Composite ceramic silicon carbide anti-corrosion daub and preparation method thereof

Through the preparation of composite ceramic silicon carbide anti-corrosion cement, the problem of equipment corrosion due to acidic wet flue gas in the existing technology is solved, and a cost-effective anti-corrosion solution is provided, which has flame retardant, crack-resistant and wear-resistant properties, and reduces the construction cost. Risks and Costs.

CN118771784APending Publication Date: 2024-10-15JIANGSU EXXON ENVIRONMENTAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410762322.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-13
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

In the existing technology, equipment and chimneys in the desulfurization system corrode due to contact with acidic wet flue gas. Existing anti-corrosion materials such as glass flake lining cement and butyl rubber are prone to fires during construction and are costly, and stainless steel composite panels are expensive. , low cost performance.

Method used

Composite ceramic silicon carbide anti-corrosion cement is used, including flame-retardant vinyl resin, silane coupling agent, fumed silica, silicon carbide, white corundum, brown corundum, zirconia, ultra-thin flake fillers and inorganic functional fillers, through vacuum It is prepared by kneading and stirring with a high-speed disperser, and then used after adding curing agent and accelerator.

Benefits of technology

The material is flame-retardant, crack-resistant, wear-resistant and has good resistance to acid and alkali corrosion, which reduces the risk of fire. It is low-cost, cost-effective, and easy to construct. Its wear-resistant performance even exceeds that of grinding wheels and whetstones.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention discloses composite ceramic silicon carbide anti-corrosion daub which is prepared from the following material components: flame-retardant vinyl resin, a silane coupling agent, fumed silica, silicon carbide, white corundum, brown corundum, zirconium oxide, flaky filler and inorganic functional filler. The inorganic functional filler is a mixed filler of aluminum hydroxide, antimonous oxide, zinc borate and calcium aluminate ammonium polyphosphate, the flaky filler is an ultrathin flaky filler, the composite ceramic silicon carbide anti-corrosion daub has the properties of flame retardance, crack resistance, wear resistance and the like, the problem that fire disasters are likely to happen during site construction of materials such as glass flake daub is solved, and the anti-corrosion performance of the daub is improved. Compared with butyl rubber, stainless steel and other materials, the manufacturing cost is greatly reduced, and the cost performance is very excellent.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of anti-corrosion materials, in particular to a composite ceramic silicon carbide anti-corrosion mortar and a preparation method thereof. Background Art

[0002] In the desulfurization system of the prior art, after the flue gas enters the desulfurization, it is converted from dry flue gas to acidic wet flue gas through slurry flushing. In addition, the current desulfurization system cancels the GGH (gas-to-gas heat exchanger), so that the emission temperature of the flue gas after desulfurization is about 45-55°C. This causes a large amount of acidic slurry to form in the wet flue gas in the desulfurization system and the chimney, which corrodes the equipment in the desulfurization system that contacts the acidic medium and the inner wall of the chimney, so it is necessary to carry out anti-corrosion treatment on the inner wall of these equipment. In addition, related equipment such as chemical systems that contact acidic and alkaline media also need to be treated with anti-corrosion.

[0003] At present, the anti-corrosion materials of the above system equipment mostly use glass flake lining mortar, butyl rubber, etc., and even directly use 316L stainless steel or titanium steel composite plate and other materials to make the equipment. The cost of directly using stainless steel or titanium steel composite plate and other materials to make equipment is too expensive and has a low cost performance; while the use of traditional glass flake mortar lining materials and butyl rubber materials is prone to fire accidents during the construction process, and butyl rubber has too high requirements on the substrate, making on-site construction difficult and its cost is relatively high. Summary of the invention

[0004] In order to overcome the technical defects in the prior art and effectively solve the technical problems in the background technology, the present invention provides the following technical solutions:

[0005] To achieve the above-mentioned purpose, the present invention provides the following technical solution: a composite ceramic silicon carbide anti-corrosion mortar, comprising the following material components: flame retardant vinyl resin, silane coupling agent, fumed silica, silicon carbide, white corundum, brown corundum, zirconium oxide, flaky filler, and inorganic functional filler.

[0006] As a preferred technical solution of the present invention, the inorganic functional filler is a mixed filler of aluminum hydroxide, antimony trioxide, zinc borate and calcium aluminate ammonium polyphosphate.

[0007] As a preferred technical solution of the present invention, the flaky filler is an ultra-thin flaky filler.

[0008] As a preferred technical solution of the present invention, it also includes a curing agent and an accelerator.

[0009] A method for preparing a composite ceramic silicon carbide anti-corrosion mortar comprises the following steps:

[0010] Step 1: Weigh a certain amount of flame retardant vinyl resin according to the stirring volume of the vacuum kneader, add silane coupling agent at a weight ratio of 1-1.5% according to the amount of the flame retardant vinyl resin, and add fumed silica at a weight ratio of 3-4%, and thoroughly disperse them in the flame retardant vinyl resin through a high-speed disperser, and the stirring time of the high-speed disperser is not less than 15 minutes;

[0011] Step 2: Pour the flame retardant vinyl resin with the fumed silica dispersed in step 1 into a vacuum kneader, add wear-resistant materials silicon carbide, white corundum, brown corundum and zirconium oxide at a weight ratio of 2.3-2.6 times the flame retardant vinyl resin (mixed in proportion according to the medium conditions), add ultra-thin flaky fillers at a weight ratio of 5-6% of the flame retardant vinyl resin, add inorganic functional fillers (i.e., aluminum hydroxide, antimony trioxide, zinc borate and calcium aluminate ammonium polyphosphate mixed fillers) at a weight ratio of 5-15% of the flame retardant vinyl resin, and vacuum knead and stir for not less than 40 minutes. The vacuum kneaded and stirred mixture is composite ceramic silicon carbide.

[0012] Step 3: Take the composite ceramic silicon carbide mixed in step 2, add curing agent and accelerator, and stir evenly to make composite ceramic silicon carbide anti-corrosion mortar for coating construction.

[0013] Compared with the prior art, the beneficial effects of the present invention are: the composite ceramic silicon carbide anti-corrosion mortar has flame retardant, crack resistance and wear resistance, which not only solves the problem of fire proneness in on-site construction of materials such as glass flake mortar, but also its cost is greatly reduced compared with materials such as butyl rubber and stainless steel, and the cost performance is very superior.

[0014] Specifically, the composite ceramic silicon carbide anticorrosive mortar of the present invention has the following advantages:

[0015] 1. Since the mixing process of materials is physical mixing and no chemical reaction occurs, the material has the characteristics of each raw material;

[0016] 2. Since the selected resin does not react with most common acids and alkalis, and each filler does not react with acids and alkalis, it has good acid and alkali corrosion resistance;

[0017] 3. It has excellent flame retardant properties. Because the selected resin is flame retardant resin and other various fillers are fire-resistant flame retardant materials, the mixture has excellent flame retardant properties and will not burn when encountering open flames, which greatly suppresses the possibility of fire during the anti-corrosion construction process;

[0018] 4. Good anti-penetration performance. Due to the addition of a certain amount of sheet filler, the sheet filler forms an irregular maze structure in the resin lining after the material is cured. The sheet filler blocks the penetration of the slurry, that is, the slurry can only penetrate through the resin layer. In addition, the fillers of different grades of this material greatly reduce the porosity of the material and greatly improve the density, that is, the penetration path of the slurry is greatly increased, which greatly enhances the anti-penetration ability of the material.

[0019] 5. A large amount of wear-resistant granular materials are added to the material, so that the material has excellent wear resistance after solidification, and its wear resistance is even greater than that of grinding wheels and grindstones;

[0020] 6. On-site construction is simple. You only need to add appropriate amount of curing agent and accelerator to the material and stir evenly before construction.

[0021] 7. The material has good thixotropic properties. If it is applied inside according to the construction requirements, the material will not flow due to its own weight.

[0022] In addition, the functions of each component of the composite ceramic silicon carbide anticorrosive mortar of the present invention are as follows:

[0023] 1. Flame retardant vinyl resin:

[0024] This type of resin has excellent acid and alkali corrosion resistance, and has high bonding strength with concrete and carbon steel. It has certain temperature resistance, especially its flame retardant performance is very good, its oxygen index is greater than 31, and it has self-extinguishing properties when exposed to open flames.

[0025] The chemical structure is shown below:

[0026]

[0027] Wherein R is H or CH3, n=1-6;

[0028] From the above, it can be clearly seen that this kind of resin has the high strength and corrosion resistance of epoxy resin, and has the advantages of easy processing of unsaturated polyester resin and excellent flame retardant properties after bromination; it does not have the disadvantages of high viscosity and difficult processing of epoxy resin.

[0029] 2. Silane coupling agent:

[0030] Since the molecular structure of the silane coupling agent contains both a reaction matrix that can chemically combine with inorganic materials and a reaction group that can chemically combine with organic materials, it can better combine the glass flakes and the resin tightly together, while improving the mechanical properties and anti-aging properties of the cement after curing, and can improve the bonding performance between the cement and the anti-corrosion matrix.

[0031] 3. Fumed silica:

[0032] The main function of fumed silica is to inhibit the falling of the mastic due to its own weight, that is, the mastic is applied on the substrate to prevent it from flowing downward due to its own weight, so that the thickness of the anti-corrosion layer after the mastic material is applied on the substrate and cured is more uniform and reliable.

[0033] 4. Silicon carbide, white corundum, brown corundum, zirconium oxide:

[0034] Silicon carbide, white corundum and brown corundum are all excellent wear-resistant materials. The addition of these materials greatly improves the wear resistance of the anti-corrosion mortar. The addition of the above materials in different proportions and different gradations can greatly improve the density of the composite ceramic material, reduce the porosity, and greatly improve the material's anti-penetration performance; at the same time, it greatly improves the material's wear resistance, and its wear resistance even exceeds that of grindstones and grinding wheels.

[0035] 5. Flaky fillers:

[0036] The addition of ultra-thin flake fillers is mainly to improve the material's anti-penetration properties.

[0037] 6. Inorganic functional fillers:

[0038] The addition of materials such as aluminum hydroxide, antimony trioxide, zinc borate, calcium aluminate ammonium polyphosphate can greatly improve the flame retardant properties of the anti-corrosion putty. In addition, a certain amount of corrosion-resistant inorganic functional fillers are added to the putty material to increase the mechanical properties, temperature resistance and mechanical properties of the material.

[0039] Furthermore, the test report of the composite ceramic silicon carbide material in the present invention is as follows:

[0040] Serial number Test items unit Detection indicators Test results Single judgment 1 Tensile Strength MPa ≥20 35.5 qualified 2 Bending Strength MPa ≥28 56.8 qualified 3 Compression strength MPa ≥70 126.6 qualified 4 Barcol hardness / ≥55 78 qualified 5 Average linear expansion coefficient K-1 ≤3×10-5 1.15×10-5 qualified 6 Primer tensile shear strength MPa ≥8 15.3 qualified 7 Heat Deflection Temperature ℃ / 205 qualified 8 Water vapor permeability coefficient g / msPa / 7.4×10-14 qualified 9 Flash point ℃ / 108 qualified 10 Ignition Point ℃ / 559 qualified 11 Oxygen Index % ≥28 35.6 qualified DETAILED DESCRIPTION

[0041] In order to make the purpose, technical solution and advantages of the present invention clearer, the technical solution in the embodiment of the present invention will be further clearly and completely described below. Obviously, the described embodiment is only a part of the embodiment of the present invention, not all the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0042] The invention provides a technical solution: a composite ceramic silicon carbide anticorrosive mortar, comprising the following material components: flame retardant vinyl resin, silane coupling agent, fumed silica, silicon carbide, white corundum, brown corundum, zirconium oxide, ultrathin flaky filler, aluminum hydroxide, antimony trioxide, zinc borate, calcium aluminate ammonium polyphosphate, a curing agent and an accelerator.

[0043] A method for preparing a composite ceramic silicon carbide anti-corrosion mortar comprises the following steps:

[0044] Step 1: Weigh a certain amount of flame retardant vinyl resin according to the stirring volume of the vacuum kneader, add silane coupling agent at a weight ratio of 1.2% according to the amount of the flame retardant vinyl resin, and add fumed silica at a weight ratio of 3.5%, and thoroughly disperse them in the flame retardant vinyl resin by a high-speed disperser, and the stirring time of the high-speed disperser is 15 minutes;

[0045] Step 2: Pour the flame retardant vinyl resin with the fumed silica dispersed in step 1 into a vacuum kneader, add wear-resistant materials silicon carbide, white corundum, brown corundum and zirconium oxide at a weight ratio of 2.5 times the flame retardant vinyl resin (mixed in proportion according to the medium conditions), add ultra-thin flaky filler at a weight ratio of 5% of the flame retardant vinyl resin, add aluminum hydroxide, antimony trioxide, zinc borate and calcium aluminate ammonium polyphosphate mixed filler at a weight ratio of 12% of the flame retardant vinyl resin, and vacuum knead and stir for 45 minutes. The vacuum kneaded and stirred mixture is composite ceramic silicon carbide.

[0046] Step 3: Take the composite ceramic silicon carbide mixed in step 2, add curing agent and accelerator, and stir evenly to make composite ceramic silicon carbide anti-corrosion mortar for coating construction.

[0047] When using:

[0048] As in step three above, the packaging barrel containing the composite ceramic silicon carbide material is opened on site, and the corresponding curing agent and accelerator are added (the curing agent and accelerator are commonly used curing agent and accelerator materials in the prior art, and the addition ratio can be added according to the conventional construction operation requirements. The operation is an existing mature technology and will not be described in detail here) and stirred evenly, and the stirred composite ceramic carbide silica gel mud can be applied to the corresponding position according to conventional operations.

[0049] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A composite ceramic silicon carbide anticorrosive mortar, characterized in that: The material components include: flame retardant vinyl resin, silane coupling agent, fumed silica, silicon carbide, white corundum, brown corundum, zirconium oxide, flaky filler and inorganic functional filler.

2. The composite ceramic silicon carbide anticorrosive mortar according to claim 1, characterized in that: The inorganic functional filler is a mixed filler of aluminum hydroxide, antimony trioxide, zinc borate and calcium aluminate ammonium polyphosphate.

3. The composite ceramic silicon carbide anticorrosive mortar according to claim 1, characterized in that: The flaky filler is an ultra-thin flaky filler.

4. The composite ceramic silicon carbide anticorrosive mortar according to claim 1, characterized in that: Also includes curing agents and accelerators.

5. The method for preparing the composite ceramic silicon carbide anticorrosive mortar according to any one of claims 1 to 4, characterized in that: The following steps are involved: Step 1: Weigh a certain amount of flame retardant vinyl resin according to the stirring volume of the vacuum kneader, add silane coupling agent at a weight ratio of 1-1.5% according to the amount of the flame retardant vinyl resin, and add fumed silica at a weight ratio of 3-4%, and thoroughly disperse them in the flame retardant vinyl resin through a high-speed disperser, and the stirring time of the high-speed disperser is not less than 15 minutes; Step 2: Pour the flame retardant vinyl resin with the fumed silica dispersed in step 1 into a vacuum kneader, add wear-resistant materials silicon carbide, white corundum, brown corundum and zirconium oxide at a weight ratio of 2.3-2.6 times the flame retardant vinyl resin (mixed in proportion according to the medium conditions), add ultra-thin flaky fillers at a weight ratio of 5-6% of the flame retardant vinyl resin, add inorganic functional fillers (i.e., aluminum hydroxide, antimony trioxide, zinc borate and calcium aluminate ammonium polyphosphate mixed fillers) at a weight ratio of 5-15% of the flame retardant vinyl resin, and vacuum knead and stir for not less than 40 minutes. The vacuum kneaded and stirred mixture is composite ceramic silicon carbide. Step 3: Take the composite ceramic silicon carbide mixed in step 2, add curing agent and accelerator, and stir evenly to make composite ceramic silicon carbide anti-corrosion mortar for coating construction.