Crude oil flow modifier and preparation method thereof
By using a three-arm star polymer as the active component of the crude oil flow modifier, the existing technology problems of insufficient applicability to high-condensation crude oil and uneven distribution of polar groups are solved, achieving wider applicability. And better fluidity and condensation reducing effect, reducing production costs and equipment update frequency.
Patent Information
- Application Number
- CN202310351351.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-04
- Publication Date
- 2024-10-15
AI Technical Summary
Existing crude oil flow modifiers are not widely applicable to high-point crude oil, and the polar groups and side chain lengths are unevenly distributed, resulting in poor dispersion and adsorption of wax crystals in crude oil, which increases production difficulty and cost.
Three-arm star polymer is used as the active component, and CTA-3 is used as the central core to copolymerize with polymer monomers such as high-carbon alcohol acrylate-maleic anhydride or vinyl acetate-maleic anhydride-styrene to form a wider range of Applicable crude oil flow modifier, improves the wax crystal morphology from rod-shaped to spherical, enhances fluidity and reduces condensation and viscosity.
It achieves wider applicability and better fluidity and condensation and viscosity reduction effects, reduces production costs and equipment update frequency, and improves the flexibility and performance of crude oil flow modifiers.
Smart Images

Figure CN118772860A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of petroleum additives, and more specifically to a crude oil flow modifier, a preparation method of the crude oil flow modifier and a three-arm star polymer used for the crude oil flow modifier. Background Art
[0002] Crude oil flow modifiers are made of oil-soluble polymers or condensates and suitable solvents, and generally include polar groups and non-polar groups. These polar groups and non-polar groups change the structure of wax crystals through eutectic and adsorption, and prevent asphaltene from aggregating to form a spatial network structure, thereby reducing the viscosity and pour point of crude oil and changing the low-temperature fluidity of crude oil.
[0003] Currently, industrialized acrylic alcohol esters and EVA crude oil flow modifiers are not universally applicable to high-viscosity crude oils. They generally generate random linear copolymers. The functional groups in the polymers are fixed. Once polymerized, the molecular structure of the polymer cannot be changed later. They are only applicable to a certain type of crude oil. When the physical properties of the crude oil change, the product performance can only be improved by adjusting the polymerization monomers. This will cause problems such as increased production difficulty, rapid equipment updates, and increased costs.
[0004] In addition, the current polymer crude oil flow modifiers are generally straight-chain, and after acting on wax crystals, rod-shaped wax crystals are formed, which have poor fluidity and require increasing the dosage to achieve the desired pour point reduction effect, which undoubtedly increases the pipeline transportation cost.
[0005] In addition, the polar groups and side chain lengths of the current polymer crude oil flow modifiers are unevenly distributed, the number of polar groups is insufficient, and the carbon chain is not long enough. After being added to crude oil, they cannot evenly disperse and adsorb wax crystals, making it difficult to achieve the ideal effect of reducing freezing point and viscosity. Summary of the invention
[0006] The object of the present invention is to provide a crude oil flow modifier and a preparation method thereof to solve at least one of the above problems existing in the prior art.
[0007] In order to achieve the above technical objectives, the technical solution adopted by the present invention is as follows:
[0008] According to a first aspect of the present invention, a crude oil flow improver is provided, which comprises an active component and an organic solvent, wherein the active component is a three-arm star polymer, the central core of the three-arm star polymer is CTA-3, and the arms of the three-arm star polymer are polymer-based crude oil flow improvers.
[0009] According to one embodiment of the present invention, the arms of the three-arm star polymer are higher carbon alcohol acrylate-maleic anhydride binary copolymer or its alcoholysis product, or vinyl acetate-maleic anhydride-styrene terpolymer or its alcoholysis product, or higher carbon alcohol acrylate-maleic anhydride-styrene terpolymer or its alcoholysis product.
[0010] According to one embodiment of the present invention, the weight percentage of each component in the crude oil flow improver is: 20% to 40% of the active component, and 60% to 80% of the organic solvent.
[0011] According to one embodiment of the present invention, the organic solvent is a mixture of one or more of dioxane, toluene, xylene, heavy aromatics, C9 aromatics, and C10 aromatics.
[0012] According to the second aspect of the present invention, there is provided a method for preparing a crude oil flow improver, which comprises the following steps: adding an organic solvent, a polymer monomer, an initiator, and CTA-3 into a reaction container in sequence, exhausting the air in the reaction container with an inert gas, and stirring the reaction at 65-90° C. for 4-16 hours to obtain a crude oil flow improver, wherein the active component of the obtained crude oil flow improver is a three-arm star polymer, the central core of the three-arm star polymer is CTA-3, and the arms of the three-arm star polymer are polymer-based crude oil flow improvers formed by polymerization of corresponding polymer monomers.
[0013] According to one embodiment of the present invention, the polymerizable monomers are acrylic acid higher alcohol ester and maleic anhydride, or vinyl acetate, maleic anhydride and styrene, or acrylic acid higher alcohol ester, maleic anhydride and styrene.
[0014] According to one embodiment of the present invention, the initiator is azobisisobutyronitrile.
[0015] According to one embodiment of the present invention, the acrylic acid ester is prepared by esterification reaction of a higher alcohol having a carbon number of 16 to 26 and acrylic acid.
[0016] According to one embodiment of the present invention, the molar ratio of the polymerized monomer to the CTA-3 is: acrylic acid higher alcohol ester: maleic anhydride: CTA-3 = 0.15 ~ 0.25: 0.15 ~ 0.2: 0.01 ~ 0.016; vinyl acetate: maleic anhydride: styrene: CTA-3 = 0.15 ~ 0.25: 0.15 ~ 0.2: 0.15 ~ 0.5: 0.01 ~ 0.016; acrylic acid higher alcohol ester: maleic anhydride: styrene: CTA-3 = 0.15 ~ 0.25: 0.15 ~ 0.2: 0.15 ~ 0.5: 0.01 ~ 0.016.
[0017] According to one embodiment of the present invention, the added amount of the initiator is 0.8%-2% of the total mass of the polymerization monomers.
[0018] According to one embodiment of the present invention, the CTA-3 is prepared by the following method: the first step: adding 2-4 g of trimethylolpropane tris(3-mercaptopropionate), 3-5 g of CS2 and 8-13 g of carbon dichloride to a reaction container in sequence, stirring evenly at room temperature, and then adding a mixture of 1.8-2.4 g of triethylamine and 13-20 g of carbon dichloride dropwise to the above mixture through a separatory funnel. After the dropwise addition is completed, stirring and reacting at room temperature for 1-3 hours; the second step: adding a mixture of 3-4.2 g of benzyl bromide and 13-20 g of carbon dichloride dropwise to the product of the first step, and after the dropwise addition is completed, continuing the reaction for 1.5-3 hours; the third step: adding 1 mol / L hydrochloric acid to the product of the second step for acidification termination reaction, washing the product with water, separating the product with a separatory funnel, adding anhydrous magnesium sulfate to the lower yellow liquid, drying at room temperature, adding an appropriate amount of methanol to the dried solution, and rotary evaporation and drying to obtain CTA-3.
[0019] According to one embodiment of the present invention, the preparation method further includes the following steps: adding high-carbon alcohol and a catalyst to the obtained crude oil flow improver, stirring and reacting at 110-130°C for 4-8 hours to obtain another crude oil flow improver, wherein the active component of the obtained another crude oil flow improver is a three-arm star polymer, the central core of the three-arm star polymer is CTA-3, and the arms of the three-arm star polymer are alcoholysis products of polymers formed by polymerization of corresponding polymerization monomers.
[0020] According to one embodiment of the present invention, the higher carbon alcohol is a higher carbon alcohol with a carbon number of 14 to 28.
[0021] According to one embodiment of the present invention, the added amount of the higher alcohol is 50-80% of the effective components in the crude oil flow improver.
[0022] According to one embodiment of the present invention, the added amount of the catalyst is 1% to 2% of the total mass of the effective components and higher alcohols in the crude oil flow improver.
[0023] According to one embodiment of the present invention, the catalyst is methanesulfonic acid.
[0024] According to a third aspect of the present invention, a three-arm star polymer for crude oil flow improver is provided, wherein the central core of the three-arm star polymer is CTA-3, and the arms of the three-arm star polymer are polymer-based crude oil flow improvers.
[0025] According to one embodiment of the present invention, the arms of the three-arm star polymer are higher carbon alcohol acrylate-maleic anhydride binary copolymer or its alcoholysis product, or vinyl acetate-maleic anhydride-styrene terpolymer or its alcoholysis product, or higher carbon alcohol acrylate-maleic anhydride-styrene terpolymer or its alcoholysis product.
[0026] The crude oil flow modifier provided by the present invention has the following beneficial effects compared with the existing polymer-based crude oil flow modifier: the crude oil flow modifier provided by the present invention has a "three-arm" star structure, and compared with the traditional comb-shaped pour point depressant, the morphology of the dispersed wax crystals has changed from the previous rod shape to a spherical shape, and has better fluidity.
[0027] Compared with the existing preparation method of the polymer crude oil flow modifier, the preparation method of the crude oil flow modifier provided by the present invention has at least one of the advantages of low synthesis cost, simple process, small dosage, easy operation and the like. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] The accompanying drawings are used to provide a further understanding of the present invention and constitute a part of the specification. Together with the following specific embodiments, they are used to explain the present invention but do not constitute a limitation of the present invention. In the accompanying drawings:
[0029] Figure 1 The structural formula of CTA-3 is shown;
[0030] Figure 2 The schematic diagram of the structure of the three-arm star polymer of acrylic acid higher alcohol ester-maleic anhydride is shown;
[0031] Figure 3 A schematic structural diagram of a vinyl acetate-maleic anhydride-styrene three-arm star polymer is shown;
[0032] Figure 4 The schematic diagram of the structure of the three-arm star polymer of acrylic acid higher alcohol ester-maleic anhydride-styrene is shown;
[0033] Figure 5 The viscosity reduction effect of the crude oil flow modifier provided by the present invention on Niger crude oil is shown;
[0034] Figure 6 The results show that the crude oil flow modifier provided by the present invention has a viscosity reducing effect on Chad crude oil. DETAILED DESCRIPTION
[0035] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with specific embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0036] According to a first aspect of the present invention, a crude oil flow improver is provided, which comprises an active component and an organic solvent, wherein the active component is a three-arm star polymer, the central core of the three-arm star polymer is CTA-3, and the arms of the three-arm star polymer are polymer-based crude oil flow improvers.
[0037] The CTA-3 mentioned in the present invention is commonly known as 2-(((benzylthio)carbonylthio)thiopropionyl)oxy)methyl)-2-ethylpropane-1,3-diylbis(((benzylthio)carbonylthio)thio)propionate), and its structural formula is as follows: Figure 1 As shown, CTA-3 is a RAFT (Reversible Addition-Fragmentation Chain Transfer Polymerization) agent. The polymer-based crude oil flow modifier that can be used as the arm of the three-arm star polymer must meet the following conditions: first, it has a double bond and is a protic monomer or an acidic or basic monomer; second, it can be used as a crude oil flow modifier, that is, it can reduce the viscosity and pour point of crude oil. By combining CTA-3 with a conventional polymer-based crude oil flow modifier, the resulting crude oil flow modifier has a "three-arm" star structure. Compared with the traditional comb-shaped crude oil flow modifier, the morphology of the dispersed wax crystals has changed from the previous rod-shaped to a spherical shape, with better fluidity and better pour point and viscosity reduction effects.
[0038] The arms of the three-arm star polymer can be a binary copolymer of acrylic acid higher alcohol ester-maleic anhydride or its alcoholysis product, a terpolymer of vinyl acetate-maleic anhydride-styrene or its alcoholysis product, or a terpolymer of acrylic acid higher alcohol ester-maleic anhydride-styrene or its alcoholysis product. The arms of the three-arm star polymer are not limited to the examples given above, and can also be a polymer-based crude oil flow modifier commonly used in the art that can react with CTA-3.
[0039] According to one embodiment of the present invention, the weight percentage of each component in the crude oil flow modifier is: 20% to 40% of active component, and 60% to 80% of organic solvent.
[0040] According to one embodiment of the present invention, the organic solvent is a mixture of one or more of dioxane, toluene, xylene, heavy aromatics, C9 aromatics, and C10 aromatics.
[0041] In the crude oil flow modifier provided by the first aspect of the present invention, the active component is a new star-shaped structure with many branches, which is shorter than the molecular chain of the traditional pour point depressant. The traditional pour point depressant disperses paraffin into rod-shaped wax crystals through adsorption, eutectic and other effects, preventing it from forming large wax crystals to improve the fluidity of crude oil. However, the "three-arm" star-shaped polymer synthesized by the present invention has short side chains, and can increase the matching carbon number side chains through alcoholysis in the later stage according to the change of the physical properties of crude oil, so that the wax crystals can be formed into "small spherules" through adsorption and eutectic effects, which have better fluidity than traditional rod-shaped wax crystals. Therefore, the star-shaped crude oil flow modifier synthesized by the present invention has a wider range of applicability. In addition, the crude oil flow modifier provided by the present invention has more polar groups and a more matching carbon skeleton chain structure. After being added to crude oil, it can evenly disperse and adsorb wax crystals, and the pour point and viscosity reduction effect is better. In addition, the polymer side chains of the crude oil flow modifier provided by the present invention can be changed. Specifically, the polymer side chains can be changed by alcoholysis, thereby making the crude oil flow modifier provided by the present invention more widely applicable to high-viscosity crude oils. For example, in the later stage, the molecular structure can be changed by alcoholysis according to the changes in the physical properties of the crude oil to adapt to the changed crude oil.
[0042] According to the second aspect of the present invention, a method for preparing a crude oil flow improver is provided, which comprises the following steps: adding an organic solvent, a polymerization monomer, an initiator, and CTA-3 into a reaction container in sequence, exhausting the air in the reaction container with an inert gas, and stirring the reaction at 65-90°C for 4-16 hours to obtain a crude oil flow improver, wherein the active component of the obtained crude oil flow improver is a three-arm star polymer, the central core of the three-arm star polymer is CTA-3, and the arms of the three-arm star polymer are copolymers formed by polymerization of corresponding polymerization monomers.
[0043] Wherein, the polymerization monomer can be acrylic acid higher alcohol ester and maleic anhydride, or can be vinyl acetate, maleic anhydride and vinylbenzene, or can be acrylic acid higher alcohol ester, maleic anhydride and vinylbenzene.These polymerization monomers can be polymerized into polymer-based crude oil flow modifier, i.e. acrylic acid higher alcohol ester-maleic anhydride binary copolymer or vinyl acetate-maleic anhydride-styrene terpolymer or acrylic acid higher alcohol ester-maleic anhydride-styrene terpolymer.Certainly the present invention is not limited to these specific monomers, protic monomers or acid and basic monomers such as acrylic acid, sodium p-vinylbenzenesulfonate, hydroxyethyl methacrylate, aminoethyl methacrylate can be polymerized smoothly, and special functional group-containing olefin monomers can undergo polymerization reaction to produce the crude oil flow modifier described in this application.
[0044] According to one embodiment of the present invention, the organic solvent is a mixture of one or more of dioxane, toluene, xylene, heavy aromatics, C9 aromatics, and C10 aromatics.
[0045] According to one embodiment of the present invention, the amount of organic solvent added is 2-3 times the total mass of the polymerized monomers. According to some embodiments of the present invention, when the polymerized monomers are acrylic acid higher alcohol esters and maleic anhydride, the molar ratio of the polymerized monomers to CTA-3 is: acrylic acid higher alcohol esters: maleic anhydride: CTA-3 = 0.15-0.25: 0.15-0.2: 0.01-0.016. According to some embodiments of the present invention, when the polymerized monomers are vinyl acetate, maleic anhydride and styrene, the molar ratio of the polymerized monomers to CTA-3 is: vinyl acetate: maleic anhydride: styrene: CTA-3 = 0.15-0.25: 0.15-0.2: 0.15-0.5: 0.01-0.016. According to some embodiments of the present invention, when the polymerizable monomers are acrylic acid higher alcohol ester, maleic anhydride and styrene, the molar ratio of the polymerizable monomers to CTA-3 is: acrylic acid higher alcohol ester: maleic anhydride: styrene: CTA-3 = 0.15-0.25: 0.15-0.2: 0.15-0.5: 0.01-0.016.
[0046] According to one embodiment of the present invention, the initiator is azobisisobutyronitrile (AIBN).
[0047] According to one embodiment of the present invention, the amount of the initiator added is 0.8%-2% of the total mass of the polymerized monomers.
[0048] According to one embodiment of the present invention, the acrylic acid higher alcohol ester is prepared by esterification reaction of a higher alcohol having a carbon number of 16 to 26 and acrylic acid.
[0049] According to one embodiment of the present invention, after the organic solvent, polymerization monomer, initiator, and CTA-3 are sequentially added to the reaction container, nitrogen is used for replacement three times to remove the air in the reaction container. The reaction container may be a reactor.
[0050] According to one embodiment of the present invention, the CTA-3 is prepared by the following method: the first step: adding 2-4 g of trimethylolpropane tris(3-mercaptopropionate), 3-5 g of CS2 and 8-13 g of carbon dichloride to a reaction container in sequence, stirring evenly at room temperature, and then adding a mixture of 1.8-2.4 g of triethylamine and 13-20 g of carbon dichloride dropwise to the above mixture through a separatory funnel. After the dropwise addition is completed, stirring and reacting at room temperature for 1-3 hours; the second step: adding a mixture of 3-4.2 g of benzyl bromide and 13-20 g of carbon dichloride dropwise to the product of the first step, and after the dropwise addition is completed, continuing the reaction for 1.5-3 hours; the third step: adding 1 mol / L hydrochloric acid to the product of the second step for acidification termination reaction, washing the product with water, separating the product with a separatory funnel, adding anhydrous magnesium sulfate to the lower yellow liquid, drying at room temperature, adding an appropriate amount of methanol to the dried solution, and rotary evaporation and drying to obtain CTA-3. Among them, trimethylolpropane tris (3-mercaptopropionate) and CS2 (carbon disulfide) are reaction monomers, carbon dichloride is a solvent, triethylamine is a catalyst, benzyl bromide is a reaction monomer, and hydrochloric acid is a reaction terminator.
[0051] According to the third aspect of the present invention, a method for preparing a crude oil flow improver is provided, which comprises the following steps: adding an organic solvent, a polymer monomer, an initiator, and CTA-3 to a reaction vessel in sequence, exhausting the air in the reaction vessel with an inert gas, stirring and reacting at 65-90°C for 4-16 hours to obtain a first crude oil flow improver; adding a high carbon alcohol and a catalyst to the first crude oil flow improver, stirring and reacting at 110-130°C for 4-8 hours to obtain a second crude oil flow improver. The active components of the first crude oil flow improver and the second crude oil flow improver are both three-arm star polymers, the central core of the three-arm star polymer is CTA-3, and the arms of the three-arm star polymer are copolymers of corresponding polymer monomers or alcoholysis products thereof.
[0052] Wherein, the polymerization monomer can be acrylic acid higher alcohol ester and maleic anhydride, or can be vinyl acetate, maleic anhydride and styrene, or can be acrylic acid higher alcohol ester, maleic anhydride and styrene. The first crude oil flow modifier is acrylic acid higher alcohol ester-maleic anhydride binary copolymer, or vinyl acetate-maleic anhydride-styrene terpolymer, or acrylic acid higher alcohol ester-maleic anhydride-styrene terpolymer, and the second crude oil flow modifier is the alcoholysis product of acrylic acid higher alcohol ester-maleic anhydride binary copolymer, or the alcoholysis product of vinyl acetate-maleic anhydride-styrene terpolymer, or the alcoholysis product of acrylic acid higher alcohol ester-maleic anhydride-styrene terpolymer. Of course, the present invention is not limited to these specific monomers, and protic monomers or acid and basic monomers such as acrylic acid, sodium p-vinylbenzenesulfonate, hydroxyethyl methacrylate, and aminoethyl methacrylate can be smoothly polymerized, and special functional group-containing olefin monomers can undergo polymerization to produce the crude oil flow modifier described in this application.
[0053] The process and parameters for obtaining the first crude oil flow modifier in this part are the same as those in the second aspect above, and will not be repeated here.
[0054] According to one embodiment of the present invention, the acrylic acid higher alcohol ester is prepared by esterification reaction of a higher alcohol having a carbon number of 16 to 26 and acrylic acid.
[0055] According to one embodiment of the present invention, the higher carbon alcohol is a higher carbon alcohol having 14 to 28 carbon atoms.
[0056] According to one embodiment of the present invention, the amount of higher alcohol added is 50-80% of the effective components in the crude oil flow improver.
[0057] According to one embodiment of the present invention, the catalyst is methanesulfonic acid (MSA).
[0058] According to one embodiment of the present invention, the amount of catalyst added is 1% to 2% of the total mass of the effective components and higher alcohols in the first crude oil flow improver.
[0059] According to a fourth aspect of the present invention, a three-arm star polymer for a crude oil flow modifier is provided, wherein the central core of the three-arm star polymer is CTA-3, and the arms of the three-arm star polymer are polymer-based crude oil flow modifiers. For example, it can be a binary copolymer of acrylic acid higher alcohol ester-maleic anhydride or its alcoholysis product (its structural schematic diagram is shown in FIG. Figure 2 ), or vinyl acetate-maleic anhydride-styrene terpolymer or its alcoholysis product (its structural schematic diagram is as shown in Figure 3 ), or acrylic acid higher alcohol ester-maleic anhydride-styrene terpolymer or its alcoholysis product (its structural schematic diagram is as shown Figure 4 shown).
[0060] The following are specific examples according to the present invention. Unless otherwise specified, the raw materials, equipment, consumables, etc. used in the following examples can be obtained by conventional commercial means.
[0061] For the parts involving numerical ranges, those skilled in the art can select any value within the numerical range defined by the present invention according to actual needs, and are not limited to the numerical values listed in the specific embodiments.
[0062] The synthesis method of RAFT agent (CTA-3) is as follows:
[0063] First, add 2-4g of trimethylolpropane tris(3-mercaptopropionate), 3-5g of CS2 and 8-13g of carbon dichloride to a 250ml round-bottomed reaction flask in sequence. After stirring evenly at room temperature, add a mixture of 1.8-2.4g of triethylamine and 13-20g of carbon dichloride dropwise to the mixture through a separatory funnel. The reaction is rapid, and the color gradually changes from light yellow to orange-yellow as the reaction proceeds. After the addition is completed, continue to stir the reaction at room temperature for 1-3 hours. In the second step, add a mixture of 3-4.2g of benzyl bromide and 13-20g of carbon dichloride dropwise to the product of the first step. This step is a click reaction with an extremely fast reaction rate. After the addition is completed, continue the reaction for 1.5-3 hours to obtain the desired product. The third step is the post-processing stage of the product. Add 1mol / L of hydrochloric acid to the product of the second step, increase the stirring speed to acidify and terminate the reaction. Wash twice with water to remove inorganic salts, separate the liquid with a separatory funnel, add anhydrous magnesium sulfate to the lower yellow liquid and dry overnight at room temperature to remove moisture. Add an appropriate amount of methanol to the dried solution, rotary evaporate to remove most of the solvent, and then place in a vacuum oven at 50-70°C to dry overnight to remove trace amounts of unreacted raw materials and solvents.
[0064] The preparation method of the crude oil flow modifier of acrylic acid higher carbon alcohol ester-maleic anhydride star copolymer is as follows:
[0065] Example 1-1
[0066] 0.15 mol of acrylic acid higher alcohol ester, 0.15 mol of maleic anhydride, 0.01 mol of CTA-3, 140.4 g of dioxane and AIBN (0.8% of the total mass of monomers) were added into a reactor, nitrogen was bubbled for 15-20 min, and the reaction was carried out at 65° C. for 4 hours to obtain a crude oil flow modifier whose active component is acrylic acid higher alcohol ester-maleic anhydride star copolymer.
[0067] Example 1-2
[0068] 0.25 mol of acrylic acid higher alcohol ester, 0.2 mol of maleic anhydride, 0.016 mol of CTA-3, 224.2 g of dioxane and AIBN (2% of the total weight of the monomers) were added into a reactor, nitrogen was bubbled for 15-20 min, and the reaction was carried out at 90° C. for 16 hours to obtain a crude oil flow modifier whose active component is acrylic acid higher alcohol ester-maleic anhydride star copolymer.
[0069] Examples 1-3
[0070] 0.20 mol of acrylic acid higher alcohol ester, 0.17 mol of maleic anhydride, 0.013 mol of CTA-3, 181 g of dioxane and AIBN (1.4% of the total mass of monomers) were added into a reactor, nitrogen was bubbled for 15-20 min, and the reaction was carried out at 77.5° C. for 10 hours to obtain a crude oil flow modifier whose active component is acrylic acid higher alcohol ester-maleic anhydride star copolymer.
[0071] The preparation method of the crude oil flow modifier of acrylic acid higher carbon alcohol ester-maleic anhydride star alcoholysis product is as follows:
[0072] Examples 1-4
[0073] To the reaction system obtained in Example 1-1, 0.3 mol of high carbon alcohol (C14) (specifically 50% of the effective component) and a catalyst (1% of the total mass of the effective component and the high carbon alcohol) were added, and the mixture was reacted at 110°C for 4 hours to obtain a crude oil flow improver whose active component is a star-shaped alcoholysis product of high carbon alcohol acrylate-maleic anhydride.
[0074] Examples 1-5
[0075] To the reaction system obtained in Example 1-1, 0.35 mol of high-carbon alcohol (C14) (specifically 65% of the effective component) and a catalyst (2% of the total mass of the effective component and the high-carbon alcohol) were added, and the mixture was reacted at 130°C for 8 hours to obtain a crude oil flow improver whose active component is a star-shaped alcoholysis product of high-carbon alcohol acrylate-maleic anhydride.
[0076] Examples 1-6
[0077] To the reaction system obtained in Example 1-1, 0.4 mol of high-carbon alcohol (C14) (specifically 80% of the effective component) and a catalyst (1.5% of the total mass of the effective component and the high-carbon alcohol) were added, and the mixture was reacted at 120°C for 6 hours to obtain a crude oil flow improver whose active component is a star-shaped alcoholysis product of high-carbon alcohol acrylate-maleic anhydride.
[0078] The preparation method of vinyl acetate-maleic anhydride-styrene star copolymer crude oil flow modifier is as follows:
[0079] Example 2-1
[0080] 0.15 mol of vinyl acetate, 0.15 mol of maleic anhydride, 0.15 mol of styrene, 0.01 mol of CTA-3, 86 g of dioxane and AIBN (0.8% of the total mass of monomers) were added into a reactor, nitrogen was bubbled for 15-20 min, and the reaction was carried out at 65° C. for 4 hours to obtain a crude oil flow modifier whose active component is a vinyl acetate-maleic anhydride-styrene star copolymer.
[0081] Example 2-2
[0082] 0.25 mol of vinyl acetate, 0.2 mol of maleic anhydride, 0.5 mol of styrene, 0.016 mol of CTA-3, 186 g of dioxane and AIBN (2% of the total mass of monomers) were added into a reactor, nitrogen was bubbled for 15-20 min, and the reaction was carried out at 90° C. for 16 hours to obtain a crude oil flow modifier whose active component is a vinyl acetate-maleic anhydride-styrene star copolymer.
[0083] Example 2-3
[0084] 0.2 mol of vinyl acetate, 0.17 mol of maleic anhydride, 0.32 mol of styrene, 0.013 mol of CTA-3, 134 g of dioxane and AIBN (1.4% of the total mass of monomers) were added into a reactor, nitrogen was bubbled for 15-20 min, and the reaction was carried out at 77.5° C. for 10 hours to obtain a crude oil flow modifier whose active component is a vinyl acetate-maleic anhydride-styrene star copolymer.
[0085] The preparation method of vinyl acetate-maleic anhydride-styrene star alcoholysis crude oil flow modifier is as follows:
[0086] Embodiment 2-4
[0087] To the reaction system of Example 2-1, 0.3 mol of high-carbon alcohol (C28) (specifically 50% of the effective component) and a catalyst (1% of the total mass of the effective component and the high-carbon alcohol) were added, and the mixture was reacted at 110°C for 4 hours to obtain a crude oil flow improver whose active component is a star-shaped alcoholysis product of vinyl acetate-maleic anhydride-styrene.
[0088] Embodiment 2-5
[0089] To the reaction system of Example 2-1, 0.35 mol of high-carbon alcohol (C28) (specifically 65% of the effective component) and a catalyst (2% of the total mass of the effective component and the high-carbon alcohol) were added, and the mixture was reacted at 130°C for 8 hours to obtain a crude oil flow improver whose active component is a star-shaped alcoholysis product of vinyl acetate-maleic anhydride-styrene.
[0090] Embodiment 2-6
[0091] To the reaction system of Example 2-1, 0.4 mol (C28) of high carbon alcohol (specifically 80% of the effective component) and a catalyst (1.5% of the total mass of the effective component and the high carbon alcohol) were added, and the mixture was reacted at 120°C for 6 hours to obtain a crude oil flow improver whose active component is a star-shaped alcoholysis product of vinyl acetate-maleic anhydride-styrene.
[0092] The preparation method of the crude oil flow modifier of acrylic acid higher carbon alcohol ester-maleic anhydride-styrene star copolymer is as follows:
[0093] Example 3-1
[0094] 0.15 mol of acrylic acid higher alcohol ester, 0.15 mol of maleic anhydride, 0.15 mol of styrene, 0.01 mol of CTA-3, 171 g of dioxane and AIBN (0.8% of the total mass of monomers) were added into a reactor, nitrogen was bubbled for 15-20 min, and the reaction was carried out at 65° C. for 4 hours to obtain a crude oil flow modifier whose active component is acrylic acid higher alcohol ester-maleic anhydride-styrene star copolymer.
[0095] Example 3-2
[0096] 0.25 mol of acrylic acid higher alcohol ester, 0.2 mol of maleic anhydride, 0.5 mol of styrene, 0.016 mol of CTA-3, 328 g of dioxane and AIBN (2% of the total mass of monomers) were added into a reactor, nitrogen was bubbled for 15-20 min, and the reaction was carried out at 90° C. for 16 hours to obtain a crude oil flow modifier whose active component is acrylic acid higher alcohol ester-maleic anhydride-styrene star copolymer.
[0097] Example 3-3
[0098] 0.2 mol of acrylic acid higher alcohol ester, 0.17 mol of maleic anhydride, 0.32 mol of styrene, 0.013 mol of CTA-3, 248 g of dioxane and AIBN (1.4% of the total mass of monomers) were added into a reactor, nitrogen was bubbled for 15-20 min, and the reaction was carried out at 77.5° C. for 10 hours to obtain a crude oil flow modifier whose active component is acrylic acid higher alcohol ester-maleic anhydride-styrene star copolymer.
[0099] The preparation method of the crude oil flow modifier of acrylic acid higher alcohol ester-maleic anhydride-styrene star alcoholysis product is as follows:
[0100] Embodiment 3-4
[0101] To the reaction system of Example 3-1, 0.3 mol of high-carbon alcohol (C21) (specifically 50% of the effective component) and a catalyst (1% of the total mass of the effective component and the high-carbon alcohol) were added, and the mixture was reacted at 110°C for 4 hours to obtain a crude oil flow improver whose active component is a high-carbon alcohol acrylate-maleic anhydride-styrene star alcoholysis product.
[0102] Embodiment 3-5
[0103] To the reaction system of Example 3-1, 0.35 mol of high-carbon alcohol (C21) (specifically 65% of the effective component) and a catalyst (2% of the total mass of the effective component and the high-carbon alcohol) were added, and the mixture was reacted at 130°C for 8 hours to obtain a crude oil flow improver whose active component is a high-carbon alcohol acrylate-maleic anhydride-styrene star alcoholysis product.
[0104] Embodiment 3-6
[0105] To the reaction system of Example 3-1, 0.4 mol of high-carbon alcohol (C21) (specifically 80% of the effective component) and a catalyst (1.5% of the total mass of the effective component and the high-carbon alcohol) were added, and the mixture was reacted at 120°C for 6 hours to obtain a crude oil flow improver whose active component is a star-shaped alcoholysis product of high-carbon alcohol acrylate-maleic anhydride-styrene.
[0106] Test Case
[0107] The crude oil samples are crude oil from the Goumeri block in Niger and the Baobab block in Chad. The physical properties of the crude oil are shown in Table 1. The crude oil pour point was determined according to the standard SY / T 0541-2009. In order to allow the crude oil flow modifier sample to fully react with the wax crystals in the crude oil, the crude oil and the crude oil with additives were heated to 80°C and kept warm for 30 minutes before the pour point test was performed. The test results are shown in Tables 2 and 3. The crude oil viscosity was determined according to the rotational viscometer equilibrium method for crude oil viscosity determination in SY / T 0520-2008. The test results are shown in Figure 5 , Figure 6 .
[0108] Table 1 Composition and physical properties of Niger crude oil and Chad crude oil
[0109]
[0110] Table 2 Effect of crude oil flow modifier on pour point reduction of Niger crude oil
[0111]
[0112] Table 3 Effect of crude oil flow modifier on pour point reduction of Chad crude oil
[0113]
[0114] From the above Table 2, Table 3 and Figure 5 , Figure 6It can be seen that the three types of star copolymer crude oil flow modifiers provided by the present invention have good pour point and viscosity reducing effects on Niger crude oil, with a pour point reduction range of more than 11.5°C and a viscosity reduction rate of more than 51.5%. The three types of star alcoholysis products provided by the present invention have good pour point and viscosity reducing effects on Chad crude oil, with a pour point reduction range of more than 12.5°C and a viscosity reduction rate of more than 56.5%.
Claims
1. A crude oil flow modifier, characterized in that: The invention comprises an active component and an organic solvent. The active component is a three-arm star polymer. The central core of the three-arm star polymer is CTA-3. The arms of the three-arm star polymer are polymer-based crude oil flow modifiers.
2. The crude oil flow improver according to claim 1, characterized in that: The arms of the three-arm star polymer are higher carbon alcohol acrylate-maleic anhydride binary copolymer or its alcoholysis product, or vinyl acetate-maleic anhydride-styrene terpolymer or its alcoholysis product, or higher carbon alcohol acrylate-maleic anhydride-styrene terpolymer or its alcoholysis product.
3. The crude oil flow improver according to claim 1, characterized in that: The weight percentage of each component in the crude oil flow modifier is: 20% to 40% of the active component and 60% to 80% of the organic solvent.
4. The crude oil flow improver according to claim 1, characterized in that: The organic solvent is a mixture of one or more of dioxane, toluene, xylene, heavy aromatics, C9 aromatics, and C10 aromatics.
5. A method for preparing a crude oil flow modifier, characterized in that: The following steps are involved: Add organic solvent, polymerization monomer, initiator and CTA-3 to the reaction container in sequence, exhaust the air in the reaction container with inert gas, stir and react at 65-90° C. for 4-16 hours to obtain a crude oil flow modifier. The active component of the obtained crude oil flow improver is a three-arm star polymer, the central core of the three-arm star polymer is CTA-3, and the arms of the three-arm star polymer are polymer-based crude oil flow improvers formed by polymerization of corresponding polymerization monomers.
6. The method for preparing the crude oil flow modifier according to claim 5, characterized in that: The polymerizable monomers are acrylic acid higher alcohol ester and maleic anhydride, or vinyl acetate, maleic anhydride and styrene, or acrylic acid higher alcohol ester, maleic anhydride and styrene.
7. The method for preparing a crude oil flow modifier according to claim 6, characterized in that: The initiator is azobisisobutyronitrile.
8. The method for preparing a crude oil flow modifier according to claim 6, characterized in that: The acrylic acid high-carbon alcohol ester is prepared by esterification reaction of high-carbon alcohol with carbon number of 16 to 26 and acrylic acid.
9. The method for preparing a crude oil flow modifier according to claim 6, characterized in that: The molar ratio of the polymerizable monomer to the CTA-3 is: Acrylic acid high alcohol ester: maleic anhydride: CTA-3 = 0.15 ~ 0.25: 0.15 ~ 0.2: 0.01 ~ 0.016; Vinyl acetate: maleic anhydride: styrene: CTA-3 = 0.15-0.25: 0.15-0.2: 0.15-0.5: 0.01-0.016; Acrylic acid high carbon alcohol ester: maleic anhydride: styrene: CTA-3 = 0.15 ~ 0.25: 0.15 ~ 0.2: 0.15 ~ 0.5: 0.01 ~ 0.
016.
10. The method for preparing a crude oil flow modifier according to claim 7, characterized in that: The added amount of the initiator is 0.8%-2% of the total mass of the polymerization monomers.
11. The method for preparing a crude oil flow modifier according to claim 5, characterized in that: The CTA-3 is prepared by the following method: Step 1: Add 2-4 g of trimethylolpropane tris(3-mercaptopropionate), 3-5 g of CS2 and 8-13 g of carbon dichloride to a reaction vessel in sequence, stir evenly at room temperature, then add a mixture of 1.8-2.4 g of triethylamine and 13-20 g of carbon dichloride dropwise into the mixture through a separatory funnel. After the addition is complete, continue stirring and reacting at room temperature for 1-3 hours; Step 2: Add a mixture of 3-4.2 g of benzyl bromide and 13-20 g of carbon dichloride dropwise to the product of the first step. After the addition is complete, continue the reaction for 1.5-3 hours; Step 3: Add 1 mol / L hydrochloric acid to the product of the second step to acidify and terminate the reaction. After washing with water, the product is separated using a separatory funnel. Anhydrous magnesium sulfate is added to the lower yellow liquid, and the solution is dried at room temperature. An appropriate amount of methanol is added to the dried solution, and CTA-3 is obtained after rotary evaporation and drying.
12. The method for preparing a crude oil flow modifier according to claim 5, characterized in that: The following steps are also included: Add high carbon alcohol and catalyst to the obtained crude oil flow improver, stir and react at 110-130° C. for 4-8 hours to obtain another crude oil flow improver. The active component of another crude oil flow modifier obtained is a three-arm star polymer, the central core of the three-arm star polymer is CTA-3, and the arms of the three-arm star polymer are alcoholysis products of polymers obtained by polymerization of corresponding polymerization monomers.
13. The method for preparing a crude oil flow modifier according to claim 12, characterized in that: The higher carbon alcohol is a higher carbon alcohol with a carbon number of 14 to 28.
14. The method for preparing a crude oil flow modifier according to claim 12, characterized in that: The added amount of the higher carbon alcohol is 50-80% of the effective components in the crude oil flow improver.
15. The method for preparing a crude oil flow modifier according to claim 12, characterized in that: The added amount of the catalyst is 1% to 2% of the total mass of the effective components and high-carbon alcohols in the crude oil flow modifier.
16. The method for preparing a crude oil flow modifier according to claim 12, characterized in that: The catalyst is methanesulfonic acid.
17. A three-arm star polymer for crude oil flow modifier, characterized in that: The central core of the three-arm star polymer is CTA-3, and the arms of the three-arm star polymer are polymer-based crude oil flow modifiers.
18. The three-arm star polymer according to claim 17, characterized in that The arms of the three-arm star polymer are higher carbon alcohol acrylate-maleic anhydride binary copolymer or its alcoholysis product, or vinyl acetate-maleic anhydride-styrene terpolymer or its alcoholysis product, or higher carbon alcohol acrylate-maleic anhydride-styrene terpolymer or its alcoholysis product.