surface treatment layer, an extrusion coating layer, and an inner covering substrate (or sealing layer). Alternatively, the final structure may consist of an outer covering substrate (or outer layer), a first adhesive layer, an outer surface surface treatment layer, a reference substrate (or barrier layer), an inner surface surface treatment layer, a second adhesive layer, an extrusion coating layer, and an inner covering substrate (or sealing layer).

[0053] In this specification, the intermediate structure refers to a structure formed in the middle during the manufacturing process of the battery pouch film, and various battery pouch intermediate structures can be generated according to the manufacturing process.

[0054] For example, there may be a first intermediate structure consisting of an outer covering substrate (or outer layer), a first adhesive layer (or outer surface adhesive layer), an outer surface surface treatment layer, a reference substrate (or barrier layer), an inner surface surface treatment layer, and a second adhesive layer (or inner surface adhesive layer). Alternatively, there may be a second intermediate structure consisting of an outer covering substrate (or outer layer), a first adhesive layer (or outer surface adhesive layer), an outer surface surface treatment layer, a reference substrate (or barrier layer), and an inner surface surface treatment layer.

[0055] In this specification, an in-line process refers to a roll-to-roll process in which the fabric performs one run between unwinding and rewinding (winding roll).

[0056] In this specification, one winding (rewinding) means winding the film on the winding roller to complete one run, and does not mean that the winding roller rotates once (of course, the winding roller can rotate multiple times). Therefore, two windings (rewinding) means completing the second run after completing one run in the preparation process and starting the second run again.

[0057] In this specification, fabric refers to the material used for the barrier layer or metal layer in the manufacturing process.

[0058] In this specification, the functional fabric refers to a resin fabric used to form a sealing layer and / or an outer layer.

[0059] In this specification, the edge portion refers to the corner portion of the molded portion. For example, when molding, the bag is prepared into a rectangular cup shape with a size of 185mm (X axis) × 85mm (Y axis) × 12mm (Z axis). The edge portion refers to the portion from the end point of the corner portion of the rectangular cup to 0.5mm × 0.5mm × 0.5mm.

[0060] In this specification, the peeling surface on the barrier layer side is not the metal surface itself as the barrier layer material, but refers to the surface of the barrier layer (peeling surface) where a part of the material peeled off from the outer layer film side remains after peeling off the outer layer and the barrier layer of the battery pouch film. Therefore, the surface roughness of the peeling surface on the barrier layer side is not the surface roughness of the metal surface itself as the barrier layer material, but refers to the surface roughness of the peeling surface on the barrier layer side where the remaining material (residue) on the barrier layer side exists after peeling off the outer layer film. The surface roughness of the peeling surface caused by the corresponding residue is different from the surface roughness of the metal layer surface itself.

[0061] Description of an exemplary implementation

[0062] An exemplary implementation of the present invention is described below.

[0063] Since cracks are easily generated at the edge when the battery bag film is highly molded, it is difficult to form a thick edge. That is, how thick the edge can be formed can be regarded as a measure to evaluate high moldability. How thick the edge can be formed can be evaluated by the residual thickness of the barrier layer at the edge after molding (thickness after molding) as follows.

[0064] The inventors arrived at the present invention by confirming the surface roughness of the peeling surface when peeling off the outer layer and the barrier layer of the battery bag film and / or the MD direction elastic modulus and TD direction elastic modulus of the outer layer of the battery bag film where the polyamide and PET are bonded together, the thickness of the edge part during high molding and their correlation with high moldability, and through research.

[0065] Specifically, in the battery pouch film of the exemplary implementation example of the present invention, after the outer layer and the barrier layer of the battery pouch film are peeled off, the surface roughness Ra on the barrier layer side is 1.5 μm or less.

[0066] In a non-limiting example, the surface roughness Ra may be 0.82 μm to 1.5 μm or 0.82 μm to 1.13 μm. In a non-limiting example, the surface roughness Ra may be 1.49 μm or less, 1.48 μm or less, 1.47 μm or less, 1.46 μm or less, 1.45 μm or less, 1.44 μm or less, 1.43 μm or less, 1.42 μm or less, 1.41 μm or less, 1.40 μm or less, 1.39 μm or less, 1.38 μm or less, 1.37 μm or less, 1.36 μm or less, 1.35 μm or less, 1.44 μm or less, 1.43 μm or less, 1.42 μm or less, 1.41 μm or less, 1.42 ... .34μm or less, 1.33μm or less, 1.32μm or less, 1.31μm or less, 1.30μm or less, 1.29μm or less, 1.28μm or less, 1.27μm or less, 1.26μm or less, 1.25μm or less, 1.24μm or less, 1.23μm or less, 1.22μm or less, 1.21μm or less, 1.20μm or less, 1.19μm or less, 1.18μm or less, 1.17μm Below, 1.16μm below, 1.15μm below, 1.14μm below, 1.13μm below, 1.12μm below, 1.11μm below, 1.10μm below, 1.09μm below, 1.08μm below, 1.07μm below, 1.06μm below, 1.05μm below, 1.04μm below, 1.03μm below, 1.02μm below, 1.01μm below, 1.0μm below, 0. 99μm or less, 0.98μm or less, 0.97μm or less, 0.96μm or less, 0.95μm or less, 0.94μm or less, 0.93μm or less, 0.92μm or less, 0.91μm or less, 0.90μm or less, 0.89μm or less, 0.88μm or less, 0.87μm or less, 0.86μm or less, 0.85μm or less, 0.84μm or less, 0.83μm or less or 0.82μm.

[0067] After peeling the outer layer of the battery pouch film and the barrier layer, when the surface roughness Ra of the barrier layer side is greater than 1.5 μm, it can be confirmed through the following experimental example that after forming 12 mm, the residual aluminum thickness at the edge portion becomes lower and the formability becomes worse.

[0068] As described above, the surface roughness of the barrier layer side can be adjusted through the following preparation process. In particular, when performing the 1P3C process, it is necessary to consider whether the drying temperature of the drying chamber after the double-sided surface treatment is additionally performed and / or the lamination of polyamide and PET, whether it is affected by the MD and TD elastic modulus of polyamide / PET, etc.

[0069] In an exemplary implementation example, preferably, in the battery pouch film, the elastic modulus of the outer layer formed by laminating polyamide and PET is less than or equal to 2450 in the MD direction and less than or equal to 2400 in the TD direction.

[0070] The evaluation method of the elastic modulus in the MD direction and the TD direction is as follows.

[0071] That is, after the above-mentioned battery bag film is prepared into 150mm×1.5mm (preparing two MD test pieces and TD test pieces) by a test piece cutting machine, Ny / PET is manually peeled off from the bag. Next, the elastic modulus is evaluated using a universal testing machine UTM. The elastic modulus evaluation conditions are speed: 50mm / min, gap (Grip gap): 50mm, room temperature 25℃, and humidity 30%. The elastic modulus evaluation is calculated using the slope of the elastic modulus interval in the SS curve (Curve).

[0072] In a non-limiting example, the elastic modulus in the MD direction of the outer layer formed by laminating polyamide and PET may be 2450 or less, 2400 or less, 2350 or less, 2300 or less, 2250 or less, 2200 or less, 2150 or less, 2100 or less, or 2050 or less. Alternatively, it may be 2000 or more, 2050 or more, 2100 or more, 2150 or more, 2200 or more, 2250 or more, 2300 or more, 2350 or more, or 2400 or more. When the elastic modulus in the MD direction is lower than the above range, the resistance to external impact is reduced.

[0073] When the elastic modulus of the outer layer formed by laminating polyamide and PET is greater than 2450 in the MD direction, it was confirmed from the following experimental examples that the moldability is deteriorated.

[0074] In a non-limiting example, the TD elastic modulus of the outer layer formed by laminating polyamide and PET may be 2400 or less, 2350 or less, 2300 or less, 2250 or less, 2200 or less, 2150 or less, 2100 or less, or 2050 or less. Alternatively, it may be 2000 or more, 2050 or more, 2100 or more, 2150 or more, 2200 or more, 2250 or more, 2300 or more, or 2350 or more. When the TD elastic modulus is lower than the above range, the resistance to external impact is reduced.

[0075] When the TD elastic modulus of the outer layer formed by laminating polyamide and PET is greater than 2400, it was confirmed from the following experimental examples that the moldability becomes poor.

[0076] The MD direction elastic modulus and TD direction elastic modulus of the outer layer formed by bonding polyamide and PET can also be adjusted through the preparation process, even if the same material is used. In particular, when performing the 1P3C process, it is necessary to consider whether the drying temperature of the drying chamber after additional double-sided surface treatment and / or the bonding of polyamide and PET, whether it is affected by the bonding of polyamide / PET, etc.

[0077] In an exemplary implementation example, the residual thickness of the metal layer at the edge of the battery pouch film (the thickness of the metal layer before molding is 60 μm) measured by the following method can be greater than 34 μm, greater than 34.5 μm, greater than 35 μm, greater than 35.5 μm, greater than 36 μm, greater than 36.5 μm, greater than 37 μm, greater than 37.5 μm, greater than 38 μm, greater than 38.5 μm, greater than 39 μm, or greater than 39.5 μm, for example, can be 34 to 40 μm.

[0078] [Measurement of thickness of residual metal layer at edge]

[0079] A 240 mm (MD) × 266 mm (TD) battery bag film was formed by a chromium (Cr) coated cup forming machine. After forming 12 mm, the edge portion was cut by a cross-section cutting machine and the maximum thickness of the metal layer cross section in the bag film was measured by SEM, that is, the residual thickness was measured. The thickness of the metal layer in the bag film before forming was 60 μm.

[0080] In an exemplary implementation example, the maximum molding depth of the battery pouch film measured according to the following method can be greater than 16 mm, greater than 16.5 mm, greater than 17 mm, greater than 17.5 mm, greater than 18 mm, greater than 18.5 mm, greater than 19 mm, greater than 19.5 mm, greater than 20 mm, greater than 20.5 mm, greater than 21 mm, greater than 21.5 mm or 22 mm.

[0081] [Moldability measurement]

[0082] The formability of a battery pouch film of 240 mm (MD) x 266 mm (TD) was measured by a cup forming machine coated with chromium (Cr).

[0083] The maximum molding depth without cracks was evaluated by measuring 10 times. During molding, the pressure was fixed at 0.3MPa, and the R value (corner curve radius value) of the molding machine was 4R (4mm). The molding size during molding was 90mm×120mm in the horizontal direction, and single molding was performed.

[0084] On the other hand, refer to Figure 1For illustration, an exemplary implementation example of the present invention may include: a sealing layer 500; an inner surface adhesive layer 400, laminated on the sealing layer 500; a barrier layer 300, laminated on the inner surface adhesive layer 400; an outer surface adhesive layer 200, laminated on the barrier layer 300; and an outer layer 100, formed on the outer surface adhesive layer 200.

[0085] In an exemplary implementation example, the outer layer 100 of the battery bag film may be polyamide, PET (polyethylene terephthalate), PBT (polybutylene terephthalate), etc. Preferably, it may be a mixed layer of polyamide and PET (a laminated film of polyamide and PET).

[0086] In an exemplary implementation example, considering the formability, the thickness of the polyamide film in the outer layer 100 is preferably 20 μm or more, more preferably 25 μm or more, but when the thickness of the polyamide film is greater than 30 μm, the insulation breakdown voltage may be reduced. Therefore, preferably, the thickness of the polyamide film is 20 μm to 30 μm, more preferably, 25 μm to 30 μm. When the polyamide film is less than 20 μm, the formability may become poor.

[0087] In an exemplary implementation example, the thickness of the PET film in the outer layer 100 is relatively thin, and the thicker the polyamide film is, the more favorable the moldability is. However, the thinner the PET film is, the more disadvantageous it may be in terms of insulation breakdown voltage. Therefore, considering this point, the PET film is preferably 7μm to 12μm.

[0088] In an exemplary implementation example, a PET film having an MD elongation and a TD elongation of 90% to 110%, 95% to 105%, or 100% can be used. The above-mentioned polyamide film having an MD elongation of 100% to 200%, 110% to 150%, or 110% to 125% and a TD elongation of 70% to 200%, 70% to 150%, or 74% to 138% can be used. For example, when the MD elongation is about 125%, a polyamide film having a TD elongation of about 75% can be used, or, when the MD elongation is about 110%, a polyamide film having a TD elongation of about 138% can be used.

[0089] In an exemplary implementation example, the sealing layer 500 may include a hot adhesive resin, that is, a sealing resin for thermal bonding. Specifically, the sealing layer may include one or more selected from the group consisting of polyolefins such as polypropylene (PP), polyethylene (PE), copolymers, terpolymers or derivatives thereof, and ethylene vinyl acetate (EVA). The copolymers (Co-polymer) or terpolymers (ter-polymer) may include ethylene / propylene copolymers or terpolymers of ethylene / propylene / butadiene, etc. As an embodiment, the sealing layer may have a thickness of 20μm to 100μm or 20μm to 80μm. The sealing layer may be multilayer. For example, the thickness of the polypropylene (CPP) layer as the sealing layer 500 may be 20μm to 80μm.

[0090] As an embodiment, the sealing layer 500 is a polypropylene layer (PP), for example, a non-stretched polypropylene (CPP) film, and the corresponding polypropylene (PP) layer and the barrier layer can be bonded by an adhesive coating layer and / or an extrusion coating (EC) layer of polypropylene resin. In addition, the sealing layer 500 itself can also be formed by extrusion. The polypropylene layer (PP) can contain various additives (rubber, elastomer, lubricant, etc.) according to the required physical properties.

[0091] In an exemplary implementation, the outer surface bonding layer 200 is an adhesive layer for bonding the barrier layer 300 and the outer layer 100 .

[0092] In an exemplary implementation, the outer surface adhesive layer 200 may include one or more of epoxy adhesive, polyurethane adhesive, phenol resin adhesive, polyolefin adhesive, and polyester adhesive. As an embodiment, the outer surface adhesive may have a thickness of 0.5 μm to 10 μm.

[0093] In an exemplary implementation, the inner surface adhesive layer 400 may be an adhesive coating layer or an extrusion coating layer for bonding the barrier layer 300 and the sealing layer 500. Alternatively, as another embodiment, the inner surface adhesive layer may include an adhesive coating layer and an extrusion coating layer.

[0094] The inner surface adhesive layer 400 may include one or more of an epoxy adhesive, a polyurethane adhesive, a phenol resin adhesive, a polyolefin adhesive, and a polyester adhesive. As an embodiment, the inner surface adhesive layer 400 may have a thickness of 0.5 μm to 10 μm. In an embodiment, the extruded resin layer may provide the bag with flexibility, adhesion, insulation, etc. As an embodiment, the extrusion coating layer may include an olefin resin such as a polypropylene resin. As an embodiment, the extrusion coating layer may have a thickness of about 5 μm to 80 μm.

[0095] In an exemplary implementation, the barrier layer 300 may include a metal layer or a surface treatment layer uniformly coated on both sides of the metal layer, and the metal layer may be a metal film or a metal vapor-deposited layer. For example, the metal film may be a metal foil. The metal vapor-deposited layer may be made by vacuum evaporation on a separate plastic film, such as a film of polyethylene terephthalate (PET), polyethylene (PE) or polypropylene (PP).

[0096] As an implementation example, there is no limitation on the metal of the metal layer, as long as it has the above-mentioned barrier properties. For example, it can be one or more metals selected from the group consisting of aluminum (Al), iron (Fe), copper (Cu), nickel (Ni), tin (Sn), zinc (Zn), indium (In) and tungsten (W) (single metal or a mixture of single metals) or two or more alloys selected therefrom. Specifically, the metal may include one or more metals selected from the group consisting of aluminum or aluminum alloys, titanium or peptide alloys, tungsten or tungsten alloys, molybdenum or molybdenum alloys, copper or copper alloys and stainless steel. More specifically, it may include aluminum. As an embodiment, in order to provide corrosion resistance to the metal, the surface treatment layer may be a layer whose surface is treated with phosphoric acid, chromium, zirconium, cerium, lanthanum, scandium, yttrium, etc.

[0097] As an implementation example, the barrier layer 300 may have a thickness of 20 μm to 80 μm. When the thickness of the barrier layer is less than 20 μm, pinholes, fine cracks, etc. may be generated during the molding process, and therefore, it is difficult to ensure safety. When the thickness of the barrier layer is greater than 80 μm, the energy density may be reduced during the battery preparation process.

[0098] In an exemplary implementation example, for example, the total thickness of the battery pouch film may be 60 μm to 185 μm. In one embodiment, the battery pouch film may be greater than 153 μm or less than 113 μm.

[0099] On the other hand, an exemplary implementation example of the present invention provides a method for preparing an adhesive battery pouch film, which is used to prepare the above-mentioned battery pouch film, and the above-mentioned method includes: a two-side surface treatment step, surface treating both sides of the metal fabric contained in the barrier layer; a step of drying the above-mentioned metal fabric that has been surface-treated on both sides; an outer surface adhesive layer coating step, applying an adhesive to one side of the above-mentioned surface-treated metal fabric to form an outer surface adhesive layer; and an outer layer laminating step, laminating an outer layer fabric to the upper part of the above-mentioned outer surface adhesive layer, and after the above-mentioned two-side surface treatment, the drying temperature of the metal fabric is above 160°C.

[0100] In connection with this, generally, the prior art includes: i) a step of applying and drying a surface treatment layer to one side of the metal layer, applying another surface treatment layer to the other side of the metal layer through a first winding step and drying, and then performing a second winding; ii) a step of forming an outer surface adhesive layer on one side of the surface-treated metal layer and attaching the outer layer to dry, and then performing a third winding; and iii) a step of forming an inner surface adhesive layer on the other side of the surface-treated metal layer and attaching the sealing layer to dry. When the above-mentioned multiple processes are repeatedly performed, not only the probability of operation loss and process defects increases, but also the formability may become poor.

[0101] In this regard, in an exemplary implementation example of the present invention, the existing battery bag film is prepared by a one-pass three-coating (1P3C, 1Pass 3Coating) method in which more than three coating processes are achieved through one operation of the fabric in one online process, rather than a preparation method in which the stacking process of each layer is repeatedly performed in the order of coating, drying and winding. Therefore, not only the problems of the prior art are solved, but also the formability can be improved.

[0102] In an exemplary implementation example, the method may include: a step of laminating polyamide and polyethylene terephthalate (PET) films for the first time; and a step of laminating the laminated polyamide and polyethylene terephthalate (PET) films to a metal layer, preferably aluminum, serving as a barrier layer.

[0103] As described above, after the polyamide (Nylon) film is first laminated to the barrier layer (usually aluminum) in the solvent dry lamination (SDL) process, the polyethylene terephthalate (PET) film is laminated thereon in the second process. In this case, since aluminum as a metal has poor elongation, it is necessary to apply maximum tension to prevent the thermal shrinkage of the polyamide in order to cope with the thermal shrinkage of the polyamide. However, in this case, if the stretched polyamide (Nylon) film becomes a bag, it is in a state where the tensile strength has been increased. As a result, the excellent moldability may be reduced.

[0104] On the contrary, when the 1P3C process is used, in a state where the polyamide film and the PET film are already bonded, if the outer layer formed by bonding the corresponding polyamide film and the PET film is bonded to the barrier layer (so that the polyamide film side is bonded toward the barrier layer), the formability can become better than the above process.

[0105] Furthermore, after the two sides of the metal fabric included in the barrier layer are surface treated, in the case of drying the metal fabric ( Figure 2 In step ⑤ of the present invention, when the drying temperature, that is, the temperature of the drying chamber is 160° C. or higher, the moldability can be further improved.

[0106] In a non-limiting example, the temperature of the drying chamber may be 160° C. to 200° C. Within the corresponding range, the prepared film has no significant difference in the change of physical properties.

[0107] For example, the temperature of the drying chamber may be 160°C or higher, 165°C or higher, 170°C or higher, 175°C or higher, 180°C or higher, 185°C or higher, 190°C or higher, or 200°C or lower, 195°C or lower, 190°C or lower, 185°C or lower, 180°C or lower, 175°C or lower, 170°C or lower, or 165°C or lower. In particular, when the chamber temperature is lower than the above range, not only the surface treatment effect is reduced, but also the physical properties (external layer peel strength, electrolytic resistance, etc.) after the surface treatment are reduced. This tendency is particularly evident when the temperature is below 140°C.

[0108] In an exemplary implementation example, the method may laminate a resin for forming a sealing layer, such as a polypropylene (PP) resin film, to the opposite side during the process of laminating the laminated polyamide and polyethylene terephthalate (PET) film to the barrier layer.

[0109] In an exemplary implementation example, the method may include: a double-sided coating step, in which the two sides of the metal layer serving as a barrier layer are subjected to a first coating and a second coating to perform surface treatment; a coating step, in which an adhesive is applied to the two sides of the surface-treated metal layer and the adhesive is dried; and a laminating step, in which a resin film and an outer layer film (polyamide and PET laminating film) for forming the sealing layer are laminated to the two sides of the metal layer coated with the adhesive and dried.

[0110] In one implementation example, in the above-mentioned two-side surface treatment step, after one side of the metal fabric is surface treated, the other side of the metal fabric is surface treated in turn without performing a drying step. In this case, the above-mentioned two-side surface treatment step can be performed by a two-side double coating device including a first coater and a second coater.

[0111] In one implementation example, the above-mentioned two-side surface treatment steps may include: a first coating execution step, applying a water-based coating liquid and a solvent-based coating liquid to one side of the metal fabric by a combination of direct coating (Direct coating) and reverse kiss coating (RKC); and a second coating execution step, applying a coating liquid to the other side of the metal fabric by RKC and film up / down coating (FiIm up / down coating) methods.

[0112] Specifically, the first coating execution step refers to the first coating of a water-based coating liquid and a solvent-based coating liquid by a combination of direct coating (Direct coating) and reverse kiss coating (RKC, Reverse Kiss Coating), and the physical properties and changes of the coating liquid can be considered. The second coating execution step refers to the second coating of the coating liquid to the other side of the metal fabric by RKC and film up / down coating (FiIm up / down coating). On the other hand, the coating uniformity and working speed can be improved by adjusting the position of the substrate contact surface used to form the outer layer and the coating roller (Coating Roll) and the doctor (Doctor). More specifically, in order to precisely control the above-mentioned coating agent, the viscosity of the coating agent can be adjusted by constructing a chamber method (closed piping), thereby preventing the entry of foreign matter from the source.

[0113] In one implementation example, more specifically, the above-mentioned two-sided surface treatment steps may include: a fabric supply process, in which the wound metal fabric is unwound and supplied; a foreign matter removal process, in which foreign matter on the surface of the supplied metal fabric is removed; a tension adjustment process, in which the tension of the metal fabric to remove surface foreign matter is adjusted; and a double-sided double coating process, in which coating is performed on both sides of the metal fabric while maintaining a specified tension.

[0114] In one implementation example, the foreign matter removal process may include a first foreign matter removal process, in which the two side surfaces of the metal fabric are subjected to discharge treatment to remove oil. Furthermore, the foreign matter removal process may also include a pinhole inspection process, in which pinholes are confirmed to be generated on the two side surfaces of the metal fabric after the oil is removed. Furthermore, the foreign matter removal process may also include a second foreign matter removal process, in which foreign matter is removed from the two side surfaces of the metal fabric after the pinhole inspection by means of a roller.

[0115] Furthermore, the method of an implementation example may further include a physical property stabilization drying step between the above-mentioned two-side surface treatment step and the outer surface adhesive layer coating step, wherein the metal fabric having been surface treated on both sides is dried in a floating manner to stabilize the physical property. According to the above-mentioned floating manner, both sides of the surface treated metal fabric can be dried simultaneously, thereby minimizing the contact between the guide roller and the fabric, thereby significantly reducing the occurrence of appearance running defects such as foreign matter transfer caused by the guide roller and dents on the fabric.

[0116] In one implementation example, the drying step in the method is a step for stabilizing physical properties, and the metal fabric with surface treatment on both sides can be dried by floating. That is, an air floating method can be used to dry the fabric with surface treatment on both sides in a non-contact manner in a floating state. In this way, the metal fabric with coating on both sides can be dried while minimizing the contact with structures such as transfer rollers. Next, it can also include: a cooling step for cooling the dried metal fabric; and a surface inspection step for inspecting the surface of the cooled metal fabric.

[0117] In one implementation example, the step of coating the outer surface bonding layer by coating the adhesive on one side of the surface-treated metal fabric to form the outer surface bonding layer is a process of coating the adhesive on one side of the metal fabric surface-treated by two coatings, which can be performed by a third coating machine, and is prepared for bonding through drying and other processes. After coating the adhesive, the metal fabric coated with the adhesive is dried to form a bonding layer, and then the thickness of the dried bonding layer can be measured and the bonding force can be enhanced by corona treatment of the surface of the bonding layer.

[0118] In one implementation example, after the above-mentioned laminating step, the above-mentioned method may further include an inner surface adhesive layer forming step, forming the inner surface adhesive layer on the other side of the above-mentioned metal fabric that is not laminating the outer layer. And, in one implementation example, after the above-mentioned inner surface adhesive layer forming step, a drying step may be included. In one implementation example, a step of laminating a sealing layer fabric to the lower part of the above-mentioned inner surface adhesive layer may also be included.

[0119] In one implementation example, in order to prevent dents and / or compression of the fabrics used in various steps before the outer layer lamination step, the above method may include two or less winding steps before preparing the final structure of the battery bag.

[0120] Specifically, the final structure of the battery pouch film may be prepared by winding the film twice or less in total, and most preferably, winding the film once in total.

[0121] In one implementation example, the winding step may be performed after the outer layer laminating step. Alternatively, the winding step may be performed after the sealing layer laminating step. Figure 2 is executed in step 10 of .

[0122] In one implementation example, the step of laminating the outer layer fabric to the upper part of the outer surface adhesive layer and the step of laminating the sealing layer fabric to the lower part of the inner surface adhesive layer are respectively used as the process of laminating the functional fabric to one side of the metal fabric coated with the adhesive, and the sealing layer fabric used to stabilize the heat resistance and cold resistance of the battery can be mainly laminating on the inner side, and the outer layer fabric used for heat resistance, pinhole resistance and wear resistance can be laminating on the outer side. In one implementation example, each of the above laminating steps can be used to laminating the outer layer fabric or the sealing fabric prepared in advance.

[0123] In one implementation example, the following steps may be included between the third coating step and the bonding step: an adhesive drying step, in which the metal fabric coated with the adhesive is dried to form an adhesive layer; an adhesive layer thickness measuring step, in which the thickness of the dried adhesive layer is measured; and an adhesive layer surface treatment step, in which the surface of the adhesive layer is subjected to corona treatment to enhance the adhesive force.

[0124] In one implementation example, after the above-mentioned bonding step, a surface inspection step may be further included to inspect the surface of the above-mentioned sealing layer or outer layer.

[0125] In one implementation example, in order to minimize the occurrence of foreign matter and scratches during the transfer of each fabric, a tendency structure that separates the substrate contact roller and the shaft from the guide roller and a shaft structure that operates as an integrated type can be used. The ordinary drive method of the guide roller is to transmit the rotation transmitted by the motor to the shaft-integrated guide roller and drive it at a speed of 1:1, while the tendency drive method is to separate the guide roller and the shaft to compensate for the small rotation speed of the roller, which can be applied to the required range. As an embodiment, a rewinder section and an unwinder section (fabric supply section) can be separately constructed so that they can be operated separately when there is a problem with the operation of the equipment due to equipment problems.

[0126] Furthermore, in one implementation example, in the process of transferring the fabric, in order to minimize the occurrence of foreign matter and scratches, a suction roller can be used in the tension control range, and in order to prevent the appearance defects (dents, scratches, etc.) caused by foreign matter adhering to the roller during operation, a contact cleaning roller for removing foreign matter can be used.

[0127] On the other hand, the exemplary implementation of the present invention may also include a aging step. In the process of preparing the battery bag film, the aging step is a necessary process for improving the reliability of adhesion, electrolyte resistance, peel strength, etc., but because the time required is long, the optimal aging process is particularly important. Preferably, in terms of productivity, only one aging process is performed for the final structure of the battery bag film to prepare the product. Specifically, the above method may include two or less aging steps. More specifically, the above method may not perform the aging step after the above two-sided surface treatment step and apply the adhesive to one side of the surface-treated metal fabric, and the above aging step may be included after the laminating step of the outer layer and / or the sealing layer. For example, if the aging step includes a two-sided surface treatment step before the above laminating step, as the film is exposed to the air for more than a specified time during the preparation process, the unlaminated surface treatment agent may fall off. For example, if the adhesive layer formation step includes a aging step, as the adhesive layer undergoes a partial reaction, the above adhesive layer may adhere to other layers.

[0128] On the other hand, the battery bag film preparation device provided by the exemplary implementation example of the present invention includes: a two-sided surface treatment device, including a first coater 3 and a second coater 4, for surface treating both sides of the metal fabric used to form a barrier layer; a third coater 7, for applying an adhesive to one side of the surface-treated metal fabric; and a bonding part 9, for bonding a functional fabric to one side of the adhesive layer. Figure 2 Schematic diagram of a battery bag film preparation device according to an embodiment of the present invention.

[0129] In one implementation example, the two-sided surface treatment device may include a fabric supply unit 1, a foreign matter removal device 2, a tension adjustment unit, a first coating machine 3, and a second coating machine 4. The fabric supply unit 1 is used to unwind and supply the wound metal fabric. The foreign matter removal device 2 is used to remove foreign matter on the surface of the supplied metal fabric. The tension adjustment unit is used to adjust the tension of the metal fabric from which the foreign matter is removed. The first coating machine 3 and the second coating machine 4 are used to coat both sides of the metal fabric while maintaining a specified tension.

[0130] In one implementation example, the foreign matter removal device 2 may include a first foreign matter removal unit for performing discharge treatment on both sides of the metal fabric to remove oil. In addition, it may also include a pinhole inspection unit for confirming whether pinholes are generated on both sides of the metal fabric after the oil is removed. It may also include a second foreign matter removal unit for removing foreign matter from both sides of the metal fabric by rollers when the confirmation result is normal.

[0131] In one implementation example, a physical property stabilization drying section 5 may be formed between the above-mentioned two-sided surface treatment device and the third coater 7, and the metal fabric coated on both sides is dried by floating to stabilize the physical properties. In this case, the air floating method can be used as a drying method to dry the coated substrate in a non-contact manner in a floating state. In this way, the metal fabric coated on both sides can be dried while minimizing the contact with structures such as transfer rollers. Then, after the dried metal fabric is cooled by the cooling section 6, the surface of the cooled metal fabric can be inspected by the surface inspection section.

[0132] In one implementation example, the third coating machine 7 and the laminating unit 9 may further include: an adhesive drying unit 8 for drying the metal fabric coated with the adhesive to form an adhesive layer; an adhesive layer measuring unit for measuring the thickness of the dried adhesive layer; and an adhesive layer surface treatment unit for performing corona treatment on the surface of the adhesive layer to enhance the adhesive force.

[0133] In an implementation example, in addition to the laminating portion 9, a surface inspection portion may also be included to inspect the surfaces of the sealing layer and the outer layer.

[0134] According to one implementation example, the battery bag film can be made of Figure 2 In one embodiment, the preparation device can be used according to the requirements. Figure 2 Between the laminating section 9 and the final winding section (End, 2nd Re-wind), a fourth coater (not shown) for applying adhesive to the other side of the surface-treated metal fabric, a drying section (not shown), a functional fabric (outer layer, sealing layer) laminating section (not shown), an extrusion section (including co-extrusion) (not shown), etc. are added.

[0135] On the other hand, the exemplary implementation of the present invention provides a secondary battery with the battery pouch film externally mounted thereon. Typically, the secondary battery may be a lithium secondary battery, and in particular, may be a large or medium-sized secondary battery for an electric vehicle (EV) or an energy storage system (ESS).

[0136] Furthermore, the secondary battery preparation method provided by the exemplary implementation example of the present invention includes the step of placing the above-mentioned battery pouch film on the outside of the secondary battery.

[0137] The following further describes the exemplary implementation examples of the present invention in detail with reference to the embodiments. The embodiments disclosed in this specification are for illustration only, and the present invention can be implemented through various implementation methods and should not be construed as being limited to the embodiments described in this specification.

[0138] [Experimental methods]

[0139] <Preparation of Examples and Comparative Examples>

[0140] The bag film of the embodiment and the comparative example is composed of an outer layer, a barrier layer, and a sealant layer. The outer layer is a laminated film of a polyethylene terephthalate (PET) film (thickness 12 μm) on the outermost side and a polyamide (Ny) film (thickness 25 μm) on the inner side. Aluminum (thickness 60 μm) is used as a barrier layer, and a polypropylene layer (thickness 80 μm) is used as a sealant layer. The total thickness including the thickness of the adhesive layer is 183 μm.

[0141] In addition to the method of bonding the outer layer and the drying process after the surface treatment on both sides ( Figure 2 The bag films of the examples and comparative examples were prepared in the same manner except that the drying chamber temperature in ⑤) was as shown in the following [Table 1].

[0142] First, a bag film of a comparative example is prepared, and the outer layer and the metal layer are bonded by a solvent dry lamination (SDL) method. Specifically, after applying a surface treatment agent to both sides of the aluminum layer as the metal layer, the polyamide as the outer layer is bonded for the first time, and then the PET is bonded on top of it for the second time. After the surface treatment, it is dried at a temperature of more than 140 degrees and less than 150 degrees. Next, the polypropylene (PP) layer as the inner layer (sealing layer) is extruded to prepare the bag film. In this process, since polyamide is easily thermally shrunk on aluminum as a hard metal, it is necessary to apply maximum tension to bond to prevent the polyamide from thermally shrinking.

[0143] On the other hand, the bag film of the example was prepared by laminating the laminated polyamide film and PET film to aluminum at one time (laminated with the polyamide film facing the aluminum), and then extruding and laminating the polypropylene (PP) layer as the inner layer (sealant layer) to the opposite side. After surface treatment, it was dried at a temperature of 160 degrees or more.

[0144] Table 1

[0145]

[0146] Each bag film was prepared to be 240 mm (MD) x 266 mm (TD).

[0147] In Examples and Comparative Examples, the peeling and barrier layer side peeling surface roughness, the aluminum residual thickness at the edge portion, and the maximum molding depth for the moldability evaluation were evaluated as follows.

[0148] <Execute Stripping>

[0149] After immersing a 2.5 cm (TD) × 15 cm (MD) bag film in a container filled with electrolyte and sealing it, the corresponding sealed container was placed in an oven at 85°C for 1 day, and then the bag film immersed in the corresponding electrolyte was taken out and cut into a size of 1.5 cm (TD) × 15 cm (MD) to prepare a sample.

[0150] In order to avoid damage to the barrier layer, only the outer layer was weakly cut, and the metal layer and the peeled sealing layer were peeled off by pulling using a universal testing machine (UTM), and then the corresponding sample was flatly adhered to a glass slide using double-sided tape. Then, the universal testing machine (UTM) was used again, with the metal layer and the peeled sealing layer at 180 degrees, and the two ends of the corresponding sample were held and peeled off by pulling for more than 30 mm (speed 50 mm / min).

[0151] <Measurement of surface roughness>

[0152] The metal (aluminum) layer side of the peeled sealant layer was cut into 1×1 cm 2 Size, use double-sided tape to stick it flat on the slide.

[0153] A surface roughness measurement device (NV-22003D profiler, a product of Nano system) was used to take a photograph of the surface curvature, and Ra in the histogram column was measured based on the acquired data using an analysis program (NanoMap, a product of Nano system).

[0154] <Measurement of elastic modulus of outer layer (polyamide / PET)>

[0155] After the battery bag film is prepared into 150mm×1.5mm by a test piece cutting machine (preparing two MD test pieces and TD test pieces), Ny / PET is manually peeled off from the bag. Next, the elastic modulus is evaluated using a universal testing machine UTM. The elastic modulus evaluation conditions are speed: 50mm / min, gap (Gripgap): 50mm, room temperature 25℃, and humidity 30%. The elastic modulus evaluation is calculated using the slope of the elastic modulus interval in the SS curve (Curve).

[0156] <Measurement of Formability and Aluminum Residual Thickness at the Edge after Forming>

[0157] The moldability and the aluminum residual thickness at the edge of the battery pouch film of 240 mm (MD)×266 mm (TD) were evaluated by a cup molding machine coated with chromium (Cr).

[0158] The results of 10 moldings were measured, and perfect molding without cracks in all 10 times was evaluated as the maximum molding depth. During molding, the pressure was fixed at 0.3MPa, and the R value (corner curvature radius value) of the molding machine was 4R (4mm). The molding size during molding was 90mm×120mm in the horizontal direction, and single molding was performed.

[0159] In order to evaluate the residual thickness of aluminum in the edge after molding, after molding 12 mm, the edge was cut by a cross-section cutter and the cross section of aluminum in the bag film was evaluated by SEM, and then the thickness of aluminum (maximum thickness, residual thickness after molding) was measured. As described above, the residual thickness of aluminum in the edge bag film (thickness after molding) is measured because the residual thickness of the barrier layer after molding greatly affects the moldability.

[0160] The evaluation results of the peeling surface roughness Ra, outer layer elastic modulus (polyamide / PET elastic modulus), edge aluminum residual thickness (unit: μm), and formability (unit: mm) of the bag films of the examples and comparative examples are shown in the following [Tables 2] to [Table 5], respectively.

[0161] Table 2

[0162]

[0163] Table 3

[0164]

[0165] Table 4

[0166]

[0167] Table 5

[0168]

[0169] As shown above, unlike the comparative example in which the peeling surface roughness Ra of the barrier layer side after peeling the outer layer and the barrier layer is greater than 1.5 μm, it can be seen that the residual aluminum thickness at the edge after forming in the embodiment with a surface roughness Ra of less than 1.5 μm is larger and the formability is better.

[0170] Furthermore, it can be seen that the aluminum residual thickness at the edge after molding is greater and better in the case where the MD direction elasticity of the outer layer of the laminated polyamide and PET is less than 2450 and the TD direction elasticity of the outer layer of the laminated polyamide and PET is less than 2400.

[0171] Although the non-limiting implementation examples and illustrative implementation examples of the present invention are described above, the technical concept of the present invention is not limited to the drawings or the above description. It is obvious that a person skilled in the art of the present invention can make various modifications to the implementation without departing from the technical concept of the present invention, and such modified implementations also fall within the scope of the protection claimed by the present invention.

Claims

1. A battery bag film, characterized in that: At least an outer layer, a barrier layer, and a sealing layer are stacked in sequence. After the outer layer and the barrier layer of the battery pouch film were peeled off, the surface roughness Ra of the peeled surface on the barrier layer side was 1.5 μm or less.

2. A battery bag film, characterized in that: At least an outer layer, a barrier layer, and a sealing layer are stacked in sequence. The outer layer is formed by laminating polyamide and polyethylene terephthalate (PET), and the elastic modulus of the outer layer in the longitudinal direction (MD direction) is less than 2450, and the elastic modulus in the transverse direction (TD direction) is less than 2400.

3. The battery pouch film according to claim 1 or 2, characterized in that: The thickness of the barrier layer before molding is 60 μm. The residual thickness of the metal layer at the edge of the battery pouch film measured by the following method is 34 μm or more. Determination of residual thickness of metal layer at edge: A battery pouch film of 240 mm (MD) × 266 mm (TD) was formed by a forming machine. After 12 mm was formed, the edge portion was cut by a cross-section cutting machine and the maximum thickness of the metal layer cross section in the battery pouch film was measured by a scanning electron microscope (SEM).

4. The battery pouch film according to claim 3, characterized in that: The maximum forming depth of the battery bag film measured by the following method is more than 16mm. Formability determination: The battery bag film was prepared into a test piece of 240 mm (MD) × 266 mm (TD), and the moldability was evaluated by a molding machine. The molding results were measured 10 times, and the molding without cracks in all 10 times was evaluated as the maximum (max) molding depth of the bag.

5. A method for preparing a battery pouch film, used for preparing the battery pouch film according to claim 1 or 2, characterized in that: include: A two-side surface treatment step, performing surface treatment on both sides of the metal fabric included in the barrier layer; A drying step, drying the metal fabric after surface treatment on both sides; an outer surface adhesive layer coating step, coating an adhesive onto one side of the surface-treated metal fabric to form an outer surface adhesive layer; and The outer layer laminating step is to laminat the outer layer fabric on the upper part of the outer surface adhesive layer. After the above two-side surface treatment, the drying temperature of the metal fabric is above 160°C.

6. The method for preparing a battery bag film according to claim 5, characterized in that: The method further comprises the following steps: after preferentially laminating the polyamide and polyethylene terephthalate (PET) films, laminating the polyamide and polyethylene terephthalate (PET) films on the barrier layer.

7. The method for preparing a battery bag film according to claim 5, characterized in that: In the above-mentioned two-side surface treatment step, after one side of the metal fabric is surface treated, the other side of the metal fabric is surface treated in turn without performing a drying step.

8. The method for preparing a battery bag film according to claim 5, characterized in that: The drying step dries the metal fabric whose two sides have been surface-treated by floating method.

9. The method for preparing a battery bag film according to claim 5, characterized in that: The above-mentioned two-side surface treatment steps include: The first coating execution step is to apply a water-based coating liquid and a solvent-based coating liquid to one side of the metal surface by a combination of direct coating and reverse contact coating (RKC); and The second coating execution step is to apply the coating liquid to the other side of the metal fabric by RKC and film upper and lower coating methods.

10. The method for preparing a battery bag film according to claim 5, characterized in that: The above methods include: After the outer layer laminating step, a first winding step is performed; After the first winding, a step of forming an inner surface bonding layer on the other side of the surface-treated metal fabric not bonded to the outer layer; The step of attaching a sealing layer fabric to the lower part of the inner surface adhesive layer; and After the sealing layer fabric is attached, a second winding step is performed.

11. A secondary battery, characterized in that: The battery pouch film according to claim 1 or 2 is used for outer packaging.

12. A method for preparing a secondary battery, characterized in that: The method comprises the step of outer packaging a secondary battery with the battery pouch film according to claim 1 or 2.

Citation Information

Patent Citations

  • Cell pouch having excellent formability

    CN108075052A

  • Battery packaging material, method for manufacturing same, and battery

    CN108886115A

  • Battery packaging material, manufacturing method therefor, battery, and aluminum alloy foil

    CN111108621A

  • Primer layer composition, secondary battery pouch film using same, and method for preparing same

    CN114132036A

  • Cell pouch with high chemical resistance and moldability

    KR1020180057926A