Recycling process of waste residues generated in titanium tetrachloride production process

By designing a recycling process for titanium tetrachloride production waste residue, including steps such as centrifugal washing, magnetic separation and ion exchange extraction, the problem of unreasonable waste residue treatment is solved, the recycling of valuable elements is realized, and environmental pollution and resources are reduced. Waste, meeting metal needs in the military and aerospace fields.

CN118773454APending Publication Date: 2024-10-15LUOYANG SUNRUI WANJI TITANIUM CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410767456.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-14
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

The solid waste residue generated during the production of titanium tetrachloride cannot be properly treated, resulting in environmental pollution and resource waste. Existing treatment methods such as incineration and landfill are unscientific and cannot solve the problem in the long term.

Method used

A process was designed that includes centrifugal washing, metal element compound particle grinding and drying, magnetic separation, gravity vibration shaker separation, ion exchange extraction and other steps. Through these steps, valuable elements in the waste residue, such as iron and aluminum, are separated and recovered. , magnesium, titanium, vanadium, zirconium, niobium, tantalum and other metals to reduce environmental pollution and resource waste.

Benefits of technology

It realizes the extraction and utilization of all valuable elements in waste residue, reduces environmental pollution, avoids incineration and landfill, improves the recycling rate of resources, fills the demand for scarce metals, and brings economic benefits.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118773454A_ABST
    Figure CN118773454A_ABST
Patent Text Reader

Abstract

The technology for recycling the waste residues generated in the titanium tetrachloride production process comprises the following steps that S1, centrifugal flushing is conducted, specifically, the waste residues and water are mixed and stirred to form slurry, centrifugal separation is conducted, calcium chloride is separated out of supernate, centrifugal separation interruption substances are carbon powder substances, and the carbon powder substances are separated out; substances centrifugally separated from the bottom layer are particulate matters of metal element compounds and a small amount of carbon powder; s2, metal element compound particles are ground and dried; s3, magnetic separation: separating out a compound of an iron element; s4, residual metal obtained after magnetic separation passes through gravity vibration shaking table equipment according to different specific gravities, and aluminum, magnesium and titanium compound particles, vanadium and zirconium compound particles and niobium and tantalum compound particles are obtained through separation; and S5, the vanadium and zirconium compound particles are subjected to ion exchange to replace vanadium and zirconium elementary elements in the compound. A reasonable waste residue recycling process and a reasonable separation sequence are designed according to different components in the waste residues, so that all the components are obtained through separation, and all valuable elements in the waste residues are extracted and utilized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of waste residue recycling, and in particular to a process for recycling waste residue generated in the production process of titanium tetrachloride. Background Art

[0002] Titanium tetrachloride is an important raw material for the preparation of titanium sponge and titanium dioxide. Currently, titanium tetrachloride is mostly produced by boiling chlorination. In the process of boiling chlorination to produce titanium tetrachloride, a large amount of solid waste residue with complex composition, heavy metals, easy to cause land salinization, and cumbersome to handle will be generated. Although the waste residue generated in the production process of titanium tetrachloride is not a hazardous solid waste, it is polluting. Direct landfill without treatment will cause soil heavy metal pollution and land salinization.

[0003] Currently, there is no process to treat this type of solid waste, and it is only treated by incineration, mine landfill, cement addition, etc. These methods are by no means scientific and long-term methods. They can only temporarily solve the current problems, and the risks still exist. With the rapid rise of the country's military industry, aerospace, and shipbuilding industries, the production capacity of titanium tetrachloride to produce titanium sponge will increase year by year, which means that with the increase in production capacity, the solid waste residue generated in the production of titanium tetrachloride will also increase year by year. Unreasonable solid waste residue treatment methods will eventually lead to accumulated environmental problems. The stable development of the titanium tetrachloride production industry requires a safe, scientific, and sustainable solid waste residue treatment process. Summary of the invention

[0004] In view of this, the present invention aims to propose a process for recycling waste residues generated in the production process of titanium tetrachloride, so as to solve the problem that the waste residues generated in the production process of titanium tetrachloride cannot be reasonably treated and utilized, thereby polluting the environment and wasting resources.

[0005] To achieve the above object, the technical solution of the present invention is achieved as follows:

[0006] A process for recycling waste residue generated in the production process of titanium tetrachloride comprises the following steps:

[0007] S1. Centrifugal washing,

[0008] Solid waste residues generated in the production process of titanium tetrachloride are mixed with water to form slurry, and the slurry is poured into a centrifugal device for centrifugal separation, calcium chloride is separated from the obtained supernatant, the interrupted substances of the centrifugal separation are carbon powder substances in the waste residues, and the substances separated by centrifugation at the bottom are particles of metal element compounds and a small amount of carbon powder;

[0009] S2. Grinding and drying of metal element compound particles;

[0010] S3. Magnetic separation, wherein the metal compound particles after drying in step S2 are fed into a magnetic separator for magnetic separation to separate the iron compound;

[0011] S4. Gravity vibration shaker separation,

[0012] After the magnetic separation in step S3, the remaining metals are separated into three groups of compound particles according to their specific gravities through a gravity vibration shaker device, namely aluminum, magnesium, titanium compound particles, vanadium, zirconium compound particles, and niobium, tantalum compound particles;

[0013] S5. Ion exchange extraction,

[0014] The vanadium and zirconium compound particles separated in step S4 are used to replace the vanadium and zirconium single elements in the compound by ion exchange.

[0015] Furthermore, in step S1, the solid waste residue and water are mixed and stirred in a ratio of 1:1.

[0016] Furthermore, in step S1, the rotation speed during centrifugation is 2500-3000 r / min, and the centrifugation time is 5-8 min.

[0017] Furthermore, in step S2, the metal element compound particles are ground to a particle size of 4 to 8 mm.

[0018] Furthermore, in step S2, after the metal element compound particles are ground, the drying temperature is 150-240°C.

[0019] Furthermore, in step S3, the magnetic field strength during magnetic separation is 0.6 to 1 T.

[0020] Furthermore, the calcium chloride can be returned to the circulating water system or the cold concentrated brine system for use after being filtered and adsorbed.

[0021] Furthermore, the carbon powder in the waste residue is attached to the outer wall of the centrifugal device and can be used for making activated carbon or as a heat source for combustion after being washed and dried.

[0022] Compared with the prior art, the process for recycling waste residue generated in the titanium tetrachloride production process of the present invention has the following advantages:

[0023] (1) According to the different components in the waste residue, a reasonable waste residue recycling process and separation sequence are designed to separate and obtain each component. All valuable elements in the waste residue are extracted and utilized, and the waste residue does not need to be processed, filled or incinerated, reducing the adverse impact on the environment;

[0024] (2) The carbon powder and calcium chloride in the waste slag generated in the titanium tetrachloride production process of the present invention can be recycled without causing pollution; the iron compound in the waste slag can be extracted and recycled after separation; the aluminum, magnesium, titanium compound, niobium, tantalum compound, vanadium, and zirconium element in the waste slag can be extracted and recycled after separation. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] The accompanying drawings constituting a part of the present invention are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the accompanying drawings:

[0026] Figure 1 The present invention provides a process flow chart for recycling waste residue generated during the production of titanium tetrachloride. DETAILED DESCRIPTION

[0027] The present invention will be further described below in conjunction with specific embodiments. It should be noted that the data in the following experimental examples are obtained by the inventor through a large number of experiments. Due to space limitations, only a part of them is shown in the specification, and those of ordinary skill in the art can understand and implement the present invention under these data. These embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content of the present invention, those skilled in the art can make various changes or modifications to the present invention, and these changes or modifications also fall within the scope protected by the present application.

[0028] It should be noted that, in the absence of conflict, the embodiments of the present invention and the features in the embodiments may be combined with each other.

[0029] The present invention will be described in detail below with reference to the accompanying drawings and in conjunction with embodiments.

[0030] Solid waste residue is generated during the production of titanium tetrachloride, and the main components of the solid waste residue are shown in Table 1. In addition to carbon powder and calcium chloride, the solid waste residue also contains many types of metals. If it is not properly treated, it will not only cause certain pollution to the environment, but also fail to reasonably utilize the resources in the waste residue, resulting in a waste of resources. The present invention designs a reasonable waste residue recycling process and separation sequence for different components in the waste residue to separate and obtain each component.

[0031] Table 1 Main components of solid waste residue

[0032]

[0033]

[0034] like Figure 1 As shown, the present invention provides a process for recycling waste residues generated in the production process of titanium tetrachloride, comprising the following steps:

[0035] S1. Centrifugal washing,

[0036] Solid waste residues generated in the production process of titanium tetrachloride are mixed with water to form slurry, and the slurry is poured into a centrifugal device for centrifugal separation, calcium chloride is separated from the obtained supernatant, the interrupted substances of the centrifugal separation are carbon powder substances in the waste residues, and the substances separated by centrifugation at the bottom are particles of metal element compounds and a small amount of carbon powder;

[0037] Specifically, a solid waste collection box is used to collect solid waste generated during the production of titanium tetrachloride. The solid waste and water are mixed and stirred in a ratio of 1:1. After the solid waste is added with water, the calcium chloride in the solid waste is dissolved in the formed slurry. After centrifugal separation, the separated supernatant, that is, the calcium chloride is separated from the water. This part of the calcium chloride can be returned to the circulating water system or the cold concentrated brine system for use after filtration and adsorption. The carbon powder in the waste is attached to the outer wall of the centrifugal equipment. After rinsing and drying, it can be used for the production of activated carbon or as a heat source for combustion. The substance separated by centrifugation at the bottom is the precipitate obtained after centrifugation. Furthermore, the speed during centrifugation is 2500-3000r / min, and the centrifugation time is 5-8min.

[0038] In this step, the yields of calcium chloride and carbon powder both reach 75%.

[0039] S2. Grinding and drying of metal element compound particles;

[0040] Specifically, the material separated by centrifugation in step S1 is ground to a particle size of 4 to 8 mm, and the drying temperature is 150 to 240° C. The metal element compounds include silicate compounds, and under this drying temperature condition, not only can these silicate compounds not be turned into a molten state to affect subsequent processing, but also the drying effect and the reaction removal of the remaining carbon powder can be ensured.

[0041] S3. Magnetic separation, wherein the metal compound particles after drying in step S2 are fed into a magnetic separator for magnetic separation to separate the iron compound;

[0042] Specifically, the magnetic field intensity during magnetic separation is 0.6 to 1 T. The yield of the compound of the iron element is 70 to 75%.

[0043] S4. Gravity vibration shaker separation,

[0044] After the magnetic separation in step S3, the remaining metals are separated into three groups of compound particles according to their specific gravities through a gravity vibration shaker device, namely aluminum, magnesium, titanium compound particles, vanadium, zirconium compound particles, and niobium, tantalum compound particles;

[0045] Specifically, after enrichment through the above process, the proportion of titanium dioxide in the aluminum, magnesium and titanium compound particles is greater than 40%, and can be directly used in the production of titanium dioxide and welding rods; the content of niobium and tantalum compound particles reaches more than 25%, meeting the national standards for niobium and tantalum ores and can be sold for processing.

[0046] In this step, the yield of aluminum, magnesium and titanium compounds reaches 75%, and the yield of niobium and tantalum compounds reaches 75%.

[0047] S5. Ion exchange extraction,

[0048] The vanadium and zirconium compound particles separated in step S4 are used to replace the vanadium and zirconium single elements in the compound by ion exchange.

[0049] Specifically, the specific gravity of the vanadium and zirconium compound particles is relatively small and cannot be used directly. The vanadium and zirconium elemental elements in the compound are replaced by ion exchange to form vanadium and zirconium metal elements, which can be sold for processing. It is a prior art to obtain vanadium and zirconium metal elements by ion exchange extraction, which will not be described in detail here. The ion exchanger used can be recycled and reused by regeneration. The yield of vanadium and zirconium metal elements reaches 57%.

[0050] After the above steps of the recycling process described in the present invention, all valuable elements in the waste slag generated in the titanium tetrachloride production process are extracted and utilized, and the waste slag does not need to be processed, filled or incinerated. The recycling process of the present invention formulates a reasonable separation order to reduce the interference of each component in the waste slag and to separate and recycle to the greatest extent. The carbon powder and calcium chloride in the waste slag generated in the titanium tetrachloride production process can be recycled without causing pollution; the iron element compounds in the waste slag can be extracted and recycled after separation; the aluminum, magnesium, titanium element compounds, niobium, tantalum element compounds, and vanadium and zirconium element compounds in the waste slag can be extracted and recycled after separation. Precious metals such as vanadium, niobium, and tantalum are all scarce metal elements needed in military industry and aerospace. They are not only utilized, but also obtain certain economic benefits, making up for the expenditure of the above process.

[0051] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A process for recycling waste residue generated in the production process of titanium tetrachloride, characterized in that: The steps include: S1. Centrifugal washing, Solid waste residues generated in the production process of titanium tetrachloride are mixed with water to form slurry, and the slurry is poured into a centrifugal device for centrifugal separation, calcium chloride is separated from the obtained supernatant, the interrupted substances of the centrifugal separation are carbon powder substances in the waste residues, and the substances separated by centrifugation at the bottom are particles of metal element compounds and a small amount of carbon powder; S2. Grinding and drying of metal element compound particles; S3. Magnetic separation, wherein the metal compound particles after drying in step S2 are fed into a magnetic separator for magnetic separation to separate the iron compound; S4. Gravity vibration shaker separation, After the magnetic separation in step S3, the remaining metals are separated into three groups of compound particles according to their specific gravities through a gravity vibration shaker device, namely aluminum, magnesium, titanium compound particles, vanadium, zirconium compound particles, and niobium, tantalum compound particles; S5. Ion exchange extraction, The vanadium and zirconium compound particles separated in step S4 are used to replace the vanadium and zirconium single elements in the compound by ion exchange.

2. The process for recycling waste residue generated in the titanium tetrachloride production process according to claim 1, characterized in that: In the step S1, the solid waste residue and water are mixed and stirred in a ratio of 1:

1.

3. The process for recycling waste residue generated in the titanium tetrachloride production process according to claim 1, characterized in that: In the step S1, the rotation speed during centrifugation is 2500-3000 r / min, and the centrifugation time is 5-8 min.

4. The process for recycling waste residue generated in the titanium tetrachloride production process according to claim 1, characterized in that: In the step S2, the metal element compound particles are ground to a particle size of 4 to 8 mm.

5. The process for recycling waste residue generated in the titanium tetrachloride production process according to claim 1, characterized in that: In the step S2, after the metal element compound particles are ground, the drying temperature is 150-240°C.

6. The process for recycling waste residue generated in the titanium tetrachloride production process according to claim 1, characterized in that: In the step S3, the magnetic field strength during magnetic separation is 0.6-1T.

7. The process for recycling waste residue generated in the titanium tetrachloride production process according to claim 1, characterized in that: The calcium chloride can be returned to the circulating water system or the cold concentrated brine system for use after being filtered and adsorbed.

8. The process for recycling waste residue generated in the titanium tetrachloride production process according to claim 1, characterized in that: The carbon powder in the waste residue is attached to the outer wall of the centrifugal device and can be used for making activated carbon or as a heat source for combustion after being washed and dried.