Silver colloid diffusion preventing agent for lead frame packaging as well as preparation method and application of silver colloid diffusion preventing agent
By using a specific formula of anti-silver glue diffusion agent in conductive silver glue, a tight hydrophobic film layer is formed, which solves the problem of conductive silver glue diffusion, achieves low silver glue diffusion rate and high storage stability, and meets higher packaging requirements. .
Patent Information
- Application Number
- CN202411016363.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-27
- Publication Date
- 2024-10-15
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Conductive silver glue is prone to silver glue diffusion in lead frame packaging, leading to poor welding and functional defects. Existing anti-silver glue diffusion agents have limited effects and cannot meet higher requirements.
An anti-silver glue diffusion agent composed of water and specific raw materials is used, including bis(3-trimethoxysilylpropyl)amine, N-(2-aminoethyl)-3-aminopropyltrimethoxy Silane, γ-aminopropyltriethoxy The formula of silane, polyol, hyperbranched polymer, polyether modified silicone oil and dispersant forms a tight hydrophobic film layer through the synergistic effect of these raw materials, increases the interaction between hydrophobicity and conductive silver colloid, and reduces the diffusivity of silver colloid.
It achieves a silver glue diffusion rate of less than 2%, increases the film contact angle, enhances the inhibitory effect on conductive silver glue seepage, meets higher requirements for silver glue diffusion prevention, and shows high storage stability.
Smart Images

Figure BDA0004965813190000051 
Figure BDA0004965813190000071 
Figure BDA0004965813190000081
Abstract
Description
Technical Field
[0001] The present application relates to the field of lead frame packaging, and more specifically, to a silver glue diffusion prevention agent for lead frame packaging, a preparation method thereof, and an application thereof. Background Art
[0002] Conductive silver paste is an adhesive that combines both bonding and electrical conductivity. It's primarily made from epoxy resin, silver powder, and additives. Due to its excellent conductivity, high linear resolution, simple operation, and environmental friendliness, it has been widely used in electronic assembly and packaging.
[0003] When conductive silver paste is used in leadframe packaging, the epoxy resin component often leaches out of the paste, a phenomenon known as silver paste diffusion. This can lead to poor soldering, functional defects, and even solder shorts. Some researchers have submerged the leadframe in an anti-diffusion agent made from γ-aminopropyltriethoxysilane. This agent forms a hydrophobic film on the leadframe surface, significantly reducing the risk of conductive silver paste leakage. However, this effectiveness is limited, with the lowest silver paste diffusion rate reaching 3.97%, which is insufficient to meet higher demands. Summary of the Invention
[0004] In order to reduce the diffusion rate of silver paste and increase the inhibitory effect of the anti-silver paste diffusion agent on the seepage of conductive silver paste, the present application provides an anti-silver paste diffusion agent for lead frame packaging, and a preparation method and application thereof.
[0005] In a first aspect, the present application provides a silver glue diffusion preventing agent for lead frame packaging, which adopts the following technical solution: a silver glue diffusion preventing agent for lead frame packaging, which is made of water and a solute; the solute includes the following raw materials in the following mass concentrations: 80-120 mg / L of bis(3-trimethoxysilylpropyl)amine, 15-25 mg / L of N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, 15-25 mg / L of γ-aminopropyltriethoxysilane, 150-250 mg / L of polyol, 90-110 mg / L of hyperbranched polymer, 250-350 mg / L of polyether-modified silicone oil, 45-55 mg / L of dispersant, and 5-15 mg / L of anti-discoloration agent; The hyperbranched polymer is obtained by grafting methyl vinyl acetate, 1,6-hexanediamine and 2-(methacryloyloxy)ethyl 2-(trimethylamino)ethyl phosphate.
[0006] The present invention's anti-silver glue diffusion agent incorporates polyols and hyperbranched polymers into its raw materials, leveraging their synergistic effects. This results in a transparent and clear appearance after 45 days of storage, without delamination, turbidity, or precipitation, demonstrating high storage stability. Furthermore, when applied to lead frame anti-silver glue diffusion treatments, the film achieves a contact angle of 84-87 degrees and a silver glue diffusion rate of less than 2%, demonstrating the advantages of low silver glue diffusion rate and high film contact angle, enhancing the inhibitory effect and meeting higher demands.
[0007] Adding γ-aminopropyltriethoxysilane, N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, and bis(3-trimethoxysilylpropyl)amine to the raw materials of the silver glue diffusion prevention agent allows them to hydrolyze and further undergo a condensation reaction, which then adsorbs onto the lead frame surface to form a hydrophobic film. γ-aminopropyltriethoxysilane contains one Si and one amino group, N-(2-aminoethyl)-3-aminopropyltrimethoxysilane contains one Si, one amino group, and one imino group, and bis(3-trimethoxysilylpropyl)amine contains two Si groups and one imino group. These three groups form an interlaced hydrophobic film, increasing the tightness of the hydrophobic film and improving the contact angle of the film. This also enhances the interaction between the hydrophobic film and the conductive silver glue, improving the inhibitory effect of the silver glue diffusion prevention agent on the leakage of the conductive silver glue.
[0008] Optionally, the weight ratio of the bis(3-trimethoxysilylpropyl)amine, N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, and γ-aminopropyltriethoxysilane is 1:0.2:0.2.
[0009] By adopting the above technical scheme, the weight ratio of di(3-trimethoxysilylpropyl)amine, N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, and γ-aminopropyltriethoxysilane is optimized to reduce the diffusion rate of silver glue and improve the use effect of the anti-silver glue diffusion agent.
[0010] Optionally, the hyperbranched polymer is prepared by the following method: Under the protection of inert gas, anhydrous ethanol is heated to 40-60° C., and vinyl methyl acetate A and 1,6-hexanediamine A are added, and the mixture is stirred for 13-17 hours; then 1,6-hexanediamine B is added, and the mixture is stirred for 13-17 hours; then vinyl methyl acetate C is added, and the mixture is stirred for 13-17 hours; then 1,6-hexanediamine D is added, and the mixture is stirred for 13-17 hours; then 2-(methacryloyloxy)ethyl 2-(trimethylamino)ethyl phosphate is added, and the mixture is stirred for 13-17 hours; and then distilled under reduced pressure to obtain a hyperbranched polymer.
[0011] Optionally, the weight ratio of anhydrous ethanol, methyl vinyl acetate A, 1,6-hexanediamine A, 1,6-hexanediamine B, methyl vinyl acetate C, 1,6-hexanediamine D, and 2-(methacryloyloxy)ethyl 2-(trimethylamino)ethyl phosphate is (500-1500):(25-35):(8-9):(30-40):(55-65):(65-75):(330-380).
[0012] By adopting the above technical solution, first, vinyl acetate methyl ester A and 1,6-hexanediamine A undergo an addition reaction, then the product undergoes an amidation reaction with 1,6-hexanediamine B, then the product undergoes an addition reaction with vinyl acetate methyl ester C, then the product undergoes an amidation reaction with 1,6-hexanediamine D, and then the product undergoes an addition reaction with 2-(methacryloyloxy)ethyl 2-(trimethylamino)ethyl phosphate, which not only increases the number of branches to form a hyperbranched polymer, but also increases the length of the branches, and introduces phosphate groups and quaternary ammonium groups at the tails of the branches, effectively increasing the anionic groups, cationic groups, and non-ionic bond groups of the hyperbranched polymer, improving the use effect of the hyperbranched polymer, and increasing the storage stability of the anti-silver glue diffusion agent.
[0013] Optionally, the polyol is one or more of sorbitol, glycerol, trimethylolethane, xylitol, and maltitol.
[0014] By adopting the above technical solution, sorbitol, glycerol, trimethylolethane, xylitol, and maltitol all contain multiple hydroxyl groups, which can reduce the surface tension of the anti-silver glue diffusion agent and increase the storage stability of the anti-silver glue diffusion agent without affecting the inhibitory effect of the anti-silver glue diffusion agent on the leakage of conductive silver glue.
[0015] Optionally, the polyether-modified silicone oil is one or more of polyether-modified silicone oil MSD-920, polyether-modified silicone oil SM-603, and polyether-modified silicone oil TS-19.
[0016] By adopting the above technical solution, the polyether-modified silicone oil is optimized, which can have a good wetting effect on the lead frame, making it easier for γ-aminopropyltriethoxysilane, N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, and bis(3-trimethoxysilylpropyl)amine to form a hydrophobic film on the surface of the lead frame.
[0017] Optionally, the dispersant is one or more of tetrabutylammonium chloride, dodecyltrimethylammonium chloride, tetraheptylammonium bromide, and n-octyltrimethylammonium bromide; The anti-discoloration agent is one or more of 1-phenyl-5-mercaptotetrazole, 2-mercaptobenzimidazole, N,N'-carbonyldiimidazole, and 2-(tert-butyloxycarbonylamino)pyridine.
[0018] By adopting the above technical solution, the dispersant and the anti-discoloration agent are optimized, which facilitates the selection of the dispersant and the anti-discoloration agent.
[0019] In a second aspect, the present application provides a method for preparing the aforementioned anti-silver paste diffusion agent for lead frame packaging, which adopts the following technical solution: A method for preparing the aforementioned anti-silver glue diffusion agent for lead frame packaging comprises the following steps: adding di(3-trimethoxysilylpropyl)amine, N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, γ-aminopropyltriethoxysilane, polyol, hyperbranched polymer, polyether-modified silicone oil, dispersant, and anti-discoloration agent to water and mixing to obtain the anti-silver glue diffusion agent.
[0020] By adopting the above technical solution, the preparation of the anti-silver glue diffusion agent is facilitated.
[0021] In a third aspect, the present application provides an application of the aforementioned anti-silver paste diffusion agent for lead frame packaging, which adopts the following technical solution: An application of the above-mentioned anti-silver glue diffusion agent for lead frame packaging is to plate the lead frame with silver and then immerse it in the anti-silver glue diffusion agent to perform a silver glue diffusion prevention treatment.
[0022] Optionally, the operating temperature of the anti-silver glue diffusion agent is 20-30° C., and the immersion time of the lead frame is 30-50 seconds.
[0023] By adopting the above technical solution, the lead frame is directly immersed in the anti-silver glue diffusion agent, which facilitates the treatment of the lead frame to prevent the silver glue from diffusing.
[0024] In summary, the present application has at least the following beneficial effects: the anti-silver glue diffusion agent of the present application adds γ-aminopropyltriethoxysilane, N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, and bis(3-trimethoxysilylpropyl)amine to the raw materials, and utilizes the synergistic effect between them to form a tight hydrophobic film on the surface of the lead frame, and introduces amino groups, imino groups, etc. into the hydrophobic film to increase the interaction between the hydrophobic film and the conductive silver glue. The film contact angle is 84-87 degrees, and the silver glue diffusion rate is less than 2%, which significantly increases the contact points of the film layer and reduces the silver glue diffusion rate. At the same time, the anti-silver glue diffusion agent is stored for 45 days and its appearance is transparent and clear, showing the advantage of high storage stability and can meet higher requirements. DETAILED DESCRIPTION
[0025] To make this application easier to understand, the following examples will be used to further illustrate this application. These examples are for illustrative purposes only and are not intended to limit the scope of application of this application. Unless otherwise specified, the raw materials or components used in this application can be obtained through commercial channels or conventional methods.
[0026] Preparation Example Preparation Example 1 A hyperbranched polymer is prepared by the following method: Nitrogen was introduced into the reaction flask to replace the air in the reaction flask with nitrogen and form a nitrogen protection. Then 1000 mg of anhydrous ethanol was added to the reaction flask and heated to 50°C. Stirring was started, and at a speed of 200 r / min, 30 mg of vinyl methyl acetate A and 8.7 mg of 1,6-hexanediamine A were added and stirred for 15 hours. Then 34.8 mg of 1,6-hexanediamine B was added and stirred for 15 hours. Then 60 mg of vinyl methyl acetate C was added and stirred for 15 hours. Then 69.6 mg of 1,6-hexanediamine D was added and stirred for 15 hours. Then 354 mg of 2-(methacryloyloxy)ethyl 2-(trimethylamino)ethyl phosphate was added and stirred for 15 hours. After that, the solvent anhydrous ethanol and the methanol obtained by the reaction were removed by reduced pressure distillation to obtain a hyperbranched polymer.
[0027] Preparation Example 2 A hyperbranched polymer is prepared by the following method: Nitrogen was introduced into the reaction flask to replace the air in the reaction flask with nitrogen and form a nitrogen protection. Then 500 mg of anhydrous ethanol was added to the reaction flask and heated to 40°C. Stirring was started, and at a speed of 150 r / min, 25 mg of vinyl methyl acetate A and 8 mg of 1,6-hexanediamine A were added and stirred for 13 hours. Then 40 mg of 1,6-hexanediamine B was added and stirred for 17 hours. Then 65 mg of vinyl methyl acetate C was added and stirred for 17 hours. Then 65 mg of 1,6-hexanediamine D was added and stirred for 13 hours. Then 330 mg of 2-(methacryloyloxy)ethyl 2-(trimethylamino)ethyl phosphate was added and stirred for 13 hours. After that, the solvent anhydrous ethanol and the methanol obtained by the reaction were removed by reduced pressure distillation to obtain a hyperbranched polymer.
[0028] Preparation Example 3 A hyperbranched polymer is prepared by the following method: Nitrogen was introduced into the reaction flask to replace the air in the reaction flask with nitrogen and form a nitrogen protection. Then 1500 mg of anhydrous ethanol was added to the reaction flask and heated to 60°C. Stirring was started, and at a speed of 250 r / min, 35 mg of methyl vinyl acetate A and 9 mg of 1,6-hexanediamine A were added and stirred for 17 hours. Then 30 mg of 1,6-hexanediamine B was added and stirred for 13 hours. Then 55 mg of methyl vinyl acetate C was added and stirred for 13 hours. Then 75 mg of 1,6-hexanediamine D was added and stirred for 17 hours. Then 380 mg of 2-(methacryloyloxy)ethyl 2-(trimethylamino)ethyl phosphate was added and stirred for 17 hours. After that, the solvent anhydrous ethanol and the methanol obtained by the reaction were removed by reduced pressure distillation to obtain a hyperbranched polymer. Example
[0029] Table 1 Raw materials of anti-silver glue diffusion agent Example 1 A silver glue diffusion preventing agent for lead frame packaging, the raw material ratio of which is shown in Table 1.
[0030] Among them, the polyol is sorbitol; the polyether-modified silicone oil is polyether-modified silicone oil MSD-920, and is selected from Qingdao Meiside Silicone Co., Ltd.; the dispersant is tetrabutylammonium chloride; the anti-discoloration agent is 1-phenyl-5-mercaptotetrazole; and the hyperbranched polymer is prepared by Preparation Example 1.
[0031] A method for preparing an anti-silver glue diffusion agent for lead frame packaging comprises the following steps: adding bis(3-trimethoxysilylpropyl)amine, N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, γ-aminopropyltriethoxysilane, polyol, hyperbranched polymer, polyether-modified silicone oil, dispersant, and anti-discoloration agent into water, and stirring for 30 minutes to obtain the anti-silver glue diffusion agent.
[0032] Examples 2-5 A silver glue diffusion preventing agent for lead frame packaging is different from Example 1 in that the raw material ratio of the silver glue diffusion preventing agent is different, and the raw material ratio of the silver glue diffusion preventing agent is shown in Table 1.
[0033] Example 6 A silver paste diffusion preventing agent for lead frame packaging is disclosed, which differs from Example 1 in that the source of the hyperbranched polymer in the raw materials of the silver paste diffusion preventing agent is different, and the hyperbranched polymer is prepared using Preparation Example 2.
[0034] Example 7 A silver paste diffusion preventing agent for lead frame packaging is disclosed, which differs from Example 1 in that the source of the hyperbranched polymer in the raw materials of the silver paste diffusion preventing agent is different, and the hyperbranched polymer is prepared using Preparation Example 3.
[0035] Comparative Example Comparative Example 1 A silver glue diffusion prevention agent for lead frame packaging, which differs from Example 1 in that, in the raw materials of the silver glue diffusion prevention agent, equal amounts of γ-aminopropyltriethoxysilane are used to replace di(3-trimethoxysilylpropyl)amine and N-(2-aminoethyl)-3-aminopropyltrimethoxysilane.
[0036] Comparative Example 2 A silver glue diffusion preventing agent for lead frame packaging is disclosed. The difference between the silver glue diffusion preventing agent and embodiment 1 is that an equal amount of N-(2-aminoethyl)-3-aminopropyltrimethoxysilane is used to replace di(3-trimethoxysilylpropyl)amine in the raw materials of the silver glue diffusion preventing agent.
[0037] Comparative Example 3 A silver glue diffusion prevention agent for lead frame packaging, which differs from Example 1 in that an equal amount of di(3-trimethoxysilylpropyl)amine is used to replace N-(2-aminoethyl)-3-aminopropyltrimethoxysilane in the raw materials of the silver glue diffusion prevention agent.
[0038] Comparative Example 4 A silver paste diffusion preventing agent for lead frame packaging is disclosed, which differs from Example 1 in that an equal amount of polyol is used to replace a hyperbranched polymer in the raw materials of the silver paste diffusion preventing agent.
[0039] Comparative Example 5 A silver paste diffusion preventing agent for lead frame packaging is different from Example 1 in that an equal amount of hyperbranched polymer is used to replace polyol in the raw materials of the silver paste diffusion preventing agent.
[0040] Application Examples Application Example 1 An application of a silver glue diffusion preventing agent for lead frame packaging comprises the following steps: The lead frame was silver-plated to form a silver coating. The lead frame, along with the silver coating, was then immersed in 50g of anti-silver paste diffusion agent at 25°C for 40 seconds. The lead frame was removed and then rinsed three times with 50g of water each time, followed by drying to complete the anti-silver paste diffusion treatment.
[0041] The lead frame is a copper sheet with a size of 40 mm×50 mm×0.3 mm, and a thickness of the silver plating layer of 2 μm. The silver paste diffusion preventing agent is prepared according to Example 1.
[0042] Application Example 2-7 An application of an anti-silver glue diffusion agent for lead frame packaging is different from Application Example 1 in that the anti-silver glue diffusion agent has different sources. The anti-silver glue diffusion agents of Application Examples 2-7 are prepared respectively using Examples 2-7.
[0043] Comparative Application Examples Comparative Application Examples 1-5 An application of an anti-silver glue diffusion agent for lead frame packaging is different from Application Example 1 in that the anti-silver glue diffusion agent has a different source. The anti-silver glue diffusion agents of Comparative Application Examples 1-5 are prepared respectively using Comparative Examples 1-5.
[0044] Performance testing (1) The anti-silver paste diffusion agents obtained in Examples 1-7 and Comparative Examples 1-5 were respectively taken as samples, and the following performance tests were performed on the samples. The test results are shown in Table 2.
[0045] The storage stability is determined by the following method: the sample is placed at 25°C for 45 days to observe whether the sample is stratified and whether turbidity or precipitation occurs.
[0046] (2) The lead frames after silver paste diffusion prevention treatment of Application Examples 1-7 and Comparative Application Examples 1-5 were respectively taken as samples, and the following performance tests were performed on the samples. The test results are shown in Table 2.
[0047] The contact angle of the sample surface was measured according to GB / T24368-2009, "Contact Angle Measurement Method for Detecting Hydrophobic Contaminants on Glass Surfaces." The closer the contact angle is to 90 degrees, the more hydrophobic the sample surface is, and the more effective it is in suppressing the leakage of the conductive silver paste.
[0048] The silver paste diffusion rate is determined using the following method: a 1mm diameter dot of conductive silver paste is applied to the silver-plated surface of the specimen using a syringe. The paste is then cured at 180°C for 30 minutes. The cured paste is then measured using a microscope, and the silver paste diffusion rate is calculated. A lower silver paste diffusion rate indicates better anti-diffusion performance.
[0049] Table 2 Test results As can be seen in Table 2, the anti-silver paste diffusion agent obtained in this application exhibits excellent stability. After 45 days of storage, the anti-silver paste diffusion agent remains transparent and clear, without delamination, turbidity, or precipitation. Furthermore, when applied to the anti-silver paste diffusion treatment of lead frames, the film contact angle is 84.11-86.12 degrees and the silver paste diffusion coefficient is 1.21-1.83%. These advantages, such as low silver paste diffusion coefficient and high film contact angle, enhance the anti-silver paste diffusion agent's ability to inhibit conductive silver paste leakage, meeting higher demands.
[0050] Compare Example 1 with Comparative Examples 4-5. In Comparative Example 4, a polyol was added to the raw materials for the anti-silver glue diffusion agent; in Comparative Example 5, a hyperbranched polymer was added to the raw materials for the anti-silver glue diffusion agent; and in Example 1, a polyol and a hyperbranched polymer were added to the raw materials for the anti-silver glue diffusion agent. It can be seen that when both the polyol and the hyperbranched polymer were added to the raw materials for the anti-silver glue diffusion agent, the anti-silver glue diffusion agent remained transparent and clear after 45 days of storage, without any delamination, turbidity, or precipitation, demonstrating enhanced storage stability.
[0051] Application Example 1 is compared with Comparative Application Examples 1-3, with Comparative Application Example 1 being the basis. Compared with Comparative Application Example 1, Comparative Application Example 2 adds N-(2-aminoethyl)-3-aminopropyltrimethoxysilane to the raw materials of the silver paste diffusion prevention agent; Compared with Comparative Application Example 1, Comparative Application Example 3 adds bis(3-trimethoxysilylpropyl)amine to the raw materials of the silver paste diffusion prevention agent; Compared with Comparative Application Example 1, Application Example 1 adds N-(2-aminoethyl)-3-aminopropyltrimethoxysilane and bis(3-trimethoxysilylpropyl)amine to the raw materials of the silver paste diffusion prevention agent. From this, it can be seen that by adding N-(2-aminoethyl)-3-aminopropyltrimethoxysilane and bis(3-trimethoxysilylpropyl)amine to the raw materials of the anti-silver glue diffusion agent, and utilizing the synergistic effect between the two, the contact points of the film layer are further increased, the diffusion rate of the silver glue is reduced, and the inhibitory effect of the anti-silver glue diffusion agent on the seepage of the conductive silver glue is increased, so that the anti-silver glue diffusion agent exhibits better performance.
[0052] It should be noted that the embodiments described above are only used to explain the present application and do not constitute any limitation to the present application. The present application has been described with reference to typical embodiments, but it should be understood that the words used therein are descriptive and explanatory words, rather than restrictive words. The present application may be modified as specified within the scope of the claims of the present application, and the invention may be revised without departing from the scope and spirit of the present application. Although the present application described therein relates to specific methods, materials and embodiments, it does not mean that the present application is limited to the specific examples disclosed therein. On the contrary, the present application can be extended to all other methods and applications with the same function.
Claims
1. A silver paste diffusion prevention agent for lead frame packaging, characterized in that: The invention is made of water and solute; the solute comprises raw materials of the following mass concentrations: 80-120 mg / L of di(3-trimethoxysilylpropyl)amine, 15-25 mg / L of N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, 15-25 mg / L of γ-aminopropyltriethoxysilane, 150-250 mg / L of polyol, 90-110 mg / L of hyperbranched polymer, 250-350 mg / L of polyether-modified silicone oil, 45-55 mg / L of dispersant, and 5-15 mg / L of anti-discoloration agent; The hyperbranched polymer is obtained by grafting methyl vinyl acetate, 1,6-hexanediamine and 2-(methacryloyloxy)ethyl 2-(trimethylamino)ethyl phosphate.
2. The anti-silver paste diffusion agent for lead frame packaging according to claim 1, characterized in that: The weight ratio of the di(3-trimethoxysilylpropyl)amine, N-(2-aminoethyl)-3-aminopropyltrimethoxysilane and γ-aminopropyltriethoxysilane is 1:0.2:0.
2.
3. The anti-silver paste diffusion agent for lead frame packaging according to claim 1, characterized in that: The hyperbranched polymer is prepared by the following method: Under the protection of inert gas, the temperature of anhydrous ethanol is raised to 40-60° C., and vinyl acetate methyl ester A and 1,6-hexanediamine A are added, and the mixture is stirred for 13-17 hours; then 1,6-hexanediamine B is added, and the mixture is stirred for 13-17 hours; then vinyl acetate methyl ester C is added, and the mixture is stirred for 13-17 hours; then 1,6-hexanediamine D is added, and the mixture is stirred for 13-17 hours; then 2-(methacryloyloxy)ethyl 2-(trimethylamino)ethyl phosphate is added, and the mixture is stirred for 13-17 hours; then, the mixture is distilled under reduced pressure to obtain a hyperbranched polymer.
4. The anti-silver paste diffusion agent for lead frame packaging according to claim 3, characterized in that: The weight ratio of anhydrous ethanol, methyl vinyl acetate A, 1,6-hexanediamine A, 1,6-hexanediamine B, methyl vinyl acetate C, 1,6-hexanediamine D, and 2-(methacryloyloxy)ethyl 2-(trimethylamino)ethyl phosphate is (500-1500):(25-35):(8-9):(30-40):(55-65):(65-75):(330-380).
5. The anti-silver paste diffusion agent for lead frame packaging according to claim 1, characterized in that: The polyol is one or more of sorbitol, glycerol, trimethylolethane, xylitol and maltitol.
6. The anti-silver paste diffusion agent for lead frame packaging according to claim 1, characterized in that: The polyether-modified silicone oil is one or more of polyether-modified silicone oil MSD-920, polyether-modified silicone oil SM-603, and polyether-modified silicone oil TS-19.
7. The anti-silver paste diffusion agent for lead frame packaging according to claim 1, characterized in that: The dispersant is one or more of tetrabutylammonium chloride, dodecyltrimethylammonium chloride, tetraheptylammonium bromide, and n-octyltrimethylammonium bromide; The anti-discoloration agent is one or more of 1-phenyl-5-mercaptotetrazole, 2-mercaptobenzimidazole, N,N'-carbonyldiimidazole, and 2-(tert-butyloxycarbonylamino)pyridine.
8. A method for preparing the silver paste diffusion preventing agent for lead frame packaging according to any one of claims 1 to 7, characterized in that: The method comprises the following steps: adding di(3-trimethoxysilylpropyl)amine, N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, gamma-aminopropyltriethoxysilane, polyol, hyperbranched polymer, polyether modified silicone oil, dispersant and anti-discoloration agent into water, and mixing the mixture to obtain an anti-silver glue diffusion agent.
9. An application of the silver paste diffusion prevention agent for lead frame packaging as claimed in any one of claims 1 to 7, characterized in that: The lead frame is silver plated and then immersed in a silver glue diffusion prevention agent for silver glue diffusion prevention treatment.
10. The use of the anti-silver paste diffusion agent for lead frame packaging according to claim 9, characterized in that: The operating temperature of the anti-silver glue diffusion agent is 20-30°C, and the immersion time of the lead frame is 30-50s.
Citation Information
Cited By
Silver colloid diffusion preventing agent as well as preparation method and application thereof
CN120737726A