Local micro-processing technology for cover plate glass
By optimizing the printing and cutting steps in the local micro-processing process of the cover glass, the problems of jagged edges, wavy lines and cutting offsets in the acid-resistant ink printing are solved, and high-precision local micro-processing of the cover glass is achieved, eliminating the need for acid protection. The film process also solves the problem of acid feeding into the film.
Patent Information
- Application Number
- CN202411207379.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2024-10-15
AI Technical Summary
In the existing cover glass thinning process, acid-resistant ink printing has serious jagged and wavy edges on the target, causing the cutting size to deviate and the accuracy cannot be guaranteed. In addition, the use of acid-proof film will lead to the problem of acid entering the film.
A local micro-processing process for the cover glass is used, including black target printing on the non-convex thinned surface, two acid-resistant ink printing, sealing and subsequent cutting. By optimizing the screen parameters and printing parameters, the target is accurately captured and Cutting accuracy.
The printing accuracy of acid-resistant ink is controlled at ±0.3mm, the cutting size is controlled at ±0.1mm, and the cutting offset is controlled at ±0.05mm. This eliminates the need for the acid-resistant film process, solves the problem of covering the film with acid, and improves the overall Craftsmanship precision and practicality.
Smart Images

Figure CN118769742A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of cover glass, and in particular to a local micro-processing process of cover glass. Background Art
[0002] With the rapid development of the touch screen industry, mobile phone cover plates are also constantly being updated. The material of the cover plate has been upgraded to glass, and the surface is required to have different patterns, hollows, bosses, etc., and the requirements for the local thinning process of the boss appearance are also constantly upgraded, and the corresponding process route is upgraded and improved. The requirements for product precision are getting higher and higher. In the cover glass thinning process, in order to produce a specific boss shape, a single large plate glass needs to use acid-proof film, acid-resistant ink, and HF acid solution. In order to protect the glass area from HF acid etching and thinning, the non-ink area is in contact with HF acid for a long time and is etched a certain amount and thinned to obtain the required appearance shape. However, the large plate thinning process will etch and deform the printed acid-resistant ink target, and the cutting cannot grasp the target, resulting in the offset of the cutting size; and because the acid-resistant ink uses a low-mesh screen, the amount of ink is large, the edge of the printed target is serrated and wavy, and the secondary printing is not easy to grasp. If the screen printing is used to position the printing side, it is easy to cause the size to deviate and the accuracy cannot be guaranteed. Therefore, it is necessary to propose an improvement measure to solve the above technical problems. Summary of the invention
[0003] The present invention provides a local micro-processing process for cover glass, which is used to solve the technical problems raised in the above background technology.
[0004] In order to achieve the above object, the present invention adopts the following technical solution: a local micro-processing process of cover glass, comprising the following steps: S1, black target printing on non-convex thinning surface; S2, first printing of acid-resistant ink on the thinned surface; S3, second printing of thinned surface acid-resistant ink; S4, place the black ink face to face and seal it; S5. Finally, thinning is performed, followed by cleaning and cutting, and the rest of the subsequent processes are performed.
[0005] Preferably, in step S1, when the first black ink is printed, the printing is performed in an edge positioning manner; 1mm*1mm square targets are generated around the large plate, and the distance between the targets and the edge of the glass is greater than 6mm.
[0006] Preferably, in step S1, the screen parameters used for the first black ink are as follows: polyester mesh 250 mesh-350 mesh, wire diameter 27um-30um, screen making tension 22±2N, screen film thickness 8um-12um, angle 22.5°-30°, double exposure method, machine printing plate spacing 3mm-4.2mm, plate lifting 8mm-12mm, scraper selection 80°, pressure 18mm-22mm, scraper pressure 20N-23N, scraping speed 100-250mm / sec.
[0007] Preferably, in step S1, the black ink is mixed in a ratio of main agent: curing agent: diluent = 100:10-12:15-16, and after mixing and stirring, it is allowed to stand for 10 minutes before use. A single ink mix can be used within 4 hours, and the screen needs to be cleaned and re-mixed if the time is exceeded; and the ink baking parameters are 100℃*10min.
[0008] Preferably, in step S2, the second acid-resistant ink printing grabs the first black ink target for precise printing, the second acid-resistant ink is printed on the thinned surface, a 0.3mm*0.3mm target is superimposed in the middle of the first target, and the target is designed to be 0.35mm away from the edge of the first target.
[0009] Preferably, in step S3, the third acid-resistant ink printing still grabs the first black ink target for printing, and is superimposed on the first acid-resistant ink. The target is designed to be 0.35 mm away from the edge of the first target and overlap with the second target; if it exceeds the overlapping part of the second target, it can also be <0.35 mm away from the edge of the first square target.
[0010] Preferably, 1%-1.5% of a slow-drying agent can be added to the acid-resistant ink before printing; the acid-resistant ink baking parameters in step S2 are 150°C*10min, the acid-resistant ink uses a 325-mesh steel screen, a wire diameter of 23um-30um, a tension of 26N-32N, a film thickness of 10um-12um, a screen angle of 45°, and the printing parameters of the matching equipment are a plate lift of 8mm-10mm, a downward pressure of 18mm-20mm, a scraper pressure of 20N-25N, a plate spacing of 4.0mm-4.3mm, and a scraping speed of 100-150mm / sec; the scraping angle is 75°.
[0011] Preferably, the acid-resistant ink screen in step S3 uses a 180-mesh polyester screen without change, and the acid-resistant ink curing time is 150-160° C.*20-30 min.
[0012] Preferably, the production parameters of 180 mesh screen are: wire diameter 55um, film thickness 24um-30um, tension 26N-28N, angle 22.5°, printing parameters lifting 10mm-12mm, pressing amount 18mm-22mm, scraper pressure 20N-25N, plate spacing 4.0mm-4.3mm, scraping speed 60-80mm / sec, and scraping glue selection 75°.
[0013] Preferably, in step S4, the sealing process is to stack two sheets of glass and place a piece of paper in the middle, with the distance between the paper and the edge of the glass being >10cm-15cm. The glue is UV acid-resistant red glue, and a sealing gun is used to apply the glue around the edges, and check for bubbles and missing parts; if there are no abnormalities, the glass is transferred to a UV furnace for curing, with a curing energy of 1800-2200mj and a transmission speed of 3.0±0.5m / min.
[0014] Compared with the prior art, the present invention has the following beneficial effects: The present invention optimizes the design of the local micro-processing process steps of the cover glass, optimizes and strictly controls the relevant parameters of each process step, and after adopting the micro-processing process of the present invention, the printing and cutting targets can be normally grasped; and the printing accuracy of the acid-resistant ink can be controlled within ±0.3mm, the cutting size can be controlled within ±0.1mm, and the cutting offset can be controlled within ±0.05mm; in addition, the micro-processing process of the present invention omits the acid-proof film process, and the sealing solves the acid ingress problem generated by the coating. The overall design is ingenious and the precision is high, which effectively ensures the normal progress of subsequent thinning, cutting and other processes, and has strong practicality. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] Figure 1 It is a schematic diagram of a square target printed on a non-acid-resistant ink surface of the present invention; Figure 2 It is a schematic diagram of the acid-resistant ink screen and the square target in step S2 of the present invention; Figure 3 It is a schematic diagram of the acid-resistant ink screen and the square target in step S3 of the present invention; Figure 4 This is a schematic diagram of the finished product effect after three layers of ink printing of the present invention; Figure 5 It is a schematic diagram of face-to-face bonding in step S4 of the present invention. DETAILED DESCRIPTION
[0016] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0017] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features. In the description of the present invention, the meaning of "plurality" is two or more, unless otherwise clearly and specifically defined.
[0018] In the present invention, unless otherwise clearly specified and limited, the terms "installed", "connected", "connected", "fixed", "provided with", etc. should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be indirectly connected through an intermediate medium, or it can be internal communication between two components. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.
[0019] Reference is now made to the accompanying drawings, wherein the purpose of each illustration is only to show certain exemplary embodiments and is not intended to limit the present invention. In each of the drawings, the same reference numerals represent the same or corresponding parts. The dimensions and proportions in each of the drawings are also only for illustration and should not be interpreted as limiting the present invention, and these dimensions may be exaggerated relative to the actual product. Example
[0020] In the original cover glass thinning process, the large plate needs to use 180 mesh polyester screen to print two acid-proof inks + apply acid-proof film for thinning, and then cut after the finished product. The overall process route is roughly: use acid-resistant ink for the first printing, then acid-resistant ink for the second printing, and then apply acid-resistant film on the non-ink surface, and finally thin, clean, tear the film, cut, and carry out the rest of the back-end processes. Because it is printed on white glass and there is no target, when the acid-resistant ink is printed for the second time, the target of the first screen printing of the acid-resistant ink is grabbed. Because a low-mesh screen is used, the edges of the printed square target pattern are severely jagged and wavy, which affects the grabbing and positioning of the target of the second printing of the ink. If the edge positioning method is used, the accuracy cannot reach ±0.3mm, and the offset cannot be guaranteed. Therefore, in the subsequent thinning process, because the size of the printed square target is a square pattern in the range of 1mm*1mm-2mm*2mm, the pattern can be changed as needed, and the target has serious jagged and wavy patterns, which causes the edge acid-resistant ink to fall off to varying degrees, the square is deformed, and the edge of the finished product is irregular. In the subsequent cutting process, due to the deformation of the square pattern, it is impossible to grasp the positioning point normally for the specified route cutting. The use of edge positioning cutting will affect the product accuracy, that is, the cutting size ±0.1mm and the cutting offset accuracy ±0.05mm cannot be achieved.
[0021] Therefore, in order to solve the above technical problems, this embodiment provides a local micro-processing process for cover glass, which specifically includes the following steps: S1, black target printing on non-convex thinning surface; S2, first printing of acid-resistant ink on the thinned surface; S3, second printing of thinned surface acid-resistant ink; S4, place the black ink face to face and seal it; S5. Finally, thinning is performed, followed by cleaning and cutting, and the rest of the subsequent processes are performed.
[0022] like Figure 1-Figure 5 As shown, in step S1, when the first black ink is printed, the edge positioning method is adopted. 1mm*1mm square targets are generated around the large plate, and the pattern can be adjusted. The distance between the target and the edge of the glass is greater than 6mm, ensuring that the targets on the four sides of the large plate fall on the glass.
[0023] In step S1, the screen parameters used for the first black ink are as follows: polyester mesh 250 mesh-350 mesh, wire diameter 27um-30um, screen making tension 22±2N, screen film thickness 8um-12um, angle 22.5°-30°, double exposure method, machine printing plate spacing 3mm-4.2mm, plate lifting 8mm-12mm, scraper selection 80°, pressure 18mm-22mm, scraper pressure 20N-23N, scraping speed 100-250mm / sec.
[0024] In step S1, the black ink is mixed in a ratio of main agent: curing agent: diluent = 100:10-12:15-16. After mixing and stirring, it is allowed to stand for 10 minutes before use. A single ink mix is used within 4 hours. If the time is exceeded, the screen needs to be cleaned and re-mixed. The ink baking parameters are 100℃*10min.
[0025] In step S2, the second acid-resistant ink printing grabs the first black ink target for precise printing, and the second acid-resistant ink is printed on the thinned surface. The 0.3mm*0.3mm target is superimposed in the middle of the first target, and the target is designed to be 0.35mm away from the edge of the first target.
[0026] In step S3, the third acid-resistant ink printing still grabs the first black ink target for printing, and is superimposed on the first acid-resistant ink to ensure that the third ink target is superimposed on the first target, and is the same size as the second target. The target is designed to be 0.35mm away from the edge of the first target and overlap with the second target; if it exceeds the overlapping part of the second target, it is also acceptable if it is less than 0.35mm from the edge of the first square target. The third acid-resistant ink printing still grabs the first black ink target for printing to ensure that the third ink target is superimposed on the first target. In this way, the second and third inks are superimposed, and the edge design distance of the boss graphics of the two is 0.3mm. When using the target grabbing printing method, the printing accuracy can be guaranteed.
[0027] Acid-resistant ink can be added with 1%-1.5% slow-drying agent before printing to ensure printing stability. The baking parameters of acid-resistant ink in step S2 are 150℃*10min, acid-resistant ink uses 325 mesh steel screen, wire diameter 23um-30um, tension 26N-32N, film thickness 10um-12um, screen angle 45°, and matching equipment printing parameters are plate lift 8mm-10mm, downward pressure 18mm-20mm, scraper pressure 20N-25N, plate spacing 4.0mm-4.3mm, scraping speed 100-150mm / sec; scraping glue is selected at 75° to improve the edge jaggedness of the boss pattern and the deformation of the wave pattern during the thinning process.
[0028] The acid-resistant ink screen in step S3 uses a 180-mesh polyester screen without change, and the acid-resistant ink curing time is 150-160°C*20-30min. Among them, the production parameters of the 180-mesh screen are: wire diameter 55um, film thickness 24um-30um, tension 26N-28N, angle 22.5°, printing parameters plate lift 10mm-12mm, pressure 18mm-22mm, scraper pressure 20N-25N, plate spacing 4.0mm-4.3mm, scraping speed 60-80mm / sec, and scraping glue selection 75°.
[0029] In step S4, the sealing process is to stack two sheets of glass and place a piece of paper in the middle. The distance between the paper and the edge of the glass is greater than 10cm-15cm. The glue is UV acid-resistant red glue. The glue is applied around the edges using a sealing gun, and then checked for bubbles and missing parts. If there are no abnormalities, it is transferred to the UV furnace for curing. The curing energy is 1800-2200mj and the transmission speed is 3.0±0.5m / min.
[0030] The present invention optimizes the design of the local micro-processing process steps of the cover glass, optimizes and strictly controls the relevant parameters of each process step, and after adopting the micro-processing process of the present invention, the printing and cutting targets can be normally grasped; and the printing accuracy of the acid-resistant ink can be controlled within ±0.3mm, the cutting size can be controlled within ±0.1mm, and the cutting offset can be controlled within ±0.05mm; in addition, the micro-processing process of the present invention omits the acid-proof film process, and the sealing solves the acid ingress problem generated by the coating. The overall design is ingenious and the precision is high, which effectively ensures the normal progress of subsequent thinning, cutting and other processes.
[0031] The above-described embodiments only express a certain implementation mode of the present invention, and the description thereof is relatively specific and detailed, but it cannot be understood as limiting the patent scope of the present invention. It should be pointed out that, for ordinary technicians in this field, several modifications and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be based on the attached claims.
Claims
1. A local micro-processing process for cover glass, characterized in that: The following steps are involved: S1, black target printing on non-convex thinning surface; S2, first printing of acid-resistant ink on the thinned surface; S3, second printing of thinned surface acid-resistant ink; S4, place the black ink face to face and seal it; S5. Finally, thinning is performed, followed by cleaning and cutting, and the rest of the subsequent processes are performed.
2. The local micro-processing process of cover glass according to claim 1, characterized in that: In step S1, when the first black ink is printed, the edge positioning method is adopted; 1mm*1mm square targets are generated around the large plate, and the distance between the targets and the edge of the glass is greater than 6mm.
3. The local micro-processing process for cover glass according to claim 2, characterized in that: In step S1, the screen parameters used for the first black ink are as follows: polyester mesh 250 mesh-350 mesh, wire diameter 27um-30um, screen making tension 22±2N, screen film thickness 8um-12um, angle 22.5°-30°, double exposure method, machine printing plate spacing 3mm-4.2mm, plate lifting 8mm-12mm, scraper selection 80°, pressure 18mm-22mm, scraper pressure 20N-23N, scraping speed 100-250mm / sec.
4. The local micro-processing process for cover glass according to claim 3, characterized in that: In step S1, the black ink is mixed in a ratio of main agent: curing agent: diluent = 100:10-12:15-16. After mixing and stirring, it is allowed to stand for 10 minutes before use. A single ink mix is used within 4 hours. If the time is exceeded, the screen needs to be cleaned and re-mixed. The ink baking parameters are 100℃*10min.
5. A local micro-processing process for cover glass according to any one of claims 1 to 4, characterized in that: In step S2, the second acid-resistant ink printing grabs the first black ink target for precise printing, and the second acid-resistant ink is printed on the thinned surface. The 0.3mm*0.3mm target is superimposed in the middle of the first target, and the target is designed to be 0.35mm away from the edge of the first target.
6. A local micro-processing process for cover glass according to claim 5, characterized in that: In step S3, the third acid-resistant ink printing still grabs the first black ink target for printing, and is superimposed on the first acid-resistant ink. The target is designed to be 0.35mm away from the edge of the first target and overlap with the second target; if it exceeds the overlapping part of the second target, it is also acceptable if the distance from the edge of the first square target is less than 0.35mm.
7. The local micro-processing process of cover glass according to claim 5, characterized in that: 1%-1.5% slow-drying agent can be added to the acid-resistant ink before printing; the baking parameters of the acid-resistant ink in step S2 are 150℃*10min, the acid-resistant ink uses a 325 mesh steel screen, a wire diameter of 23um-30um, a tension of 26N-32N, a film thickness of 10um-12um, a screen angle of 45°, and the printing parameters of the matching equipment are a plate lift of 8mm-10mm, a downward pressure of 18mm-20mm, a scraper pressure of 20N-25N, a plate spacing of 4.0mm-4.3mm, and a scraping speed of 100-150mm / sec; the scraping glue is selected at 75°.
8. The local micro-processing process of cover glass according to claim 6, characterized in that: The acid-resistant ink screen in step S3 uses a 180-mesh polyester screen without change, and the acid-resistant ink curing time is 150-160° C.*20-30 min.
9. A local micro-processing process for cover glass according to claim 8, characterized in that: The production parameters of 180 mesh screen are: wire diameter 55um, film thickness 24um-30um, tension 26N-28N, angle 22.5°, printing parameters lifting plate 10mm-12mm, pressing amount 18mm-22mm, scraper pressure 20N-25N, plate spacing 4.0mm-4.3mm, scraping speed 60-80mm / sec, scraping glue selection 75°.
10. The local micro-processing process of cover glass according to claim 1, characterized in that: In step S4, the sealing process is to stack two sheets of glass and place a piece of paper in the middle. The distance between the paper and the edge of the glass is greater than 10cm-15cm. The glue is UV acid-resistant red glue. The glue is applied around the edges using a sealing gun, and then checked for bubbles and missing parts. If there are no abnormalities, it is transferred to the UV furnace for curing. The curing energy is 1800-2200mj and the transmission speed is 3.0±0.5m / min.
Citation Information
Patent Citations
Manufacturing method of curved-surface touch screen glass cover plate
CN105528114A
Manufacturing method of white OGS touch screen
CN106598333A
OLED single side thinning method
CN106698958A
Preparation method of glass surface with partial frosted area
CN107414683A
Cover plate glass preparation method
CN114455821A