A method for preparing defective cadmium selenide nanowires

By preparing defective cadmium selenide nanowires through hydrothermal reaction in ethylenediamine solvent, the problems of complex preparation and poor photocatalytic activity of CdSe nanomaterials were solved, and nanowires with controllable morphology and uniform size were realized, exhibiting excellent photocatalytic performance.

CN118771317BActive Publication Date: 2026-11-17GUANGXI UNIV
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411059580.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-04
Publication Date
2026-11-17
Estimated Expiration
2044-08-04

AI Technical Summary

Technical Problem

Existing CdSe nanomaterials have complex preparation processes, high energy consumption, and uneven size, resulting in poor photocatalytic activity, which limits their applications.

Method used

Using ethylenediamine as a solvent and reducing agent, a mixture of selenite and cadmium salt was heated in a hydrothermal reactor to prepare defective cadmium selenide nanowires in one step, avoiding high-temperature treatment. The product was treated with hydrogen peroxide to control defects, resulting in nanowires with controllable morphology and uniform size.

Benefits of technology

The prepared defective cadmium selenide nanowires have controllable morphology and uniform size, and exhibit excellent photocatalytic activity, making them suitable for applications such as photocatalytic water splitting for hydrogen production and degradation of organic pollutants.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118771317B_ABST
    Figure CN118771317B_ABST
Patent Text Reader

Abstract

This invention discloses a method for preparing defective cadmium selenide nanowires, comprising the following steps: S1: Adding 1.7294–2.0515 g of selenite and 2.5647–3.0842 g of cadmium salt to 50–100 ml of ethylenediamine solution, and stirring thoroughly to obtain a mixture; S2: Transferring the mixture obtained in step S1 to a hydrothermal reactor, and placing the hydrothermal reactor in a drying oven for constant temperature reaction at 160–200 °C for 24–48 h, then naturally cooling to room temperature; S3: Centrifuging, washing, and drying the product obtained in step S2 to obtain cadmium selenide nanowires; S4: Adding 0.2 g of the product obtained in step S3 to 20 ml of hydrogen peroxide with a mass concentration of 0.25%–1.25%, ultrasonically vibrating for 2–4 h, centrifuging, washing, and drying to obtain defective cadmium selenide nanowires. The defective cadmium selenide nanowires obtained by the method of this invention have uniform morphology and excellent visible light photocatalytic activity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of inorganic material preparation technology, specifically a method for preparing defective cadmium selenide nanowires. Background Technology

[0002] The increasing severity of fossil fuel shortages and environmental pollution has drawn significant attention, prompting efforts to develop new, pollution-free, and sustainable energy sources. Hydrogen, with its high energy density and environmentally friendly characteristics, shows great potential in replacing fossil fuels. Current hydrogen storage materials primarily include hydrogen-containing compounds (such as NaBH4, hydrazine hydrate, and organic hydrogen-containing compounds) and water, which are the sources of hydrogen. Among these substances, producing hydrogen by splitting water does not emit any greenhouse gases during the conversion process; however, this process requires external energy input. If this external energy source is sustainable, such as solar energy, then hydrogen is naturally considered a green energy source. Furthermore, hydrogen can become the best alternative to fossil fuels for powering equipment. As early as 1972, Fujishima and Honda discovered the photoelectrocatalytic water splitting of n-type semiconductor TiO2 to produce hydrogen. Therefore, solar energy can be used to achieve semiconductor-based photocatalytic hydrogen production, and this strategy has been considered the most effective method for solving the current global energy problem. The key to implementing this strategy is the development of photocatalysts with highly efficient and stable photocatalytic performance.

[0003] CdSe is a typical II-VI group semiconductor material with a band gap of 1.74 eV. Its emission spectrum is relatively narrow, and the microparticles exhibit good photoelectric and catalytic properties, making them widely applicable in technologies such as solar cells, light-emitting diodes, and communication technologies. CdSe nanoparticles also possess a narrow, symmetrically distributed fluorescence spectrum, high fluorescence quantum efficiency, and a wide excitation range. The position of the emission peak varies depending on the particle size, making these microparticles suitable as fluorescent markers for applications in medical detection and bioanalysis.

[0004] In recent years, the study and exploration of semiconductor nanoparticles has attracted widespread interest from researchers both domestically and internationally. Scientists from various countries have tried many methods and have successfully synthesized CdSe nanoparticles, such as organometallic synthesis, solvothermal synthesis, photochemical synthesis, sonicochemical synthesis, and ultrasonic hydrothermal synthesis. Among these methods, solvothermal synthesis has achieved significant breakthroughs. Li Yadong of Tsinghua University attempted to use solvents such as pyridine, benzene, and diethylamine in experiments. These solutions were added to selenium and cadmium powders and heated under hot pressure at 120-200℃ to form various forms of CdSe nanomaterials. With the development of synthesis technology, the application of CdSe nanomaterials in various fields will inevitably be promoted, thus playing an important role in research and replacing currently used fluorescent fuel molecules.

[0005] The aforementioned CdSe nanomaterials suffer from numerous drawbacks, including complex preparation processes and high energy consumption. Furthermore, the resulting CdSe nanomaterials exhibit uneven size and poor photocatalytic activity, significantly limiting their applications. Therefore, a method that simplifies the preparation process, yields uniformly sized CdSe nanowires, and provides superior photocatalytic activity remains to be sought. Summary of the Invention

[0006] The technical problem to be solved by the present invention is to provide a method for preparing defective cadmium selenide nanowires. The method is simple, and the prepared defective cadmium selenide nanowires have controllable morphology, uniform size, and excellent photocatalytic activity.

[0007] The present invention solves the above-mentioned technical problems by means of the following technical solution:

[0008] The method for preparing defective cadmium selenide nanowires according to the present invention includes the following steps:

[0009] S1: Add 1.7294–2.0515 g of selenite and 2.5647–3.0842 g of cadmium salt to 50–100 ml of ethylenediamine solution and stir thoroughly to obtain a mixture for later use;

[0010] S2: Transfer the mixture obtained in step S1 to a hydrothermal reactor, place the hydrothermal reactor in a drying oven and react at a constant temperature of 160-200℃ for 24-48 hours, and then cool naturally to room temperature;

[0011] S3: Centrifuge, wash and dry the product obtained in step S2 to obtain cadmium selenide nanowires.

[0012] S4: Add 0.2g of the product obtained in step S3 to 20ml of hydrogen peroxide with a mass concentration of 0.25% to 1.25%, sonicate for 2 to 4 hours, centrifuge, wash and dry to obtain defective cadmium selenide nanowires.

[0013] The cadmium salt mentioned in step S1 of this invention is cadmium sulfate or cadmium nitrate.

[0014] The selenite in step S1 of this invention is sodium selenite or potassium selenite.

[0015] In step S3 of this invention, the washing is performed by alternating washing with anhydrous ethanol and deionized water three times each, and the drying refers to placing the washed product in a vacuum drying oven and drying it at 80°C for 24 hours.

[0016] In step S4 of this invention, the washing process involves first washing with deionized water, then washing with anhydrous ethanol, repeating this cycle three times, and finally placing the washed product in a vacuum drying oven and drying it at 80°C for 24 hours.

[0017] The frequency of the ultrasonic oscillation in step S4 of this invention is 400-700 Hz.

[0018] In step S1 of this invention, the stirring time is 15 to 30 minutes.

[0019] In step S2 of this invention, the hydrothermal reactor is a hydrothermal reactor lined with polytetrafluoroethylene.

[0020] The ethylenediamine (C2H8N2) described in this invention is of analytical grade with a purity ≥99.5%.

[0021] The cadmium sulfate (CdSO4·8 / 3H2O) described in this invention is of analytical grade with a purity ≥99.0%.

[0022] The sodium selenite (Na2SeO3) described in this invention is of analytical grade with a purity ≥99.0%.

[0023] Compared with the prior art, the present invention has the following beneficial effects:

[0024] (1) In this invention, cadmium salt is selected as raw material, selenite which is highly soluble in ethylenediamine is used as selenium source, and ethylenediamine is used as solvent. The reaction occurs in a solvothermal environment, and cadmium selenide nanowires can be obtained in one step.

[0025] (2) The defective cadmium selenide nanowires prepared by the method of the present invention do not require high-temperature treatment, thus avoiding the influence of high-temperature treatment on the morphology and stability of the product, and also avoiding the alteration of defects.

[0026] (3) The defective cadmium selenide nanowires obtained by the method of the present invention have controllable morphology and uniform size; the nanowires are about 200-300 nm long and about 20 nm in diameter, with relatively uniform distribution and controllable defect amount. Moreover, the defective cadmium selenide nanowires prepared have excellent visible light photocatalytic activity and have broad application prospects in the fields of photocatalytic water splitting for hydrogen production and degradation of organic pollutants.

[0027] (4) In this invention, ethylenediamine is used as the reaction solvent. Ethylenediamine has a high boiling point of 117°C and can be heated to 160-200°C; it is also strongly alkaline. The ethylenediamine used in this invention acts as both a solvent and a reducing agent, preventing the formation of Se during the reaction. 4+ Oxidation to Se 6+ Therefore, no reducing agent needs to be added. Attached Figure Description

[0028] Figure 1 These are scanning electron microscope (SEM) images of defective cadmium selenide nanowires and pure cadmium selenide nanowires from Example 1 of the present invention.

[0029] (a) Pure CdSe; (b) Defective CdSe.

[0030] Figure 2 The following is a mapping diagram of the defective cadmium selenide nanowire sample in Example 1 of the present invention. (a) is the elemental EDS diagram of the selected sample; (b) and (c) are the mapping diagrams of Cd and Se elements, respectively; (d) is the SEM image of the selected sample; and (e) is the elemental content distribution diagram of the sample.

[0031] Figure 3 The image shows the Raman (PL) spectrum of the defective cadmium selenide nanowires in Example 1 of this invention. (a) is the full spectrum from 50 to 1000 nm; (b) is the spectrum at a wavenumber of 301 cm⁻¹. -1 A comparison diagram of Raman spectral peaks.

[0032] Figure 4 This is a comparison of the photocatalytic degradation of methyl orange by the defective cadmium selenide nanowires of this invention under visible light. (a) Pure CdSe; (b) 1.25CdSe; (c) 0.75CdSe; (d) 0.25CdSe. Detailed Implementation

[0033] The present invention will be further described below with reference to specific embodiments. Unless otherwise specified, the experimental methods used in the following embodiments are conventional methods; the raw materials and auxiliaries used are commercially available and can be purchased from the conventional market unless otherwise specified.

[0034] Example 1:

[0035] The method for preparing defective cadmium selenide nanowires of the present invention is as follows:

[0036] 1.7294 g of sodium selenite (Na2SeO3, purity ≥99.0%) and 2.5647 g of cadmium sulfate (CdSO4·8 / 3H2O, purity ≥99.0%) were added to beakers containing 50 ml of ethylenediamine (C2H8N2, purity ≥99.5%). After stirring for 25 min, the mixture was transferred to a hydrothermal reactor lined with polytetrafluoroethylene (PTFE), tightened, and placed in a vacuum drying oven for hydrothermal reaction at 200 °C for 24 h. After naturally cooling to room temperature, the mixture was centrifuged and washed three times each with anhydrous ethanol and deionized water. The sample was then dried in a vacuum drying oven at 80 °C for 24 h to obtain cadmium selenide nanowires (i.e., pure CdSe).

[0037] Weigh 0.2000 g of the obtained cadmium selenide nanowire sample and add it to 20 ml of hydrogen peroxide (mass concentration of 0.25%). Sonicate the sample (frequency of 700 Hz) for 2 h, centrifuge, wash the sample with deionized water first, then wash it with anhydrous ethanol, and repeat the washing cycle 3 times. Finally, place the product in a vacuum drying oven and dry it at 80 °C for 24 h to obtain defective cadmium selenide nanowires (i.e. defective CdSe).

[0038] Example 2

[0039] The method for preparing defective cadmium selenide nanowires of the present invention is as follows:

[0040] 1.7294 g of sodium selenite (Na2SeO3, purity ≥99.0%) and 2.5647 g of cadmium sulfate (CdSO4·8 / 3H2O, purity ≥99.0%) were added to beakers containing 70 ml of ethylenediamine (C2H8N2, purity ≥99.5%). After stirring for 15 min, the mixture was transferred to a hydrothermal reactor lined with polytetrafluoroethylene (PTFE), tightened, and placed in a vacuum drying oven for hydrothermal reaction at 160 °C for 24 h. After naturally cooling to room temperature, the mixture was centrifuged and washed three times each with anhydrous ethanol and deionized water. The sample was then dried in a vacuum drying oven at 80 °C for 24 h to obtain cadmium selenide nanowires.

[0041] Weigh 0.2000 g of the obtained cadmium selenide nanowire sample and add it to 20 ml of hydrogen peroxide (mass concentration of 0.75%). Sonicate the sample (frequency of 400 Hz) for 4 h, centrifuge, wash the sample with deionized water first, then wash it with anhydrous ethanol, and repeat the washing cycle 3 times. Finally, place the product in a vacuum drying oven and dry it at 80 °C for 24 h to obtain defective cadmium selenide nanowires.

[0042] Example 3

[0043] The method for preparing defective cadmium selenide nanowires of the present invention is as follows:

[0044] 1.7294 g of sodium selenite (Na2SeO3, purity ≥99.0%) and 3.0842 g of cadmium nitrate (Cd(NO3)2·4H2O, purity ≥99.0%) were added to beakers containing 100 ml of ethylenediamine (C2H8N2, purity ≥99.5%). After stirring for 20 min, the mixture was transferred to a hydrothermal reactor lined with polytetrafluoroethylene (PTFE), tightened, and placed in a vacuum drying oven for hydrothermal reaction at 200 °C for 24 h. After naturally cooling to room temperature, the mixture was centrifuged and washed three times each with anhydrous ethanol and deionized water. The sample was then dried in a vacuum drying oven at 80 °C for 48 h to obtain cadmium selenide nanowires.

[0045] Weigh 0.2000 g of the obtained cadmium selenide nanowire sample and add it to 20 ml of hydrogen peroxide (mass concentration of 1.25%). Sonicate the sample (frequency of 500 Hz) for 3 h, centrifuge, wash the sample with deionized water first, then wash it with anhydrous ethanol, and repeat the washing cycle 3 times. Finally, place the product in a vacuum drying oven and dry it at 80 °C for 48 h to obtain defective cadmium selenide nanowires.

[0046] Example 4

[0047] The method for preparing defective cadmium selenide nanowires of the present invention is as follows:

[0048] 2.0515 g of potassium selenite (K₂SeO₃, purity ≥99.0%) and 2.5647 g of cadmium sulfate (CdSO₄·8 / 3H₂O, purity ≥99.0%) were added to beakers containing 70 ml of ethylenediamine (C₂H₈N₂, purity ≥99.5%). After stirring for 30 min, the mixture was transferred to a hydrothermal reactor lined with polytetrafluoroethylene (PTFE), tightened, and placed in a vacuum drying oven for hydrothermal reaction at 200 °C for 24 h. After naturally cooling to room temperature, the mixture was centrifuged and washed three times each with anhydrous ethanol and deionized water. The sample was then dried in a vacuum drying oven at 80 °C for 48 h to obtain cadmium selenide nanowires.

[0049] Weigh 0.2000 g of the obtained cadmium selenide nanowire sample and add it to 20 ml of hydrogen peroxide (mass concentration of 1.25%). Sonicate the sample (frequency of 600 Hz) for 2 h, centrifuge, wash the sample with deionized water first, then wash it with anhydrous ethanol, and repeat the washing cycle 3 times. Finally, place the product in a vacuum drying oven and dry it at 80 °C for 48 h to obtain defective cadmium selenide nanowires.

[0050] The morphology and structure of the defective cadmium selenide nanowires prepared in Example 1 are analyzed as follows:

[0051] The defective cadmium selenide nanowires obtained in Example 1 of this invention were subjected to morphological and compositional analysis using a LEO1530VP field emission scanning electron microscope (SEM). The results are shown in [Figure 1]. Figure 1 and Figure 2 As shown, the defective cadmium selenide nanowires in the sample are linear, approximately 200-300 nm long and 20 nm in diameter, and contain elements such as Se and Cd. Pure CdSe has an irregular structure with a small number of linear and blocky structures, approximately 100-200 nm long. After ultrasonic treatment with hydrogen peroxide, the morphology of the resulting defective CdSe changes significantly, exhibiting numerous linear structures and a small number of irregular structures. This demonstrates that hydrogen peroxide can significantly alter the crystal morphology. Photocatalytic performance is directly related to the crystal structure and defects of the photocatalyst. Defective CdSe with altered crystal structure exhibits superior photocatalytic performance.

[0052] from Figure 2 It can be seen that the main components of the obtained defective cadmium selenide nanowire sample are Se and Cd, with a molar ratio of approximately 1:1, indicating that the defective cadmium selenide nanowire sample was successfully prepared.

[0053] from Figure 3 As can be seen in (a), the CdSe Raman spectrum has two distinct peaks, located at 301 cm⁻¹. -1 and 612cm-1 For a wavenumber of 301 cm⁻¹ -1 The Raman peaks are further magnified (e.g. Figure 3 As shown in (b), it was found that the wavenumber redshifted significantly with the increase of hydrogen peroxide content, indicating that the oxidation of hydrogen peroxide promoted the increase of cadmium selenide surface defects.

[0054] Evaluation of the photocatalytic activity of the defective cadmium selenide nanowires of this invention:

[0055] The photocatalytic activity evaluation reaction was conducted in a 200ml quartz glass reactor on an XPS-VII type reactor (manufactured by Nanjing Xujiang Electromechanical Plant). A 1000W xenon lamp was used as the ultraviolet-visible light source, and a self-made filtrate was used to absorb the ultraviolet light source to obtain the visible light source. The filtrate used 2M NaNO3 to absorb light with wavelengths below 400nm. This solution layer was located in the interlayer between the lamp tube and the circulating cooling water, so that after further absorption of ultraviolet light by the water layer, the ultraviolet light absorption rate reached over 98%. 20mg of the defective cadmium selenide nanowires of this invention were added to 200ml of methyl orange solution (20mg / l), and ultrasonically dispersed in a dark room for 15min to obtain a good dispersion state. To achieve desorption-adsorption equilibrium, magnetic stirring was performed for 1h with air flowing at 200ml / min before turning on the lamp, followed by photocatalytic reaction at room temperature. During the reaction, 8 ml samples were taken at regular intervals. The resulting suspension was centrifuged in a high-speed centrifuge for 10 min to remove the catalyst suspended in the solution. The supernatant was then tested for concentration using a Hitachi UV-3010 spectrophotometer.

[0056] The decolorization efficiency of methyl orange can be calculated using the following formula:

[0057] X% = (A0-A) / A0 × 100%;

[0058] Where: A0 is the absorbance of 20 mg / L MO at 465 nm:

[0059] A represents the absorbance of methyl orange samples taken at different times.

[0060] The photocatalytic degradation effects of pure cadmium selenide nanowires (i.e., pure CdSe) obtained in the first step of Example 1 of this invention and defective cadmium selenide nanowires obtained by the method of this invention under sunlight were compared. For details, please refer to [link to relevant documentation]. Figure 4 Among them, (a) pure CdSe; (b) 1.25CdSe; (c) 0.75CdSe; and (d) 0.25CdSe. The 1.25CdSe, 0.75CdSe, and 0.25CdSe refer to defective cadmium selenide nanowires obtained by treatment with hydrogen peroxide of different mass concentrations.

[0061] Depend on Figure 4 It was found that under visible light, the degradation rate of methyl orange by pure CdSe was only 27% within 150 minutes, while CdSe treated with hydrogen peroxide showed significantly better degradation performance than pure CdSe. The photocatalytic effect of 0.25% CdSe was the best, with a degradation rate approaching 100%. The photocatalytic efficiency of defective cadmium selenide nanowires first increased and then decreased with increasing cadmium selenide content. This may be due to the increase in CdSe defects, which become recombination centers for photogenerated charges, leading to a decrease in photocatalytic activity.

Claims

1. A method for preparing defective cadmium selenide nanowires, characterized in that, The method includes the following steps: S1: Add 1.7294–2.0515 g of selenite and 2.5647–3.0842 g of cadmium salt to 50–100 ml of ethylenediamine solution and stir thoroughly to obtain a mixed solution for later use; wherein the selenite is sodium selenite or potassium selenite; wherein the cadmium salt is cadmium sulfate or cadmium nitrate; S2: Transfer the mixture obtained in step S1 to a hydrothermal reactor, place the hydrothermal reactor in a drying oven and react at a constant temperature of 160-200℃ for 24-48 hours, and then cool naturally to room temperature; S3: Centrifuge, wash and dry the product obtained in step S2 to obtain cadmium selenide nanowires. S4: Add 0.2g of the product obtained in step S3 to 20ml of hydrogen peroxide with a mass concentration of 0.25%-1.25%, sonicate for 2-4 hours, centrifuge, wash, and dry to obtain defective cadmium selenide nanowires.

2. The method for preparing defective cadmium selenide nanowires according to claim 1, characterized in that, In step S3, the washing involves alternating between washing with anhydrous ethanol and deionized water three times each, and the drying involves placing the washed product in a vacuum drying oven and drying it at 80°C for 24 hours.

3. The method for preparing defective cadmium selenide nanowires according to claim 1 or 2, characterized in that, In step S4, the washing process involves first washing with deionized water, then washing with anhydrous ethanol, repeating this cycle three times. Finally, the washed product is placed in a vacuum drying oven and dried at 80°C for 24 hours.

4. The method for preparing defective cadmium selenide nanowires according to claim 1 or 2, characterized in that, The frequency of the ultrasonic oscillation in step S4 is 400-700 Hz.

5. The method for preparing defective cadmium selenide nanowires according to claim 1 or 2, characterized in that, The hydrothermal reactor mentioned in step S2 is a hydrothermal reactor with a polytetrafluoroethylene liner.

6. The method for preparing defective cadmium selenide nanowires according to claim 1 or 2, characterized in that, In step S1, the stirring time is 15 to 30 minutes.

Citation Information

Patent Citations

  • Method of manufacturing cadmium selenide nano thread

    CN101108725A

  • Preparation method of out-phase junction CdS nanowire

    CN113860357A