Polyurethane composite foam material, preparation method thereof and application of polyurethane composite foam material in battery
Through the preparation of polyurethane composite foaming materials, hydrophobic aerogel and isocyanate are used to form a prepolymer and condensed with polyol, which solves the problems of complex production process and insufficient material performance of cylindrical battery modules, and achieves good fixation and stabilization of battery cells. Thermal isolation meets the needs of battery module lightweight and safety performance.
Patent Information
- Application Number
- CN202410788718.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-18
- Publication Date
- 2024-10-15
Smart Images

Figure BDA0004899472700000091 
Figure BDA0004899472700000101
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of lithium batteries, and in particular to a polyurethane composite foaming material, a preparation method thereof and application in batteries. Background Art
[0002] With the country's high attention and the rapid development of new energy vehicles, the share of new energy vehicles in China's automobile market will continue to grow in the next few years. The safety of electric vehicles has always been the focus of consumers. As the core component of new energy vehicles, improving the safety performance of power batteries is the key to improving the safety performance of new energy vehicles.
[0003] Power batteries mainly include square batteries and cylindrical batteries. At present, there are many studies and reports on the thermal protection of square battery modules, and the research on thermal insulation protection of square battery modules has been perfected. However, since the regularity of the internal structure of cylindrical battery modules is lower than that of square battery modules, preformed materials are often used between the cells of cylindrical power battery modules to block the heat transfer and diffusion between the cells, and the cells need to be fixed by cell holders, which makes the production process of cylindrical power battery modules complicated, which is not conducive to mass production and cost reduction; more importantly, the preformed materials currently used in cylindrical power battery modules have a large density, and their flow properties, flame retardancy and fixation performance of the cells cannot meet the requirements at the same time, and the standard of module lightweighting is low, which cannot meet the needs of lightweight design of battery modules. Summary of the invention
[0004] In order to provide a thermal insulation protective material with good fluidity, high strength, low thermal conductivity and excellent thermal insulation performance so as to achieve the effect of efficiently blocking heat transfer between battery cells, fixing battery cells and meeting the lightweight requirements of battery modules, the present application provides a polyurethane composite foam material, a preparation method thereof and its application in batteries.
[0005] In a first aspect, the present application provides a polyurethane composite foam material, which adopts the following technical solution:
[0006] A polyurethane composite foaming material includes component A and component B; component A includes the following raw materials in parts by weight: 30-50 parts of polyol, 4-5 parts of cross-linking agent, and 0.2-0.4 parts of foaming agent; component B includes the following raw materials in parts by weight: 45-55 parts of isocyanate, and 1-2 parts of hydrophobic aerogel. For example, the polyol can be 30 parts, 40 parts, and 50 parts, the cross-linking agent can be 4 parts, 4.5 parts, 4.8 parts, and 5 parts, the foaming agent can be 0.2 parts, 0.3 parts, and 0.4 parts, the isocyanate can be 45 parts, 50 parts, and 55 parts, and the hydrophobic aerogel can be 1 part, 1.5 parts, and 2 parts, but it is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0007] The present invention uses hydrophobic aerogel. A small amount of hydroxyl groups exist on the surface of the hydrophobic aerogel, which can cooperate with isocyanate to form an intermediate with a terminal -NCO group, namely a prepolymer. On the one hand, the prepolymer can not only reduce the viscosity of the system, so that the polyurethane composite foam material has a longer reaction operation time, which is convenient for industrial production, but also the addition of the hydrophobic aerogel can increase the distance between molecules in the system, reduce the interaction force between molecules, and reduce the number of entanglement points in the reaction system, thereby improving the fluidity of the polyurethane composite foam material, so that the polyurethane composite foam material can be fully filled in the gap between two adjacent battery cells, and the polyurethane composite foam material can be fully contacted with the battery cell while improving its heat absorption effect and fixation effect on the battery cell; on the other hand, the prepolymer can condense with the hydroxyl group in the polyol to form an amide bond, thereby effectively improving the strength and heat resistance stability of the homogeneous foaming composite material, so that the battery module can absorb the stress generated by the outside, the energy and heat generated by the impact, and strengthen the fixation effect and heat insulation effect of the polyurethane composite foam material on the battery cell in the battery module.
[0008] In summary, the polyurethane composite foam material prepared by the above formula is a low-viscosity liquid. The encapsulation process can be used to make the above material flow and fill the gaps between the battery cells before foaming and forming. After foaming, it has low density, high strength, small thermal conductivity, excellent thermal insulation performance, flame retardancy reaching 3mm V0 level and meets halogen-free environmental protection requirements; it can play a good role in fixing the battery cells in the cylindrical battery module, effectively block the heat transfer between the battery cells, and at the same time meet the requirements of lightweight cylindrical battery modules.
[0009] Preferably, the mass ratio of the component A to the component B is 1-3:1-3, for example, 1:3, 3:1, 1:1, 2:1, but not limited to the listed values, and other values not listed in the numerical range are also applicable.
[0010] By controlling the amount of component A and component B, adjusting the amount of prepolymer in the reaction system, improving the mixing between component A and component B, and preventing the occurrence of side reactions while adjusting the viscosity of the reaction system, the thermal insulation stability of the polyurethane composite foam material and the fixation effect on the battery cell are improved.
[0011] Preferably, the NCO content of the isocyanate is 28%-33%, and the viscosity of the isocyanate is 200-400 cps. For example, the NCO content of the isocyanate may be 28%, 29.5%, 30%, 33%, and the viscosity of the isocyanate may be 200 cps, 300 cps, 400 cps, but the values are not limited to the values listed, and other values not listed in the numerical range are also applicable.
[0012] Preferably, NCO refers to the mass of isocyanate (—NCO) groups contained in 100 g of an isocyanate sample.
[0013] Preferably, the isocyanate includes at least one of 2,4-toluene diisocyanate, 2,6-toluene diisocyanate, isophorone diisocyanate, p-phenylene diisocyanate, polymethylene polyphenyl polyisocyanate, and carbodiimide-modified MDI (carbodiimide-modified diphenylmethane diisocyanate).
[0014] By using isocyanate containing NCO in the above range, the stability of the reaction between isocyanate and hydrophobic aerogel can be improved, and a sufficient amount of prepolymer can be generated, which is helpful to improve the strength and elongation at break of the polyurethane composite foam material, so that the polyurethane composite foam material will not crack or break during thermal expansion and contraction, thereby improving the stability of the battery cells in the battery module.
[0015] Preferably, the density of the hydrophobic aerogel is 45-60 kg / m 3 , thermal conductivity is 0.010-0.015Wm -1 .K -1 For example, the density of hydrophobic aerogel can be 45 kg / m 3 , 53kg / m 3 , 58kg / m 3 、60kg / m 3 , the thermal conductivity of hydrophobic aerogel can be 0.010Wm -1 .K -1 、0.012Wm -1 .K -1 、0.015Wm -1 .K -1 , but not limited to the listed values, other unlisted values within the numerical range are also applicable.
[0016] Preferably, the hydrophobic aerogel comprises hydrophobic silica aerogel.
[0017] By selecting hydrophobic aerogel with suitable density and thermal conductivity, the hydrophobic aerogel can maintain a relatively high porosity and a multi-level fractal pore microstructure, thereby significantly improving the thermal conductivity of the polyurethane composite foam material.
[0018] Preferably, the viscosity of the polyol is 1000-1500 cps, and the hydroxyl value of the polyol is 100-500 mgKOH. For example, the viscosity of the polyol may be 1000 cps, 1300 cps, 1500 cps, and the hydroxyl value of the polyol may be 100 mgKOH, 200 mgKOH, 400 mgKOH, 500 mgKOH, but the polyol is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0019] Preferably, the polyol includes at least one of castor oil-modified polyether polyol, soybean oil-modified polyol, bisphenol A-modified polyol and polyester polyol.
[0020] By using the vegetable oil-modified polyol with the above hydroxyl value, the reaction rate of the polyol and the prepolymer in component B can be adjusted, the number of amide bonds generated by condensation can be increased, and the strength and thermal insulation performance of the polyurethane composite foam material can be improved.
[0021] Preferably, the A component further comprises the following raw materials in parts by weight: 5-10 parts of halogen-free flame retardant, 0.1-0.5 parts of foam stabilizer, 0.2-0.3 parts of catalyst, and 1-3 parts of plasticizer. For example, the halogen-free flame retardant can be 5 parts, 8 parts, and 10 parts, the foam stabilizer can be 0.1 parts, 0.3 parts, 0.4 parts, and 0.5 parts, the catalyst can be 0.2 parts, 0.25 parts, and 0.3 parts, and the plasticizer can be 1 part, 2 parts, and 3 parts, but the values listed are not limited thereto, and other values not listed within the numerical range are also applicable.
[0022] Furthermore, the hydrophobic aerogel can be combined with the halogen-free flame retardant. The three-dimensional porous network structure of the hydrophobic aerogel can be combined with the halogen-free flame retardant to effectively prevent air convection. When the battery releases a large amount of heat, it can absorb heat at an extremely fast rate, and form an effective thermal barrier between the various battery cells of the battery module, thereby further reducing the thermal conductivity of the polyurethane foam composite material and improving the flame retardant effect of the battery module.
[0023] Preferably, the cross-linking agent includes at least one of glycerol and trihydroxypropane; and the foaming agent includes at least one of water and cyclopentane.
[0024] Preferably, the halogen-free flame retardant includes at least one of polyphosphate and triethyl phosphate.
[0025] Preferably, the foam stabilizer includes a polyether-modified silicone surfactant; the catalyst includes at least one of an organic tin catalyst, N,N-dimethylcyclohexylamine, bis-(dimethylaminoethyl ether), and triethylenediamine; the plasticizer includes at least one of γ-(2,3-epoxypropoxy)propyltrimethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltriethoxysilane, γ-aminopropyltriethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, and (3-mercaptopropyl)trimethoxysilane.
[0026] In a second aspect, the present application provides a method for preparing a polyurethane composite foam material, using the following technical solution:
[0027] A method for preparing a polyurethane composite foam material comprises the following steps:
[0028] S1, preparing the component A: mixing the raw materials constituting the component A and stirring them under vacuum, and discharging the materials after cooling to obtain the component A;
[0029] Preparation of the B component: mixing the raw materials constituting the B component and stirring in a vacuum environment to obtain a prepolymer, and cooling to obtain the B component;
[0030] S2, mixing the component A and the component B, stirring and letting stand to obtain the polyurethane composite foaming material.
[0031] By first mixing the isocyanate with the hydrophobic aerogel to obtain a prepolymer, and then mixing the A component with the prepolymer, it is helpful to adjust the condensation reaction rate of the prepolymer and the polyol, increase the number of amide bonds in the polyurethane composite foam material, and thus significantly improve the strength and heat resistance of the polyurethane composite foam material; and, at this time, the hydrophobic aerogel can also form a uniform hollow three-dimensional network structure in the reaction system, which is helpful to be used in combination with the halogen-free flame retardant in the A component, and significantly reduce the thermal conductivity and flame retardant properties of the polyurethane composite foam material.
[0032] Preferably, in S1, the temperature of component A during stirring is 25-30°C, the vacuum degree is -0.8MPa to 1MPa, and the stirring time is 2-4h; the temperature of component B during stirring is 25-30°C, the vacuum degree is -0.8MPa to 1MPa, and the stirring time is 2-4h; in S2, the stirring time is 1-3min, and the stirring speed is 1500-3000rpm. For example, the temperature of component A during stirring can be 25°C, 28°C, or 30°C, the vacuum degree can be -0.8MPa, 0.5MPa, or 1MPa, and the stirring time can be 2h, 3h, or 4h; the temperature of component B during stirring can be 25°C, 27°C, or 30°C, the vacuum degree can be -0.8MPa, 0.6MPa, or 1MPa, and the stirring time can be 2h, 3h, or 4h; in S2, the stirring time can be 1min, 2min, or 3min, and the stirring speed can be 1500rpm, 2000rpm, or 3000rpm; but the values are not limited to the values listed, and other values not listed within the numerical range are also applicable.
[0033] In a third aspect, the present application provides an application of a polyurethane composite foam material in a battery module, using the following technical solution:
[0034] The invention discloses an application of a polyurethane composite foam material in a cylindrical battery module. DETAILED DESCRIPTION
[0035] For better understanding and implementation, the technical solution of the present invention will be clearly and completely described below in conjunction with embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments.
[0036] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used in the specification of the present invention herein are only for the purpose of describing specific embodiments and are not intended to limit the present invention.
[0037] Unless otherwise indicated, all numerical values expressing quantities of ingredients, reaction conditions, and so forth used in the specification and claims are to be understood as modified by the term “about.” Accordingly, unless indicated to the contrary, the numerical parameters set forth herein are approximations that can vary depending upon the desired properties desired to be obtained.
[0038] As used herein, "and / or" means one or all of the mentioned elements.
[0039] As used herein, “including” and “comprising” encompasses the case where only the stated elements are present as well as the case where there are other elements other than the stated elements.
[0040] All percentages in the present invention are by weight, unless otherwise specified.
[0041] Unless otherwise indicated, "a", "an", "an" and "the" used in this specification are intended to include "at least one" or "one or more". For example, "a component" means one or more components, so more than one component may be considered and may be employed or used in the implementation of the embodiment.
[0042] Example 1
[0043] The polyurethane composite foam material comprises a component A and a component B in a mass ratio of 1:1;
[0044] Taking component A as a reference, component A includes the following raw materials in parts by weight: castor oil-modified polyether polyol, soybean oil-modified polyol, (viscosity 1000cps, hydroxyl value 300mgKOH / g) 38 parts, glycerol 4 parts, water 0.3 parts, polyphosphate ester 5 parts, polyether-modified silicone surfactant 0.1 parts, N,N-dimethylcyclohexylamine 0.2 parts, γ-(2,3-epoxypropoxy)propyltrimethoxysilane 2 parts;
[0045] Based on component B, component B includes the following raw materials in parts by weight: 48 parts of isocyanate (NCO content is 32%, viscosity is 200cps), hydrophobic silica aerogel (thermal conductivity is 0.011Wm -1 .K-1 , density is 55kg.m -3 )2 copies.
[0046] The polyurethane composite foam material is prepared by the following steps:
[0047] S1, preparation of component A: the raw materials constituting component A are mixed, stirred for 2 hours in a vacuum environment of 28°C and -0.8MPa, cooled to 25°C and then discharged to obtain component A;
[0048] Preparation of component B: The raw materials constituting component B are mixed, stirred for 2 hours in a vacuum environment of 28° C. and -0.8 MPa, and then cooled to 25° C. to obtain component B.
[0049] S2, mixing component A and component B, and mixing at a rotation speed of 3000 rpm for 1 min to obtain a polyurethane composite foam material.
[0050] The polyurethane composite foam material is quickly poured into the spaces between the cells of the cylindrical battery module and allowed to stand for foaming and forming.
[0051] Example 2
[0052] The polyurethane composite foam material comprises a component A and a component B in a mass ratio of 1:3;
[0053] Taking component A as a reference, component A includes the following raw materials in parts by weight: 50 parts of soybean oil-modified polyol (viscosity 1500cps, hydroxyl value 100mgKOH / g), 5 parts of trihydroxypropane, 0.3 parts of water, 10 parts of triethyl phosphate, 0.5 parts of polyether-modified silicone surfactant, 0.2-0.3 parts of bis-(dimethylaminoethyl ether), and 3 parts of 2-(3,4-epoxycyclohexyl)ethyltriethoxysilane;
[0054] Based on component B, component B includes the following raw materials by weight: 45 parts of isocyanate (NCO content is 28%, viscosity is 400cps), hydrophobic silica aerogel (thermal conductivity is 0.015Wm -1 .K -1 , density is 70kg.m -3 )1 copy.
[0055] The polyurethane composite foam material is prepared by the following steps:
[0056] S1, preparation of component A: the raw materials constituting component A are mixed, stirred for 4 hours in a vacuum environment at 25°C and 1 MPa, cooled to 25°C, and then discharged to obtain component A;
[0057] Preparation of component B: The raw materials constituting component B are mixed, stirred for 4 hours in a vacuum environment of 25 and 1 MPa, and then cooled to 25°C to obtain component B.
[0058] S2, mixing component A and component B, and mixing at a rotation speed of 1500 rpm for 3 minutes to obtain a polyurethane composite foam material.
[0059] The polyurethane composite foam material is quickly poured into the spaces between the cells of the cylindrical battery module and allowed to stand for foaming and forming.
[0060] Example 3
[0061] The polyurethane composite foam material comprises a component A and a component B in a mass ratio of 3:1;
[0062] Taking component A as a reference, component A includes the following raw materials in parts by weight: 30 parts of bisphenol A modified polyol (viscosity 1200cps, hydroxyl value 500mgKOH / g), 4 parts of glycerol, 0.2 parts of water, 5 parts of triethyl phosphate, 0.2 parts of polyether modified silicone surfactant, 0.2 parts of triethylenediamine, and 1 part of γ-aminopropyltriethoxysilane;
[0063] Based on component B, component B includes the following raw materials in parts by weight: 55 parts of isocyanate (NCO content of 33%, viscosity of 300cps), hydrophobic silica aerogel (thermal conductivity of 0.010Wm -1 .K -1 , density is 45kg.m -3 )2 copies.
[0064] The polyurethane composite foam material is prepared by the following steps:
[0065] S1, preparation of component A: the raw materials constituting component A are mixed, stirred for 3 hours in a vacuum environment at 30°C and 0.5MPa, cooled to 25°C, and then discharged to obtain component A;
[0066] Preparation of component B: The raw materials constituting component B are mixed, stirred for 3 hours in a vacuum environment at 30° C. and 0.5 MPa, and then cooled to 25° C. to obtain component B.
[0067] S2, mixing component A and component B, and mixing at a rotation speed of 2500 rpm for 2 minutes to obtain a polyurethane composite foam material.
[0068] The polyurethane composite foam material is quickly poured into the spaces between the cells of the cylindrical battery module and allowed to stand for foaming and forming.
[0069] Example 4
[0070] The difference between this embodiment and embodiment 1 is that the NCO content of the isocyanate used in component B is 20%; the other steps and parameters are consistent with those in embodiment 1.
[0071] Example 5
[0072] The difference between this embodiment and embodiment 1 is that the NCO content of the isocyanate used in component B is 40%; the other steps and parameters are consistent with those in embodiment 1.
[0073] Example 6
[0074] The difference between this embodiment and embodiment 1 is that the viscosity of the isocyanate used in component B is 100 cps; the rest is consistent with embodiment 1.
[0075] Example 7
[0076] The difference between this embodiment and embodiment 1 is that the viscosity of the isocyanate used in component B is 600 cps; the other steps and parameters are consistent with those in embodiment 1.
[0077] Example 8
[0078] The difference between this embodiment and embodiment 1 is that the thermal conductivity of the hydrophobic silica aerogel is 0.025 Wm -1 .K -1 , density is 100kg.m -3 ; Other steps and parameters are consistent with Example 1.
[0079] Example 9
[0080] The difference between this embodiment and embodiment 1 is that the plasticizer in component A is replaced by an equal weight of hydrophobic aerogel, and the hydrophobic aerogel in component B is replaced by an equal weight of plasticizer; other steps and parameters are consistent with embodiment 1.
[0081] Example 10
[0082] The difference between this embodiment and embodiment 1 is that the hydrophobic aerogel is a hydrophobic alumina aerogel; the other steps and parameters are consistent with those in embodiment 1.
[0083] Comparative Example 1
[0084] The difference between this comparative example and Example 1 is that no hydrophobic silica aerogel is used in component B; other steps and parameters are consistent with Example 1.
[0085] Comparative Example 2
[0086] The difference between this comparative example and Example 1 is that an equal weight of hydrophilic silica aerogel is used to replace the hydrophobic silica aerogel in component B; the other steps and parameters are consistent with Example 1.
[0087] Test Method
[0088] 1. Performance test of polyurethane composite foam material
[0089] 1. Viscosity test
[0090] The viscosity of the polyurethane composite foam materials in the above examples and comparative examples was tested, and the specific test method was based on GB / T 2794-2013 "Determination of viscosity of adhesives - Single cylinder rotational viscometer method".
[0091] 2. Thermal conductivity test
[0092] The polyurethane composite foam materials in the above examples and comparative examples were tested for thermal conductivity, and the specific test method was based on GB / T 10295-2008 "Measurement of Steady-State Thermal Resistance and Related Properties of Insulating Materials - Heat Flow Meter Method".
[0093] 3. Strength test
[0094] The polyurethane composite foam materials in the above examples and comparative examples were subjected to strength tests, and the specific test methods were based on GB / T 528 "Determination of steady-state thermal resistance and related properties of insulation materials - Heat flow meter method".
[0095] 4. Flame retardant grade test
[0096] The polyurethane composite foam materials in the above examples and comparative examples were subjected to strength tests, and the specific test methods were carried out in accordance with the UL94 standard.
[0097] 2. Lithium battery thermal runaway performance test
[0098] The lithium batteries in the above embodiments and comparative examples were subjected to thermal runaway performance tests. The specific test methods refer to GB38031-2020 "Safety Requirements for Power Batteries 8.2 Safety of Battery Packs or Systems".
[0099] Table 1
[0100]
[0101]
[0102] In combination with Examples 1-3, Comparative Examples 1-2 and Table 1, it can be seen that by selecting hydrophobic silica aerogel as the raw material of the polyurethane composite foam material, the hydrophobic silica aerogel helps to improve the strength and flame retardant grade of the polyurethane composite foam material, and reduce the thermal conductivity; this is because the hydrophobic silica aerogel can first react with the isocyanate to form a prepolymer, adjust the viscosity of the reaction system, and the prepolymer can react with the hydroxyl group in the polyol to form an amide bond, thereby achieving the effect of improving the strength of the polyurethane composite foam material and reducing the thermal conductivity; further, the combination of the hydrophobic silica aerogel and the halogen-free flame retardant can also further improve the flame retardant properties of the polyurethane composite material, so that the polyurethane composite foam material has excellent comprehensive properties.
[0103] When hydrophilic silica aerogel is used instead of hydrophobic silica aerogel to prepare the polyurethane composite foam material in Comparative Example 2, due to the presence of a large number of hydroxyl groups on the surface of the hydrophilic silica aerogel, it is easy to absorb water during the preparation process, resulting in increased capillary force and structural collapse, which seriously affects the strength and thermal insulation properties of the polyurethane composite foam material.
[0104] In combination with Example 1, Examples 4-5 and Table 1, it can be seen that when the NCO content in the isocyanate is too low, the strength of the polyurethane composite foam material decreases, which is not conducive to its fixation to the battery core, and the pore volume in the polyurethane foam composite material is reduced, so that its thermal insulation performance decreases; therefore, compared with the polyurethane composite foam material in Example 1, the strength of the polyurethane composite foam material in Example 4 is low and the flame retardant grade is low; and when the NCO content in the isocyanate is too high, the viscosity of the polyurethane composite foam material decreases, which is not conducive to the industrial production of the polyurethane composite foam material, and the number of closed cells in the polyurethane foam composite material is reduced, so that its thermal insulation performance decreases; therefore, compared with the polyurethane composite foam material in Example 1, the strength of the polyurethane composite foam material in Example 5 is low and the flame retardant grade is low.
[0105] In combination with Example 1, Examples 6-7 and Table 1, it can be seen that when the viscosity of the isocyanate is too low or too high, the isocyanate and other raw materials cannot produce a polyurethane composite foam material with suitable viscosity; compared with the polyurethane composite foam material in the examples, the viscosity of the polyurethane composite foam material in Examples 6-7 is reduced, which is not conducive to the industrial production of the polyurethane composite foam material.
[0106] In combination with Example 1, Example 8 and Table 1, it can be seen that when the density of the hydrophobic silica aerogel is too large and the thermal conductivity is too high, the porosity in the hydrophobic silica is low and the fractal of the pore microstructure is poor, which is not conducive to the effect of its coordination with the halogen-free flame retardant. Compared with the polyurethane composite foam material in Example 1, the thermal conductivity of the polyurethane composite foam material in Example 8 is significantly increased, and the flame retardant grade is reduced.
[0107] In combination with Example 1, Example 9 and Table 1, it can be seen that when the application order of the hydrophobic silica aerogel in the process of preparing the polyurethane composite foam material is changed, the hydrophobic silica aerogel cannot react with the isocyanate to generate a sufficient number of prepolymers first, which will further affect the number of amide bonds generated by the subsequent condensation of the prepolymer and the hydroxyl group. Compared with the polyurethane composite foam material in Example 1, the strength of the polyurethane composite foam material in Example 9 decreases, the thermal conductivity increases, and the flame retardant grade decreases.
[0108] In combination with Example 1, Example 10 and Table 1, it can be seen that when the type of hydrophobic aerogel is changed and hydrophobic alumina aerogel is used instead of hydrophobic silica aerogel, the thickening effect of the hydrophobic alumina aerogel is higher than the thickening effect of the hydrophobic silica aerogel, resulting in the density of the polyurethane composite foam material prepared in Example 10 being too large, which is not conducive to improving its strength and exerting its thermal insulation performance.
[0109] The above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit the protection scope of the present invention. Although the present invention is described in detail with reference to the above embodiments, ordinary technicians in the relevant field should understand that the technical solutions of the present invention can be modified or equivalently replaced, but these modifications or replacements are all within the protection scope of the present invention.
Claims
1. A polyurethane composite foam material, characterized in that: It includes component A and component B; The component A comprises the following raw materials in parts by weight: 30-50 parts of polyol, 4-5 parts of cross-linking agent, and 0.2-0.4 parts of foaming agent; The B component comprises the following raw materials in parts by weight: 45-55 parts of isocyanate and 1-2 parts of hydrophobic aerogel.
2. The polyurethane composite foam material according to claim 1, characterized in that: The mass ratio of the A component to the B component is 1-3:1-3.
3. The polyurethane composite foam material according to claim 1, characterized in that: The NCO content of the isocyanate is 28%-33%, and the viscosity of the isocyanate is 200-400 cps.
4. The polyurethane composite foam material according to claim 3, characterized in that: The isocyanate includes at least one of 2,4-toluene diisocyanate, 2,6-toluene diisocyanate, isophorone diisocyanate, p-phenylene diisocyanate, polymethylene polyphenyl polyisocyanate, and carbodiimide modified MDI.
5. The polyurethane composite foam material according to claim 1, characterized in that: The density of the hydrophobic aerogel is 45-60 kg / m 3 , thermal conductivity is 0.010-0.015Wm -1 .K -1 .
6. The polyurethane composite foam material according to claim 5, characterized in that: The hydrophobic aerogel includes a hydrophobic silica aerogel.
7. The polyurethane composite foam material according to claim 1, characterized in that: The viscosity of the polyol is 1000-1500 cps, and the hydroxyl value of the polyol is 100-500 mgKOH.
8. The polyurethane composite foam material according to claim 7, characterized in that: The polyol includes at least one of castor oil-modified polyether polyol, soybean oil-modified polyol, bisphenol A-modified polyol and polyester polyol.
9. The polyurethane composite foam material according to claim 1, characterized in that: The cross-linking agent includes at least one of glycerol and trihydroxypropane; the foaming agent includes at least one of water and cyclopentane.
10. The polyurethane composite foam material according to any one of claims 1 to 9, characterized in that: The component A also includes the following raw materials in parts by weight: 5-10 parts of halogen-free flame retardant, 0.1-0.5 parts of foam stabilizer, 0.2-0.3 parts of catalyst, and 1-3 parts of plasticizer.
11. The polyurethane composite foam material according to claim 10, characterized in that: The halogen-free flame retardant includes at least one of polyphosphate and triethyl phosphate.
12. The polyurethane composite foam material according to claim 10, characterized in that: The foam stabilizer includes a polyether-modified silicone surfactant; the catalyst includes at least one of an organic tin catalyst, N,N-dimethylcyclohexylamine, bis-(dimethylaminoethyl ether), and triethylenediamine; the plasticizer includes at least one of γ-(2,3-epoxypropoxy)propyltrimethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltriethoxysilane, γ-aminopropyltriethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, and (3-mercaptopropyl)trimethoxysilane.
13. The method for preparing the polyurethane composite foam material according to any one of claims 1 to 12, characterized in that: The steps include: S1, preparing the component A: mixing the raw materials constituting the component A and stirring them under vacuum, and discharging the materials after cooling to obtain the component A; Preparation of the B component: mixing the raw materials constituting the B component and stirring in a vacuum environment to obtain a prepolymer, and cooling to obtain the B component; S2, mixing the component A and the component B, stirring and standing to obtain the urethane composite foaming material.
14. The method for preparing the polyurethane composite foam material according to claim 13, characterized in that: In S1, the temperature of component A during stirring is 25-30°C, the vacuum degree is -0.8MPa to 1MPa, and the stirring time is 2-4h; the temperature of component B during stirring is 25-30°C, the vacuum degree is -0.8MPa to 1MPa, and the stirring time is 2-4h; In S2, the stirring time is 1-3 min, and the stirring speed is 1500-3000 rpm.
15. Use of the polyurethane composite foam material according to any one of claims 1 to 12 in a battery module.
Citation Information
Cited By
Preparation method of polyurethane and silicon dioxide aerogel composite material
CN119859306A
Polyurethane foam material and preparation method thereof
CN120484215A
Insulating fabric
JP2026132997A
Insulating fabric
JP7875327B1
Heat-insulating fabric
WO2026168148A1