InP-based core-shell structure quantum dot and preparation method thereof
By growing the ZnSe inner shell and the ZnS outer shell in situ on InP@ZnSe-based quantum dots, the problem of reduced fluorescence quantum yield of InP-based quantum dot light-emitting diodes is solved, and large-size, high quantum yield and narrow half-peak width are achieved. , improving device performance.
Patent Information
- Application Number
- CN202411002889.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-25
- Publication Date
- 2024-10-15
AI Technical Summary
The fluorescence quantum yield of InP-based green quantum dot light-emitting diodes decreases sharply when the particle size reaches above 8 nm, resulting in poor device performance.
Using InP@ZnSe/ZnSe/ZnS-based core-shell structure quantum dots, InP@ZnSe-based quantum dots are prepared under oxygen-free conditions, and a ZnSe inner shell layer and a ZnS outer shell layer are grown in situ on the surface to adjust the structure of the quantum dots. to improve fluorescence quantum yield.
The large-sized (above 12 nm) high quantum yield and narrow half-peak width of InP-based core-shell structure quantum dots have been achieved, which improves the performance of quantum dot light-emitting diodes and meets the application needs in the field of lighting display.
Smart Images

Figure CN118772889A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a large-size InP-based core-shell structure quantum dot and a preparation method thereof, and belongs to the field of quantum dot luminescent materials. Background Art
[0002] Semiconductor quantum dot luminescent materials have many excellent optical properties such as high quantum yield, good photochemical stability, high monochromaticity and continuously adjustable emission spectrum. Therefore, quantum dot-based light-emitting diode devices (QLEDs) are expected to become the new generation of mainstream luminescent display technology. Currently, high-performance QLEDs are mostly based on II-VI group quantum dots. Due to the inherent toxicity of heavy metal quantum dots such as Cd, Pb, and Hg, their actual device applications are strictly restricted. As the best substitutes for heavy metal quantum dots, InP, ZnSe, and ZnTeSe-based quantum dots have photoelectric properties that are almost comparable to those of Cd / Pb-based quantum dots, and are considered to be a new generation of "green" environmentally friendly luminescent materials. At present, the external quantum efficiency of InP-based red and ZnTeSe-based blue environmentally friendly QLEDs has exceeded 20%, and the brightness exceeds or approaches 100,000 cd m -2 , T of red InP-based QLEDs 95 @1000 cd m -2 The lifetime (the time it takes for the brightness to drop to 95% of the initial brightness) exceeds 500 h, while the T 50 @100 cd m -2 The lifetime has exceeded 15,000 h, which is close to the basic requirement for industrial applications. In recent years, although green InP-based QLEDs have also achieved rapid development, compared with red InP-based QLEDs, green InP-based QLEDs have low efficiency (usually less than 16.3%) and low brightness (52,730 cd m -2 ) is insufficient, stability (T 95 @1000 cd m -2 These problems have become the key bottlenecks for green light InP-based QLEDs in display and lighting applications.
[0003] InP quantum dots have a small effective mass of electrons (0.077 m0, in contrast, CdSe has a value of 0.13 m0, where m0 is the free mass of electrons) and a high conduction band energy level, which results in insufficient electron confinement by InP quantum dots. This not only results in insufficient effective radiation recombination centers in quantum dots, but also reduces device efficiency because electrons are easily coupled to defects in the hole transport layer (HTL). ZnS can effectively confine electrons as a quantum dot shell due to its higher conduction band energy level, but it has a large lattice mismatch with InP (7.7%) and produces more defects. In order to reduce the lattice mismatch between the InP core and the ZnS outer shell, ZnSe, ZnSeS, and GaP are often used as intermediate shells. However, the sizes of the InP / ZnSeS / ZnS and InP / ZnSe / ZnS core-shell structure QDs reported so far are basically in the range of 7-8 nm, which is relatively small. After the quantum dots are formed into films, the energy resonance transfer is severe, resulting in a low quantum yield of the light-emitting layer film, which in turn leads to poor device performance. Summary of the invention
[0004] The present invention provides an InP-based core-shell structure quantum dot and a preparation method thereof, which aims to solve the problem in the prior art that the fluorescence quantum yield of the InP-based core-shell structure quantum dot decreases sharply when the particle size reaches 8 nm or more.
[0005] The technical solution of the present invention is: an InP-based core-shell structure quantum dot, whose structure includes a core body, an inner shell layer, and an outer shell layer; the inner shell layer is coated on the surface of the core body, the outer shell layer is coated on the outer surface of the inner shell layer, and the inner shell layer is located between the core body and the outer shell layer; the core body is an InP-based quantum dot.
[0006] Furthermore, the particle size of the InP-based quantum dots is 2.0 nm to 3.0 nm; the thickness of the inner shell layer is 2.0 nm to 4.5 nm, and the thickness of the outer shell layer is 0.5 nm to 1.0 nm; the inner shell layer is a ZnSe shell layer; and the outer shell layer is a ZnS shell layer.
[0007] Furthermore, the InP-based quantum dots are InP@ZnSe-based quantum dots; the InP@ZnSe-based quantum dots include an InP-based core and a ZnSe core membrane, and the ZnSe core membrane is coated on the surface of the InP-based core.
[0008] A method for preparing InP-based core-shell structure quantum dots, the method comprising: Step 1) preparing an InP@ZnSe-based quantum dot dispersion under oxygen-free conditions; Step 2) maintaining an oxygen-free condition, adding an etchant to the InP@ZnSe-based quantum dot dispersion to etch the surface of the InP@ZnSe-based quantum dots to form an InP-based quantum dot etching dispersion; Step 3) under oxygen-free conditions, adding the mixture of inner shell material sources to the InP@ZnSe-based quantum dot etching dispersion, in-situ growing the inner shell on the surface of the etched InP@ZnSe-based quantum dots, to obtain an intermediate dispersion; Step 4) Under anaerobic conditions, a mixture of shell layer material sources is added to the intermediate dispersion to in-situ grow a shell layer on the outer surface of the inner shell layer.
[0009] Furthermore, the etchant is one or a combination of hydrofluoric acid, zinc fluoride, indium fluoride, zinc trifluoroacetate, and zinc tetrafluoroborate.
[0010] Furthermore, the step 1) preparing an InP@ZnSe-based quantum dot dispersion under anaerobic conditions specifically comprises: 1-1) Under anaerobic conditions, indium acetate, zinc acetate, palmitic acid, (TMS)3P (tri(trimethylsilyl)phosphine) are added to octadecene to obtain an InP-based core dispersion; 1-2) Adding selenium-tri-n-octylphosphine solution to the InP-based core dispersion liquid obtains an InP@ZnSe-based quantum dot dispersion liquid containing InP@ZnSe-based quantum dots.
[0011] Furthermore, the molar ratio of the indium acetate, zinc acetate, palmitic acid, and (TMS)3P is (0.1-0.2):(0.05-0.1):(0.4-0.8):(0.05-0.1), the concentration of the indium acetate in octadecene is (0.01-0.02) mol / L, the concentration of selenium in the selenium-tri-n-octylphosphine solution is (0.5-2) mol / L, and the molar ratio of the indium acetate to the selenium in the selenium-tri-n-octylphosphine solution is 1:(0.3-1.6).
[0012] Furthermore, the step 2) maintains oxygen-free conditions, and adds an etchant to the InP@ZnSe-based quantum dot dispersion to etch the surface of the InP@ZnSe-based quantum dots to form an InP-based quantum dot etching dispersion, specifically comprising: 2-1) preparing a mixed solution of zinc oleate and liquid paraffin; the volume ratio of zinc oleate to liquid paraffin in the mixed solution of zinc oleate and liquid paraffin is 3:3 to 3:8; the zinc oleate is a zinc oleate solution prepared by mixing zinc acetate and oleic acid, the concentration of zinc oleate in the zinc oleate solution is calculated as zinc ion, and the concentration of zinc oleate in the zinc oleate solution is (0.4 to 1) mol / L; 2-2) Add zinc fluoride and a mixed solution of zinc oleate and liquid paraffin to the InP@ZnSe-based quantum dot dispersion to form an InP@ZnSe-based quantum dot etching dispersion; wherein the ratio of the amount of indium acetate added in the process of preparing the InP@ZnSe-based quantum dot dispersion to the amount of zinc fluoride and zinc oleate added here is (0.05-0.15):(0.2-1):(1.5-3).
[0013] Furthermore, the step 3) adds the mixture of inner shell material sources to the InP@ZnSe-based quantum dot etching dispersion under anaerobic conditions, and in situ grows the inner shell on the surface of the etched InP@ZnSe-based quantum dots to obtain an intermediate dispersion, specifically comprising: heating the InP@ZnSe-based quantum dot etching dispersion to 240°C to 350°C under nitrogen protection; directly adding the selenium-tri-n-octylphosphine solution to the InP@ZnSe-based quantum dot etching dispersion, wherein the concentration of selenium in the selenium-tri-n-octylphosphine solution is (0.5 to 2) mol / L, and the volume ratio of the selenium-tri-n-octylphosphine solution added here to the InP@ZnSe-based quantum dot etching dispersion is 1: (4.5 to 18), and the reaction is carried out for 0.5 h to 3.0 h.
[0014] Furthermore, the step 4) adds the mixture of the shell layer material source to the intermediate dispersion under anaerobic conditions, and in situ grows the shell layer on the outer surface of the inner shell layer, specifically comprising: adding a sulfur-tri-n-octylphosphine solution to the intermediate solution, wherein the sulfur concentration in the sulfur-tri-n-octylphosphine solution is (0.5-2) mol / L, and the volume ratio of the sulfur-tri-n-octylphosphine solution to the intermediate solution is (0.02-0.08):1, reacting for 10 min to 50 min, to obtain an InP-based core-shell structure quantum dot solution, i.e., an InP@ZnSe / ZnSe / ZnS quantum dot solution.
[0015] Beneficial effects of the present invention: The InP-based core-shell structure quantum dots prepared by the present invention have large size (can reach more than 12 nm), high quantum yield, and narrow half-peak width, and can be applied to quantum dot light-emitting diodes to meet the application in the field of lighting display. It is a thick-shell large-size InP-based core-shell structure quantum dot that can ensure both better carrier confinement in the device and carrier injection concentration; so that the InP-based core-shell structure quantum dots can still maintain a high fluorescence quantum yield when the particle size reaches more than 12 nm. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] Attached Figure 1 TEM test results of the InP-based core, InP@ZnSe-based quantum dots and InP@ZnSe / ZnSe / ZnS quantum dots prepared in Example 1.
[0017] Attached Figure 2 The fluorescence emission spectra of the InP-based core and InP@ZnSe-based quantum dots generated in the preparation process of Example 1 before and after being etched by zinc fluoride-generated hydrofluoric acid.
[0018] Attached Figure 3 These are the fluorescence emission spectra of the InP@ZnSe / ZnSe / ZnS quantum dots prepared in Example 1 and the InP@ZnSe / ZnSe / ZnS quantum dots prepared in Example 2.
[0019] Attached Figure 4 This is a TEM image of InP@ZnSe / ZnSe / ZnS quantum dots prepared in Example 2 without zinc fluoride-generated hydrofluoric acid etching.
[0020] Attached Figure 5 This is a TEM image of InP@ZnSe / ZnSe / ZnS quantum dots prepared in Example 3 without zinc fluoride-generated hydrofluoric acid etching.
[0021] Attached Figure 6 This is a comparison chart of the quantum yield stability test results of the InP@ZnSe / ZnSe / ZnS quantum dots prepared in Example 1 and the InP@ZnSe / ZnSe / ZnS quantum dots prepared in Example 2.
[0022] Attached Figure 7 This is a comparison chart of the quantum yield test results of InP@ZnSe / ZnSe / ZnS quantum dots prepared in Example 1, Example 2, and Example 3, respectively.
[0023] Attached Figure 8 This is a simulation diagram of the tunneling probability and ratio of electron injection and leakage in the quantum dot light-emitting diode constructed by preparing InP@ZnSe / ZnSe / ZnS quantum dots in Example 1.
[0024] Attached Fig. 9 This is a device performance diagram of the quantum dot light-emitting diode prepared in Example 1.
[0025] Attached Fig.10 This is a device life graph of the quantum dot light-emitting diode prepared in Example 1. DETAILED DESCRIPTION
[0026] An InP-based core-shell structure quantum dot, which comprises a core, an inner shell and an outer shell; the inner shell is coated on the surface of the core, the outer shell is coated on the outer surface of the inner shell, and the inner shell is located between the core and the outer shell; the core is an InP-based quantum dot.
[0027] The particle size of the InP-based quantum dots is 2.0 nm to 3.0 nm; the thickness of the inner shell layer is 2.0 nm to 4.5 nm, and the thickness of the outer shell layer is 0.5 nm to 1.0 nm.
[0028] The InP-based quantum dots include an InP-based core and a core membrane coated on the surface of the InP-based core; the InP-based quantum dots are preferably InP@ZnSe-based quantum dots; the InP@ZnSe-based quantum dots include an InP-based core and a ZnSe core membrane, and the ZnSe core membrane is coated on the surface of the InP-based core; the particle size of the InP-based core is preferably 1.0 nm to 2.5 nm, and the thickness of the ZnSe core membrane is preferably 0.25 nm to 1 nm; in the present invention, the ZnSe core membrane can enhance the fluorescent luminescence effect of the InP-based core, and can also inhibit the Oswald ripening of the InP crystal core at high temperature.
[0029] The inner shell layer is a ZnSe shell layer; the outer shell layer is a ZnS shell layer; the inner shell layer is m layers of ZnSe, wherein m is the number of monomolecular layers of the ZnSe inner shell layer, and m is preferably 4-15.
[0030] The InP-based core-shell structure quantum dots are InP@ZnSe / ZnSe / ZnS quantum dots.
[0031] A method for preparing InP-based core-shell structure quantum dots, the method comprising the following steps: Step 1) preparing an InP@ZnSe-based quantum dot dispersion under oxygen-free conditions; Step 2) maintaining oxygen-free conditions, adding an etchant to the InP@ZnSe-based quantum dot dispersion to etch the surface of the InP@ZnSe-based quantum dots to form an InP-based quantum dot etching dispersion; the etchant is preferably one or a combination of hydrofluoric acid (HF), zinc fluoride, indium fluoride, zinc trifluoroacetate, and zinc tetrafluoroborate; and further preferably, zinc fluoride and zinc oleate in situ generate hydrofluoric acid (HF) to in situ etch the surface of the InP@ZnSe-based quantum dots; Step 3) under oxygen-free conditions, adding the mixture of inner shell material sources to the InP@ZnSe-based quantum dot etching dispersion, in-situ growing the inner shell on the surface of the etched InP@ZnSe-based quantum dots, to obtain an intermediate dispersion; Step 4) Under anaerobic conditions, a mixture of shell layer material sources is added to the intermediate dispersion to in-situ grow a shell layer on the outer surface of the inner shell layer.
[0032] The step 1) preparing an InP@ZnSe-based quantum dot dispersion under anaerobic conditions specifically comprises: 1-1) Under anaerobic conditions, indium acetate, zinc acetate, palmitic acid, (TMS)3P (tri(trimethylsilyl)phosphine) are added to octadecene to obtain an InP-based core dispersion; 1-2) Adding selenium-tri-n-octylphosphine solution to the InP-based core dispersion to obtain an InP@ZnSe-based quantum dot dispersion containing InP@ZnSe-based quantum dots; the molar ratio of the indium acetate, zinc acetate, palmitic acid, and (TMS)3P is preferably (0.1-0.2):(0.05-0.1):(0.4-0.8):(0.05-0.1), the concentration of the indium acetate in octadecene is preferably (0.01-0.02) mol / L, the concentration of selenium in the selenium-tri-n-octylphosphine solution is preferably (0.5-2) mol / L, and the molar ratio of the indium acetate to the selenium in the selenium-tri-n-octylphosphine solution is preferably 1:(0.3-1.6).
[0033] The step 2) maintaining an oxygen-free condition, adding an etchant to the InP@ZnSe-based quantum dot dispersion to etch the surface of the InP@ZnSe-based quantum dots to form an InP-based quantum dot etching dispersion, specifically includes: 2-1) preparing a mixed solution of zinc oleate and liquid paraffin; the volume ratio of zinc oleate to liquid paraffin in the mixed solution of zinc oleate and liquid paraffin is preferably 3:3 to 3:8, and more preferably the volume ratio of zinc oleate to liquid paraffin is 3:5; the zinc oleate is preferably a zinc oleate solution prepared by mixing zinc acetate and oleic acid, the concentration of zinc oleate in the zinc oleate solution is calculated as zinc ions, and the concentration of zinc oleate in the zinc oleate solution, i.e., the zinc ion concentration, is preferably (0.4 to 1) mol / L; 2-2) Add zinc fluoride and a mixed solution of zinc oleate and liquid paraffin to the InP@ZnSe-based quantum dot dispersion to form an InP@ZnSe-based quantum dot etching dispersion; wherein the ratio of the amount of indium acetate added in the process of preparing the InP@ZnSe-based quantum dot dispersion to the amount of zinc fluoride and zinc oleate added here is preferably (0.05-0.15): (0.2-1): (1.5-3).
[0034] The step 3) adds the mixture of inner shell material sources to the InP@ZnSe-based quantum dot etching dispersion under anaerobic conditions, and in-situ grows the inner shell layer on the surface of the etched InP@ZnSe-based quantum dots to obtain an intermediate dispersion, specifically comprising: heating the InP@ZnSe-based quantum dot etching dispersion to 240°C to 350°C, preferably 340°C, under nitrogen protection; directly adding the selenium-tri-n-octylphosphine solution to the InP@ZnSe-based quantum dot etching dispersion, wherein the concentration of selenium in the selenium-tri-n-octylphosphine solution is (0.5-2) mol / L, and the volume ratio of the selenium-tri-n-octylphosphine solution added here to the InP@ZnSe-based quantum dot etching dispersion is 1: (4.5-18), reacting for 0.5 h to 3.0 h, preferably reacting for 2 h, to obtain an intermediate dispersion, i.e., InP@ZnSe / ZnSe quantum dot solution.
[0035] The step 4) adds the mixture of shell layer material sources to the intermediate dispersion under anaerobic conditions, and in-situ grows the shell layer on the outer surface of the inner shell layer, specifically comprising: adding sulfur-tri-n-octylphosphine solution to the intermediate solution, wherein the concentration of sulfur in the sulfur-tri-n-octylphosphine solution is (0.5-2) mol / L, and the volume ratio of sulfur-tri-n-octylphosphine solution to the intermediate solution is preferably (0.02-0.08):1, reacting for 10 min to 50 min to obtain an InP-based core-shell structure quantum dot solution, i.e., an InP@ZnSe / ZnSe / ZnS quantum dot solution; and in-situ grows the shell layer material on the outer surface of the inner shell layer to obtain thick-shell InP-based quantum dots that can ensure both good carrier confinement and carrier injection concentration.
[0036] The present invention provides a thick-shell large-size InP-based core-shell structure quantum dot which can ensure both good carrier confinement and carrier injection concentration. In the present invention, the inner shell layer is relatively thick, which can ensure both good carrier confinement and carrier injection concentration. In the traditional InP / ZnSeS / ZnS structure, although the alloy ZnSeS inner shell layer can effectively confine electrons, its conduction band energy level is relatively high, which significantly hinders the injection of electrons. In the traditional InP / ZnSe / ZnS structure, although the thinner ZnSe inner shell layer is conducive to the injection of electrons, due to the higher conduction band energy level of the InP quantum dot and the weaker electron confinement ability of the ZnSe inner shell layer, the electrons injected into the quantum dot are not injected into the quantum dot. The electrons may couple with the defects in the hole transport layer through the tunneling effect, causing serious electron leakage. Based on the InP@ZnSe-based quantum dots, the present invention promotes surface-specific growth and reduces lattice disorder by adding hydrofluoric acid. The hydrofluoric acid etching causes specific growth on the surface of the ZnSe core membrane. The specific growth changes the spherical growth law of the quantum dots. When the ZnSe inner shell layer is further grown on the surface of the InP@ZnSe-based quantum dots, the specific growth at different positions on the surface of the ZnSe core membrane forms anisotropic growth of the ZnSe inner shell layer, and finally forms a non-spherical, approximately cubic-shaped InP-based core-shell structure quantum dot with few defects. The present invention maintains a high PL On the basis of QY, the thickness of the ZnSe inner shell can be significantly increased to form cubic InP-based core-shell structure quantum dots with few defects. The thicker ZnSe inner shell effectively reduces electron leakage. At the same time, the thicker ZnSe inner shell in the present invention does not obviously hinder the injection of electrons. In addition, the ZnS outer shell of a certain thickness can well confine electrons and holes, confine excitons to emit light inside the quantum dots, increase the quantum yield, and the ZnS outer shell has much higher environmental tolerance than ZnSe and is more stable.
[0037] The InP-based core-shell structure quantum dots prepared by the present invention are suitable for quantum dot light-emitting diodes. When the InP-based core-shell structure quantum dots prepared by the present invention are used to prepare quantum dot light-emitting diodes, it is only necessary to use the conventional quantum dot light-emitting diode preparation method in the prior art. The difference is that when preparing quantum dot light-emitting diodes using the prior art, the conventionally used quantum dots are replaced with the InP-based core-shell structure quantum dots prepared by the present invention. Example 1
[0038] A method for preparing InP@ZnSe / ZnSe / ZnS quantum dots, the method comprising the following steps: Step 1) Under anaerobic conditions, indium acetate, zinc acetate, palmitic acid, and (TMS)3P (tri(trimethylsilyl)phosphine) are added to octadecene and mixed to obtain an InP-based core dispersion; the molar ratio of the indium acetate, zinc acetate, palmitic acid, and (TMS)3P is 0.15:0.075:0.575:0.1, and the concentration of the indium acetate in octadecene is 0.015 mol / L; then, a selenium-tri-n-octylphosphine solution is added to the InP-based core dispersion to obtain an InP@ZnSe-based quantum dot dispersion containing InP@ZnSe-based quantum dots; the concentration of selenium in the selenium-tri-n-octylphosphine solution is 1 mol / L, and the molar ratio of the added indium acetate to the selenium in the added selenium-tri-n-octylphosphine solution is 1:1.
[0039] Step 2) preparing a mixed solution of zinc oleate and liquid paraffin; the volume ratio of zinc oleate to liquid paraffin in the mixed solution of zinc oleate and liquid paraffin is 3:5, the zinc oleate is a zinc oleate solution generated by mixing zinc acetate and oleic acid, the concentration of zinc oleate in the zinc oleate solution is calculated as zinc ions, and the concentration of zinc oleate in the zinc oleate solution, i.e., the zinc ion concentration, is 0.8 mol / L; maintaining anaerobic conditions, adding zinc fluoride and a mixed solution of zinc oleate and liquid paraffin to the InP@ZnSe-based quantum dot dispersion to form an InP@ZnSe-based quantum dot etching dispersion; wherein the ratio of the amount of indium acetate added in step 1) to the amount of zinc fluoride and zinc oleate added in step 2) is 1:5:24.
[0040] Step 3) Under nitrogen protection, the InP@ZnSe-based quantum dot etching dispersion is heated to 340°C. At this temperature, the selenium-tri-n-octylphosphine solution is added to the InP@ZnSe-based quantum dot etching dispersion; wherein the concentration of selenium in the selenium-tri-n-octylphosphine solution is 1 mol / L, and the volume ratio of the selenium-tri-n-octylphosphine solution added here to the InP@ZnSe-based quantum dot etching dispersion is 1:4.5, and the reaction is carried out for 2 h to obtain an intermediate dispersion, namely, the InP@ZnSe / ZnSe quantum dot solution; 4) Under anaerobic conditions, adding sulfur-tri-n-octylphosphine solution to the intermediate solution, wherein the concentration of sulfur in the sulfur-tri-n-octylphosphine solution is 1 mol / L, and the volume ratio of the sulfur-tri-n-octylphosphine solution to the intermediate solution is preferably 0.06:1, and reacting for 30 min to obtain an InP-based core-shell structure quantum dot solution containing InP-based core-shell structure quantum dots, that is, an InP@ZnSe / ZnSe / ZnS quantum dot solution containing InP@ZnSe / ZnSe / ZnS quantum dots.
[0041] The InP-based core-shell structure quantum dots prepared in this embodiment are used to construct quantum dot light-emitting diodes: the conventional quantum dot light-emitting diode preparation method in the prior art is used to construct quantum dot light-emitting diodes. The difference is that when using the prior art to prepare quantum dot light-emitting diodes, the conventional quantum dots are replaced with the InP-based core-shell structure quantum dots prepared in this embodiment.
[0042] Attached Figure 1 TEM test results of the InP-based core, InP@ZnSe-based quantum dots and InP@ZnSe / ZnSe / ZnS quantum dots prepared in Example 1; Figure 1 It can be seen that the size of the prepared InP-based core is 1.5 nm to 2 nm, the particle size of the InP@ZnSe-based quantum dots is 2.5 nm to 3.0 nm, and the particle size of the InP@ZnSe / ZnSe / ZnS quantum dots reaches more than 12 nm, indicating that the target quantum dots obtained in this embodiment have a thicker shell layer, and the finally prepared InP@ZnSe / ZnSe / ZnS quantum dots are approximately cubic in shape.
[0043] Attached Figure 2 The fluorescence emission spectra of the InP-based core and InP@ZnSe-based quantum dots generated in the preparation process of Example 1 before and after hydrofluoric acid etching; Figure 2 It can be clearly seen that the InP-based core has no obvious fluorescence effect, but after the InP-based core is coated with a ZnSe core membrane, an obvious fluorescence effect appears. After the InP@ZnSe-based quantum dots are etched with hydrofluoric acid (HF) by adding zinc fluoride, the fluorescence effect is further enhanced and a blue shift occurs due to the influence on the ZnSe core membrane.
[0044] Attached Figure 8 The tunneling probability and ratio of electron injection and leakage after the quantum dot light-emitting diode is constructed using the InP@ZnSe / ZnSe / ZnS quantum dots prepared in Example 1 are simulated; Figure 8 It can be seen that with the increase of ZnSe shell thickness, the ratio of electron injection / electron leakage shows an upward trend, ensuring the overall improvement of device performance.
[0045] Attached Fig.10 The device life graph of the quantum dot light-emitting diode constructed using the InP@ZnSe / ZnSe / ZnS quantum dots prepared in Example 1 is shown in the attached figure. Fig.10 It can be seen that at the initial brightness of 6718 cd m -2 Under the same conditions, the T of the quantum dot light-emitting diode device constructed using the InP@ZnSe / ZnSe / ZnS quantum dots prepared in Example 1 95 The life span is 35.9 h. According to the formula L0 n. T95 =C (L0 is the initial brightness, T 95 is the time taken for the device brightness to drop to 95%, n is the acceleration factor, and C is a constant. -2 Under the same conditions, the T of the quantum dot light-emitting diode device constructed using the InP@ZnSe / ZnSe / ZnS quantum dots prepared in Example 1 95 The lifespan is 1240 hours. Example 2
[0046] A method for preparing InP@ZnSe / ZnSe / ZnS quantum dots, the method comprising the following steps: Step 1) Under anaerobic conditions, indium acetate, zinc acetate, palmitic acid, and (TMS)3P (tri(trimethylsilyl)phosphine) are added to octadecene and mixed to obtain an InP-based core dispersion; the molar ratio of the indium acetate, zinc acetate, palmitic acid, and (TMS)3P is 0.15:0.075:0.575:0.1, and the concentration of the indium acetate in octadecene is 0.015 mol / L; then, a selenium-tri-n-octylphosphine solution is added to the InP-based core dispersion to obtain an InP@ZnSe-based quantum dot dispersion containing InP@ZnSe-based quantum dots; the concentration of selenium in the selenium-tri-n-octylphosphine solution is 1 mol / L, and the molar ratio of the added indium acetate to the selenium in the added selenium-tri-n-octylphosphine solution is 1:1.
[0047] Step 2) preparing a mixed solution of zinc oleate and liquid paraffin; the volume ratio of zinc oleate to liquid paraffin in the mixed solution of zinc oleate and liquid paraffin is 3:5, the zinc oleate is a zinc oleate solution generated by mixing zinc acetate and oleic acid, the concentration of zinc oleate in the zinc oleate solution is calculated as zinc ions, and the concentration of zinc oleate in the zinc oleate solution, i.e., the zinc ion concentration, is 0.8 mol / L; maintaining anaerobic conditions, adding the mixed solution of zinc oleate and liquid paraffin to the InP@ZnSe-based quantum dot dispersion to form an intermediate dispersion, then heating to 340°C, at this temperature, adding selenium-tri-n-octylphosphine solution to the intermediate dispersion; wherein the concentration of selenium in the selenium-tri-n-octylphosphine solution is 1 mol / L, the volume ratio of the selenium-tri-n-octylphosphine solution added here to the InP@ZnSe intermediate dispersion is 1:4.5, reacting for 2 h to obtain an intermediate dispersion; Step 3) Under anaerobic conditions, a sulfur-tri-n-octylphosphine solution is added to the intermediate solution, wherein the concentration of sulfur in the sulfur-tri-n-octylphosphine solution is 1 mol / L, and the volume ratio of the sulfur-tri-n-octylphosphine solution to the intermediate solution is preferably 0.06:1. The reaction is carried out for 30 minutes to obtain an InP-based core-shell structure quantum dot solution containing InP@ZnSe / ZnSe / ZnS quantum dots without hydrofluoric acid etching.
[0048] The difference between Example 2 and Example 1 is that zinc fluoride is not added in the whole process, and the process of in-situ generation of hydrofluoric acid (HF) by zinc fluoride and zinc oleate to in-situ etch the surface of InP@ZnSe-based quantum dots is missing.
[0049] The construction of quantum dot light-emitting diodes using the InP-based core-shell structure quantum dots prepared in this embodiment is the same as that in Example 1: the conventional quantum dot light-emitting diode preparation method in the prior art is used to construct the quantum dot light-emitting diode. The difference is that when preparing quantum dot light-emitting diodes using the prior art, the conventional quantum dots are replaced with the InP-based core-shell structure quantum dots prepared in this embodiment.
[0050] Attached Figure 3 The fluorescence emission spectra of the InP@ZnSe / ZnSe / ZnS quantum dots prepared in Example 1 and the InP@ZnSe / ZnSe / ZnS quantum dots prepared in Example 2 are shown in FIG. Figure 3 It can be seen that the emission spectrum of the InP@ZnSe / ZnSe / ZnS quantum dots prepared in Example 1 is in the green light range, and the fluorescence effect is stronger and the half-peak width is narrower than that of the InP@ZnSe / ZnSe / ZnS quantum dots prepared without zinc fluoride-generated hydrofluoric acid etching.
[0051] Attached Figure 4 TEM image of InP@ZnSe / ZnSe / ZnS quantum dots prepared in Example 2 without zinc fluoride generation and hydrofluoric acid etching, as shown in the attached Figure 4 It can be seen that the particle size of the InP@ZnSe / ZnSe / ZnS quantum dots prepared in Example 2 also reaches 12 nm, but the InP@ZnSe / ZnSe / ZnS quantum dots finally prepared in Example 2 are spherical, and the overall shape is significantly different from the three-dimensional shape of the InP@ZnSe / ZnSe / ZnS quantum dots prepared in Example 1. Example 3
[0052] A method for preparing InP@ZnSe / ZnSe / ZnS quantum dots, the method comprising the following steps: Step 1) Under anaerobic conditions, indium acetate, zinc acetate, palmitic acid, and (TMS)3P (tri(trimethylsilyl)phosphine) are added to octadecene and mixed to obtain an InP-based core dispersion; the molar ratio of the indium acetate, zinc acetate, palmitic acid, and (TMS)3P is 0.15:0.075:0.575:0.1, and the concentration of the indium acetate in octadecene is 0.015 mol / L; then, a selenium-tri-n-octylphosphine solution is added to the InP-based core dispersion to obtain an InP@ZnSe-based quantum dot dispersion containing InP@ZnSe-based quantum dots; the concentration of selenium in the selenium-tri-n-octylphosphine solution is 1 mol / L, and the molar ratio of the added zinc acetate to the selenium in the added selenium-tri-n-octylphosphine solution is 1:1.
[0053] Step 2) preparing a mixed solution of zinc oleate and liquid paraffin; the volume ratio of zinc oleate to liquid paraffin in the mixed solution of zinc oleate and liquid paraffin is 3:5, the zinc oleate is a zinc oleate solution generated by mixing zinc acetate and oleic acid, the concentration of zinc oleate in the zinc oleate solution is calculated as zinc ions, and the concentration of zinc oleate in the zinc oleate solution, i.e., the zinc ion concentration, is 0.8 mol / L; maintaining anaerobic conditions, adding the mixed solution of zinc oleate and liquid paraffin to the InP@ZnSe-based quantum dot dispersion to form an intermediate dispersion, then heating to 340°C, at this temperature, adding selenium-tri-n-octylphosphine solution to the intermediate dispersion; wherein the concentration of selenium in the selenium-tri-n-octylphosphine solution is 1 mol / L, the volume ratio of the selenium-tri-n-octylphosphine solution added here to the InP@ZnSe intermediate dispersion is 1:20, reacting for 1 h to obtain an intermediate dispersion; Step 3) Under anaerobic conditions, a sulfur-tri-n-octylphosphine solution is added to the intermediate solution, wherein the concentration of sulfur in the sulfur-tri-n-octylphosphine solution is 1 mol / L, and the volume ratio of the sulfur-tri-n-octylphosphine solution to the intermediate solution is preferably 0.06:1. The reaction is carried out for 30 minutes to obtain an InP-based core-shell structure quantum dot solution containing InP@ZnSe / ZnSe / ZnS quantum dots without hydrofluoric acid etching.
[0054] The difference between Example 3 and Example 2 is that the thickness of the ZnSe intermediate shell layer and the particle size of the InP-based core-shell structure quantum dots finally prepared are reduced by reducing the amount of selenium-tri-n-octylphosphine solution added and the reaction time. Figure 5 The particle size of the InP@ZnSe / ZnSe / ZnS quantum dots prepared in Example 3 is 8 nm. In the entire process of Example 3, zinc fluoride is not added, and there is no process in which zinc fluoride and zinc oleate in situ generate hydrofluoric acid (HF) to in situ etch the surface of the InP@ZnSe-based quantum dots.
[0055] The construction of quantum dot light-emitting diodes using the InP-based core-shell structure quantum dots prepared in this embodiment is the same as that in Embodiment 1 and Embodiment 2: the conventional quantum dot light-emitting diode preparation method in the prior art is used to construct the quantum dot light-emitting diode. The difference is that when the quantum dot light-emitting diodes are prepared using the prior art, the conventional quantum dots are replaced with the InP-based core-shell structure quantum dots prepared in this embodiment.
[0056] Attached Figure 6 The quantum yield stability test results of the InP@ZnSe / ZnSe / ZnS quantum dots prepared in Example 1 and the InP@ZnSe / ZnSe / ZnS quantum dots prepared in Example 2 are compared; Figure 6 It can be seen that the InP@ZnSe / ZnSe / ZnS quantum dots prepared in Example 1 have better quantum yield stability.
[0057] Attached Figure 7 The quantum yield (PL QY) test results of InP@ZnSe / ZnSe / ZnS quantum dots prepared in Example 1, Example 2, and Example 3 are compared. Figure 7 It can be seen that, relative to the small-sized InP@ZnSe / ZnSe / ZnS quantum dots prepared in Example 3, the quantum yield of the unetched InP@ZnSe / ZnSe / ZnS quantum dots prepared in Example 2 is significantly reduced at a larger size (12 nm), while the quantum yield of the InP@ZnSe / ZnSe / ZnS quantum dots generated by in-situ etching of the surface of the InP@ZnSe-based quantum dots by in-situ generation of hydrofluoric acid (HF) by zinc fluoride and zinc oleate in Example 1 can still be maintained above 90% at a larger size (12 nm), and relative to the small-sized InP@ZnSe / ZnSe / ZnS quantum dots prepared in Example 3, the quantum yield of the InP@ZnSe / ZnSe / ZnS quantum dots prepared in Example 1 is increased.
[0058] Attached Fig. 9 The device performance diagrams of quantum dot light-emitting diodes constructed by using the InP@ZnSe / ZnSe / ZnS quantum dots prepared in Example 1, Example 2, and Example 3 are shown in the accompanying drawings. Figure 6 It can be seen that the maximum brightness of the quantum dot light-emitting diode obtained in Example 1 is 270,000 cd m -2 , current efficiency is 112.56 cd A -1 , the external quantum efficiency is 26.68%; the maximum brightness of the quantum dot light-emitting diode obtained in Example 2 is 86343 cd m -2 , the maximum current efficiency is 52.88 cdA -1, the maximum external quantum efficiency is 12.52%; the maximum brightness of the quantum dot light-emitting diode obtained in Example 3 is 181037 cdm -2 , the maximum current efficiency is 63.98 cd A -1 , the maximum external quantum efficiency is 15.12%; it can be seen that the device performance of the quantum dot light-emitting diode constructed by using the InP@ZnSe / ZnSe / ZnS quantum dots prepared in Example 1 is better; from the comparison of Example 2 and Example 3, it can be seen that the device performance of the quantum dot light-emitting diode constructed by the InP@ZnSe / ZnSe / ZnS quantum dots formed after in-situ etching of the surface of the InP@ZnSe-based quantum dots without hydrofluoric acid (HF) is as the InP@ZnSe / ZnSe / ZnS quantum dots The particle size increases, the brightness and efficiency of the device decrease significantly; for the same InP@ZnSe / ZnSe / ZnS quantum dots with a particle size of 12nm, the device performance of the quantum dot light-emitting diode formed by the InP@ZnSe / ZnSe / ZnS quantum dots formed after in-situ etching of the surface of the InP@ZnSe-based quantum dots in Example 1 is better.
Claims
1. An InP-based core-shell quantum dot, characterized in that It comprises a core body, an inner shell layer and an outer shell layer; the inner shell layer is coated on the surface of the core body, the outer shell layer is coated on the outer surface of the inner shell layer, and the inner shell layer is located between the core body and the outer shell layer; the core body is an InP-based quantum dot.
2. The InP-based core-shell quantum dot according to claim 1, characterized in that The particle size of the InP-based quantum dots is 2.0 nm to 3.0 nm; the thickness of the inner shell layer is 2.0 nm to 4.5 nm, and the thickness of the outer shell layer is 0.5 nm to 1.0 nm; the inner shell layer is a ZnSe shell layer; and the outer shell layer is a ZnS shell layer.
3. The InP-based core-shell quantum dot according to claim 1, characterized in that The InP-based quantum dots are InP@ZnSe-based quantum dots; the InP@ZnSe-based quantum dots include an InP-based core and a ZnSe core membrane, and the ZnSe core membrane is coated on the surface of the InP-based core.
4. A method for preparing InP-based core-shell structure quantum dots, characterized in that include: Step 1) preparing an InP@ZnSe-based quantum dot dispersion under oxygen-free conditions; Step 2) maintaining an oxygen-free condition, adding an etchant to the InP@ZnSe-based quantum dot dispersion to etch the surface of the InP@ZnSe-based quantum dots to form an InP-based quantum dot etching dispersion; Step 3) under oxygen-free conditions, adding the mixture of inner shell material sources to the InP@ZnSe-based quantum dot etching dispersion, in-situ growing the inner shell on the surface of the etched InP@ZnSe-based quantum dots, to obtain an intermediate dispersion; Step 4) Under anaerobic conditions, a mixture of shell layer material sources is added to the intermediate dispersion to in-situ grow a shell layer on the outer surface of the inner shell layer.
5. The method for preparing an InP-based core-shell structure quantum dot according to claim 4, characterized in that The etchant is one or a combination of hydrofluoric acid, zinc fluoride, indium fluoride, zinc trifluoroacetate, and zinc tetrafluoroborate.
6. The method for preparing an InP-based core-shell structure quantum dot according to claim 4, characterized in that The step 1) preparing an InP@ZnSe-based quantum dot dispersion under anaerobic conditions specifically comprises: 1-1) Under anaerobic conditions, indium acetate, zinc acetate, palmitic acid, and (TMS)3P are added to octadecene to obtain an InP-based core dispersion; 1-2) Adding selenium-tri-n-octylphosphine solution to the InP-based core dispersion liquid obtains an InP@ZnSe-based quantum dot dispersion liquid containing InP@ZnSe-based quantum dots.
7. The method for preparing InP-based core-shell quantum dots according to claim 6, characterized in that The molar ratio of the indium acetate, zinc acetate, palmitic acid, and (TMS)3P is (0.1-0.2):(0.05-0.1):(0.4-0.8):(0.05-0.1), the concentration of the indium acetate in octadecene is (0.01-0.02) mol / L, the concentration of selenium in the selenium-tri-n-octylphosphine solution is (0.5-2) mol / L, and the molar ratio of the indium acetate to the selenium in the selenium-tri-n-octylphosphine solution is 1:(0.3-1.6).
8. The method for preparing InP-based core-shell quantum dots according to claim 4, characterized in that The step 2) maintaining an oxygen-free condition, adding an etchant to the InP@ZnSe-based quantum dot dispersion to etch the surface of the InP@ZnSe-based quantum dots to form an InP-based quantum dot etching dispersion, specifically includes: 2-1) preparing a mixed solution of zinc oleate and liquid paraffin; the volume ratio of zinc oleate to liquid paraffin in the mixed solution of zinc oleate and liquid paraffin is 3:3 to 3:8; the zinc oleate is a zinc oleate solution prepared by mixing zinc acetate and oleic acid, the concentration of zinc oleate in the zinc oleate solution is calculated as zinc ion, and the concentration of zinc oleate in the zinc oleate solution is (0.4 to 1) mol / L; 2-2) Add zinc fluoride and a mixed solution of zinc oleate and liquid paraffin to the InP@ZnSe-based quantum dot dispersion to form an InP@ZnSe-based quantum dot etching dispersion; wherein the ratio of the amount of indium acetate added in the process of preparing the InP@ZnSe-based quantum dot dispersion to the amount of zinc fluoride and zinc oleate added here is (0.05-0.15):(0.2-1):(1.5-3).
9. The method for preparing InP-based core-shell quantum dots according to claim 4, characterized in that The step 3) adds the mixture of inner shell material sources to the InP@ZnSe-based quantum dot etching dispersion under anaerobic conditions, and in situ grows the inner shell layer on the surface of the etched InP@ZnSe-based quantum dots to obtain an intermediate dispersion, specifically comprising: heating the InP@ZnSe-based quantum dot etching dispersion to 240°C to 350°C under nitrogen protection; directly adding the selenium-tri-n-octylphosphine solution to the InP@ZnSe-based quantum dot etching dispersion, wherein the concentration of selenium in the selenium-tri-n-octylphosphine solution is (0.5 to 2) mol / L, and the volume ratio of the selenium-tri-n-octylphosphine solution added here to the InP@ZnSe-based quantum dot etching dispersion is 1: (4.5 to 18), and the reaction is carried out for 0.5 h to 3.0 h.
10. The method for preparing InP-based core-shell quantum dots according to claim 4, characterized in that The step 4) adds the mixture of shell layer material sources to the intermediate dispersion under anaerobic conditions to in-situ grow the shell layer on the outer surface of the inner shell layer, specifically comprising: adding a sulfur-tri-n-octylphosphine solution to the intermediate solution, wherein the sulfur concentration in the sulfur-tri-n-octylphosphine solution is (0.5-2) mol / L, and the volume ratio of the sulfur-tri-n-octylphosphine solution to the intermediate solution is (0.02-0.08):1, reacting for 10 min to 50 min to obtain an InP-based core-shell structure quantum dot solution, i.e., an InP@ZnSe / ZnSe / ZnS quantum dot solution.
Citation Information
Patent Citations
InP core-shell quantum dot with low oxidation defect and preparation method thereof
CN115124993A
Core-shell quantum dot as well as preparation method and application thereof
CN118006335A